High-conductivity polymer solid electrolyte and preparation method thereof

Through the combination technology of ultrasonic dispersion and metal organic frame materials, the low conductivity and mechanical performance of solid electrolytes are solved, and polymer electrolytes with high conductivity are prepared, which improves the performance and stability of the battery and is suitable for all-solid state batteries. .

CN119092810APending Publication Date: 2024-12-06ZHEJIANG ZHIBANG LITHIUM BATTERY NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196593.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing solid electrolytes have problems such as low ionic conductivity, poor interface compatibility, and insufficient mechanical properties, which are difficult to meet the requirements of high-performance batteries.

Method used

Through ultrasonic dispersion reduction of graphene oxide powder, combined with metal organic frame (MOF) materials, graphene modified polyimide is prepared by multi-step reaction method to form a material rich in carboxylic acid groups on the surface, and perform molecular self-assembly to improve the Ion conductivity and mechanical properties of electrolytes.

Benefits of technology

It significantly improves the ionic conductivity and mechanical properties of the electrolyte, enhances the charging and discharging efficiency and safety of the battery, ensures the thermal stability and environmental adaptability of the material, and is suitable for use in all-solid state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005016580750000061
    Figure BDA0005016580750000061
  • Figure BDA0005016580750000071
    Figure BDA0005016580750000071
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-conductivity polymer solid electrolyte. The preparation method comprises the following steps: S1, ultrasonically dispersing reduced graphene oxide powder into an aromatic tetracarboxylic dibasic ester solution; s2, mixing the graphene modified polyimide with a catalyst, and adding diamine for reaction to obtain graphene modified polyimide; s3, carrying out strong alkali treatment on the graphene modified polyimide, then adding a carboxylic acid derivative to carry out swelling reaction, and then carrying out hydrolysis reaction to obtain graphene modified polyimide with the surface rich in carboxylic acid groups; s4, immersing the polyimide substrate into a mixed solution composed of a metal salt solution and polycarboxylic acid for molecular self-assembly reaction to obtain an ionic conductor material of an MOF material grown on the surface of the polyimide substrate in situ; and S5, mixing with a lithium salt to obtain the high-conductivity polymer solid electrolyte. The polymer solid electrolyte prepared by the invention not only has excellent conductivity and mechanical strength, but also ensures the long-term durability and stability of the polymer solid electrolyte under different environmental conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid electrolytes, and in particular to a high-conductivity polymer solid electrolyte and a preparation method thereof. Background Art

[0002] With the development of new energy technologies, the demand for efficient and safe electrochemical energy storage systems is growing. Traditional liquid electrolytes have problems such as flammability, easy leakage, and poor stability in lithium-ion batteries, which limits the further improvement of battery performance. Solid-state electrolytes are regarded as the development direction of the next generation of battery technology due to their advantages such as high safety and high energy density. However, existing solid-state electrolytes generally have defects such as low ionic conductivity, poor interface compatibility, and insufficient mechanical properties, which make it difficult to meet the requirements of high-performance batteries. Therefore, the development of solid-state electrolyte materials with high conductivity, good interface compatibility and excellent mechanical properties is of great significance to promote the development of all-solid-state battery technology.

[0003] The present invention aims to solve the deficiencies of the prior art through an innovative preparation method and provide a high-conductivity polymer solid electrolyte with better performance. Summary of the invention

[0004] In view of the above shortcomings of the prior art, the present invention provides a method for preparing a high-conductivity polymer solid electrolyte to solve the problems of low ion conductivity, poor interface compatibility, insufficient mechanical properties, and low electrochemical stability of traditional solid electrolytes. Through innovative preparation steps, the present invention aims to provide a solid electrolyte with better comprehensive performance, significantly improving its electrochemical performance and application potential in all-solid-state batteries.

