Sodium nickelate cathode material synthesis using persulfate sodium removal and oxidation and use thereof
Through sulfate treatment and desodium nicode oxide materials, combined with electrolytic manganese dioxide and graphite, the problem of unstable nicode material at high temperatures is solved, the chemical stability and performance of the battery is improved, and the use of the battery is extended life.
Patent Information
- Application Number
- CN202380032791.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-15
- Filing Date
- 2023-04-17
- Publication Date
- 2024-12-06
AI Technical Summary
In existing alkaline electrochemical cell units, the nicate material is unstable at high temperatures, resulting in electrochemical reduction and electrode capacity loss, limiting the shelf life of the battery.
The chemical stability and battery performance of the material are improved by pre-aging treatment using a sulfate-treated desodium and oxidized nicate material, combined with electrolytic manganese dioxide and graphite.
It significantly improves the chemical stability and battery performance of nicate materials, extends the shelf life of the battery, and maintains high discharge capacity and efficiency under high temperature conditions.
Smart Images

Figure HDA0005072743150000011 
Figure HDA0005072743150000021 
Figure HDA0005072743150000031
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Provisional Application Serial No. 63 / 363,059, filed on April 15, 2022, which is hereby incorporated by reference in its entirety for all of its teachings. Background Art
[0003] Alkaline electrochemical cells are commercially available in cell sizes commonly referred to as LR6 (AA), LR03 (AAA), LR14 (C), and LR20 (D). The cylindrical shape of the cell must conform to dimensional standards established by organizations such as the International Electrotechnical Commission. The electrochemical cells are used by consumers to power a variety of electrical devices, such as clocks, radios, toys, electronic games, film cameras that typically include flash units, and digital cameras. Such electrical devices have a variety of discharge conditions, such as from low drain to relatively high drain.
[0004] Since the shape and size of batteries are generally fixed, battery manufacturers must modify battery cell characteristics to improve performance. Attempts to solve the problem of how to improve battery performance in a particular device, such as a digital camera, often involve changing the internal construction of the battery cell. For example, the battery cell construction has been modified by increasing the amount of active material used within the battery cell.
[0005] High-valent nickel materials including nickel oxyhydroxide (NiOOH), nickel dioxide (NiO2), and various forms of nickel oxide, nickelate, and nickel oxyhydroxide can be used as cathode materials in alkaline systems due to their high capacity and cell voltage. x The oxidation state of NiO2 (where x<<1) is higher than 3+, which potentially enables a much higher discharge capacity than that of EMD (MnO2). x NiO2 is inherently unstable and degrades rapidly at high temperatures. In addition, these materials are thermodynamically unstable in aqueous electrolytes, which results in electrochemical reduction of the nickel cathode (loss of electrode capacity). Therefore, the shelf life of alkaline batteries with high-priced nickel cathodes is limited compared to batteries containing some other cathode materials. Summary of the invention
[0006] One embodiment of the present invention is a nickelate material having an X-ray diffraction (XRD) pattern including a first peak at about 12°-14° 2θ, a second peak at about 18°-21° 2θ, a third peak at about 24°-25° 2θ, and a fourth peak set at about 36°-43° 2θ. In an alternative embodiment, the sodium-removed nickelate material has an XRD pattern having at least one, two, three, or four of the four peaks or peak sets.
[0007] One embodiment is a method of preparing a sulfate-treated desodiumed and oxidized nickelate, the method comprising contacting sodium nickelate with a persulfate solution to produce the sulfate-treated desodiumed and oxidized nickelate.
[0008] One embodiment is a nickelate material prepared by any of the methods described herein.
[0009] One embodiment is an alkaline cathode composition comprising any of the nickelate materials described herein and electrolytic manganese dioxide (EMD).
[0010] One embodiment is an alkaline cathode composition comprising any of the desodiumated and oxidized nickelate materials described herein, electrolytic manganese dioxide, graphite, and a binder.
[0011] One embodiment is a pre-aged beta nickelate material having an X-ray diffraction (XRD) pattern including a first peak at about 50.0°-52.0° 2θ, a second peak at about 53.6°-56.8° 2θ, a third peak at about 60.8°-62.6° 2θ, a fourth peak at about 66.4°-67.5° 2θ, and a fifth peak at about 67.4°-68.6° 2θ. In an alternative embodiment, the sodium-depleted nickelate material has an XRD pattern having at least 1, 2, 3, 4, or 5 of these five peaks.
[0012] One embodiment is a method of preparing a pre-aged beta nickelate material, the method comprising contacting a beta nickelate with a pre-aging solution comprising a hydroxide to produce the pre-aged nickelate material.
[0013] One embodiment is a beta nickelate material prepared by any of the methods described herein.
[0014] One embodiment is an alkaline cathode composition including any of the beta nickelate materials described herein and electrolytic manganese dioxide (EMD).
[0015] One embodiment is a composition comprising any of the beta nickelate materials described herein, electrolytic manganese dioxide, graphite, and a binder.
[0016] One embodiment is an alkaline electrochemical cell comprising any of the nickelate materials or compositions described herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a cross-sectional elevation view of an alkaline electrochemical cell according to one embodiment.
[0018] Figure 2 The yields and chemistries of acid desodiumization / disproportionation and persulfate desodiumization / oxidation are presented.
[0019] Figure 3 An X-ray diffraction (XRD) pattern of sodium nickel oxide is shown.
[0020] Figure 4 An X-ray diffraction (XRD) pattern of desodiumated sodium nickel oxide is shown.
[0021] Figure 5 Shown is an X-ray diffraction (XRD) pattern of desodiumed and oxidized sodium nickel oxide using persulfate.
[0022] Figure 6 Shown are the discharge capacities (10 mA / g) before and after aging the dry powders at 70° C. / 50% RH for 4 weeks.
[0023] Figure 7 The X-ray diffraction (XRD) pattern of LiOH pre-aged β-nickelate is shown.
[0024] Figure 8 The discharge curves at O / C=1 are shown before and after LiOH pre-aging of β-nickelate.
[0025] Fig. 9 Shown are discharge curves before and after LiOH pre-aged β-nickelate mixed with EMD and O / C = 14.5.
