Multilayer film

By using metallocene-catalyzed multimodal polyethylene copolymer and recovery blend in multilayer films, the density and fluidity of the core layer are optimized, and the mechanical and optical properties balance and sealing of multilayer films in recovered polymers are solved. The problem of insufficient performance has achieved efficient packaging materials application.

CN119095725APending Publication Date: 2024-12-06北欧化工公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380032621.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-06
Filing Date
2023-04-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing multilayer films are difficult to achieve a good balance between recovery and mechanical properties and optical properties, and there is also the problem of insufficient sealing properties, especially when the recovered polymer is included.

Method used

A multilayer film structure consisting of a surface layer, a core layer and a sealing layer, wherein the core layer uses a metallocene-catalyzed multimodal polyethylene copolymer (MMCP) composed of ethylene-1-butene and ethylene-1-hexene polymers. , combined with the recovery of blends, optimize density and melt flow rate to improve mechanical properties and sealing properties.

Benefits of technology

It achieves a good balance between mechanical and optical properties of multilayer films in the presence of recovered polymers, and significantly improves sealing performance, which is suitable for packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005071324850000091
    Figure BDA0005071324850000091
  • Figure BDA0005071324850000101
    Figure BDA0005071324850000101
  • Figure BDA0005071324850000111
    Figure BDA0005071324850000111
Patent Text Reader

Abstract

The invention relates to a multilayer film comprising a skin layer (SKL), a core layer (CL) and a sealing layer (SL); wherein at least the core layer comprises a specific metallocene catalyzed multimodal polyethylene copolymer (MMCP). The invention also relates to the use of said multilayer film as a packaging material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a multilayer film comprising a skin layer (SKL), a core layer (CL) and a seal layer (SL), wherein at least one of the layers comprises a specific metallocene-catalyzed multimodal polyethylene copolymer (MMCP). The present invention also relates to the use of the multilayer film as a packaging material.

[0002] Polyethylene is widely used in various fields of daily life, such as packaging, due to its excellent cost-performance ratio. Due to different needs, multilayer films with different types of materials are now used, which meets the needs from one side, but the disadvantage is that the recycling of such films is difficult. From the recycling point of view, a single material solution would be preferred. In addition, a multilayer film that allows the presence of recycled polymers and at the same time exhibits acceptable properties is required.

[0003] Single-material solutions and multilayer films containing recycled polymers are known in the prior art.

[0004] WO 2021 / 259910 A1 relates to a tubular film intended to form a stretch hood. The tubular film has a core layer and at least one skin layer. The core layer comprises, by weight of the core layer: 30 to 80% of recycled polyethylene, 10 to 35% of a polymer booster selected from thermoplastic elastomers and polyolefin plastomers, and 0 to 40% of virgin ethylene polymers and / or virgin ethylene-based copolymers.

[0005] WO 2021 / 173771 A1 relates to a multilayer film, a packaging article and a method for making a packaging article from the multilayer film. The multilayer film has a waste content of at least 25%, a compatibilizer and an antioxidant, and can be used for food packaging. The waste includes a polymer mixture recovered and recycled from a waste stream.

[0006] EP 3 838 587 A1 relates to a multilayer stretch wrap film, in particular a polyolefin stretch film comprising at least 20 wt % of PCR plastic waste, a method for its preparation and the use of the multilayer stretch film according to the invention in stretch wrapping operations for goods.

[0007] WO 2021 / 074697 A1 relates to a shrink film, which may include at least one layer comprising a blended ethylene-based polymer composition, wherein the blended ethylene-based polymer composition has a PCR content varying from greater than 5 wt% to less than 95 wt% and a virgin resin content varying from greater than 5 wt% to less than 95 wt%, wherein the virgin resin is selected from HDPE, LLDPE, LDPE, or a combination thereof.

[0008] Starting from this, one object of the present invention is to provide a multilayer film which is not only easy to recycle but also has a good balance of mechanical and optical properties, has excellent sealing properties and tolerates the presence of already recycled polymers.

[0009] These objects have been solved by a multilayer film according to claim 1, comprising a skin layer (SKL), a core layer (CL) and a seal layer (SL); wherein at least the core layer (CL) comprises a metallocene-catalyzed multimodal polyethylene copolymer (MMCP) comprising

[0010] (i) 35.0 to 50.0 wt% of an ethylene-1-butene polymer component (A), based on the total weight of the MMCP; and

[0011] (ii) 50.0 to 65.0 wt% of an ethylene-1-hexene polymer component (B), based on the total weight of the MMCP; wherein

[0012] The ethylene-1-butene polymer component (A) has

[0013] ·920 to 960 kg / m 3 Density within the range (ASTM D792);

[0014] MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 3.0 to 300.0 g / 10 min;

[0015] · a 1-butene content in the range of 0.1 to 3.0 mol% based on the ethylene-1-butene polymer component (A); and

[0016] The ethylene-1-hexene polymer component (B) has

[0017] 880 to 920 kg / m 3 Density within the range (ASTM D792);

[0018] MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.001 to 1.0 g / 10 min;

[0019] · a 1-hexene content in the range of 1.5 to 10.0 mol% based on the ethylene-1-hexene polymer compound (B); and

[0020] Metallocene-catalyzed multimodal polyethylene copolymers (MMCPs) have

[0021] ·910 to 930 kg / m 3 Density within the range (ASTM D792);

[0022] MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 1.4 g / 10 min; and

[0023] MFR in the range of 22 to 70 21 (190℃, 21.6kg, ISO 1133) and MFR2 (190℃,

[0024] 2.16kg, ISO 1133) Ratio MFR 21 / MFR2;

[0025] wherein the core layer further comprises a mixed plastic-polyethylene recycled blend having an MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 1.2 g / 10 min and a 3 Density (ASTM D792).

[0026] Advantageous embodiments of the multilayer film according to the invention are specified in dependent claims 2 to 14. The invention also relates to the use of the multilayer film according to the invention according to claim 15 as packaging material.

[0027] definition

[0028] Metallocene-catalyzed (linear low density) polyethylene is defined in the present invention as a (linear low density) polyethylene copolymer produced in the presence of a metallocene catalyst.

[0029] Ziegler-Natta catalyzed (linear low density) polyethylene is defined in the present invention as a (linear low density) polyethylene copolymer produced in the presence of a Ziegler-Natta catalyst.

[0030] For the purposes of the present invention, the metallocene-catalyzed (linear low density) polyethylene composed of an ethylene-1-butene polymer component (A) and an ethylene-1-hexene polymer component (B) means that the polymers are produced in at least a two-stage sequential polymerization process, wherein component (A) is first produced and then, in a subsequent polymerization step, component (B) is produced in the presence of component (A) to produce the metallocene-catalyzed (linear low density) polyethylene, or vice versa, i.e., component (B) is first produced and then, in a subsequent polymerization step, component (A) is produced in the presence of component (B) to produce the metallocene-catalyzed (linear low density) polyethylene.

[0031] In the context of multimodal metallocene-catalyzed (linear low density) polyethylene, the term "multimodal" refers herein to the multimodality with respect to the melt flow rate (MFR) of at least ethylene polymer components (A) and (B), i.e. ethylene polymer components (A) and (B) have different MFR values. The multimodal metallocene-catalyzed (linear low density) polyethylene may have additional multimodality between ethylene polymer components (A) and (B) with respect to one or more other properties (such as density, comonomer type and / or comonomer content), which will be described below.

[0032] For the purpose of this specification and the subsequent claims, the term "recycled LDPE" is used to indicate that the material is recovered from post-consumer waste and / or industrial waste. That is, post-consumer waste refers to items that have completed at least the first use cycle (or life cycle), that is, items that have reached their first purpose; while industrial waste refers to manufacturing waste that does not usually reach the hands of consumers. In the gist of the present invention, "recycled LDPE" may also contain up to 20wt%, preferably up to 15wt%, more preferably up to 10wt%, even more preferably up to 5wt% of other components, such as LLDPE, MDPE, HDPE, based on the total weight of the recycled LDPE. Correspondingly, the term "virgin" refers to materials and / or items that are newly produced before the first use and have not been recycled. In the absence of explicit mention of the source of the polymer, the polymer is a "virgin" polymer.

[0033] Low density polyethylene (LDPE) is defined in the present invention as a low density polyethylene copolymer preferably produced in a high pressure process.

[0034] Ethylene homopolymers are polymers consisting essentially of ethylene monomer units. Due to impurities, especially impurities in industrial polymerization processes, ethylene homopolymers may contain up to 1.0 mol% of comonomer units, preferably up to 0.5 mol% of comonomer units, most preferably up to 0.01 mol% of comonomer units.

[0035] A single material film in the context of the present invention may be a film that uses primarily one polymer (eg polyethylene) but not a significant amount of other polymers. However, in the case where the film is based on polyethylene, different polyethylenes may be present.

[0036] Where the term "comprising" is used in the present description and claims, it does not exclude other, not specifically stated, elements of major or minor functional importance. For the purposes of the present invention, the term "consisting of" is considered to be a preferred embodiment of the term "comprising". If a group is defined hereinafter as comprising at least a certain number of embodiments, this is also to be understood as disclosing the group, which preferably consists only of these embodiments.

[0037] Whenever the terms "including" or "having" are used, these terms are meant to be equivalent to "comprising" as defined above.