[0005] In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0006] A method for preparing a high-conductivity polymer solid electrolyte, the preparation method comprising the following steps:

[0007] S1: using an aromatic tetracarboxylic acid dibasic ester solution as a dispersed phase, and ultrasonically dispersing reduced graphene oxide powder in the dispersed phase to obtain a reduced graphene oxide aromatic tetracarboxylic acid dibasic ester dispersion;

[0008] S2: mixing the reduced graphene oxide aromatic tetracarboxylic acid dibasic ester dispersion obtained in step S1 with a catalyst to obtain a mixture; adding a diamine and stirring evenly, and heating the mixture to obtain a graphene-modified polyimide;

[0009] S3: treating the graphene-modified polyimide obtained in step S2 with a strong base, then adding it to a carboxylic acid derivative solution for swelling reaction for a certain period of time, and then performing a hydrolysis reaction to obtain a graphene-modified polyimide with a surface rich in carboxylic acid groups;

[0010] S4: immersing the graphene-modified polyimide matrix obtained in step S3 into a mixed solution consisting of a metal salt solution and a polycarboxylic acid to perform a molecular self-assembly reaction, thereby obtaining an ionic conductor material of an MOF material in situ grown on the surface of the polyimide matrix;

[0011] S5: mixing the ion conductor material obtained in step S4 with lithium salt and an organic solvent, heating and stirring the mixture to obtain the high-conductivity polymer solid electrolyte after vacuum drying.

[0012] As a preferred technical solution, the solute of the aromatic tetracarboxylic acid dibasic ester solution is at least one of dimethyl pyromellitic acid, diethyl pyromellitic acid, di-n-propyl pyromellitic acid, 3,3',4,4'-dimethyl benzophenone tetracarboxylate, 3,3',4,4'-diethyl benzophenone tetracarboxylate, 3,3',4,4'-dimethyl diphenyl ether tetracarboxylate, and 3,3',4,4'-diethyl diphenyl ether tetracarboxylate.

[0013] As a preferred technical solution, the ultrasonic dispersion operating conditions are: operating temperature 20-60°C, operating power 100-500W, and operating time 20-180min.

[0014] As a preferred technical solution, the catalyst is at least one of triethanolamine, triethylenediamine, stannous octoate, and dibutyltin dilaurate.

[0015] As a preferred technical solution, the diamine is at least one of p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, and 1,4-bis(4-aminophenoxy)benzene.

[0016] As a preferred technical solution, the carboxylic acid derivative is at least one of acetic acid, propionic acid, butyric acid, acetic anhydride, propionic anhydride, and butyric anhydride.

[0017] As a preferred technical solution, the solute of the metal salt solution is composed of at least one metal element selected from zirconium, silver, copper, aluminum, iron and nickel as cations and at least one selected from chloride ions, nitrate ions and sulfate ions as anions.

[0018] As a preferred technical solution, the polycarboxylic acid is 3,4-dimethylthieno(2,3-b)thiophene-2,5-dicarboxylic acid and / or thieno[3,4-c]pyridine-1,3-dicarboxylic acid.

[0019] As a preferred technical solution, the lithium salt is at least one of lithium perchlorate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium tetrachloroaluminate, lithium trifluoromethanesulfonate, and lithium bis(trifluoromethanesulfonyl)imide.

[0020] Another aspect of the present invention is to provide a high-conductivity polymer solid electrolyte, wherein the solid electrolyte is prepared by the above-mentioned preparation method of the high-conductivity polymer solid electrolyte.

[0021] In step S1 of the present invention, the reduced graphene oxide powder is uniformly dispersed in the aromatic tetracarboxylic acid dibasic ester solution by ultrasonic dispersion technology to form a stable dispersion, which lays the foundation for the conductivity and mechanical properties of the subsequent materials. In step S2, under the action of a catalyst, the aromatic tetracarboxylic acid dibasic ester and the diamine undergo a polycondensation reaction to form a graphene-modified polyimide. This composite material combines the high conductivity of graphene and the thermal stability of polyimide, showing good electrical conductivity and mechanical strength. Further, step S3 introduces carboxylic acid groups on the surface of the polyimide matrix by strong alkali treatment and the swelling reaction of carboxylic acid derivatives, which not only provides abundant active sites for the in-situ growth of MOF materials, but also enhances the hydrophilicity and ion adsorption capacity of the material, thereby improving the ion transport performance. In step S4, the MOF material grows in-situ on the surface of the polyimide matrix to form a continuous ion transport channel. This process significantly improves the ionic conductivity of the electrolyte, while enhancing the mechanical properties and electrochemical stability of the material, providing a guarantee for the safety and stability of the battery. Finally, in step S5, a polymer solid electrolyte with high electrical conductivity is prepared by compounding the ion conductor material with the lithium salt.