[0026] Fig.10 A comparison of the discharge energies of β-nickelate after aging at 60° C. and sodium nickel oxide after sulfate desodiumization and oxidation is shown.
[0027] Fig.11 Shown are discharge curves for EMD mixed with various levels of sodium nickel oxide that has been desodiumated with sulfate and oxidized.
[0028] Fig.12 The discharge efficiency and energy in the EMD / nickelate blends are shown versus Ni wt%. DETAILED DESCRIPTION
[0029] Various embodiments will now be described more fully below with reference to the accompanying drawings, in which some but not all embodiments are shown. In fact, various embodiments can be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein; on the contrary, these embodiments are provided so that the present disclosure will satisfy applicable legal requirements. Throughout the text, the same reference numerals refer to the same elements. In the following description, each component can be identified as having a specific value or parameter; however, these items are provided as exemplary embodiments. In fact, the exemplary embodiments do not limit the various aspects and concepts of the embodiments, because many comparable parameters, sizes, ranges and / or values can be implemented. The terms "first", "second", etc., "primary", "exemplary", "minor", etc. do not represent any order, quantity or importance, but are used to distinguish one element from another element. Further, the terms "one (a)", "an" and "the" do not represent a limitation on quantity, but represent that there is "at least one" referenced item.
[0030] This embodiment is designed in an effort to overcome the limitations of existing electrochemical battery cells. x NiO2, Na produced from acid leached NaNiO2 x The yield of NiO2 is lower and the chemical stability is lower. An oxidation / de-sodiumization method is disclosed, which improves the chemical stability of the sodium nickelate material at high temperature compared to the commonly used acid leaching method, and the yield of the nickelate material obtained by the oxidation / de-sodiumization method is higher.
[0031] It is contemplated that each embodiment disclosed herein is applicable to each of the other disclosed embodiments.All combinations and sub-combinations of the various elements described herein are within the scope of the embodiments.
[0032] It should be understood that where a parameter range is provided, the embodiments also provide all integers and ranges within the range, as well as tenths and hundredths thereof. For example, "5-10%" includes 5%, 6%, 7%, 8%, 9% and 10%; 5.0%, 5.1%, 5.2%, ... 9.8%, 9.9% and 10.0%; and 5.00%, 5.01%, 5.02%, ... 9.98%, 9.99% and 10.00%, and, for example, 6-9%, 5.1%-9.9% and 5.01%-9.99%.
[0033] As used herein, "about" in the context of a numerical value or a range means within ±10%, ±5%, or ±1% of the recited or claimed numerical value or range.
[0034] As used herein, "nickelate" refers to a salt containing a nickel-containing anion, or a compound including nickel and at least one other element in combination with oxygen.
[0035] As used herein, "nickel compound" refers to any compound that includes nickel.
[0036] As used herein, "nickel precursor" refers to a compound that includes nickel that reacts with a sodium-containing compound to produce a different compound that includes nickel.
[0037] As used herein, "oxide" refers to a chemical compound containing at least one oxygen atom and one other element. As used herein, "nickel oxide" refers to any oxide containing nickel. Nickel oxide may include other cations and anions. Non-limiting examples include nickel dioxide (NiO2), nickel hydroxide (Ni(OH)2), and hydrated alkaline nickel oxide (such as Na x NiO2·n(H2O)).
[0038] As used herein, "oxyhydroxide" refers to a chemical compound or complex containing an oxide group and a hydroxide group. As used herein, "nickel oxyhydroxide" refers to any oxyhydroxide containing nickel. The nickel oxyhydroxide may include other cations and anions. A non-limiting example is nickel oxyhydroxide (NiOOH).
[0039] As used herein, "persulfate" refers to any salt comprising a persulfate anion (SO5 2- or S2O8 2- ) compounds. Non-limiting examples include sodium persulfate (NaS2O8), ammonium persulfate (NH4)2S2O8, and potassium persulfate (K2S2O8).
[0040] As used herein, "sodium compound" refers to any compound that includes sodium. In one embodiment, the sodium compound includes both sodium and oxygen. Non-limiting examples include NaOH (sodium hydroxide), Na2O (sodium oxide), NaO2 (sodium peroxide), and Na x NiO2 (sodium nickel oxide).
[0041] As used herein, "improvement" with respect to storage stability means that storage stability (i.e., "shelf life") is increased. Generally, an "improvement" in a property or performance indicator of a material or electrochemical cell means that the property or performance indicator is different (compared to a property or performance indicator of a different material or electrochemical cell) in a way that a user or manufacturer of the material or cell would expect (i.e., costs less, lasts longer, provides more power, is more durable, is easier or faster to manufacture, etc.).
[0042] As used herein, "alkali metal" is an element from Group IA of the Periodic Table of Elements. Non-limiting examples include Li, Na, K, Rb, and Cs.
[0043] As used herein, "alkaline earth metals" are elements from Group IIA of the Periodic Table of Elements. Non-limiting examples include Mg, Ca, and Sr.
[0044] As used herein, a "transition metal" is an element from Groups IB-VIIIB of the Periodic Table of the Elements. Non-limiting examples include Co, Mn, Zn, Y, Nb, and Ti.
[0045] As used herein, "other metals" or "another metal" includes all metals on the periodic table not included in the previously mentioned groups, including Al, Ga, In, Sn, Tl, Pb, and Bi.
[0046] As used herein, a "primary" electrochemical cell is a non-rechargeable (ie, disposable) electrochemical cell. A "secondary" electrochemical cell is a rechargeable electrochemical cell.
[0047] As used herein, "electrical conductivity" refers to the ability of a given material to conduct an electric current. This is usually measured in Siemens per meter (S / m).
[0048] As used herein, the terms "pre-aging" or "pre-aged" refer to a controlled process that converts a material over time into a more stable resulting phase or mixture of different phases when used in a final product. For example, a cathode material can be pre-aged using the processes discussed herein to provide a more shelf-stable cathode material when included in a battery. In certain embodiments, the nickelate oxide is pre-aged by exposing the material to a specific concentration of LiOH, NaOH, KOH, and / or other oxides or hydroxides at a specific temperature and for a specified time period. Other hypotheses are that pre-aging can also form a protective film on the high oxidation state surface of the nickel particles to slow down the decomposition reaction from the high nickel oxidation state to the low nickel oxidation state.