[0038] When an indefinite or definite article is used when referring to a singular noun, for example "a", "an" or "the", this includes a plural of that noun unless otherwise stated.

[0039] Metallocene-catalyzed multimodal polyethylene copolymers (MMCP)

[0040] At least the core layer in the multilayer film according to the present invention comprises a specific metallocene-catalyzed multimodal polyethylene copolymer (MMCP).

[0041] The specific copolymer (MMCP) comprises, preferably consists of (i) 35.0 to 50.0 wt% of an ethylene-1-butene polymer component (A) based on the total weight of the MMCP and (ii) 50.0 to 65.0 wt% of an ethylene-1-hexene polymer component (B) based on the total weight of the MMCP.

[0042] The ethylene-1-butene polymer component (A) has a molecular weight of 920 to 960 kg / m 3 range (ASTM D792), MFR2 (190° C., 2.16 kg, ISO 1133) in the range of 3.0 to 300.0 g / 10 min, and a 1-butene content in the range of 0.1 to 3.0 mol % based on the ethylene-1-butene polymer component (A).

[0043] The ethylene-1-hexene polymer component (B) has a molecular weight of 880 to 920 kg / m 3 range (ASTM D792), MFR2 (190° C., 2.16 kg, ISO 1133) within the range of 0.001 to 1.0 g / 10 min, 1-hexene content within the range of 1.5 to 10.0 mol % based on the ethylene-1-hexene polymer compound (B).

[0044] The metallocene-catalyzed multimodal polyethylene copolymer (MMCP) has a molecular weight of 910 to 930 kg / m 3 Density in the range (ASTM D792), MFR in the range of 0.1 to 1.4 g / 10min 21 (190°C, 21.6 kg, ISO 1133); and MFR in the range of 22 to 70 21 Ratio of MFR (190℃, 21.6kg, ISO 1133) to MFR2 (190℃, 2.16kg, ISO 1133) 21 / MFR2.

[0045] In a preferred embodiment of the present invention, the ethylene-1-butene polymer component (A) consists of ethylene polymer fractions (A-1) and (A-2).

[0046] In case the ethylene-1-butene polymer component (A) consists of ethylene polymer fractions (A-1) and (A-2), the MFR2 of the ethylene polymer fractions (A-1) and (A-2) may be the same as or different from each other.

[0047] The MFR2 (190°C, 2.16 kg, ISO 1133) of the ethylene polymer portion (A-1) and / or (A-2) is in the range of 3.0 to 300.0 g / 10 min, preferably 3.0 to 10.0 g / 10 min or 80 to 150.0 g / 10 min, more preferably 4.0 to 7.0 g / 10 min or 6.0 to 8.0 g / 10 min or 115 to 125 g / 10 min.

[0048] In a preferred embodiment the MFR2 of ethylene polymer components (A) and (B) are different from each other.

[0049] The MFR2 (190°C, 2.16 kg, ISO 1133) of the ethylene polymer component (A) is preferably in the range of 3.0 to 200 g / 10 min, more preferably 3.5 to 11 g / 10 min or 100 to 130 g / 10 min, more preferably 4.0 to 9.0 g / 10 min or 115 to 128 g / 10 min, even more preferably 4.5 to 8.5 g / 10 min or 120 to 125 g / 10 min.

[0050] The MFR2 (190°C, 2.16 kg, ISO 1133) of the ethylene polymer component (B) is in the range of 0.001 to 1.0 g / 10 min, preferably 0.005 to 0.8 g / 10 min, more preferably 0.2 to 0.6 g / 10 min, even more preferably 0.01 to 0.5 g / 10 min.

[0051] The multimodal copolymer (MMCP) has an MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 1.35 g / 10min, more preferably 0.4 to 1.30 g / 10min or 0.5 to 0.7 g / 10min.

[0052] Of course, in addition to multimodality with respect to (i.e. a difference between) the MFR2 of the ethylene polymer components (A) and (B), the multimodal PE of the present invention may also be multimodal, for example with respect to one or both of two other properties: multimodality with respect to, i.e. a difference between, the densities of the ethylene polymer components (A) and (B).

[0053] Preferably, the multimodal copolymer (MMCP) is further multimodal with respect to the comonomer content of the ethylene polymer components (A) and (B).

[0054] The comonomer type of polymer fractions (A-1) and (A-2) is the same, so both fractions have 1-butene as a comonomer.

[0055] The comonomer content of components (A) and (B) can be measured or, in a preferred case, in a so-called multi-stage process, one component is first produced and then the other component is produced in the presence of the first component, then the comonomer content of the first produced component, e.g. component (A), can be measured and the comonomer content of the other component, e.g. component (B), can be calculated according to the following equation:

[0056] The comonomer content in component B (mol% or wt%) = (the comonomer content in the final product (mol% or wt%) - (the weight fraction of component A) * Comonomer content in component A (mol% or wt%)

[0057] / (weight fraction of component B).

[0058] MFR of multimodal copolymers (MMCP) 21 Ratio of MFR (190℃, 21.6kg, ISO 1133) to MFR2 (190℃, 2.16kg, ISO1133) 21 / MFR2 is in the range of 22 to 70, preferably 22 to 50, more preferably 23 to 50, even more preferably 28 to 46.

[0059] According to a preferred embodiment of the present invention, the content of the ethylene-1-butene polymer component (A) is in the range of 35 to 50 wt%, preferably 36 to 48 wt%, more preferably 38 to 45 wt%, based on the total weight of the MMCP, and / or the content of the ethylene-1-hexene polymer component (B) is in the range of 50 to 65 wt%, preferably 52 to 64 wt%, more preferably 55 to 62 wt%, based on the total weight of the MMCP.

[0060] The total amount of 1-butene, based on the multimodal polymer (MMCP), is preferably in the range of 0.1 to 1.0 mol%, more preferably 0.2 to 0.8 mol%, more preferably 0.3 to 0.7 mol%.

[0061] The total amount of 1-hexene, based on the multimodal polymer (MMCP), is preferably in the range of 1.5 to 8.0 mol%, more preferably 2.0 to 6.0 mol%, even more preferably 2.2 to 4.0 mol%.

[0062] The total amount of 1-butene present in the ethylene-1-butene polymer component (A) is 0.1 to 3.0 mol%, preferably 0.3 to 2.6 mol%, more preferably 0.5 to 2.0 mol%, even more preferably 0.6 to 1.8 mol%, based on the ethylene-1-butene polymer component (A).

[0063] The total amount (mol%) of 1-hexene present in the ethylene-1-hexene polymer component (B) is 1.5 to 10.0 mol%, preferably 3.0 to 8.0 mol%, more preferably 3.5 to 7.0 mol%, based on the ethylene-1-hexene polymer component (B).

[0064] Even more preferably, the multimodal polymer (MMCP) of the present invention is further multimodal with respect to the density difference between ethylene polymer component (A) and ethylene polymer component (B). Preferably, the density of ethylene polymer component (A) is different from, preferably higher than, the density of ethylene polymer component (B).

[0065] The density of the ethylene polymer component (A) is 920 to 960 kg / m 3 , preferably 925 to 955 kg / m 3 , more preferably 930 to 950 kg / m 3 and / or the density of the ethylene polymer component (B) is in the range of 880 to 920 kg / m 3 , preferably 885 to 915 kg / m 3 And more preferably 890 to 910 kg / m 3 within the range.

[0066] The density of the polymer part (A-1) and / or (A-2) is 925 to 960 kg / m 3 , preferably 925 to 955 kg / m 3 , more preferably 930 to 950 kg / m 3 within the range.

[0067] The densities of the polymer parts (A-1) and (A-2) may be the same as or may be different from each other.

[0068] The metallocene-catalyzed multimodal copolymer (MMCP) is preferably a linear low density polyethylene (LLDPE) which has a well-known meaning.

[0069] The density of the multimodal copolymer (MMCP) is between 910 and 930 kg / m 3 , choose 912.0 to 925kg / m 3 , more preferably 913.0 to 918.0 kg / m 3 within the range.

[0070] More preferably, the multimodal copolymer (MMCP) is multimodal (i.e. there is a difference between them) at least with respect to MFR2, the comonomer content and the density of the ethylene polymer components (A) and (B) is multimodal (i.e. there is a difference between them), as defined above, below or in the claims, the claims including any preferred ranges or embodiments of the polymer composition.

[0071] Furthermore, the multimodal copolymer (MMCP) may also have a molecular weight distribution (Mw / Mn) determined by GPC in the range of at least 3.5 to at most 7.2, preferably in the range of 4.0 to 7.0, more preferably in the range of 4.5 to 6.8.

[0072] Furthermore, the multimodal copolymer (MMCP) has a ratio of the soluble fraction at 35°C determined by cross fractionation chromatography (CFC) as described in the experimental part to the density of the multimodal polyethylene copolymer (MMCP), SF@35°C / density, of less than 0.007, preferably less than 0.006, more preferably less than 0.005, e.g. in the range of 0.001 to less than 0.007, preferably 0.001 to less than 0.006, more preferably 0.001 to less than 0.005 or less than 0.050. MMCP .

[0073] The amount of the soluble fraction at 35°C is in the range of 0.5 to 6.0 wt%, preferably 0.8 to 5.0 wt%, more preferably 1.0 to 4.0 wt% or 39 to 43 wt%, based on the total multimodal polyethylene copolymer (MMCP).

