Organic long afterglow material and preparation method thereof
By mixing organic fluorescent dyes with photocuring glue and performing photocuring process, the complex process problems in the existing technology are solved, and the simple preparation and stable performance of organic long afterglow materials are achieved. It is suitable for a variety of application scenarios, especially in Car clothing safety instructions and metal flaw detection showed excellent results.
Patent Information
- Application Number
- CN202411214173.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-31
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the preparation of organic long afterglow materials with visible light excitation has a complex process, which is not conducive to simple and economical preparation and application.
The organic fluorescent dye is mixed with a photocuring glue, removed the solvent and cured with ultraviolet light to prepare an organic long afterglow material with good afterglow properties.
The afterglow emission of traditional fluorescent dyes under white light excitation is achieved, and a flat and smooth material is obtained, with stable afterglow performance and is suitable for applications in various scenarios, especially in terms of vehicle clothing safety indication and metal flaw detection.
Smart Images

Figure CN119081680A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic long afterglow materials, and in particular to an organic long afterglow material and a preparation method thereof. Background Art
[0002] In recent years, the research and development of organic long-persistent luminescence materials (OLPLMs) has attracted widespread attention due to their low price, green and simple preparation process, adjustable luminescence properties (color, brightness or duration, etc.), and sensitive external environment response characteristics (pressure, temperature or humidity, etc.). They have shown unique performance advantages in the fields of biosensing and imaging, information encryption or anti-counterfeiting, three-dimensional display, etc.
[0003] A large number of studies on OLPLMs have shown that the rigid matrix of the material is conducive to stabilizing the triplet radiation decay, thereby obtaining a long afterglow luminescent material. By doping or copolymerizing the luminophore to form a rigid amorphous polymer matrix, molecular vibration can be effectively suppressed, thereby obtaining efficient continuous LPL emission, and is conducive to achieving flexible and large-area preparation, expanding the application range of OLPLMs.
[0004] Organic long afterglow materials based on visible light excitation are beneficial for daily applications, such as display, information encryption, and lighting equipment, but usually require modification of the chemical structure of organic molecules, often involving complex molecular design and chemical synthesis, which hinders researchers' further exploration. Many common commercial fluorescent dyes, such as acridine and its derivatives, have charge transfer characteristics, which are helpful for absorption in the visible light region, but their afterglow performance is poor, and they often show very weak luminescence in the solid state. The use of polymer curing, such as photocuring and thermal curing, has been proven to effectively induce long afterglow. For example, a Chinese patent application document with publication number CN116768489A discloses a method for preparing a pure organic fluorescent long afterglow film excited by visible light, including: using a polyhydroxy polymer matrix material and a solvent to configure a main solution; using fluorescent dye molecules and a solvent to configure a guest solution; using a mixed solution of the main solution and the guest solution to configure a target solution; dripping the target solution on a glass sheet to remove the solvent in the target solution to obtain a pure organic fluorescent long afterglow film excited by visible light; wherein hydrogen bonds are formed between the polyhydroxy polymer matrix material and the fluorescent dye molecules. The obtained film can be used in the field of color-adjustable lighting sources, industrial product manufacturing and anti-counterfeiting labels, but its process is complicated and is not conducive to its application in metal flaw detection and other aspects. Summary of the invention
[0005] The technical problem to be solved by the present invention is how to simply prepare an organic long afterglow material excited by visible light.
[0006] The present invention solves the above technical problems through the following technical means:
[0007] A method for preparing an organic long afterglow material comprises the following steps: uniformly mixing an organic fluorescent dye, a solvent and a photocurable adhesive, removing the solvent and curing the organic long afterglow material with ultraviolet light;
[0008] Wherein, the organic fluorescent dye is a mixture of one or more of quinacridone, acridinium yellow, acridinium yellow G, acridinium yellow hydrochloride, proflavine sulfate, acridinium orange, acridinone, ethidium bromide, and 9-aminoacridine; the light-curing adhesive is a mixture of one or more of UV glue D-606, UV curing adhesive 3491, UV curing adhesive YY1181, V3218, and UV curing adhesive 3492;
[0009] Alternatively, the organic fluorescent dye is a mixture of one or more of acridine yellow, proflavine sulfate, acridine orange, and 9-aminoacridine, and the photocurable adhesive is V3018.
[0010] Preferably, the UV curing adhesive 3491 is from Henkel Loctite (China) Co., Ltd. AA3491, UV curing adhesive 3491 of Guangdong Youyang New Materials Co., Ltd., or a mixture of two thereof; the UV curing adhesive 3492 is Henkel Loctite (China) Co., Ltd. AA3492, UV curing adhesive 3492 of Guangdong Youyang New Materials Co., Ltd., or a mixture of two of them.