[0049] One embodiment is a nickelate material having an X-ray diffraction (XRD) pattern including a first peak at about 12°-14° 2θ, a second peak at about 18°-21° 2θ, a third peak at about 24°-25° 2θ, and a fourth peak set at about 36°-43° 2θ. In an alternative embodiment, the sodium-depleted nickelate material has an XRD pattern having at least 1, 2, 3, or 4 of these four peaks or peak sets.
[0050] In one embodiment, the nickelate material is a desodiumized and oxidized sodium nickelate material.
[0051] In one embodiment, the desodiumed and oxidized nickelate material is a desodiumed nickelate hydride comprising the following phases:
[0052] i) 40-90 wt% of a compound having the formula (Na x NiO2·nH2O), wherein 0.2≤x<1, and 0 <n<2;
[0053] ii) nickel oxide (NiO2) in an amount of 5-40 wt%; and
[0054] iii) β-nickel hydroxide (NiOOH) in an amount of 5-20 wt%.
[0055] One embodiment is a method of preparing a sulfate-treated desodiumed and oxidized nickelate, the method comprising contacting sodium nickelate with a persulfate solution to produce the sulfate-treated desodiumed and oxidized nickelate.
[0056] In one embodiment, the nickelate that has been desodiumized and oxidized by sulfate is a mixture of nickel oxide, sodium nickel oxide hydrate and / or nickel oxide hydroxide.
[0057] In one embodiment, the sulfate-treated, desodiumated and oxidized nickelate comprises the following phases:
[0058] i) 40-90 wt% of a compound having the formula (Na x NiO2·nH2O), wherein 0.2≤x<1, and 0 <n<2;
[0059] ii) nickel oxide (NiO2) in an amount of 5-40 wt%; and
[0060] iii) β-nickel hydroxide (NiOOH) in an amount of 5-20 wt%.
[0061] This is a mixed phase nickelate. In one embodiment, x is at least, at most, or about 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1, or within a range defined by any two of these values. In one embodiment, n is at least, at most, or about 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2, or within a range defined by any two of these values. In one embodiment, the molar ratio of persulfate to nickel is about 2-4. In one embodiment, the molar ratio is at least, at most, or about 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, or 4, or within a range bounded by any two of these values.
[0062] In one embodiment, the sodium nickelate is contacted with the persulfate solution for a period of about 1-72 hours. In one embodiment, the period of time is at least, at most, or about 1 hour, 2 hours, 4 hours, 8 hours, 12 hours, 16 hours, 20 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 hours, 54 hours, 60 hours, 66 hours, or 72 hours, or within a range bounded by any two of these values.
[0063] In one embodiment, the method is carried out at a temperature less than or equal to 50° C. In one embodiment, the temperature is at least, at most, or about 0° C., 5° C., 10° C., 15° C., 20° C., 25° C., 30° C., 35° C., 40° C., 45° C., or 50° C., or within a range bounded by any two of these values.
[0064] In one embodiment, the pH of the persulfate solution is about 12-14. In one embodiment, the pH of the persulfate solution is at least, at most, or about 12, 12.1, 12.2, 12.3, 12.4, 12.5, 12.6, 12.7, 12.8, 12.9, 13, 13.1, 13.2, 13.3, 13.4, 13.5, 13.6, 13.7, 13.8, 13.9, or 14, or within a range bounded by any two of these values.
[0065] In one embodiment, the persulfate solution comprises a persulfate selected from the group consisting of potassium persulfate and sodium persulfate. In one embodiment, the persulfate is potassium persulfate. In one embodiment, the persulfate is sodium persulfate.
[0066] One embodiment is a nickelate material prepared by any of the methods described herein.
[0067] One embodiment is an alkaline cathode composition comprising any of the nickelate materials described herein and electrolytic manganese dioxide (EMD).
[0068] In one embodiment, the ratio of nickel to manganese is about 99: 1 to 1: 99 by weight. In one embodiment, the ratio of nickel to manganese is at least, at most, or about 99: 1, 95:5, 90: 10, 80:20, 70:30, 60:40, 50:50, 40:60, 30:70, 20:80, 10:90, 5:95, or 1:99, or within a range bounded by any two of these values.
[0069] One embodiment is an alkaline cathode composition comprising any of the desodiumated and oxidized nickelate materials described herein, electrolytic manganese dioxide, graphite, and a binder.
[0070] In one embodiment, the desodiumized and oxidized nickelate material is present in an amount of about 8.8-45.1 wt.%, electrolytic manganese dioxide (EMD) is present in an amount of about 48-84.3 wt.%, graphite is present in an amount of about 3-8 wt.%, and the binder is present in an amount of about 0.1-1.0 wt.%, relative to the total weight of the nickelate, EMD, graphite and binder. In one embodiment, the nickelate is at least, at most, or about 8.8 wt.%, 9 wt.%, 10 wt.%, 11 wt.%, 12 wt.%, 13 wt.%, 14 wt.%, 15 wt.%, 16 wt.%, 17 wt.%, 18 wt.%, 19 wt.%, 20 wt.%, 21 wt.%, 22 wt.%, 23 wt.%, 24 wt.%, 25 wt.%, 26 wt.%, 27 wt.% %, 28wt.%, 29wt.%, 30wt.%, 31wt.%, 32wt.%, 33wt.%, 34wt.%, 35wt.%, 36wt.%, 37wt.%, 38wt.%, 39wt.%, 40wt.%, 41wt.%, 42wt.%, 43wt.%, 44wt.%, 45wt.% or 45.1wt.%, or in an amount within the range defined by any two of these values.