[0022] The polymer solid electrolyte prepared by the present invention exhibits excellent ionic conductivity and interface impedance performance in electrochemical tests, and is suitable for use in all-solid-state batteries. In addition, the electrolyte of the present invention also exhibits good environmental stability, and can maintain performance even in oxygen-containing and water-containing atmospheres, ensuring the reliability and durability of the battery under different environmental conditions. In general, the high-conductivity polymer solid electrolyte of the present invention not only improves the charge and discharge efficiency and safety of the battery, but also provides an important material basis for the development of all-solid-state battery technology by enhancing the mechanical properties and thermal stability of the material.

[0023] Beneficial effects of the present invention:

[0024] The preparation method of the high-conductivity polymer solid electrolyte of the present invention not only achieves high conductivity and excellent mechanical properties, but also achieves good interface compatibility with electrode materials by innovatively introducing reduced graphene oxide and combining metal organic framework (MOF) materials. This design not only enhances the ion transmission efficiency of the electrolyte, but also maintains the thermal stability and electrochemical stability of the material, which helps to improve the charge and discharge efficiency and cycle stability of the all-solid-state battery.

[0025] In general, the polymer solid electrolyte prepared by the present invention not only has excellent electrical conductivity and mechanical strength, but also ensures its long-term durability and stability under different environmental conditions. It has strong overall comprehensive performance and environmental adaptability, can meet the promotion and use of high energy density and high safety batteries, and has broad application prospects and market potential. DETAILED DESCRIPTION

[0026] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.

[0027] Example 1

[0028] The method for preparing the high conductivity polymer solid electrolyte of this embodiment comprises the following steps:

[0029] S1: Using 20 g of dimethyl pyromellitic acid in N,N-dimethylformamide solution (100 mL) as the dispersed phase, 0.1 g of reduced graphene oxide powder was ultrasonically dispersed in the dispersed phase to obtain a reduced graphene oxide dimethyl pyromellitic acid dispersion; the ultrasonic dispersion operating conditions were: operating temperature 50°C, operating power 300 W, and operating time 90 min.

[0030] S2: Mix the reduced graphene oxide dimethyl pyromellitic acid dispersion obtained in step S1 and dibutyl tin dilaurate to obtain a mixture; add 4,4'-diaminodiphenyl ether and stir evenly, first subject to a low-temperature polycondensation reaction at 110°C for 3 hours, and then subject to a high-temperature reaction at 250°C for 3 hours to obtain graphene-modified polyimide; the mass ratio of the reduced graphene oxide dimethyl pyromellitic acid dispersion, dibutyl tin dilaurate and 4,4'-diaminodiphenyl ether is 100:8:150.

[0031] S3: The graphene-modified polyimide obtained in step S2 is first added to a sodium hydroxide solution with a pH of 12 for strong alkaline treatment. After the operation for 30 minutes, it is washed and filtered with deionized water and anhydrous ethanol for multiple times, and then added to a carboxylic acid derivative solution composed of acetic acid and acetic anhydride in a molar ratio of 1:1 for swelling reaction for 1 hour. After filtering, deionized water is added, and then hydrolysis reaction is carried out for 2 hours to obtain a graphene-modified polyimide with rich carboxylic acid groups on the surface; the weight ratio of the graphene-modified polyimide to the volume of the carboxylic acid derivative solution is 1:5.