[0011] Preferably, the UV glue D-606 comes from Foshan Jinggu Adhesive Co., Ltd., the UV curing adhesive YY1181 comes from Guangdong Youyang New Materials Co., Ltd., and the V3218 comes from Dongguan Lelai Adhesive Products Co., Ltd.
[0012] Preferably, the usage ratio of the organic fluorescent dye to the solvent is 1-5 mg: 1-10 ml.
[0013] Preferably, the mass ratio of the photocurable adhesive to the organic fluorescent dye is 300-40000:1.
[0014] Preferably, the solvent is ethanol.
[0015] Preferably, the wavelength of the ultraviolet light is 365 nm, and the irradiation curing time is 20 to 40 seconds.
[0016] Preferably, before removing the solvent, the method further comprises coating a solution obtained by uniformly mixing the organic fluorescent dye, the solvent and the photocurable adhesive on the substrate.
[0017] Preferably, the coating is carried out by dripping or brushing.
[0018] The present invention also provides an organic long afterglow material, which is prepared by adopting the preparation method of the organic long afterglow material.
[0019] Preferably, the organic long afterglow material is a coating or a film.
[0020] The present invention also provides a method for inducing long afterglow emission of organic fluorescent dyes, comprising the following steps: uniformly mixing the organic fluorescent dyes, solvents and photocurable adhesive, removing the solvents and curing with ultraviolet light to induce long afterglow emission of the organic fluorescent dyes.
[0021] The advantages of the present invention are:
[0022] (1) By mixing traditional fluorescent dyes with photocurable adhesives and performing a photocuring process, afterglow emission of traditional fluorescent dyes acridine and its derivatives under white light excitation can be induced;
[0023] (2) The preparation method of the present invention can obtain a flat and smooth material with good afterglow performance and stable afterglow performance. The material does not require any heating process and the conditions are mild and not harsh, which will be very beneficial to the application of LPL materials in various scenarios.
[0024] (3) The present invention discloses an application of long afterglow emission stimulated by white light in the safety indication of vehicle clothing. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The macroscopic LPL images of the coating obtained in Example 1 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 6s after turning off the white light);
[0026] Figure 2 The macroscopic LPL images of the coating obtained in Example 2 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 6s after turning off the white light);
[0027] Figure 3 The macroscopic LPL images of the coating obtained in Example 3 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 6s after turning off the white light);
[0028] Figure 4 The macroscopic LPL images of the coating obtained in Example 4 of the present invention at room temperature (from left to right: when excited by white light, 1s after turning off the white light, and 3s after turning off the white light);
[0029] Figure 5 The macroscopic LPL images of the coating obtained in Example 5 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0030] Figure 6 This is a macroscopic LPL image of the coating obtained in Example 41 of the present invention at room temperature (from left to right: when excited by white light and 1 second after turning off the white light lamp);
[0031] Figure 7 The macroscopic LPL images of the coating obtained in Example 6 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0032] Figure 8 The macroscopic LPL images of the coating obtained in Example 7 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0033] Fig. 9 The macroscopic LPL images of the coating obtained in Example 8 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0034] Fig.10 The macroscopic LPL images of the coating obtained in Example 9 of the present invention at room temperature (from left to right: when excited by white light, 1s after turning off the white light, and 3s after turning off the white light);
[0035] Fig.11 The macroscopic LPL images of the coating obtained in Example 10 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0036] Fig.12 The macroscopic LPL images of the coating obtained in Example 11 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 6s after turning off the white light);
[0037] Fig.13 The macroscopic LPL images of the coating obtained in Example 12 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 6s after turning off the white light);
[0038] Fig.14 The macroscopic LPL images of the coating obtained in Example 13 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 6s after turning off the white light);
[0039] Fig.15This is a macroscopic LPL image of the coating obtained in Example 14 of the present invention at room temperature (from left to right: when excited by white light, 1s after turning off the white light lamp, and 3s after turning off the white light lamp);
[0040] Fig.16 This is a macroscopic LPL image of the coating obtained in Example 15 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0041] Fig.17 This is a macroscopic LPL image of the coating obtained in Example 16 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0042] Fig.18 This is a macroscopic LPL image of the coating obtained in Example 17 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0043] Fig.19 This is a macroscopic LPL image of the coating obtained in Example 18 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0044] Fig. 20 This is a macroscopic LPL image of the coating obtained in Example 19 of the present invention at room temperature (from left to right: when excited by white light, 1s after turning off the white light lamp, and 3s after turning off the white light lamp);
[0045] Fig.21 This is a macroscopic LPL image of the coating obtained in Example 20 of the present invention at room temperature (from left to right: when excited by white light, 1s after turning off the white light lamp, and 4s after turning off the white light lamp);
[0046] Fig. 22 This is a macroscopic LPL image of the coating obtained in Example 42 of the present invention at room temperature (from left to right: when excited by white light and 1 second after turning off the white light lamp);