[0071] In one embodiment, the EMD is at least, at most, or about 48 wt.%, 49 wt.%, 50 wt.%, 51 wt.%, 52 wt.%, 53 wt.%, 54 wt.%, 55 wt.%, 56 wt.%, 57 wt.%, 58 wt.%, 59 wt.%, 60 wt.%, 61 wt.%, 62 wt.%, 63 wt.%, 64 wt.%, 65 wt.%, 66 wt.%, 67 wt.%, %, 68 wt.%, 69 wt.%, 70 wt.%, 71 wt.%, 72 wt.%, 73 wt.%, 74 wt.%, 75 wt.%, 76 wt.%, 77 wt.%, 78 wt.%, 79 wt.%, 80 wt.%, 81 wt.%, 82 wt.%, 83 wt.%, 84 wt.% or 84.3 wt.%, or in an amount within a range defined by any two of these values. In an embodiment, graphite is present in an amount of at least, at most or about 3 wt.%, 4 wt.%, 5 wt.%, 6 wt.%, 7 wt.%, or 8 wt.%, or in an amount within a range defined by any two of these values. In one embodiment, the binder is present in an amount of at least, at most, or about 0.1 wt.%, 0.2 wt.%, 0.3 wt.%, 0.4 wt.%, 0.5 wt.%, 0.6 wt.%, 0.7 wt.%, 0.8 wt.%, 0.9 wt.%, or 1.0 wt.%, or within a range defined by any two of these values.
[0072] In one embodiment, the desodiumed and oxidized nickelate material and EMD are present together in an amount of about 92-97 wt.%, graphite is present in an amount of about 3-8 wt.%, and the binder is present in an amount of about 0.1-1.0 wt.%. In one embodiment, the desodiumed and oxidized nickelate material and EMD are present together in an amount of at least, at most, or about 92 wt.%, 93 wt.%, 94 wt.%, 95 wt.%, 96 wt.%, or 97 wt.%, or in an amount within a range defined by any two of these values. In one embodiment, graphite is present in an amount of at least, at most, or about 3 wt.%, 4 wt.%, 5 wt.%, 6 wt.%, 7 wt.%, or 8 wt.%, or in an amount within a range defined by any two of these values. In one embodiment, the binder is present in an amount of at least, at most, or about 0.1 wt.%, 0.2 wt.%, 0.3 wt.%, 0.4 wt.%, 0.5 wt.%, 0.6 wt.%, 0.7 wt.%, 0.8 wt.%, 0.9 wt.%, or 1.0 wt.%, or within a range defined by any two of these values.
[0073] One embodiment is a pre-aged beta nickelate material having an X-ray diffraction (XRD) pattern including a first peak at about 50.0°-52.0° 2θ, a second peak at about 53.6°-56.8° 2θ, a third peak at about 60.8°-62.6° 2θ, a fourth peak at about 66.4°-67.5° 2θ, and a fifth peak at about 67.4°-68.6° 2θ. In an alternative embodiment, the sodium-depleted nickelate material has an XRD pattern having at least 1, 2, 3, 4, or 5 of these five peaks.
[0074] In one embodiment, the pre-aged beta nickelate material has been prepared by pre-aging the beta nickelate using a pre-aging solution including a hydroxide.
[0075] In one embodiment, the hydroxide is selected from the group consisting of alkali metal hydroxides and alkaline earth metal hydroxides. In one embodiment, the hydroxide is selected from the group consisting of LiOH, NaOH, KOH and Ca(OH)2. In one embodiment, the hydroxide is LiOH, NaOH or KOH. In one embodiment, the hydroxide is LiOH. In one embodiment, the hydroxide is NaOH. In one embodiment, the hydroxide is KOH.
[0076] In one example, the pre-aging solution has a hydroxide concentration of about 0.005 M to about 1 M. In one example, the hydroxide concentration is at least, at most, or about 0.005 M, 0.01 M, 0.02 M, 0.05 M, 0.1 M, 0.2 M, 0.3 M, 0.4 M, 0.5 M, 0.6 M, 0.7 M, 0.8 M, 0.9 M, or 1.0 M, or within a range bounded by any two of these values.
[0077] In one embodiment, the ratio of pre-aging solution to beta nickelate is from about 1 mL / g to about 200 mL / g. In one embodiment, the ratio is at least, at most, or about 1 mL / g, 2 mL / g, 5 mL / g, 10 mL / g, 20 mL / g, 30 mL / g, 40 mL / g, 50 mL / g, 60 mL / g, 70 mL / g, 80 mL / g, 90 mL / g, 100 mL / g, 110 mL / g, 120 mL / g, 130 mL / g, 140 mL / g, 150 mL / g, 160 mL / g, 170 mL / g, 180 mL / g, 190 mL / g, or 200 mL / g, or within a range bounded by any two of these values.
[0078] In one embodiment, the beta nickelate is pre-aged for about 1-60 minutes. In one embodiment, the beta nickelate precursor is pre-aged for about 1-30 minutes or about 1-20 minutes. In one embodiment, the beta nickelate is pre-aged for at least, at most, or about 1 minute, 2 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, or 60 minutes, or within a range defined by any two of these values.
[0079] In one embodiment, the beta nickelate is pre-aged at a temperature of about 0° C. to about 40° C. In one embodiment, the beta nickelate is pre-aged at a temperature of at least, at most, or about 0° C., 5° C., 10° C., 15° C., 20° C., 25° C., 30° C., 35° C., or 40° C., or within a range bounded by any two of these values.
[0080] In one embodiment, the pre-aged β-nickelate comprises β-nickelate, nickel oxide, β-nickel oxyhydroxide or a combination thereof.
[0081] One embodiment is a method of preparing a pre-aged beta nickelate material, the method comprising contacting a beta nickelate with a pre-aging solution comprising a hydroxide to produce the pre-aged nickelate material.
[0082] In one embodiment, the hydroxide is selected from the group consisting of alkali metal hydroxides and alkaline earth metal hydroxides. In one embodiment, the hydroxide is selected from the group consisting of LiOH, NaOH, KOH and Ca(OH)2. In one embodiment, the hydroxide is LiOH, NaOH or KOH. In one embodiment, the hydroxide is LiOH. In one embodiment, the hydroxide is NaOH. In one embodiment, the hydroxide is KOH.
[0083] In one example, the pre-aging solution has a hydroxide concentration of about 0.005 M to about 1 M. In one example, the hydroxide concentration is at least, at most, or about 0.005 M, 0.01 M, 0.02 M, 0.05 M, 0.1 M, 0.2 M, 0.3 M, 0.4 M, 0.5 M, 0.6 M, 0.7 M, 0.8 M, 0.9 M, or 1.0 M, or within a range bounded by any two of these values.