[0074] In one embodiment of the invention the multimodal polyethylene copolymer (MMCP) is further characterised in that the ratio of the molecular weight (Mw) of the low crystalline fraction (LCF) to the molecular weight (Mw) of the high crystalline fraction (HCF) Mw(Tp(LCF) / Mw(Tp(HCF) determined as described in the experimental part is in the range of >1.0 to 10.0, preferably in the range of 2.0 to 8.0, more preferably in the range of 2.2 to 6.0, and / or

[0075] The ratio of width at half height (LCF) / (98-Tp(LCF)) is in the range of 0.10 to 1.50, preferably in the range of 0.15 to 1.2, more preferably in the range of 0.20 to 1.0, and / or the difference of Mw(LCF)-Mw(HCF) is at least 5000 to at most 200000 g / mol, preferably 50000 to 180000 g / mol, more preferably 80000 to 150000 g / mol or 5000 to 7000 g / mol.

[0076] Within the scope of the present invention, the first and second ethylene polymer parts (A-1 and A-2) of the ethylene polymer component (A) are present in a weight ratio of 4:1 to 1:4, such as 3:1 to 1:3, or 2:1 to 1:2, or 1:1.

[0077] The ethylene polymer component (A) is present in an amount of 35.0 to 50.0 wt%, preferably in an amount of 36.0 to 48.0 wt%, even more preferably in an amount of 38.0 to 45.0 wt%, based on the multimodal copolymer (MMCP).

[0078] Accordingly, the ethylene polymer component (B) is present in an amount of 50.0 to 65.0 wt%, preferably in an amount of 52.0 to 64.0 wt%, more preferably in an amount of 55.0 to 62.0 wt%, based on the multimodal copolymer (MMCP).

[0079] The metallocene-catalyzed multimodal copolymer (MMCP) can be produced in a two-stage process, which preferably comprises a slurry reactor (loop reactor), wherein the slurry (loop) reactor is connected in series with a gas phase reactor (GPR), whereby ethylene polymer component (A) is produced in the loop reactor and ethylene polymer component (B) is produced in the GPR in the presence of ethylene polymer component (A) to produce the multimodal copolymer (MMCP).

[0080] In case the ethylene component (A) of the multimodal copolymer (MMCP) consists of ethylene polymer fractions (A-1) and (A-2), the multimodal copolymer (MMCP) may be produced in a three-stage process, which preferably comprises a first slurry reactor (loop reactor 1), wherein the first slurry loop reactor is connected in series to a further slurry reactor (loop reactor 2) such that the first ethylene polymer fraction (A-1) produced in the loop reactor 1 is fed to the loop reactor 2, where the second ethylene polymer fraction (A-2) is produced in the presence of the first fraction (A-1). Thus, the loop reactor 2 is connected in series to a gas phase reactor (GPR) such that the first ethylene polymer fraction (A) leaving the second slurry reactor is fed to the GPR, to produce a trimodal polyethylene copolymer. In this case, the reaction conditions in the two slurry reactors are selected such that products different in MFR and / or density are produced in the two slurry reactors.

[0081] Such processes are described in particular in WO 2016 / 198273 A1, WO 2021 / 009189 A1, WO 2021 / 009190 A1, WO 2021 / 009191 A1 and WO 2021 / 009192. Full details of how to prepare suitable metallocene-catalyzed multimodal copolymers (MMCPs) can be found in these references.

[0082] Metallocene-catalyzed multimodal copolymers (MMCPs) are produced by using a metallocene catalyst. The metallocene catalyst preferably comprises a metallocene complex and a cocatalyst. The metallocene compound or complex is also referred to herein as an organometallic compound (C).

[0083] The organometallic compound (C) comprises a transition metal (M) from Groups 3 to 10 of the Periodic Table of Elements (IUPAC 2007) or from the actinides or lanthanides.

[0084] According to the present invention, the term "organometallic compound (C)" includes any metallocene or non-metallocene compound of a transition metal, which carries at least one organic (coordinating) ligand and exhibits catalytic activity alone or together with a cocatalyst. Transition metal compounds are well known in the art, and the present invention encompasses compounds of metals from Groups 3 to 10, e.g. Groups 3 to 7, or Groups 3 to 6, e.g. Groups 4 to 6, of the Periodic Table (IUPAC 2007), as well as lanthanides or actinides.

[0085] In one embodiment, the organometallic compound (C) has the following formula (I):

[0086]

[0087] Wherein each X is independently a halogen atom, C 1-6 -alkyl, C 1-6 - alkoxy, phenyl or benzyl;

[0088] Each Het is independently a monocyclic heteroaromatic group containing at least one heteroatom selected from O or S;

[0089] L is -R'2Si-, wherein each R' is independently a C substituted with an alkoxy group having 1 to 10 carbon atoms. 1-20 -Hydrocarbon or C 1-10 -alkyl;

[0090] M is Ti, Zr or Hf;

[0091] Each R 1 Same or different, is C 1-6 -alkyl or C 1-6 - alkoxy;

[0092] Each n is 1 to 2;

[0093] Each R 2 Same or different, is C 1-6 -alkyl, C 1-6 -alkoxy or -Si(R)3 group;

[0094] Each R is optionally replaced by 1 to 3 C 1-6-alkyl substituted C 1-10 -alkyl or phenyl; and each p is 0 to 1.

[0095] Preferably, the compound of formula (I) has the structure

[0096]

[0097] Wherein each X is independently a halogen atom, C 1-6 -alkyl, C 1-6 -alkoxy, phenyl or benzyl; L is Me2Si-;

[0098] Each R 1 Same or different and C 1-6 - alkyl, for example methyl or tert-butyl;

[0099] Each n is 1 to 2;

[0100] R 2 is -Si(R)3alkyl; each p is 1;

[0101] Each R is C 1-6 -alkyl or phenyl.

[0102] Highly preferred complexes of formula (I) are

[0103]

[0104] Most preferably, the complex dimethylsilanediylbis[2-(5-trimethylsilylfuran-2-yl)-4,5-dimethylcyclopentadien-1-yl]zirconium dichloride is used.

[0105] More preferably, the ethylene polymer components (A) and (B) of the multimodal copolymer (MMCP) are prepared using, ie in the presence of, the same metallocene catalyst.

[0106] To form the catalyst, a cocatalyst, also called an activator, well known in the art is used. Cocatalysts containing Al or B are well known and can be used here. Preferably, an aluminoxane (such as MAO) or a boron-based cocatalyst (such as a borate) is used.

[0107] In contrast to Ziegler Natta catalysis, polyethylene copolymers produced using single-site catalysis have characteristics that distinguish them from Ziegler Natta materials. In particular, the comonomer distribution is more uniform. This can be shown using TREF or Crystaf techniques. Catalyst residues can also indicate the catalyst used. Ziegler Natta catalysts do not contain group (IV) metals such as Zr or Hf.

[0108] Multilayer film

[0109] A preferred embodiment of the multilayer film according to the invention provides that the thickness of the skin layer (SKL) of the multilayer film is in the range of 1 to 100 μm; preferably in the range of 5 to 80 μm, more preferably in the range of 10 to 15 μm.

[0110] According to another preferred embodiment of the present invention, the thickness of the core layer (CL) of the multilayer film is in the range of 10 to 200 μm; preferably in the range of 20 to 80 μm, more preferably in the range of 30 to 45 μm.

[0111] In another preferred embodiment according to the present invention, the thickness of the sealing layer (SL) of the multilayer film is in the range of 1 to 50 μm; preferably in the range of 5 to 25 μm, more preferably in the range of 10 to 15 μm.

[0112] In another preferred embodiment according to the present invention, the thickness of the multilayer film is in the range of 12 to 350 μm; preferably in the range of 40 to 150 μm, more preferably in the range of 50 to 70 μm.

[0113] According to another preferred embodiment of the present invention, the multilayer film consists of a skin layer (SKL), a core layer (CL) and a sealing layer (SL). It goes without saying that the core layer (CL) is located between the skin layer (SKL) and the sealing layer (SL).

[0114] The core layer (CL) comprises at least a metallocene-catalyzed multimodal polyethylene copolymer (MMCP) and a mixed plastic-polyethylene recycled blend having an MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 30.0 g / 10 min and a 3 Density within the range (ASTM D792).

[0115] In a preferred embodiment, the core layer (CL) comprises 10 to 35 wt%, preferably 15 to 30 wt%, more preferably 18 to 25 wt%, based on the total weight of the core layer (CL), of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP), the MMCP preferably having a molecular weight in the range of 912 to 925 kg / m 3 , preferably 913 to 918 kg / m 3 Density in the range of 1.5 to 2.0 g / 10 min (ASTM D792) and MFR2 in the range of 0.5 to 1.4 g / 10 min (190°C, 2.16 kg, ISO 1133), and

[0116] 50 to 90 wt%, preferably 55 to 85 wt%, more preferably 68 to 82 wt%, based on the total weight of the core layer (CL), of a mixed plastic-polyethylene recycled blend, the blend having an MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 1.2 g / 10min, preferably 0.3 to 1.1 g / 10min and a MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 910 to 945 kg / m 3 , preferably 915 to 930 kg / m 3 , most preferably 920 to 927 kg / m 3 Density within the range (ASTM D792).