[0047] Fig.23 This is a macroscopic LPL image of the coating obtained in Example 21 of the present invention at room temperature (from left to right: when excited by white light, 1s and 2s after turning off the white light);
[0048] Fig.24 This is a macroscopic LPL image of the coating obtained in Example 22 of the present invention at room temperature (from left to right: when excited by white light, 1s and 2s after turning off the white light);
[0049] Fig.25 This is a macroscopic LPL image of the coating obtained in Example 23 of the present invention at room temperature (from left to right: when excited by white light, 1s and 2s after turning off the white light);
[0050] Fig.26 This is a macroscopic LPL image of the coating obtained in Example 24 of the present invention at room temperature (from left to right: when excited by white light, 1s and 2s after turning off the white light lamp);
[0051] Fig. 27 This is a macroscopic LPL image of the coating obtained in Example 25 of the present invention at room temperature (from left to right: when excited by white light, 1s and 2s after turning off the white light lamp);
[0052] Fig.28 This is a macroscopic LPL image of the coating obtained in Example 43 of the present invention at room temperature (from left to right: when excited by white light and 1 second after turning off the white light);
[0053] Fig.29 This is the attenuation spectrum of the afterglow performance of the coating obtained in Example 26 of the present invention;
[0054] Fig.30 This is a macroscopic LPL image of the coating obtained in Example 27 of the present invention at room temperature (from left to right: when excited by white light and 1 second after turning off the white light);
[0055] Fig.31 This is the attenuation spectrum of the afterglow performance of the coating obtained in Example 31 of the present invention;
[0056] Fig.32 This is the attenuation spectrum of the afterglow performance of the coating obtained in Example 32 of the present invention;
[0057] Fig.33 This is a macroscopic LPL image of the coating obtained in Example 36 of the present invention at room temperature (from left to right: when excited by white light, 1s after turning off the white light lamp, and 3s after turning off the white light lamp);
[0058] Fig.34 This is a macroscopic LPL image of the coating obtained in Example 37 of the present invention at room temperature (from left to right: when excited by white light, 1s after turning off the white light lamp, and 3s after turning off the white light lamp);
[0059] Fig.35 This is the attenuation spectrum of the afterglow performance of the coating obtained in Example 38 of the present invention;
[0060] Fig.36 This is a macroscopic LPL image of the coating obtained in Example 39 of the present invention at room temperature (from left to right: when excited by white light and 1 second after turning off the white light);
[0061] Fig.37 This is a macroscopic LPL picture of the organic long afterglow coating obtained in Example 2 of the present invention applied on a car cover for safety indication application (from left to right: under ambient light, when excited by white light, and 1s, 3s, and 5s after turning off the white light);
[0062] Fig.38 The macroscopic LPL images of the film obtained in Example 46 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 6s after turning off the white light);
[0063] Fig.39 This is the attenuation spectrum of the afterglow performance of the thin film obtained in Example 46 of the present invention;
[0064] Fig.40 The macroscopic LPL images of the film obtained in Example 47 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0065] Fig.41 The macroscopic LPL images of the film obtained in Example 48 of the present invention at room temperature (from left to right: when excited by white light, 1s, 3s, and 5s after turning off the white light);
[0066] Fig.42 The macroscopic LPL images of the film obtained in Example 49 of the present invention at room temperature (from left to right: when excited by white light, 1s, 2s, and 3s after turning off the white light);
[0067] Fig.43 This is the attenuation spectrum of the afterglow performance of the thin film obtained in Example 50 of the present invention;
[0068] Fig.44 This is a macroscopic LPL image of the film obtained in Example 51 of the present invention at room temperature (from left to right: when excited by white light, 1s and 2s after turning off the white light);
[0069] Fig.45 This is the attenuation spectrum of the afterglow performance of the thin film obtained in Example 51 of the present invention;
[0070] Fig.46 This is the attenuation spectrum of the afterglow performance of the thin film obtained in Example 52 of the present invention;
[0071] Fig.47 This is the attenuation spectrum of the afterglow performance of the thin film obtained in Example 53 of the present invention;
[0072] Fig.48 This is the attenuation spectrum of the afterglow performance of the thin film obtained in Example 54 of the present invention;
[0073] Fig.49 The present invention is an application of the afterglow excited by white light obtained by Example 46 and Example 49 in large-area safety indication;
[0074] Fig.50 The present invention is an application of the white light excited afterglow obtained from Example 46 in metal flaw detection. DETAILED DESCRIPTION
[0075] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0076] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0077] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0078] In the following Examples 1 to 44 and Comparative Examples 1 to 14, the organic fluorescent dye luminophores were purchased from Tianjin Xiens Biochemical Technology Co., Ltd. (purity: 98%); the photocuring adhesive was purchased from Henkel Loctite (China) Co., Ltd. AA3491; Guangdong Youyang New Materials Co., Ltd., UV curing adhesive 3491 / YY1181; Foshan Jinggu Adhesive Co., Ltd., UV glue D-606; Dongguan Lelai Adhesive Products Co., Ltd., V-3218 / V-3018. Among them, AA 3491 and UV glue D-606 are acrylic adhesives. AA 3491 is a transparent, low viscosity, modified acrylic ester liquid adhesive that cures after a few seconds of 365nm ultraviolet irradiation. UV curing adhesives 3491 / YY1181, V-3218 / V-3018 are polyurethane acrylate adhesives that can be cured after a few seconds of 365nm ultraviolet irradiation.