[0084] In one embodiment, the ratio of pre-aging solution to beta nickelate is from about 1 mL / g to about 200 mL / g. In one embodiment, the ratio is at least, at most, or about 1 mL / g, 2 mL / g, 5 mL / g, 10 mL / g, 20 mL / g, 30 mL / g, 40 mL / g, 50 mL / g, 60 mL / g, 70 mL / g, 80 mL / g, 90 mL / g, 100 mL / g, 110 mL / g, 120 mL / g, 130 mL / g, 140 mL / g, 150 mL / g, 160 mL / g, 170 mL / g, 180 mL / g, 190 mL / g, or 200 mL / g, or within a range bounded by any two of these values.
[0085] In one embodiment, the beta nickelate is pre-aged for about 1-60 minutes. In one embodiment, the beta nickelate precursor is pre-aged for about 1-30 minutes or about 1-20 minutes. In one embodiment, the beta nickelate is pre-aged for at least, at most, or about 1 minute, 2 minutes, 5 minutes, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes, or 60 minutes, or within a range defined by any two of these values.
[0086] In one embodiment, the temperature is about 0° C. to about 40° C. In one embodiment, the temperature is at least, at most, or about 0° C., 5° C., 10° C., 15° C., 20° C., 25° C., 30° C., 35° C., or 40° C., or within a range bounded by any two of these values.
[0087] One embodiment is a beta nickelate material prepared by any of the methods described herein.
[0088] One embodiment is an alkaline cathode composition including any of the beta nickelate materials described herein and electrolytic manganese dioxide (EMD).
[0089] In one embodiment, the ratio of nickel to manganese is about 99: 1 to 1: 99 by weight. In one embodiment, the ratio of nickel to manganese is at least, at most, or about 99: 1, 95:5, 90: 10, 80:20, 70:30, 60:40, 50:50, 40:60, 30:70, 20:80, 10:90, 5:95, or 1:99, or within a range bounded by any two of these values.
[0090] One embodiment is a composition comprising any of the beta nickelate materials described herein, electrolytic manganese dioxide, graphite, and a binder.
[0091] In one embodiment, the nickel from the beta nickelate material is present in an amount of about 8.8-45.1 wt.%, the electrolytic manganese dioxide is present in an amount of about 48-84.3 wt.%, the graphite is present in an amount of about 3-8 wt.%, and the binder is present in an amount of about 0.1-1.0 wt.%, relative to the total weight of the nickelate, EMD, graphite, and binder. In one embodiment, the nickel is present in an amount of at least, at most, or about 8.8 wt.%, 9 wt.%, 10 wt.%, 11 wt.%, 12 wt.%, 13 wt.%, 14 wt.%, 15 wt.%, 16 wt.%, 17 wt.%, 18 wt.%, 19 wt.%, 20 wt.%, 21 wt.%, 22 wt.%, 23 wt.%, 24 wt.%, 25 wt.%, 26 wt.%, 27 wt.%, 28 wt.%, 29 wt.%, 30 wt.%, 31 wt.%, 32 wt.%, 33 wt.%, 34 wt.%, 35 wt.%, 36 wt.%, 37 wt.%, 38 wt.%, 39 wt.%, 40 wt.%, 41 wt.%, 42 wt.%, 43 wt.%, 44 wt.%, 45 wt.%, 46 wt.%, 47 wt.%, 48 wt.%, 49 wt.%, 50 wt.%, 51 wt.%, 52 wt.%, 53 wt.%, 54 wt.%, 55 wt.%, 56 wt.%, 57 wt.%, 58 wt.%, 59 wt.%, 60 wt.%, %, 28wt.%, 29wt.%, 30wt.%, 31wt.%, 32wt.%, 33wt.%, 34wt.%, 35wt.%, 36wt.%, 37wt.%, 38wt.%, 39wt.%, 40wt.%, 41wt.%, 42wt.%, 43wt.%, 44wt.%, 45wt.% or 45.1wt.%, or in an amount within the range defined by any two of these values.
[0092] In one embodiment, the EMD is at least, at most, or about 48 wt.%, 49 wt.%, 50 wt.%, 51 wt.%, 52 wt.%, 53 wt.%, 54 wt.%, 55 wt.%, 56 wt.%, 57 wt.%, 58 wt.%, 59 wt.%, 60 wt.%, 61 wt.%, 62 wt.%, 63 wt.%, 64 wt.%, 65 wt.%, 66 wt.%, 67 wt.%, %, 68 wt.%, 69 wt.%, 70 wt.%, 71 wt.%, 72 wt.%, 73 wt.%, 74 wt.%, 75 wt.%, 76 wt.%, 77 wt.%, 78 wt.%, 79 wt.%, 80 wt.%, 81 wt.%, 82 wt.%, 83 wt.%, 84 wt.% or 84.3 wt.%, or in an amount within a range defined by any two of these values. In an embodiment, graphite is present in an amount of at least, at most or about 3 wt.%, 4 wt.%, 5 wt.%, 6 wt.%, 7 wt.%, or 8 wt.%, or in an amount within a range defined by any two of these values. In one embodiment, the binder is present in an amount of at least, at most, or about 0.1 wt.%, 0.2 wt.%, 0.3 wt.%, 0.4 wt.%, 0.5 wt.%, 0.6 wt.%, 0.7 wt.%, 0.8 wt.%, 0.9 wt.%, or 1.0 wt.%, or within a range defined by any two of these values.
[0093] In one embodiment, the beta nickelate material and EMD are present together in an amount of about 92-97 wt.%, graphite is present in an amount of about 3-8 wt.%, and the binder is present in an amount of about 0.1-1.0 wt.%. In one embodiment, the desodiumated and oxidized nickelate material and EMD are present together in an amount of at least, at most, or about 92 wt.%, 93 wt.%, 94 wt.%, 95 wt.%, 96 wt.%, or 97 wt.%, or in an amount within a range defined by any two of these values. In one embodiment, graphite is present in an amount of at least, at most, or about 3 wt.%, 4 wt.%, 5 wt.%, 6 wt.%, 7 wt.%, or 8 wt.%, or in an amount within a range defined by any two of these values. In one embodiment, the binder is present in an amount of at least, at most, or about 0.1 wt.%, 0.2 wt.%, 0.3 wt.%, 0.4 wt.%, 0.5 wt.%, 0.6 wt.%, 0.7 wt.%, 0.8 wt.%, 0.9 wt.%, or 1.0 wt.%, or within a range defined by any two of these values.