[0117] The core layer (CL) may further comprise 0 to 15 wt%, more preferably 0 to 12 wt%, still more preferably 8 to 12 wt%, based on the total weight of the core layer (CL) of a Ziegler-Natta catalyzed linear low density polyethylene, preferably a multimodal α-olefin terpolymer, preferably having a molecular weight in the range of 920 to 970 kg / m 3 , more preferably 935 to 950 kg / m 3 The core layer (CL) is a polyethylene having a density in the range of 0.1 to 2.5 g / 10 min, preferably a MFR2 in the range of 1.0 to 1.8 g / 10 min (190° C., 2.16 kg, ISO 1133); and / or 0 to 15 wt %, more preferably 0 to 12 wt %, more preferably 6 to 10 wt % of a high density polyethylene based on the total weight of the core layer (CL), the high density polyethylene being preferably bimodal and having a density in the range of 950 to 975 kg / m 3 , more preferably 955 to 965 kg / m 3 The density (ASTM D792) is in the range of 0.1 to 1.5 g / 10 min, preferably in the range of 0.5 to 1.0 g / 10 min.

[0118] The skin layer (SKL) preferably comprises 65 to 95 wt%, 80 to 95 wt%, more preferably 82 to 93 wt%, still more preferably 88 to 92 wt% of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP), preferably having a molecular weight in the range of 912 to 925 kg / m 3 , more preferably 913 to 918 kg / m 3 The invention relates to a surface layer (SKL) having a density in the range of 910 to 930 kg / m3 , preferably 920 to 925 kg / m 3 The density (ASTM D792) is in the range of 0.5 to 4 g / 10 min, preferably in the range of 0.7 to 2 g / 10 min.

[0119] The sealing layer (SL) preferably comprises 0 to 90 wt%, or 50 to 90 wt%, preferably 70 to 85 wt%, based on the total weight of the sealing layer (SL), of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP), preferably having a molecular weight of 912 to 925 kg / m 3 , more preferably 913 to 918 kg / m 3 The present invention relates to a sealing layer (SL) having a density in the range of 0.5 to 1.4 g / 10 min (ASTM D792) and an MFR2 in the range of 0.5 to 1.4 g / 10 min (190° C., 2.16 kg, ISO 1133); and 0 to 80 wt%, or 10 to 70 wt%, preferably 15 to 25 wt% of a plastomer based on the total weight of the sealing layer (SL), the plastomer being preferably a copolymer of ethylene and 1-octene, preferably having a molecular weight of 860 to 910 kg / m 3 , preferably 895 to 905 kg / m 3 and a density (ASTM D792) in the range of 0.5 to 10 g / 10 min, preferably 1.0 to 1.5 g / 10 min and an MFR2 (190° C., 2.16 kg, ISO 1133) in the range of 0.5 to 10 g / 10 min, preferably 1.0 to 1.5 g / 10 min; and 0 to 50 wt%, preferably 35 to 45 wt%, based on the total weight of the sealing layer (SL), of a multimodal metallocene-catalyzed linear low density polyethylene, which is preferably a bimodal ethylene / 1-butene / 1-hexene terpolymer, preferably having a molecular weight in the range of 910 to 930 kg / m 3 , more preferably 916 to 925 kg / m 3 The invention relates to a polymer having a density in the range of 0.1 to 0.2 g / 10 min (ASTM D792) and an MFR2 in the range of 0.5 to 2 g / 10 min (190°C, 2.16 kg, ISO 1133).

[0120] According to another preferred embodiment of the invention it is provided that the skin layer (SKL), the core layer (CL) and the sealing layer (SL) comprise a metallocene-catalyzed multimodal polyethylene copolymer (MMCP).

[0121] The polymers used in the multilayer films according to the invention may contain additives and fillers in amounts which are customary in the field of film applications. Examples of such additives are, inter alia, antioxidants, processing stabilizers, UV stabilizers, pigments, fillers, antistatic additives, antiblocking agents, nucleating agents, acid scavengers and polymer processing aids (PPAs).

[0122] It should be understood herein that any additive and / or filler may optionally be added in the form of a so-called masterbatch comprising the respective additive(s) and a carrier polymer. In this case, the carrier polymer is not calculated in the polymer component of the metallocene-catalyzed multimodal polyethylene copolymer (MMCP), but in the amount of the respective additive, based on the total amount (100 wt%) of the polymer composition.

[0123] According to another preferred embodiment of the present invention, the multilayer film has an MD tensile modulus (ISO 527-3) in the range of 150 to 300 MPa, preferably in the range of 190 to 240 MPa; and / or a TD tensile modulus (ISO 527-3) in the range of 150 to 400 MPa, preferably in the range of 200 to 300 MPa and / or a dart drop strength (ISO 7765-1) in the range of 230 to 800 g, preferably in the range of 350 to 600 g.

[0124] In another preferred embodiment according to the present invention, the multilayer film has a haze (ASTM D1003-00) in the range of 5% to 15%, preferably in the range of 8% to 13%; and / or a seal initiation temperature determined as described in the description in the range of 60 to 70°C or 78 to 85°C, preferably in the range of 63 to 68°C or 79 to 81°C; and / or a hot tack force determined as described in the description in the range of 6.0 to 8.0N or 5.2 to 5.8N, preferably in the range of 6.2 to 7.5N or 5.4 to 5.6N; and / or a hot tack temperature determined as described in the description in the range of 60 to 90°C, preferably in the range of 63 to 86°C.

[0125] According to a further preferred embodiment of the invention, it is provided that the multilayer film consists of a polyethylene-based polymer.

[0126] method

[0127] Another aspect of the present invention relates to a method of producing a multilayer film.

[0128] The multilayer films according to the invention are generally produced by conventional processes in which the layers of the film are coextruded.

[0129] The different polymer components in any layer of the film are usually intimately mixed before the layer is formed, for example using a twin screw extruder, preferably a counter-rotating extruder or a co-rotating extruder. The blend is then converted into a coextruded film.

[0130] Generally, the multilayer film according to the invention can be produced by a blown film or cast film process, preferably by a blown film process.

[0131] To make such films, at least three polymer melt streams are simultaneously extruded (ie, coextruded) through, for example, a multi-channel tubular, annular or circular die to form a tube which is inflated, expanded and / or cooled with air to form the film. The manufacture of blown films is a well-known process.

[0132] Blown (co)extrusion may be carried out at a temperature of 150 to 230°C, more preferably 160 to 225°C, and cooled by blowing gas (typically air) at a temperature of 10 to 40°C, more preferably 12 to 16°C, to provide a frost line height of 0.5 to 4 times, more preferably 1 to 2 times, the die diameter.

[0133] The blow up ratio (BUR) should generally be in the range of 1.5 to 3.5, preferably 2.0 to 3.0, more preferably 2.1 to 2.8.

[0134] use

[0135] Another aspect of the present invention relates to the use of the multilayer film as packaging material, preferably for food and / or medical products.

[0136] The invention will now be described with reference to the following non-limiting examples.

[0137] Experimental Section

[0138] A. Test Method

[0139] Unless otherwise defined, the following definitions of terms and determination methods apply to the above general description of the invention as well as to the following examples.

[0140] Melt flow rate:

[0141] The melt flow rate (MFR) is determined according to ISO 1133 - Thermoplastics - Determination of melt mass-flow rate (MFR) and melt volume-flow rate (MVR) - Part 1: Standard method and is expressed in g / 10 min. The MFR is an indication of the flowability of the polymer and therefore of its processability. The higher the melt flow rate, the lower the viscosity of the polymer. The MFR of polyethylene is determined at 190°C. The MFR can be determined at different loads, for example 2.16 kg (MFR2), 5 kg (MFR5) or 21.6 kg (MFR 21 ).

[0142] Calculation of MFR2 of component B and part (A-2)

[0143] logA=x·logB+(1-x)·logC

[0144]

[0145] For component B:

[0146] B = MFR2 of component (A)

[0147] C = MFR2 of component (B)

[0148] A = Final MFR2 of the multimodal polyethylene copolymer (P) (blend)

[0149] X = weight fraction of component (A)

[0150] For part (A-2):

[0151] B = MFR2 of the first part (A-1)

[0152] C = MFR2 of the second part (A-2)

[0153] A = Final MFR2 of cyclic polymer (= component (A)) (mixture)

[0154] X = weight fraction of the first part (A-1).

[0155] density

[0156] The density of the polymer is measured in kg / m according to ASTM; D792, method B (density at 23°C by balance) on compression molded specimens prepared according to EN ISO 1872-2. 3 .

[0157] DSC analysis, melting temperature (T m ) and crystallization temperature (T c )

[0158] Data can be measured with a TA Instruments Q2000 Differential Scanning Calorimetry (DSC) on 5 to 7 mg samples.DSC is run according to ISO 11357 / Part 3 / Method C2 in the temperature range of -30 to +225°C with a scan rate of 10°C / min in a hot / cold / hot cycle.

[0159] Crystallization temperature (T c ) and crystallization enthalpy (H c ) is determined by the cooling step, while the melting temperature (T m ) and melting enthalpy (H m ) is determined by the second heating step.

[0160] Dart Drop Intensity (DDI): Determination of impact resistance by free falling dart method

[0161] DDI was measured according to ISO 7765-1:1988 / Method A on films produced as shown below. This test method covers the determination of the energy that will cause film failure under specified conditions of impact by a dart falling freely from a specified height, which will cause 50% of the test specimens to fail (Step Method A). A uniform increment of the missile mass was used during the test, and after each specimen test, the missile weight was reduced or increased by a uniform increment depending on the observed result (failure or no failure) of the specimen.