[0079] The structural formula of the organic fluorescent dye used is shown below:
[0080]
[0081] The following examples and comparative examples are used in the following tests:
[0082] Ocean Optics multi-band spectrometer;
[0083] Room temperature: 20-25℃;
[0084] The substrate may be glass, paper, polyurethane car cover film, etc. In the following embodiments and comparative examples, the substrate is glass or polyurethane car cover film.
[0085] In the following Examples 1-44 and Comparative Examples 1-14, the power of the UV lamp is 15W (365nm), and the power of the white light lamp is 20W.
[0086] Embodiments 1 to 44
[0087] A specific method for preparing a photocurable organic long afterglow coating is as follows: stirring an organic fluorescent dye luminophore in a solvent for 10 minutes to completely dissolve it to obtain a luminophore solution, then mixing the luminophore solution with a photocurable adhesive, stirring for 2 minutes at room temperature to obtain a solution, taking 0.5 mL of the solution and drop-coating it on a glass substrate, standing for 1 hour, and after the solvent in the solution is completely evaporated, irradiating and curing it with a 15W ultraviolet lamp for 30 seconds to obtain a coating, wherein, in terms of mass fraction, the ratio of the photocurable adhesive to the organic fluorescent dye luminophore is 20000:1, the ratio of the mass fraction of the organic fluorescent dye luminophore to the volume fraction of the solvent is 2:1, the unit of the mass fraction is mg, the unit of the volume fraction is ml, and the solvent is ethanol.
[0088] The organic fluorescent dyes, photocurable adhesive types and their afterglow times in different embodiments are shown in Table 1.
[0089] Comparative Examples 1 to 14
[0090] A specific method for preparing a photocurable organic long afterglow coating is as follows: stirring an organic fluorescent dye luminophore in a solvent for 10 minutes to completely dissolve it to obtain a luminophore solution, then mixing the luminophore solution with a photocurable adhesive, stirring for 2 minutes at room temperature to obtain a solution, taking 0.5 mL of the solution and applying it dropwise on a glass substrate, standing for 1 hour, and after the solvent in the above solution is completely evaporated, irradiating and curing it with a 15W ultraviolet lamp for 30 seconds to obtain a coating, wherein, by mass, the ratio of the photocurable adhesive to the organic fluorescent dye luminophore is 20000:1, the ratio of the mass fraction of the organic fluorescent dye luminophore to the volume fraction of the solvent is 2:1, the unit of mass fraction is mg, the unit of volume fraction is ml, and the solvent is ethanol. The organic fluorescent dyes, photocurable adhesive types and their afterglow times of different comparative examples are shown in Table 1.
[0091] Table 1
[0092]
[0093]
[0094]
[0095]
[0096]
[0097]
[0098]
[0099]
[0100]
[0101]
[0102] Figure 1 This is a macroscopic LPL picture of the coating obtained in Example 1 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 6 seconds. It can be seen that the coating emits light more evenly.
[0103] Figure 2 This is a macroscopic LPL picture of the coating obtained in Example 2 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 6 seconds. It can be seen that the coating emits light more evenly.
[0104] Figure 3 This is a macroscopic LPL picture of the coating obtained in Example 3 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 6 seconds. It can be seen that the coating emits light more evenly.
[0105] in, Figure 1-3 In the image, there is still afterglow at 6s, and the brightness captured by the camera is much lower than that observed by the naked eye, resulting in very low brightness.
[0106] Figure 4 This is a macroscopic LPL picture of the coating obtained in Example 4 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 3 seconds. It can be seen that the coating emits light more evenly.
[0107] Figure 5 This is a macroscopic LPL picture of the coating obtained in Example 5 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the coating emits light more evenly.
[0108] Figure 6 This is a macroscopic LPL picture of the coating obtained from Example 41 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 1 second. It can be seen that the coating emits light more uniformly, but the afterglow performance is weaker than that of the coating obtained from Examples 1-5.
[0109] Figure 7 This is a macroscopic LPL picture of the coating obtained in Example 6 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the coating emits light more evenly.
[0110] Figure 8 This is a macroscopic LPL picture of the coating obtained in Example 7 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the coating emits light relatively evenly.