[0094] In one embodiment, any nickelate material described herein is a nickelate cathode material.
[0095] One embodiment is an alkaline electrochemical cell comprising any of the nickelate materials or compositions described herein.
[0096] refer to Figure 1 The embodiments will be better understood with the figures showing a cylindrical battery cell 1 in elevation cross section, wherein the battery cell has a nail-type or spool-type configuration and is sized comparable to a conventional LR6 (AA) sized alkaline battery cell, which is particularly suitable for these embodiments. However, it should be understood that the battery cells according to these embodiments may have other sizes and shapes (such as a prismatic shape or a button-type shape) and other electrode configurations as known in the art. Figure 1 The materials and designs of the components of the electrochemical cell shown in the drawings are for illustration purposes only, and other materials and designs may be substituted. In addition, in certain embodiments, the cathode material and the anode material may be coated onto the surface of the separator and / or the current collector and may be rolled to form a "jelly roll" configuration.
[0097] exist Figure 1In the embodiment, an electrochemical cell 1 is shown, which includes a container or can 10 having a closed bottom end 24, a top end 22, and a side wall 26 located therebetween. The closed bottom end 24 includes a terminal cover 20, which includes a protrusion. The can 10 has an inner wall 16. In the embodiment, the positive terminal cover 20 is welded or otherwise attached to the bottom end 24. In one embodiment, the terminal cover 20 can be formed of electroplated steel (e.g., electroplated steel with a small piece protruding at its central area). The container 10 can be formed of a metal such as steel, preferably electroplated with nickel, cobalt and / or other metals or alloys or other materials having sufficient structural properties compatible with various inputs in the electrochemical cell. The label 28 can be formed around the outer surface of the container 10 and can be formed on the outer peripheral edges of the positive terminal cover 20 and the negative terminal cover 46, as long as the negative terminal cover 46 is electrically insulated from the container 10 and the positive terminal 20.
[0098] Disposed within the container 10 are the first electrode 18 and the second electrode 12 and the separator 14 therebetween. The first electrode 18 is disposed within a space defined by the separator 14 and a closure assembly 40 secured to the open end 22 of the container 10. The closed end 24, the sidewall 26, and the closure assembly 40 define a cavity in which the electrodes of the battery cell are housed.
[0099] The closed assembly 40 includes a closed member 42 such as a gasket, a current collector 44, and a conductive terminal 46 in electrical contact with the current collector 44. The closed member 42 preferably contains a pressure relief port that will allow the closed member to rupture when the internal pressure of the battery cell becomes excessive. The closed member 42 can be formed of a polymer or elastomeric material (e.g., nylon-6,6), an injection moldable polymer blend (e.g., a polypropylene matrix combined with poly(phenylene oxide) or polystyrene), or another material (e.g., a metal), provided that the current collector 44 and the conductive terminal 46 are electrically insulated from the container 10 that serves as the current collector of the second electrode 12. In the embodiment shown, the current collector 44 is an elongated nail or spool-shaped component. The current collector 44 is made of a metal or metal alloy (e.g., copper or brass), a conductively plated metal or plastic current collector, etc. Other suitable materials can be used. The current collector 44 is inserted through a preferably centrally located hole in the closed member 42.
[0100] The first electrode 18 is preferably a negative electrode or anode. The negative electrode comprises a mixture of one or more active materials, a conductive material, solid zinc oxide, and a surfactant. The negative electrode may optionally contain other additives, such as a binder or a gelling agent, etc.
[0101] Zinc is an example primary active material for the negative electrode of the described embodiments. Mercury and magnesium may also be used. Preferably, the volume of active material used in the negative electrode is sufficient to maintain the desired particle-to-particle contact and the desired anode to cathode (A:C) ratio.
[0102] Particle-to-particle contact should be maintained during the useful life of the battery. If the volume of active material in the negative electrode is too low, the voltage of the cell may suddenly drop to an unacceptably low value when the cell is powered to a device. It is believed that the voltage drop is caused by the loss of continuity of the conductive matrix of the negative electrode. The conductive matrix can be formed by undischarged active material particles, conductive electrochemically formed oxides, or a combination thereof. The voltage drop may occur after the oxide begins to form, but before a sufficient network is established to bridge all active material particles present.
[0103] The alkaline electrolyte aqueous solution may include an alkaline metal hydroxide, such as potassium hydroxide (KOH), sodium hydroxide (NaOH), etc., or a mixture thereof. Potassium hydroxide is preferred. The alkaline electrolyte used to form the gelled electrolyte of the negative electrode contains an alkaline metal hydroxide in an amount of about 26 wt % to about 36 wt % (e.g., about 26 wt % to about 32 wt %, and specifically, about 26 wt % to about 30 wt %) based on the total weight of the alkaline electrolyte. There is an interaction between the negative electrode alkali metal hydroxide and the added solid zinc oxide, and it is found that lower alkali metal hydroxides improve DSC service. Electrolytes with lower alkalinity are preferred, but they may result in rapid electrolyte separation of the anode. An increase in the concentration of alkali metal hydroxides produces a more stable anode, but may reduce DSC service.
[0104] A gelling agent well known in the art is preferably utilized in the negative electrode, such as a cross-linked polyacrylic acid, such as that available from Noveon, Inc. of Cleveland, Ohio, USA. 940. Carboxymethyl cellulose, polyacrylamide and sodium polyacrylate are examples of other gelling agents suitable for alkaline electrolyte solutions. In order to maintain a substantially uniform dispersion of zinc and solid zinc oxide particles in the negative electrode, a gelling agent is desirable. The amount of gelling agent present is selected so that a low electrolyte separation rate is obtained and the anode viscosity at yield stress is not too large, which may cause anode dispersion problems.