[0032] S4: The graphene-modified polyimide substrate obtained in step S3 is immersed in a mixed solution consisting of an aqueous solution of 0.1M zirconium chloride and 0.4M 3,4-dimethylthieno(2,3-b)thiophene-2,5-dicarboxylic acid, and a molecular self-assembly reaction is performed at 60°C for 24 hours to obtain an ionic conductor material with in-situ growth of MOF material on the surface of the polyimide substrate.

[0033] S5: Mix the ionic conductor material obtained in step S4 with 1M lithium bis(trifluoromethanesulfonyl)imide and an appropriate amount of N,N-dimethylformamide, heat to 60° C. and stir for 2 h to fully mix them, and then dry them in a vacuum drying oven for 24 h to obtain the high conductivity polymer solid electrolyte.

[0034] Example 2

[0035] The method for preparing the high conductivity polymer solid electrolyte of this embodiment comprises the following steps:

[0036] S1: Using 25 g of 3,3',4,4'-dimethylbenzophenonetetracarboxylate N,N-dimethylformamide solution (100 mL) as the dispersed phase, 0.15 g of reduced graphene oxide powder was ultrasonically dispersed in the dispersed phase to obtain a reduced graphene oxide aromatic tetracarboxylic acid dibasic ester dispersion; the ultrasonic dispersion operating conditions were: operating temperature 60°C, operating power 500W, and operating time 60min.

[0037] S2: Mix the reduced graphene oxide aromatic tetracarboxylic acid dibasic ester dispersion obtained in step S1 and dibutyltin dilaurate to obtain a mixture; add 1,4-bis(4-aminophenoxy)benzene and stir evenly, first subject to a low-temperature polycondensation reaction at 150°C for 2 hours, and then subject to a high-temperature reaction at 280°C for 1 hour to obtain graphene-modified polyimide; the mass ratio of the reduced graphene oxide aromatic tetracarboxylic acid dibasic ester dispersion, dibutyltin dilaurate and diamine is 80:5:120.

[0038] S3: The graphene-modified polyimide obtained in step S2 is first added to a sodium hydroxide solution with a pH of 12 for strong alkaline treatment. After the operation for 30 minutes, it is washed and filtered with deionized water and anhydrous ethanol for multiple times, and then added to a carboxylic acid derivative solution composed of propionic acid and propionic anhydride in a molar ratio of 1:1 for swelling reaction for 2 hours. After filtering, deionized water is added, and then hydrolysis reaction is carried out for 4 hours to obtain a graphene-modified polyimide with rich carboxylic acid groups on the surface; the weight ratio of the graphene-modified polyimide to the volume of the carboxylic acid derivative solution is 1:5.

[0039] S4: The graphene-modified polyimide substrate obtained in step S3 is immersed in a mixed solution consisting of an aqueous solution of 0.1 M silver nitrate and 0.1 M thieno[3,4-c]pyridine-1,3-dicarboxylic acid, and a molecular self-assembly reaction is performed at 60° C. for 24 hours to obtain an ionic conductor material having an in-situ grown MOF material on the surface of the polyimide substrate.

[0040] S5: Mix the ionic conductor material obtained in step S4 with 1M lithium trifluoromethanesulfonate and an appropriate amount of N,N-dimethylformamide, heat to 60° C. and stir for 2 hours to fully mix them, and then dry them in a vacuum drying oven for 24 hours to obtain the high-conductivity polymer solid electrolyte.

[0041] Example 3

[0042] The method for preparing the high conductivity polymer solid electrolyte of this embodiment comprises the following steps:

[0043] S1: Using 30 g of 3,3',4,4'-diphenyl ether tetraacid diethyl ester in N,N-dimethylformamide solution (100 mL) as the dispersed phase, 0.2 g of reduced graphene oxide powder was ultrasonically dispersed in the dispersed phase to obtain a reduced graphene oxide aromatic tetracarboxylic acid dibasic ester dispersion; the ultrasonic dispersion operating conditions are: operating temperature 60°C, operating power 500W, and operating time 90min.