[0162] Standard conditions:

[0163] Adjustment time: >96h

[0164] Test temperature: 23℃

[0165] Dart head material: phenolic resin

[0166] Dart diameter: 38mm

[0167] Drop height: 660mm

[0168] result:

[0169] Impact failure weight - 50% [g]

[0170] Tensile modulus (TM)

[0171] The tensile modulus (MPa) of film samples prepared as described below was measured in the machine direction (MD) and / or transverse direction (TD) according to ISO 527-3 with a crosshead speed of 1 mm / min.

[0172] Haze

[0173] The haze was measured according to ASTM D1003-00 on the films produced as shown below.

[0174] Sealing start temperature (SIT); Sealing end temperature (SET), Sealing range

[0175] This method determines the sealing temperature range (sealing range) of polyethylene films, in particular blown films or cast films. The sealing temperature range is the temperature range over which the film can be sealed according to the conditions given below.

[0176] The lower limit (heat seal initiation temperature (SIT)) is the sealing temperature at which a seal strength of ≥ 5 N is achieved. The upper limit (seal end temperature (SET)) is reached when the film sticks to the sealing device.

[0177] The measurements were performed according to a slightly modified ASTM F1921-12, where the test parameters sealing pressure, delay time and gripper separation rate were modified. The force / temperature curve was continued until thermal failure of the membrane.

[0178] The sealing range was determined on a J&B Universal Sealer Model 4000 on films produced as shown below, using the following additional parameters:

[0179] Adjustment time: >96h

[0180] Sample width: 25mm

[0181] Sealing pressure: 0.4N / mm 2 (PE)

[0182] Sealing time: 1 second

[0183] Delay time: 30 seconds

[0184] Sealing jaws size: 50x5 mm

[0185] Sealing jaws shape: flat

[0186] Sealing jaw coating: Niptef

[0187] Sealing temperature: ambient temperature -240℃

[0188] Sealing temperature interval: 5°C

[0189] Starting temperature: 50℃

[0190] Grip separation rate: 42 mm / sec

[0191] Hot Tack Temperature (HTT) and Hot Tack Force (HTF)

[0192] HTT (lowest temperature to obtain maximum hot tack) and HTF (maximum hot tack) were measured according to ASTM F 1921 Method B on films produced as shown below with a thickness of 60 μm (three-layer blown film) with the following settings:

[0193] Q-name Instrument: Hot Tack-Seal Tester

[0194] Model: J&B 4000MB

[0195] Sealing strip length: 50[mm]

[0196] Sealing strip width: 5[mm]

[0197] Sealing strip shape: flat

[0198] Sealing pressure: 0.15N / mm 2

[0199] Sealing time: 1s

[0200] Sealing strip coating:

[0201] Roughness of coated seal strip 1[μm]

[0202] Film sample width: 25mm

[0203] Cooling time: 0.2s

[0204] Peeling speed: 200mm / s

[0205] Starting temperature: 50℃

[0206] End temperature: burn-through and / or shrinkage

[0207] Increment: 5℃

[0208] All film samples were prepared in a standard atmosphere for conditioning and testing at 23°C (±2°C) and 50% (±10%) relative humidity. The minimum conditioning time for the samples in the standard atmosphere before testing was at least 40 hours. The minimum standing time between extrusion of the film samples and the start of testing was at least 88 hours. The hot tack measurement determines the strength of the heat seal formed in the film and is performed immediately after the seal is completed and before it cools to ambient temperature.

[0209] The HTF is measured as a function of temperature within a temperature range and with temperature increments as described above. The number of test specimens per temperature is at least 3. The HTF is evaluated as the maximum force (maximum peak value) at failure mode "peeling".

[0210] Gel content

[0211] The gel content was measured using a gel counting device consisting of a measuring extruder ME 25 / 5200 V1, 25 * 25D, adapter and slit die (opening 0.5 * 150mm), the extruder has five temperature adjustment zones, adjusted to a temperature distribution of 170 / 180 / 190 / 190 / 190°C. Connected to it is a cooling roll unit (diameter 13cm, temperature set to 50°C), a line camera (CCD 4096 pixels, for dynamic digital processing of grayscale images) and a winding unit. For gel count content measurement, the material is extruded at a screw speed of 30 revolutions per minute, a drawing speed of 3-3.5m / min and a cooling roll temperature of 50°C to prepare a thin cast film with a thickness of 70μm and a width of about 110mm.

[0212] The resolution of the camera on the membrane was 25 μm x 25 μm. The camera was operated in transmission mode with constant gray value (automatically set margin level = 170). The system is able to decide between 256 gray values ​​from black = 0 to white = 256. For detection of gels, a sensitivity level dark of 25% was used.

[0213] For each material, a line scan camera is used to check the 2 The average number of gel spots on the membrane surface area. The line scan camera is set to distinguish the size of the gel spots according to the following:

[0214] Gel size (size of the longest dimension of the gel)

[0215] 300μm to 599μm

[0216] 600μm to 999μm

[0217] Above 1000μm

[0218] Dynamic shear measurement (frequency sweep measurement)

[0219] The characterization of the polymer composition or the melt of the polymer by dynamic shear measurement as described above or below complies with ISO standards 6721-1 and 6721-10 and is carried out as described on pages 15 to 17 of WO 2021 / 105299 A1.

[0220] Strain Hardening (SH) Modulus

[0221] The strain hardening modulus was determined as described in WO 2021 / 233818 A1, pages 36 to 38.

[0222] Comonomer content - quantification of microstructure by NMR spectroscopy

[0223] Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the comonomer content of the polymers.

[0224] A Bruker Avance III 400 MHz NMR spectrometer was used to analyze the 1 H and 13 C was operated at 500.13 and 125.76 MHz and quantitative data were recorded in the molten state. 13 C{ 1 H}NMR spectra. All spectra were obtained using 13The spectra were recorded at 150 °C using a C-optimized 7 mm magic angle spinning (MAS) probe head with nitrogen used for all pneumatics. Approximately 200 mg of material was loaded into a 7 mm outer diameter zirconium oxide MAS rotor and spun at 4 kHz. This setup was chosen primarily for the high sensitivity required for rapid identification and accurate quantification {klimke06, parkinson07, castignolles09}. Standard single pulse excitation was used, utilizing NOE {pollard04, klimke06} with a short recycle delay of 3 s and an RS-HEPT decoupling scheme {fillip05, griffin07}. A total of 1024 (1k) transients were acquired for each spectrum.

[0225] Quantitative 13 C{ 1 H} NMR spectra were processed, integrated, and the relevant quantitative properties were determined from the integration. All chemical shifts were internally referenced to the bulk methylene signal (δ+) at 30.00 ppm.

[0226] The amount of ethylene is quantified using the integration of the methylene (δ+) sites at 30.00 ppm and taking into account the number of reported sites per monomer:

[0227] E=I δ+ / 2

[0228] Correction for the presence of isolated comonomer units is based on the number of isolated comonomer units present:

[0229] E total = E + (3 * B+2 * H) / 2

[0230] where B and H are defined for their respective comonomers. Corrections are made in a similar manner when there is continuous and discontinuous comonomer incorporation.

[0231] Characteristic signals corresponding to the incorporation of 1-butene were observed and the comonomer fraction was calculated as the fraction of 1-butene in the polymer relative to all monomers in the polymer:

[0232] fB total = B total / (E total + B total + H total)

[0233] The amount of isolated 1-butene incorporated into the EEBEE sequence was quantified using the integration of the *B2 site at 39.8 ppm and taking into account the number of reporter sites per comonomer:

[0234] B=I *B2

[0235] If present, the amount of continuously incorporated 1-butene in the EEBBEE sequence was quantified using the integration of the ααB2B2 site at 39.4 ppm and taking into account the number of reported sites for each comonomer:

[0236] BB=2 * IααB2B2

[0237] If present, the amount of non-reporting sites per comonomer:

[0238] HEH=2 * IββB4B4

[0239] No HHH sequence was observed. The total 1-hexene content was calculated based on the sum of isolated, continuous and discontinuously incorporated 1-hexene:

[0240] Total H = H + HH + HEH

[0241] The total mole fraction of 1-hexene in the polymer was then calculated as:

[0242] fH=H total / (E total+B total+H total)

[0243] The mole percentage of comonomer incorporation is calculated from the mole fraction:

[0244] B [mol%] = 100 * f

[0245] H [mol%] = 100 * f

[0246] The weight percent of comonomer incorporation is calculated from the mole fraction:

[0247] B [wt%] = 100 * (fB * 56.11) / ((fB * 56.11)+(fH * 84.16)+((1-(fB+fH)) * 28.05))

[0248] H [wt%] = 100 * (fH * 84.16) / ((fB * 56.11)+(fH * 84.16)+((1-(fB+fH)) * 28.05))

[0249] References:

[0250] Klimke,K.,Parkinson,M.,Piel,C.,Kaminsky,W.,Spiess,H.W.,Wilhelm,M.,Macromol.Chem.Phys.2006;207:382.

[0251] Parkinson,M.,Klimke,K.,Spiess,H.W.,Wilhelm,M.,Macromol.Chem.Phys.2007;208:2128.

[0252] Pollard,M.,Klimke,K.,Graf,R.,Spiess,H.W.,Wilhelm,M.,Sperber,O.,Piel,C.,Kaminsky,W.,Macromolecules 2004;37:813.