[0111] Fig. 9 This is a macroscopic LPL picture of the coating obtained in Example 8 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the coating emits light more evenly.
[0112] Fig.10 This is a macroscopic LPL picture of the coating obtained in Example 9 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 3 seconds. It can be seen that the coating emits light more evenly.
[0113] Fig.11 This is a macroscopic LPL picture of the coating obtained in Example 10 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the coating emits light more evenly.
[0114] Fig.12 This is a macroscopic LPL picture of the coating obtained in Example 11 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 6 seconds. It can be seen that the coating emits light relatively evenly.
[0115] Fig.13 This is a macroscopic LPL picture of the coating obtained in Example 12 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 6 seconds. It can be seen that the coating emits light relatively evenly.
[0116] Fig.14 This is a macroscopic LPL picture of the coating obtained in Example 13 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 6 seconds. It can be seen that the coating emits light relatively evenly.
[0117] Fig.15 This is a macroscopic LPL picture of the coating obtained in Example 14 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 3 seconds. It can be seen that the coating emits light relatively evenly.
[0118] Fig.16 This is a macroscopic LPL picture of the coating obtained in Example 15 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the coating emits light relatively evenly.
[0119] Fig.17This is a macroscopic LPL picture of the coating obtained in Example 16 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the coating emits light relatively evenly.
[0120] Fig.18 This is a macroscopic LPL picture of the coating obtained in Example 17 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the coating emits light relatively evenly.
[0121] Fig.19 This is a macroscopic LPL picture of the coating obtained in Example 18 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the coating emits light relatively evenly.
[0122] Fig. 20 This is a macroscopic LPL picture of the coating obtained in Example 19 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 3 seconds. It can be seen that the coating emits light relatively evenly.
[0123] Fig.21 This is a macroscopic LPL picture of the coating obtained in Example 20 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 4 seconds. It can be seen that the coating emits light relatively evenly.
[0124] Fig. 22 This is a macroscopic LPL picture of the coating obtained from Example 42 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 1 second. It can be seen that the coating emits light more uniformly, but the afterglow performance is weaker than that of the coating obtained from Examples 16-20.
[0125] Fig.23 This is a macroscopic LPL picture of the coating obtained in Example 21 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 2 seconds. It can be seen that the coating emits light relatively evenly.
[0126] Fig.24 This is a macroscopic LPL picture of the coating obtained in Example 22 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 2 seconds. It can be seen that the coating emits light relatively evenly.
[0127] Fig.25 This is a macroscopic LPL picture of the coating obtained in Example 23 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 2 seconds. It can be seen that the coating emits light relatively evenly.
[0128] Fig.26This is a macroscopic LPL picture of the coating obtained in Example 24 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 2 seconds. It can be seen that the coating emits light relatively evenly.
[0129] Fig. 27 This is a macroscopic LPL picture of the coating obtained in Example 25 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 2 seconds. It can be seen that the coating emits light relatively evenly.
[0130] Fig.28 This is a macroscopic LPL picture of the coating obtained from Example 43 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 1 second. It can be seen that the coating emits light more uniformly, but the afterglow performance is weaker than that of the coating obtained from Examples 21-25.
[0131] Fig.29 This is the afterglow performance attenuation diagram of the coating obtained in Example 26. It can be seen from the figure that from -2s to 0s is the coating prepared in Example 26 irradiated with a white light lamp, and the coating exhibits photoluminescence characteristics; from 0s to 1s is the long afterglow luminescence of the coating after the white light lamp is removed, and the afterglow time is about 1s.
[0132] Fig.30 This is a macroscopic LPL picture of the coating obtained in Example 27 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 1 second. It can be seen that the coating emits light relatively evenly.
[0133] Fig.31 This is the afterglow performance attenuation diagram of the coating obtained in Example 31. It can be seen from the figure that from -2s to 0s is the coating prepared in Example 31 irradiated with white light, and the coating exhibits photoluminescence characteristics; from 0s to 2s is the long afterglow luminescence of the coating after the white light is removed, and the afterglow time is about 2s.
[0134] Fig.32 This is the afterglow performance attenuation diagram of the coating obtained in Example 32. It can be seen from the figure that from -2s to 0s is the coating prepared in Example 32 irradiated with white light, and the coating exhibits photoluminescence characteristics; from 0s to 2s is the long afterglow luminescence of the coating after the white light is removed, and the afterglow time is about 2s.
[0135] Fig.33 This is a macroscopic LPL picture of the coating obtained in Example 36 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 3 seconds. It can be seen that the coating emits light relatively evenly.
[0136] Fig.34This is a macroscopic LPL picture of the coating obtained in Example 37 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 3 seconds. It can be seen that the coating emits light relatively evenly.