[0105] Other components that may optionally be present in the negative electrode include, but are not limited to, gassing inhibitors, organic or inorganic corrosion inhibitors, plating agents, binders, or other surfactants. Examples of gassing inhibitors or corrosion inhibitors may include indium salts (such as indium hydroxide), perfluoroalkyl ammonium salts, alkali metal sulfides, and the like. In one embodiment, dissolved zinc oxide is preferably present by dissolving in the electrolyte to improve electroplating on bobbins or nail-type current collectors and reduce negative electrode shelf gassing. The added dissolved zinc oxide is separate and different from the solid zinc oxide present in the anode composition. In one embodiment, a level of dissolved zinc oxide in an amount of about 1% by weight based on the total weight of the negative electrode electrolyte is preferred. The BET surface area of soluble or dissolved zinc oxide measured using a Tristar 3000 BET specific surface area analyzer from Micrometrics (the analyzer has a multi-point calibration after zinc oxide is degassed at 150°C for one hour) is generally about 4 m 2 / g or less; and the particle size D50 (median diameter) measured using the CILAS particle size analyzer as indicated above is generally about 1 micron. In a further embodiment, in the negative electrode, in order to substantially prevent the battery cell from shorting through the separator during discharge of the battery cell, an amount of about 0.3 wt % sodium silicate based on the total weight of the negative electrode electrolyte is preferred.
[0106] The negative electrode can be formed in a variety of different ways known in the art. For example, the negative electrode components can be dry blended and added to the battery cell, with the alkaline electrolyte added separately, or as in a preferred embodiment, using a pre-gelled negative electrode process.
[0107] The second electrode 12 (also referred to herein as the positive electrode or cathode) has a nickelate compound (or "nickelate cathode material") as its electrochemically active material. The active material is present in an amount of generally about 80 wt% to about 98 wt%, and preferably about 81 wt% to 97 wt%, based on the total weight of the positive electrode (i.e., nickelate cathode material, binder, conductive material, positive electrode electrolyte, and additives (if present)).
[0108] The active cathode material can be a blend of nickelate cathode material with other active materials such as electrolytic manganese dioxide (EMD), chemical manganese dioxide (CMD), copper oxide, etc. The weight % of the nickel-containing compound can range from 5% to 100% of the total active cathode material. The positive electrode is formed by combining and mixing the desired components of the electrode, followed by dispersing a certain amount of the mixture into the open end of the container, and then using a punch to mold the mixture into a solid tubular configuration, the solid tubular configuration defining a cavity within the container, and the diaphragm 14 and the first electrode 18 are then placed in the cavity (referred to as impact molding). Figure 1As shown, the second electrode 12 has a ledge 30 and an inner surface 32. Alternatively, the positive electrode may be formed by preforming a plurality of rings from a mixture comprising the nickelate cathode material and then inserting the rings into a container to form a tubular shaped second electrode (referred to as ring molding). Figure 1 The cell shown would typically contain 3 or 4 rings.
[0109] The active material can be in the form of particles of any size suitable for use in an electrode mixture. In one embodiment, the active material is in the form of particles having an average size of about 1-20 microns, or 1-10 microns, or 1-5 microns, or 7-10 microns. In one embodiment, the active material is in the form of particles having a size in the range of 0.1-40 microns.
[0110] The cathode also includes a binder, which can be any binder known in the art. Non-limiting examples of binders include polyvinylidene fluoride (PVDF), polyethylene, polystyrene- and ethylene / propylene-based copolymers (such as those sold by Kraton Corporation (Houston, TX)), and polyvinylidene fluoride (PVDF). The binder may be in the form of particles of any size suitable for use in an electrode mixture.
[0111] The cathode also includes a conductive material, which can be conductive carbon. The conductive carbon can be graphite, and the graphite can be expanded graphite. The graphite can be in the form of particles of any size suitable for the electrode mixture. In one embodiment, the graphite is in the form of particles with an average size ranging from nanoparticle size to 65 microns. In one embodiment, the maximum size of the graphite particles is 110 microns.
[0112] An example of another cathode additive is barium sulfate (BaSO4), which is commercially available from Bario E. Derivati SpA of Massa, Italy. Barium sulfate is present in an amount generally from about 1 wt% to about 2 wt%, based on the total weight of the positive electrode. Other additives may include, for example, barium acetate, titanium dioxide, a binder (such as (Axalta Coating Systems, Glen Mills, PA) and calcium stearate.
[0113] One of the parameters used by cell designers characterizes the cell design as the ratio of the electrochemical capacity of one electrode to the electrochemical capacity of the opposite electrode, such as the ratio of the anode (A) to the cathode (C), i.e., the A:C ratio. For an LR6-type alkaline primary cell utilizing zinc in the negative electrode or anode and MnO2 in the positive electrode or cathode, the A:C ratio may be greater than 1.1:1, such as greater than 1.2:1, and specifically, 1.3:1 for an impact molded positive electrode. The A:C ratio of a ring molded positive electrode may be from about 1.3:1 to about 1.1:1.
[0114] A separator 14 is provided to separate the first electrode 18 from the second electrode 12. The separator 14 maintains the physical dielectric separation of the electrochemically active material of the positive electrode from the electrochemically active material of the negative electrode and allows ions to be transported between the electrode materials. In addition, the separator acts as a wicking medium for the electrolyte and a sleeve that prevents the fragmented portion of the negative electrode from contacting the top of the positive electrode. The separator 14 can be a layered ion-permeable nonwoven fiber fabric. Typical separators typically contain two or more layers of paper. Conventional separators are typically formed by preforming the separator material into a cup-shaped basket, which is then inserted under the cavity defined by the second electrode 12 and the closed end 24 and any positive electrode material located on the closed end; or during battery cell assembly, two rectangular separators are inserted into the cavity to form a basket with the materials rotated 90° relative to each other. Conventional preformed separators are typically made of a piece of nonwoven fabric that is rolled into a cylindrical shape that conforms to the inner wall of the second electrode and has a closed bottom end.
[0115] All references cited above and all patents, patent publications, and non-patent references cited herein are incorporated by reference in their entirety.
[0116] Although the embodiments have been shown and described in detail above, such illustrations and descriptions are to be regarded as illustrative or exemplary, rather than restrictive. It will be understood that changes and modifications may be made by those of ordinary skill in the art within the scope and spirit of the following claims. Specifically, the embodiments include any combination of features from the different embodiments described above and below.