[0253] Filip,X.,Tripon,C.,Filip,C.,J.Mag.Resn.2005,176,239.

[0254] Griffin,J.M.,Tripon,C.,Samoson,A.,Filip,C.,and Brown,S.P.,Mag.Res.inChem.2007 45,S1,S198.

[0255] Castignolles,P.,Graf,R.,Parkinson,M.,Wilhelm,M.,Gaborieau,M.,Polymer50(2009)2373.

[0256] Busico,V.,Cipullo,R.,Prog.Polym.Sci.26(2001)443.

[0257] Busico,V.,Cipullo,R.,Monaco,G.,Vacatello,M.,Segre,A.L.,Macromoleucles30(1997)6251.

[0258] Zhou,Z.,Kuemmerle,R.,Qiu,X.,Redwine,D.,Cong,R.,Taha,A.,Baugh,D.Winniford,B.,J.Mag.Reson.187(2007)225.

[0259] Busico,V.,Carbonniere,P.,Cipullo,R.,Pellecchia,R.,Severn,J.,Talarico,G.,Macromol.Rapid Commun.2007,28,1128.

[0260] Resconi,L.,Cavallo,L.,Fait,A.,Pimontesi,F.,Chem.Rev.2000,100,1253.

[0261] Molecular weight, molecular weight distribution (M n 、M w , MWD)

[0262] The average molecular weight (M z 、M w and M n ), molecular weight distribution (MWD) and its breadth described by the polydispersity index PDI = Mw / Mn (where Mn is the number average molecular weight and Mw is the weight average molecular weight) are calculated by gel permeation chromatography (GPC) according to ASTM D 6474-12 using the following formula:

[0263]

[0264] For a constant elution volume interval ΔV i , where A i and M i and elution volume V i The associated chromatographic peak slice area and the polyolefin molecular weight (MW), where N equals the number of data points obtained from the chromatogram between the integration limits.

[0265] A high temperature GPC instrument equipped with an infrared (IR) detector (IR4 or IR5 from PolymerChar (Valencia, Spain)) or a differential refractometer (RI) from Agilent Technologies, equipped with 3x Agilent-PLgel Olexis and 1x Agilent-PLgel Olexis Guard columns was used. 1,2,4-Trichlorobenzene (TCB) stabilized with 250 mg / L 2,6-di-tert-butyl-4-methylphenol was used as solvent and mobile phase. The chromatographic system was operated at 160°C with a constant flow rate of 1 mL / min. 200 μL of sample solution was injected for each analysis. Data collection was performed using Agilent Cirrus software version 3.3 or PolymerChar GPC-IR control software.

[0266] The column set was calibrated using universal calibration with 19 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11500 kg / mol. The PS standards were dissolved at room temperature for several hours. The conversion of polystyrene peak molecular weight to polyolefin molecular weight was accomplished by using the Mark Houwink equation and the following Mark Houwink constants:

[0267] K PS =19x 10 -3 mL / g, α PS =0.655

[0268] K PE =39x 10 -3 mL / g, α PE =0.725

[0269] A third-order polynomial fit was used to fit the calibration data.

[0270] For PE, all samples were prepared in the concentration range of 0.5–1 mg / ml and dissolved at 160 °C for 3 h with continuous gentle shaking.

[0271] Determination of chemical heterogeneity by cross fractionation chromatography (CFC)

[0272] The chemical composition distribution at a certain elution temperature (polymer crystallinity in solution) as well as the molecular weight distribution and the corresponding molecular weight average values ​​(Mn, Mw and Mv) are determined by the fully automated cross-fractionation chromatography (CFC) method described in Ortin A., Monrabal B., Sancho-Tello J., Macromol. Symp., 2007, 257, 13-28 and WO 2018 / 210893 A1 on pages 18 and 19.

[0273] Soluble part SF@35℃

[0274] The soluble fraction SF@35°C is the polymer fraction eluted at 35°C.

[0275] Mw(Tp(LCF, Mw(Tp(HCF), half peak width Tp(LCF), half peak width Tp(HCF)

[0276] In order to determine the weight average molecular weight at the maximum peak of the low crystalline part (Mw(Tp(LCF)) or the weight average molecular weight at the maximum peak of the high crystalline part (Mw(Tp(HCF)) and the half peak widths of Tp(LCF) and Tp(HCF) in the first step, an a-TREF curve is obtained from the above CFC analysis,

[0277] The peak maximum of the high crystalline fraction (HCF) peak (Tp(HCF)) and the peak maximum of the low crystalline fraction (LCF) peak (Tp(LCF)) are determined from the a-TREF curve. The elution temperature of Tp(HCF) is higher than that of Tp(LCF), but lower than 99°C. Typically, the high crystalline fraction is in the range of 90°C to 99°C, and the low crystalline fraction is the polymer fraction eluted from 35°C to 90°C. In Figure 1 of WO2018 / 210893, the a-TREF obtained from CFC analysis of IE1 and CE1 is shown.

[0278] The half-peak width of HCF and LCF is defined as the elution temperature difference between the front temperature and the back temperature at half the maximum peak height of Tp(LCF) or Tp(HCF), respectively. If the peaks are not well separated, the corresponding front temperature at half the maximum is taken from 35°C forward, while the back temperature at half the maximum is taken from 100°C backward. If LCF is well separated from HCF, the back temperature is taken after HCF.

[0279] In the next step, the Mw at the elution temperatures Tp(LCF) and Tp(HCF) is determined. Thus, the Mw at Tp(LCF) (Mw(Tp(LCD)) is calculated by linear interpolation between the Mw values ​​measured by GPC at elution temperatures above Tp(LCF) and below Tp(LCF). This is achieved by using the "TREND" function in Excel. The same procedure is performed to determine the Mw at Tp(HCF).

[0280] Based on the determined Mw(Tp(LCF), Mw(Tp(HCF), half-peak width(LCF), half-peak width(HCF) and Tp(LCF), the following parameters can be directly calculated:

[0281] -Mw(Tp(LCF) / Mw(Tp(HCF)

[0282] -Difference of Mw(TP(LCF))-Mw(TP(HCF) (g / mol) = Mw(TP(LCF)

[0283] -Mw(TP(HCF)[g / mol]

[0284] - Half peak width (LCF) / (98°C - Tp (LCF)).

[0285] B. Materials used

[0286] FB5600 is a type of FB5600 purchased bimodal high-density polyethylene (MFR2 (190℃ / 2.16kg): 0.70g / 10min, density: 960kg / m 3 , Tm 132℃).

[0287] FT5236 is a low density polyethylene (MFR2 (190°C / 2.16kg): 0.75g / 10min, density: 923kg / m 3 , Tm 112°C, produced by Tubular Technology) and contains anti-blocking agents, antioxidants and slip additives. FK1820 is a product available from Borouge as Anteo TM FK1820 commercially available bimodal ethylene / 1-butene / 1-hexene terpolymer (MFR2 (190°C / 2.16kg): 1.5g / 10min, density: 931kg / m 3 , T m 122°C, produced with a metallocene catalyst) and contains antioxidants and processing aids.

[0288] Queo0201 is a product available from Borealis AG as Queo TM 0201 Single-modal vinyl 1-octene plastomer (MFR2 (190°C / 2.16kg): 1.1g / 10min, density: 902kg / m 3 , T m 97°C, produced in a solution polymerization process using a metallocene catalyst) and containing a processing stabilizer.

[0289] NAV 101 is a low density polyethylene (LDPE) post-consumer recyclate blend available from Ecoplast Kunststoffrecycling GmbH. The properties of NAV 101 are shown in Table 1.

[0290] Table 1: Characteristics of NAV 101.

[0291] Ethylene content) wt% 90.67 Isolated C3 content wt% 0 C4 content wt% 2.23 C6 content wt% 2.73 C7 content wt% 0.48 iPP content wt% 3.89 LDPE content wt% 33.00 density <![CDATA[kg / m 3 ]]> 923.9 <![CDATA[MFR2]]> g / 10min 1.02 <![CDATA[MFR5]]> g / 10min 3.57 <![CDATA[MFR 21 ]]> g / 10min 41.56 SHI2.7 / 210 22.16 eta0.05 Pa·s 16187 eta300 Pa·s 618 PI <![CDATA[s -1 ]]> 1.46 SH modulus MPa 14.3 Gel content (>1000μm) <![CDATA[1 / m 2 ]]> 16.9 Gel content (600-1000μm) <![CDATA[1 / m 2 ]]> 175.1 Gel content (300-599 (μm)) <![CDATA[1 / m 2 ]]> 885.9 Tc ℃ 109 Tm1 ℃ 122 Tm2 ℃ 109 Hm1 J / g 125 Hm2 J / g 290

[0292] ZNCP is a multimodal α-olefin terpolymer (MFR5 (190℃ / 5kg): 1.5g / 10min, density: 941kg / m 3 , T m 128°C, produced with a Ziegler-Natta catalyst) and was produced as follows.

[0293] The polymerization was carried out in a Borstar pilot plant with a 3-reactor set-up (loop 1 - loop 2 - GPR) and a prepolymerization loop reactor according to the conditions given in Table 2. A solid polymerization catalyst component prepared as described in Example 1 of EP 1 378 528 A1 was introduced into the reactor together with a triethylaluminum cocatalyst such that the molar ratio Al / Ti was about 15.