[0137] Fig.35 This is the afterglow performance attenuation diagram of the coating obtained in Example 38. It can be seen from the figure that from -2s to 0s is the coating prepared in Example 38 irradiated with a white light lamp, and the coating exhibits photoluminescence characteristics; from 0s to 3s is the long afterglow luminescence of the coating after the white light lamp is removed, and the afterglow time is about 3s.
[0138] Fig.36 This is a macroscopic LPL picture of the coating obtained in Example 39 at room temperature. It is excited by a white light lamp, and the light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 1 second. It can be seen that the coating emits light relatively evenly.
[0139] Embodiment 45
[0140] Preparation of light-cured organic long afterglow coating and its application in car cover safety indication. The specific method includes the following steps:
[0141] Step 1, stirring the organic fluorescent dye luminophore in a solvent for 10 minutes to completely dissolve it, obtaining a luminophore solution, and then mixing the luminophore solution with a photocurable adhesive, stirring for 2 minutes at room temperature to obtain a solution, wherein the photocurable adhesive, the organic fluorescent dye luminophore material and the solvent are the same as those in Example 2. In terms of mass fractions, the ratio of the photocurable adhesive to the organic fluorescent dye luminophore is 20000:1, the ratio of the mass fraction of the organic fluorescent dye luminophore to the volume fraction of the solvent is 2:1, the unit of mass fraction is mg, the unit of volume fraction is ml, and the solvent is ethanol.
[0142] Step 2, apply the solution on the car cover film, let it stand at room temperature for 0.5 hours, and after the ethanol evaporates completely, cure it with a 365nm ultraviolet lamp for 30 seconds, and after curing, irradiate the car cover surface with a white light lamp for 3 seconds, and after turning off the excitation light source, observe afterglow on the car cover surface. In this embodiment, the car cover is made of polyurethane (TPU) material.
[0143] like Fig.37 As shown, after turning off the white light, the car cover film can be seen emitting a long yellow-green afterglow, and safety indication can be achieved through the afterglow phenomenon.
[0144] In the above-mentioned embodiments 1-45, by AA3491 replaced AA3492 can achieve the same technical effect; by replacing UV curing adhesive 3491 (Guangdong Youyang New Materials Co., Ltd.) with UV curing adhesive 3492 (Guangdong Youyang New Materials Co., Ltd.), the same technical effect can be achieved.
[0145] In the following Examples 46-54 and Comparative Examples 15-16, the power of the UV lamp is 15W (365nm), and the power of the white light lamp is 30W.
[0146] Examples 46-54
[0147] Mix the photocurable adhesive, organic fluorescent dye and solvent, stir for 5 minutes at room temperature of 20-25°C to obtain a solution, take 0.5 mL of the solution and drop it on the substrate, let it stand for 2 hours at room temperature to allow the solvent in the solution to evaporate completely, and cure it with a 15W ultraviolet lamp for 30 seconds to obtain a film, wherein the ratio of the organic fluorescent dye to the photocurable adhesive is 1:300 by mass, the ratio of the mass fraction of the photocurable adhesive to the volume fraction of the solvent is 3:10, the unit of mass fraction is g, the unit of volume fraction is mL, and the solvent is ethanol. The organic fluorescent dyes of different embodiments and their afterglow time are shown in Table 2. The photocurable adhesive was purchased from: Henkel Loctite (China) Co., Ltd. ( AA3491).
[0148] Comparative Examples 15-16
[0149] The only difference from Example 46 is that the organic fluorescent dye used is different from that in Example 46, and the rest is the same as Example 46. The organic fluorescent dyes of different comparative examples and their afterglow times are shown in Table 2.
[0150] Table 2
[0151]
[0152]
[0153]
[0154] In the present invention, an LPL film with relatively uniform luminescence can be obtained by mixing an organic fluorescent dye and a photocurable adhesive and performing a photocuring process.
[0155] Fig.38 This is a macroscopic LPL picture of the film obtained in Example 46 at room temperature. The film is excited by a white light lamp. The white light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 6 seconds. It can be seen that the film emits light relatively evenly.
[0156] Fig.39 This is the afterglow performance attenuation diagram of the film obtained by Example 46. It can be seen from the figure that -2s to 0s is the time when the film prepared by Example 46 is irradiated with a white light lamp, and the film exhibits photoluminescence characteristics; 0s to 6s is the long afterglow luminescence of the film after the white light lamp is removed, and the afterglow time is about 6s, which is similar to the afterglow time observed by the naked eye.
[0157] Fig.40 This is a macroscopic LPL picture of the film obtained in Example 47 at room temperature. The film is excited by a white light lamp. The white light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the film emits light relatively evenly.
[0158] Fig.41 This is a macroscopic LPL picture of the film obtained from Example 48 at room temperature. The film is excited by a white light lamp. The white light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 5 seconds. It can be seen that the film emits light relatively evenly.