[0044] S2: Mix the reduced graphene oxide aromatic tetracarboxylic acid dibasic ester dispersion obtained in step S1 and dibutyltin dilaurate to obtain a mixture; add p-phenylenediamine and stir evenly, first subject to a low-temperature polycondensation reaction at 90°C for 5 hours, and then subject to a high-temperature reaction at 250°C for 2 hours to obtain graphene-modified polyimide; the mass ratio of the reduced graphene oxide aromatic tetracarboxylic acid dibasic ester dispersion, dibutyltin dilaurate and diamine is 50:4:75.

[0045] S3: The graphene-modified polyimide obtained in step S2 is first added to a sodium hydroxide solution with a pH of 12 for strong alkaline treatment. After the operation for 30 minutes, it is washed and filtered with deionized water and anhydrous ethanol for multiple times, and then added to a carboxylic acid derivative solution composed of butyric acid and butyric anhydride in a molar ratio of 1:1 for swelling reaction for 3 hours. After filtering, deionized water is added, and then hydrolysis reaction is carried out for 6 hours to obtain a graphene-modified polyimide with rich carboxylic acid groups on the surface; the weight ratio of the graphene-modified polyimide to the volume ratio of the carboxylic acid derivative solution is 1:5.

[0046] S4: The graphene-modified polyimide substrate obtained in step S3 is immersed in a mixed solution consisting of an aqueous solution of 0.1M copper chloride and 0.2M 3,4-dimethylthieno(2,3-b)thiophene-2,5-dicarboxylic acid, and a molecular self-assembly reaction is performed at 60°C for 24 hours to obtain an ionic conductor material with in-situ growth of MOF material on the surface of the polyimide substrate.

[0047] S5: Mix the ionic conductor material obtained in step S4 with 1M lithium hexafluorophosphate and an appropriate amount of N,N-dimethylformamide, heat to 60° C. and stir for 2 h to fully mix them, and then dry them in a vacuum drying oven for 24 h to obtain the high-conductivity polymer solid electrolyte.

[0048] The polymer solid electrolytes prepared in Examples 1 to 3 were made into disc samples with a diameter of 10 mm and a thickness of 1 mm for performance testing. The performance results are shown in Table 1:

[0049] Among them, the mechanical strength performance test method is: the example sample is cut into long strips with a length of 120 mm and a width of 15 mm. The mechanical strength of the polymer solid electrolyte is evaluated by a tensile test on a universal material testing machine, with tensile strength and elongation at break as evaluation indicators.

[0050] For the ionic conductivity performance test, the polymer solid electrolyte samples prepared in Examples 1 to 3 were connected to an AC impedance spectroscopy measuring instrument to test the ionic conductivity of the polymer solid electrolyte by AC impedance spectroscopy.

[0051] For the interface impedance performance test, the polymer solid electrolyte samples of Examples 1 to 3 were sandwiched between the positive and negative electrode materials (the positive electrode material was lithium manganese oxide, and the negative electrode material was lithium titanate) to form a complete button battery structure; an electrochemical workstation was used to perform an electrochemical impedance spectroscopy test on the interface impedance between the polymer solid electrolyte and the positive and negative electrode materials.

[0052] Environmental stability performance test, first, prepare 6 samples with similar ionic conductivity and interface impedance performance in Examples 1 to 3, and then number them A1-A3 (oxygen-containing atmosphere) and B1-B3 (water-containing atmosphere), respectively; secondly, expose them in reaction vessels with oxygen-containing atmosphere (pure oxygen with a concentration of 99.99%) and water-containing atmosphere (relative humidity of 85%) for 72 hours, respectively; finally, test the ionic conductivity of the polymer solid electrolyte by AC impedance spectroscopy, calculate the average values ​​of ionic conductivity and interface impedance of the 6 samples in each example, and evaluate the environmental stability of the polymer solid electrolyte by taking the change rate of the average value of ionic conductivity and interface impedance as evaluation indicators. Table 1

[0053] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention, and these changes and improvements fall within the scope of the present invention claimed.