[0294] Table 2: Polymerization conditions.

[0295] Prepolymerization reactor Temperature(℃) 70 Pressure(kPa) 5783 Split (wt%) 2 First loop reactor Temperature(℃) 95 Pressure(kPa) 5512 C2(mol%) 4.7 H2 / C2(mol / kmol) 306 MFR2(g / 10min) 195 Divided into (wt%) 18 Second loop reactor Temperature(℃) 95 Pressure(kPa) 5382 C2(mol%) 5.5 H2 / C2(mol / kmol) 563 Divided into (wt%) 26 <![CDATA[MFR2(g / 10min)]]> 390 Gas Phase Reactor Temperature(℃) 82 Pressure(kPa) 1988 C2(mol%) 13.1 H2 / C2(mol / kmol) 22.0 C4 / C2(mol / kmol) 94.4 C6 / C2(mol / kmol) 123.5 Divided into (wt%) 54

[0296] The polymer powder was mixed with 1200 ppm Irganox B561 (available from BASF SE) and 400 ppm calcium stearate under nitrogen atmosphere, and then compounded and extruded into pellets using a JSW CIMP90 twin-screw extruder under nitrogen atmosphere.

[0297] MMCP1, MMCP2 and MMCP3 are multimodal copolymers prepared as follows:

[0298] Catalyst preparation (CAT)

[0299] SiO2 loading:

[0300] 10 kg of silica (PQ Corporation ES757, calcined at 600°C) was added from a feed bucket and inerted in the reactor until the O2 level reached less than 2 ppm.

[0301] Preparation of MAO / tol / MC:

[0302] At 25°C (oil circulation temperature) and 95rpm stirring, a 30wt% MAO toluene solution (14.1kg) was added from a balance to another reactor, followed by toluene (4.0kg). After adding toluene, the stirring speed was increased from 95rpm to>200rpm, with a stirring time of 30 minutes. Metallocene racemic-dimethylsilanediylbis{2-(5-(trimethylsilyl)furan-2-yl)-4,5-dimethylcyclopentadiene-1-yl}zirconium dichloride 477g was added from a metal cylinder, followed by 4kg toluene rinse (total toluene was 8.0kg). The reactor stirring speed was changed to 95rpm for MC feeding, returned to 200rpm and continued for 3h reaction time. After the reaction time, the MAO / tol / MC solution was transferred to a feed container.

[0303] Preparation of catalyst:

[0304] The reactor temperature was set to 10°C (oil circulation temperature) and stirring was adjusted to 40 rpm during the addition of MAO / tol / MC. MAO / tol / MC solution (22.2 kg) was added over 205 minutes, followed by a stirring time of 60 minutes (oil circulation temperature was set to 25°C). After stirring, the "dry mix" was stabilized at 25°C (oil circulation temperature) for 12 hours with a stirring speed of 0 rpm. The reactor was rotated 20° (back and forth) and stirred several times per hour at a speed of 5 rpm.

[0305] After stabilization, the catalyst was dried at 60°C (oil circulation temperature) for 2 hours under a 2 kg / h nitrogen flow, followed by 13 hours under vacuum (same nitrogen flow rate, stirring at 5 rpm). The dried catalyst was sampled and the HC content was measured using a Sartorius moisture analyzer (model MA45) in a glove box using thermogravimetry. The target HC level was <2% (actual 1.3%).

[0306] polymerization:

[0307] The polymerization was carried out in a Borstar pilot plant with a 3-reactor set-up (Loop 1 - Loop 2 - GPR) and a prepolymerization loop reactor according to the conditions given in Table 3.

[0308] Table 3: Polymerization conditions.

[0309]

[0310]

[0311] The polymer (MMCP1-3) was mixed with 2400 ppm of Irganox B561 (available from BASF) and 270 ppm of Dynamar FX 5922 (available from 3M), compounded and extruded into pellets using a JSW extruder under a nitrogen atmosphere so that the SEI was 230 kWh / kg and the melt temperature was 250° C. Table 4 summarizes some properties of MMCP1-3 and FK1820.

[0312] Table 4: Properties of multimodal copolymers.

[0313]

[0314]

[0315] *: HCF: High Crystalline Fraction / LCF: Low Crystalline Fraction. CFC data.

[0316] C. Fabrication of three-layer membrane

[0317] 3-layer films with a total thickness of 60 μm and the composition shown in Table 6 were produced on a Collin 3-layer lab line (BUR=1:2.5, winding speed=7 m / min, frost line 120 mm, melt temperature=210° C.).

[0318] D. Results

[0319] Table 5: Composition and properties of the three-layer membranes.

[0320]

[0321] E. Discussion of Results

[0322] As can be seen from Table 5 above, the films according to the present invention (IE1-4) not only show better mechanical properties (high dart impact strength and tensile modulus) than the films according to the comparative example (CE1), but also have excellent sealing properties (see seal initiation temperature SIT, hot tack temperature and hot tack force).

Claims

1. A multilayer film comprising a skin layer (SKL), a core layer (CL) and a sealing layer (SL); wherein At least the core layer (CL) comprises a metallocene-catalyzed multimodal polyethylene copolymer (MMCP) comprising (i) 35.0 to 50.0 wt% of an ethylene-1-butene polymer component (A), based on the total weight of the MMCP; and (ii) 50.0 to 65.0 wt% of an ethylene-1-hexene polymer component (B), based on the total weight of the MMCP; wherein The ethylene-1-butene polymer component (A) has ·920 to 960 kg / m 3 Density within the range (ASTM D792); MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 3.0 to 300.0 g / 10 min; · a 1-butene content in the range of 0.1 to 3.0 mol% based on the ethylene-1-butene polymer component (A); and The ethylene-1-hexene polymer component (B) has 880 to 920 kg / m 3 Density within the range (ASTM D792); MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.001 to 1.0 g / 10 min; · a 1-hexene content in the range of 1.5 to 10.0 mol% based on the ethylene-1-hexene polymer compound (B); and The metallocene-catalyzed multimodal polyethylene copolymer (MMCP) has ·910 to 930 kg / m 3 Density within the range (ASTM D792); MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 1.4 g / 10 min; and MFR in the range of 22 to 70 21 Ratio of MFR (190℃, 21.6kg, ISO 1133) to MFR2 (190℃, 2.16kg, ISO1133) 21 / MFR2; wherein the core layer (CL) further comprises Mixed plastics - polyethylene recycled blends having an MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 1.2 g / 10 min and a 3 Density (ASTM D792).

2. The multilayer film according to claim 1, characterized in that The metallocene-catalyzed multimodal polyethylene copolymer (MMCP) has a ratio of the soluble fraction at 35°C to the density of the MMCP, SF@35°C / density, as determined by cross fractionation chromatography (CFC) as described in the experimental section, of less than 0.007 or less than 0.

050. MMCP , wherein the amount of the soluble portion at 35° C. is in the range of 0.5 to 6.0 wt % or 39 to 43 wt % based on the total weight of the MMCP; and / or MFR in the range of 22 to 50, preferably 28 to 46 21 Ratio of MFR (190℃, 21.6kg, ISO 1133) to MFR2 (190℃, 2.16kg, ISO 1133) 21 / MFR2.

3. The multilayer film according to claim 1 or 2, characterized in that The thickness of the skin layer (SKL) of the multilayer film is in the range of 1 to 100 μm; preferably in the range of 5 to 80 μm, more preferably in the range of 10 to 15 μm; and / or The thickness of the core layer (CL) of the multilayer film is in the range of 10 to 200 μm; preferably in the range of 20 to 80 μm, more preferably in the range of 30 to 45 μm; and / or The thickness of the sealing layer (SL) of the multilayer film is in the range of 1 to 50 μm; preferably in the range of 5 to 25 μm, more preferably in the range of 10 to 15 μm; and / or The thickness of the multilayer film is in the range of 12 to 350 μm; preferably in the range of 40 to 150 μm, more preferably in the range of 50 to 70 μm.

4. The multilayer film according to any one of the preceding claims, characterized in that The multilayer film consists of a skin layer (SKL), a core layer (CL) and a sealing layer (SL); and The surface layer (SKL) comprises 65 to 95 wt%, preferably 80 to 95 wt%, more preferably 82 to 93 wt%, more preferably 88 to 92 wt%, based on the total weight of the skin layer (SKL), of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP), the metallocene-catalyzed multimodal polyethylene copolymer (MMCP) preferably having a molecular weight in the range of 912 to 925 kg / m 3 , more preferably 913 to 918 kg / m 3 Density in the range of 1.5 to 2.0 g / 10 min (ASTM D792) and MFR2 in the range of 0.5 to 1.4 g / 10 min (190°C, 2.16 kg, ISO 1133); and 5 to 35 wt%, preferably 5 to 20 wt%, preferably 7 to 18 wt%, more preferably 8 to 12 wt% of LDPE based on the total weight of the skin layer (SKL), the LDPE having a molecular weight of 910 to 930 kg / m 3 , preferably 920 to 925 kg / m 3 The density (ASTM D792) is within the range of 0.5 to 4 g / 10 min, and the MFR2 (190° C., 2.16 kg, ISO 1133) is within the range of 0.7 to 2 g / 10 min.