[0159] Fig.42 This is a macroscopic LPL picture of the film obtained in Example 49 at room temperature. The film is excited by a white light lamp. The white light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 3 seconds. It can be seen that the film emits light relatively evenly.
[0160] Fig.43 This is a graph of the afterglow performance attenuation of the film obtained from Example 50. As can be seen from the graph, from -2s to 0s is the white light lamp irradiating the film prepared by Example 50, and the film exhibits photoluminescence characteristics; from 0s to 5s is the long afterglow luminescence of the film after the white light lamp is removed, and the afterglow time is about 5s.
[0161] Fig.44 This is a macroscopic LPL picture of the film obtained in Example 51 at room temperature. The film is excited by a white light lamp. The white light source is turned off after irradiation for 3 seconds. The afterglow can be maintained for 2 seconds. It can be seen that the film emits light relatively evenly.
[0162] Fig.45 This is the afterglow performance attenuation diagram of the film obtained in Example 51. It can be seen from the figure that -2s to 0s is the time when the film prepared in Example 51 is irradiated by a white light lamp, and the film exhibits photoluminescence characteristics; 0s to 2s is the long afterglow luminescence of the film after the white light lamp is removed, and the afterglow time is about 2s, which is similar to the afterglow time observed by the naked eye.
[0163] Fig.46 This is the afterglow performance attenuation diagram of the film obtained in Example 52. It can be seen from the figure that from -2s to 0s is the white light lamp irradiating the film prepared in Example 52, and the film exhibits photoluminescence characteristics; 0s to 1s is the long afterglow luminescence of the film after the white light lamp is removed, and the afterglow time is about 1s.
[0164] Fig.47 This is the afterglow performance attenuation diagram of the film obtained by Example 53. It can be seen from the figure that from -2s to 0s is the white light lamp irradiating the film prepared by Example 53, and the film exhibits photoluminescence characteristics; 0s to 1s is the long afterglow luminescence of the film after the white light lamp is removed, and the afterglow time is about 1s.
[0165] Fig.48This is the afterglow performance attenuation diagram of the film obtained by Example 54. It can be seen from the figure that from -2s to 0s is the white light lamp irradiating the film prepared by Example 54, and the film exhibits photoluminescence characteristics; 0s to 1s is the long afterglow luminescence of the film after the white light lamp is removed, and the afterglow time is about 1s.
[0166] Depend on Figure 1-48 It can be seen that the present invention can induce afterglow emission of the fluorescent dye under white light excitation by mixing the organic fluorescent dye and the photocurable adhesive and performing a photocuring process.
[0167] Embodiment 55
[0168] The afterglow emission of organic fluorescent dyes induced by photocurable adhesives under white light excitation is applied to large-area safety indication. The specific method includes the following steps:
[0169] Step 1, mixing a photocurable adhesive, an organic fluorescent dye and a solvent, stirring for 5 minutes at room temperature of 20 to 25° C. to obtain a solution, wherein the photocurable adhesive, the organic fluorescent dye and the solvent are the same as those in Example 46. In terms of mass fractions, the ratio of the fluorescent dye to the photocurable adhesive is 1:300, the ratio of the mass fraction of the photocurable adhesive to the volume fraction of the solvent is 3:10, the unit of mass fraction is g, the unit of volume fraction is mL, and the solvent is ethanol.
[0170] Step 2, mixing a photocurable adhesive, an organic fluorescent dye and a solvent, stirring for 5 minutes at room temperature of 20 to 25° C. to obtain a solution, wherein the photocurable adhesive, the organic fluorescent dye and the solvent are the same as those in Example 49. In terms of mass fractions, the ratio of the fluorescent dye to the photocurable adhesive is 1:300, the ratio of the mass fraction of the photocurable adhesive to the volume fraction of the solvent is 3:10, the unit of mass fraction is g, the unit of volume fraction is mL, and the solvent is ethanol.
[0171] Step 3, apply the solution to a large area of the "No Left Turn" safety sign, wherein the "left turn arrow" is coated with the solution obtained in Example 46, and the "No" is coated with the solution obtained in Example 49. After the solvent evaporates, irradiate with a 365nm ultraviolet lamp for curing ( Fig.49 a).
[0172] Step 4, when providing safety instructions, use a white light to illuminate the safety sign. After turning off the white light illumination source, an afterglow can be observed on the sign, thereby serving as a safety instruction.
[0173] like Fig.49 As shown in the figure, when the white light is irradiated, the "No Left Turn" sign can be observed. When the white light source is removed, the "Left Turn Arrow" shows a yellow-green afterglow and the "No" shows an orange afterglow ( Fig.49 b) so that the road signs have both reflective and afterglow characteristics, which can better serve as safety instructions (such as Fig.49 , using a 1 yuan coin as a reference, you can compare the size of the sign).