Claims

1. A method for preparing a high conductivity polymer solid electrolyte, characterized in that: The preparation method comprises the following steps: S1: using an aromatic tetracarboxylic acid dibasic ester solution as a dispersed phase, and ultrasonically dispersing reduced graphene oxide powder in the dispersed phase to obtain a reduced graphene oxide aromatic tetracarboxylic acid dibasic ester dispersion; S2: mixing the reduced graphene oxide aromatic tetracarboxylic acid dibasic ester dispersion obtained in step S1 with a catalyst to obtain a mixture; adding a diamine and stirring evenly, and heating the mixture to obtain a graphene-modified polyimide; S3: treating the graphene-modified polyimide obtained in step S2 with a strong base, then adding it to a carboxylic acid derivative solution for swelling reaction for a certain period of time, and then performing a hydrolysis reaction to obtain a graphene-modified polyimide with a surface rich in carboxylic acid groups; S4: immersing the graphene-modified polyimide matrix obtained in step S3 into a mixed solution consisting of a metal salt solution and a polycarboxylic acid to perform a molecular self-assembly reaction, thereby obtaining an ionic conductor material of an MOF material in situ grown on the surface of the polyimide matrix; S5: mixing the ion conductor material obtained in step S4 with lithium salt and an organic solvent, heating and stirring the mixture to obtain the high-conductivity polymer solid electrolyte after vacuum drying.

2. The method for preparing a high conductivity polymer solid electrolyte according to claim 1, characterized in that: The solute of the aromatic tetracarboxylic acid dibasic ester solution is at least one of dimethyl pyromellitic acid, diethyl pyromellitic acid, di-n-propyl pyromellitic acid, 3,3',4,4'-dimethyl benzophenone tetracarboxylate, diethyl 3,3',4,4'-diethyl benzophenone tetracarboxylate, 3,3',4,4'-dimethyl diphenyl ether tetracarboxylate, and diethyl 3,3',4,4'-diphenyl ether tetracarboxylate.

3. The method for preparing a high conductivity polymer solid electrolyte according to claim 1, characterized in that: The ultrasonic dispersion operation conditions are: operation temperature 20-60° C., operation power 100-500 W, and operation time 20-180 min.

4. The method for preparing a high conductivity polymer solid electrolyte according to claim 1, characterized in that: The catalyst is at least one of triethanolamine, triethylenediamine, stannous octoate and dibutyltin dilaurate.

5. The method for preparing a high conductivity polymer solid electrolyte according to claim 1, characterized in that: The diamine is at least one of p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, and 1,4-bis(4-aminophenoxy)benzene.

6. The method for preparing a high conductivity polymer solid electrolyte according to claim 1, characterized in that: The carboxylic acid derivative is at least one of acetic acid, propionic acid, butyric acid, acetic anhydride, propionic anhydride and butyric anhydride.

7. The method for preparing a high conductivity polymer solid electrolyte according to claim 1, characterized in that: The solute of the metal salt solution is composed of at least one metal element selected from zirconium, silver, copper, aluminum, iron and nickel as a cation and at least one metal element selected from chloride ion, nitrate ion and sulfate ion as an anion.

8. The method for preparing a high conductivity polymer solid electrolyte according to claim 1, characterized in that: The polycarboxylic acid is 3,4-dimethylthieno(2,3-b)thiophene-2,5-dicarboxylic acid and / or thieno[3,4-c]pyridine-1,3-dicarboxylic acid.

9. The method for preparing a high conductivity polymer solid electrolyte according to claim 1, characterized in that: The lithium salt is at least one of lithium perchlorate, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium tetrachloroaluminate, lithium trifluoromethanesulfonate, and lithium bis(trifluoromethanesulfonyl)imide.

10. A high conductivity polymer solid electrolyte, characterized in that: The solid electrolyte is prepared by the method for preparing a high-conductivity polymer solid electrolyte as claimed in any one of claims 1 to 9.