5. The multilayer film according to any one of the preceding claims, characterized in that The multilayer film consists of a skin layer (SKL), a core layer (CL) and a sealing layer (SL); and The core layer (CL) comprises 10 to 35 wt%, more preferably 15 to 30 wt%, more preferably 18 to 25 wt%, based on the total weight of the core layer (CL), of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP), the metallocene-catalyzed multimodal polyethylene copolymer (MMCP) preferably having a molecular weight of 912 to 925 kg / m 3 , more preferably 913 to 918 kg / m 3 Density in the range of 1.5 to 2.0 g / 10 min (ASTM D792) and MFR2 in the range of 0.5 to 1.4 g / 10 min (190°C, 2.16 kg, ISO 1133); and 50 to 90 wt%, preferably 55 to 85 wt%, more preferably 68 to 82 wt%, based on the total weight of the core layer (CL), of a mixed plastic-polyethylene recycled blend having an MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.1 to 1.2 g / 10min, preferably 0.3 to 1.1 g / 10min and a MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 910 to 945 kg / m 3 , preferably 915 to 930 kg / m 3 , most preferably 920 to 927 kg / m 3 Density within the range (ASTM D792); and 0 to 15 wt%, preferably 0 to 12 wt%, more preferably 8 to 12 wt%, based on the total weight of the core layer (CL) of a Ziegler-Natta catalyzed linear low density polyethylene (ZNCP), the Ziegler-Natta catalyzed linear low density polyethylene (ZNCP) preferably being a multimodal α-olefin terpolymer, preferably having a molecular weight in the range of 920 to 970 kg / m 3 , more preferably 935 to 950 kg / m 3 A density in the range of 1.5 to 2.5 g / 10 min (ASTM D792) and an MFR2 (190° C., 2.16 kg, ISO 1133) in the range of 0.1 to 2.5 g / 10 min, preferably 1.0 to 1.8 g / 10 min; and 0 to 15 wt%, more preferably 0 to 12 wt%, more preferably 6 to 10 wt% of a high density polyethylene, based on the total weight of the core layer (CL), the high density polyethylene preferably being bimodal and having a density of 950 to 975 kg / m 3 , more preferably 955 to 965 kg / m 3 The preferred embodiment of the present invention has a density in the range of 0.1 to 1.5 g / 10 min, preferably a MFR2 (190° C., 2.16 kg, ISO 1133) in the range of 0.5 to 1.0 g / 10 min.

6. The multilayer film according to any one of the preceding claims, characterized in that The multilayer film consists of a skin layer (SKL), a core layer (CL) and a sealing layer (SL); and / or The sealing layer (SL) comprises 0 to 90 wt% or 50 to 90 wt%, more preferably 70 to 85 wt%, based on the total weight of the sealing layer (SL), of a metallocene-catalyzed multimodal polyethylene copolymer (MMCP), the metallocene-catalyzed multimodal polyethylene copolymer (MMCP) preferably having a molecular weight in the range of 912 to 925 kg / m 3 , more preferably 913 to 918 kg / m 3 Density in the range of 1.5 to 2.0 g / 10 min (ASTM D792) and MFR2 in the range of 0.5 to 1.4 g / 10 min (190°C, 2.16 kg, ISO 1133), and 0 to 80 wt %, preferably 10 to 70 wt %, more preferably 15 to 25 wt % of a plastomer, based on the total weight of the sealing layer (SL), the plastomer being preferably a copolymer of ethylene and 1-octene, preferably having a molecular weight of 860 to 910 kg / m 3 , preferably 895 to 905 kg / m 3 A density in the range of 0.5 to 10 g / 10 min, preferably in the range of 1.0 to 1.5 g / 10 min, MFR2 (190° C., 2.16 kg, ISO 1133); and 0 to 50 wt%, preferably 35 to 45 wt%, based on the total weight of the sealing layer (SL), of a multimodal metallocene-catalyzed linear low density polyethylene, preferably a bimodal ethylene / 1-butene / 1-hexene terpolymer, preferably having a molecular weight in the range of 910 to 930 kg / m 3 , more preferably 916 to 925 kg / m 3 range (ASTM D792); and MFR2 (190° C., 2.16 kg, ISO 1133) in the range of 0.5 to 2 g / 10 min.

7. The multilayer film according to any one of the preceding claims, characterized in that The skin layer (SKL), the core layer (CL) and the sealant layer (SL) comprise a metallocene-catalyzed multimodal polyethylene copolymer (MMCP).

8. The multilayer film according to any one of the preceding claims, characterized in that Metallocene-catalyzed multimodal polyethylene copolymers (MMCPs) have the ratio of the molecular weight (Mw) of the low crystalline fraction (LCF) to the molecular weight (Mw) of the high crystalline fraction (HCF) determined as described in the experimental part in the range of >1.0 to 10.0, Mw(Tp(LCF) / Mw(Tp(HCF), and / or a width at half height ratio (LCF) / (98-Tp(LCF)) in the range of 0.10 to 1.50, and / or • A difference of Mw(LCF)-Mw(HCF) of at least 5000 and at most 200000 g / mol.

9. The multilayer film according to any one of the preceding claims, characterized in that The component (A) of the metallocene-catalyzed multimodal polyethylene copolymer (MMCP) consists of an ethylene polymer fraction (A-1) and an ethylene polymer fraction (A-2); wherein; The ethylene polymer portion (A-1) preferably has 925 to 960 kg / m 3 , preferably 925 to 955 kg / m 3 , more preferably 930 to 950 kg / m 3 Density within the range (ASTM D792); and / or 3.0 to 300.0 g / 10 min, preferably 3.0 to 10.0 g / 10 min or 80 to 150 g / 10 min, More preferably, the MFR2 (190°C, 2.16kg, ISO 1133), and / or The ethylene polymer portion (A-2) preferably has 925 to 960 kg / m 3 , preferably 925 to 955 kg / m 3 , more preferably 930 to 950 kg / m 3 Density within the range (ASTM D792), and / or 3.0 to 300.0 g / 10 min, preferably 3.0 to 10.0 g / 10 min or 80 to 150 g / 10 min, More preferably, the MFR2 (190°C, 2.16kg, ISO 1133).

10. The multilayer film according to any one of the preceding claims, characterized in that Metallocene-catalyzed multimodal copolymers (MMCPs) have a total amount of 1-butene in the range of 0.1 to 1.0 mol%, preferably 0.2 to 0.8 mol%, more preferably 0.3 to 0.7 mol%, based on the multimodal polymer (MMCP); and / or A total amount of 1-hexene in the range of 1.5 to 8.0 mol%, preferably 2.0 to 6.0 mol%, more preferably 2.2 to 4.0 mol% based on the multimodal polymer (MMCP); and / or 35 to 50 wt%, preferably 36 to 48 wt%, more preferably 38 to 45 wt% of the ethylene-1-butene polymer component (A), based on the total weight of the MMCP; and / or 50 to 65 wt %, preferably 52 to 64 wt %, more preferably 55 to 62 wt %, based on the total weight of MMCP Content of ethylene-1-hexene polymer component (B) in wt%.

11. The multilayer film according to any one of the preceding claims, characterized in that Metallocene-catalyzed multimodal copolymers (MMCPs) are produced in the presence of a metallocene complex of formula (I): Wherein each X is independently a halogen atom, C 1-6 -alkyl, C 1-6 - alkoxy, phenyl or benzyl; Each Het is independently a monocyclic heteroaromatic group containing at least one heteroatom selected from O or S; L is -R'2Si-, wherein each R' is independently a C substituted with an alkoxy group having 1 to 10 carbon atoms. 1-20 -Hydrocarbon or C 1-10 -alkyl; M is Ti, Zr or Hf; Each R1 is the same or different, is C 1-6 -alkyl or C 1-6 - alkoxy; Each n is 1 to 2; Each R2 is the same or different, and is C 1-6 -alkyl, C 1-6 -alkoxy or -Si(R)3 group; Each R is optionally replaced by 1 to 3 C 1-6 -alkyl substituted C 1-10 - alkyl or phenyl; and Each p is from 0 to 1.

12. The multilayer film according to any one of the preceding claims, characterized in that The multilayer film has a longitudinal tensile modulus in the range of 150 to 300 MPa, preferably in the range of 190 to 240 MPa (ISO 527-3); and / or a transverse tensile modulus (ISO 527-3) in the range of 150 to 400 MPa, preferably in the range of 200 to 300 MPa; and / or • Dart drop strength (ISO 7765-1) in the range of 230 to 800 g, preferably in the range of 350 to 600 g.

13. The multilayer film according to any one of the preceding claims, characterized in that The multilayer film has A haze (ASTM D1003-00) in the range of 5 to 15%, preferably in the range of 8 to 13%; and / or a sealing initiation temperature determined as described in the description in the range of 60 to 70°C or 78 to 85°C, preferably in the range of 63 to 68°C or 79 to 81°C; and / or A hot tack force determined as described in the description in the range of 6.0 to 8.0 N or 5.2 to 5.8 N, preferably in the range of 6.2 to 7.5 N or 5.4 to 5.6 N; and / or - A hot sticking temperature determined as described in the specification in the range of 60 to 90°C, preferably in the range of 63 to 86°C.

14. The multilayer film according to any one of the preceding claims, characterized in that The multilayer film consists of a polyethylene-based polymer.

15. Use of the multilayer film according to any of the preceding claims as packaging material, preferably for food and / or medical products.

Citation Information

Patent Citations

  • Multilayer film

    CN103068574A

  • Multimodal ethylene copolymer

    WO2022018239A1