[0174] Embodiment 56
[0175] The afterglow emission of organic fluorescent dyes induced by light-curing adhesives under white light excitation is applied to metal flaw detection. The specific method includes the following steps:
[0176] Step 1, mixing a photocurable adhesive, an organic fluorescent dye and a solvent, stirring for 5 minutes at room temperature of 20 to 25° C. to obtain a solution, wherein the photocurable adhesive, the organic fluorescent dye and the solvent are the same as those in Example 46. In terms of mass fractions, the ratio of the fluorescent dye to the photocurable adhesive is 1:300, the ratio of the mass fraction of the photocurable adhesive to the volume fraction of the solvent is 3:10, the unit of mass fraction is g, the unit of volume fraction is mL, and the solvent is ethanol.
[0177] Step 2, apply the solution obtained in step 1 on the metal surface, use ethanol as a cleaning agent to wipe off the excess solution on the metal surface, after the ethanol evaporates, use a 365nm ultraviolet lamp to solidify, and use the long afterglow material in the solution as a penetrant and developer for penetrant flaw detection: use a white light lamp to illuminate the metal surface, and judge the position and size of the defect by the afterglow. When there is an open defect on the metal surface, the open defect emits a long afterglow, and when there is no open defect on the metal surface, no long afterglow is emitted.
[0178] like Fig.50 As shown in the figure, after turning off the white light, you can see that the opening defect emits a long yellow-green afterglow. The location and size of the defect can be determined through the afterglow phenomenon, thereby realizing non-destructive testing of metal flaw detection.
[0179] In the above-mentioned Examples 46-54, by AA3491 replaced AA3492 can achieve consistent technical results.
[0180] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing an organic long afterglow material, characterized in that: The method comprises the following steps: uniformly mixing an organic fluorescent dye, a solvent and a light-curing adhesive, removing the solvent and curing the mixture with ultraviolet light to obtain the organic long afterglow material; Wherein, the organic fluorescent dye is a mixture of one or more of quinacridone, acridinium yellow, acridinium yellow G, acridinium yellow hydrochloride, proflavine sulfate, acridinium orange, acridinone, ethidium bromide, and 9-aminoacridine; the light-curing adhesive is a mixture of one or more of UV glue D-606, UV curing adhesive 3491, UV curing adhesive YY1181, V3218, and UV curing adhesive 3492; Alternatively, the organic fluorescent dye is a mixture of one or more of acridine yellow, proflavine sulfate, acridine orange, and 9-aminoacridine, and the photocurable adhesive is V3018.
2. The method for preparing the organic long afterglow material according to claim 1, characterized in that: The UV curing adhesive 3491 is from Henkel Loctite (China) Co., Ltd. AA3491, UV curing adhesive 3491 of Guangdong Youyang New Materials Co., Ltd., or a mixture of two thereof; the UV curing adhesive 3492 is Henkel Loctite (China) Co., Ltd. AA3492, UV curing adhesive 3492 of Guangdong Youyang New Materials Co., Ltd., or a mixture of two of them.
3. The method for preparing the organic long afterglow material according to claim 1, characterized in that: The UV glue D-606 comes from Foshan Jinggu Adhesive Co., Ltd., the UV curing adhesive YY1181 comes from Guangdong Youyang New Materials Co., Ltd., and the V3218 comes from Dongguan Lelai Adhesive Products Co., Ltd.
4. The method for preparing the organic long afterglow material according to claim 1, characterized in that: The usage ratio of the organic fluorescent dye and the solvent is 1-5 mg: 1-10 ml.
5. The method for preparing the organic long afterglow material according to claim 1, characterized in that: The mass ratio of the photocurable adhesive to the organic fluorescent dye is 300-40000:
1.
6. The method for preparing an organic long afterglow material according to claim 1, characterized in that: The solvent is ethanol.
7. The method for preparing an organic long afterglow material according to claim 1, characterized in that: The wavelength of the ultraviolet light is 365 nm, and the irradiation curing time is 20 to 40 seconds.
8. The method for preparing an organic long afterglow material according to any one of claims 1 to 7, characterized in that: Before removing the solvent, the method further comprises coating the solution obtained by uniformly mixing the organic fluorescent dye, the solvent and the light-curing adhesive on the substrate.
9. An organic long afterglow material, characterized in that: The organic long afterglow material is prepared by the preparation method of any one of claims 1 to 8.
10. A method for inducing long afterglow emission of an organic fluorescent dye, characterized in that: The following steps are involved: The organic fluorescent dye and solvent according to any one of claims 1 to 3 are uniformly mixed with the photocurable adhesive according to any one of claims 1 to 3, and after removing the solvent, ultraviolet light is used for curing to induce long afterglow emission of the organic fluorescent dye.
Citation Information
Patent Citations
Preparation method and application of pure organic fluorescent long afterglow film excited by visible light
CN116768489A