[0117] The embodiments are further described by way of the following illustrative non-limiting examples that provide a better understanding of the embodiments and their many advantages. The following examples are included to illustrate the preferred embodiments. It should be understood by those skilled in the art that the techniques disclosed in the following examples represent the techniques used in the embodiments to work well in the practice of the embodiments and therefore can be considered to constitute the preferred mode of their practice. However, in light of the present disclosure, it should be understood by those skilled in the art that many changes may be made to the specific embodiments disclosed and still similar or similar results may be obtained without departing from the spirit and scope of the embodiments.
[0118] Discussion and Examples
[0119] Example 1: NaNiO2 synthesis
[0120] Granular Na2O2 ordered from Sigma Aldrich was poured into a Spex grinding vial until 1 / 3 full. The material was pre-ground for 30 minutes to reduce particle size. The desired amount of Ni(OH)2 was weighed into a crucible and the crucible was covered with a lid. The Ni(OH)2 was heated in a furnace at 650°C for 6 hours to be converted into NiO, which was verified by XRD. 13.1 g of the converted NiO was weighed out into a Spex grinding container and 9.3 g of pre-ground Na2O2 was added. The Spex grinding container was sealed with tape and ground for 5 minutes. The ground reagent mixture was transferred to a crucible with a lid; and heated at 680°C for 30 hours in air or oxygen. The final product was ground on a Spex mill for 10 minutes, if necessary. The final product must be handled in an argon glove box because the sample is sensitive to moisture in the air. The powder XRD patterns of the synthesized materials were analyzed using a D-8Advance X-ray diffractometer, and the phases identified were mainly NaNiO2, such as Figure 3 shown.
[0121] Example 2: Sodium removal / disproportionation by acid leaching
[0122] 17.4 g of the sample from Example 1 was leached with concentrated sulfuric acid to remove sodium (de-sodium). After acid leaching, the sample was filtered and washed with DI water through filter paper until the pH of the filtrate matched the pH of the DI water. The powder was dried at 71°C overnight. The final weight of the dried sample was 2.2 g, so the calculated yield was about 13%. The dried powder was identified by XRD as having sodium nickel hydride oxide (Na 0.33 NiO20.5 (H2O), PDF 04-015-9998), nickel oxyhydroxide (β-NiOOH, PDF 04-016-9895) and nickel oxide (NiO2, PDF 04-010-4751) mixed phase compounds, such as Figure 4 shown.
[0123] Example 3: Desodiumization and Oxidation with Persulfate
[0124] 100mL deionized (DI) water is added to a 250mL beaker. 43.2g Na2S2O8 purchased from GFS Chemicals (GFSChemical) is slowly added to a beaker of DI water stirred with a magnetic bar. The solution is stirred continuously until it is clear. 1.58g 50wt% NaOH is slowly added and stirred for 1 hour. 9.0g NaNiO2 synthesized in Example 1 is added to the solution very slowly in an exhaust hood because the reaction is exothermic and adding powder too quickly may cause bubbling overflow (the molar ratio of the obtained sodium persulfate to sodium nickel oxide is 2.3). After the powder is added, the beaker with the stirring set is moved to a Thermotron oven and the temperature is ramped to 40°C. The solution is stirred continuously for 20 hours at 40°C. The Thermotron is disconnected and the powder is allowed to settle for 15-30 minutes until the powder settles. The powder is filtered and washed with DI water through filter paper until the pH of the filtrate matches the pH of the DI water. The powder was dried at 71° C. overnight. The final weight of the dried sample was 7.2 g, which resulted in a yield of 80%, which is much higher than the yield (13%) in Example 2. The dried powder was identified as sodium nickel oxide hydride (Na 0.33 NiO20.5(H2O), PDF 04-015-9998), such as Figure 5 For better visualization, the Figure 5 The 2θ of sample 2 in the figure shifts to the right by 0.3 degrees.
[0125] Example 4: α-nickelate Li x NiO2 Synthesis
[0126] A lithium nickel oxide (LiNiO2) precursor is prepared and delithiated by acid leaching in a sulfuric acid solution (H.Arai and Y.Sakurai, J.Power Sources, 81-82 (1999) 401-405). The XRD pattern shows that the delithiated product is α-lithium nickel oxide (Li 0.09 Ni 0.01 )(NiO2), PDF 01-085-1976), and based on inductively coupled plasma atomic emission spectroscopy (ICP-AES), the composition is Li 0.104 NiO2.
[0127] Example 5: Half-cell testing on both fresh samples and samples aged at 70°C at 50% RH for 4 weeks
[0128] Some samples of dry powders from both Examples 3 and 4 were aged at 70°C at 50% relative humidity (RH) for 4 weeks. Both fresh and aged samples from Examples 3 and 4 were then discharged in a half-cell test apparatus to determine the electrochemical discharge capacity as follows: 49 wt% of the active material was mixed with 49% SFG 15 graphite and 2% coathylene binder to form a cathode mixture. 200 mg of the cathode mixture was pressed into a 357 coin cell can with a force of 5,000 lbf. The coin cell was placed into an acrylic plastic test fixture filled with 40 wt% KOH and 6 wt% ZnO; and the coin cell was discharged at a rate of 10 mA / g with a 1 hour rest for every 5 hours of discharge to observe voltage recovery. The discharge rate is based on the active material. Figure 6 The discharge curve of the material is shown. It can be seen from the figure that the fresh capacity of the α-nickelate in Example 4 (409 mAh / g at 1.0 V) is higher than the fresh capacity in Example 3 (sodium nickel oxyhydroxide Na 0.33 NiO20.5(H2O) (347 mAh / g)) has a higher cutoff voltage. However, the discharge capacity of the alpha nickelate material in Example 4 dropped dramatically to 157 mAh / g after the sample was aged at 70°C at 50% RH for 4 weeks. Under the same aging conditions, the discharge capacity of the sodium oxide nickel hydride material from Example 3 only slightly dropped to 327 mAh / g at 1.0 V. Therefore, in addition to its high yield, the sodium oxide nickel hydride sample from Example 3 is chemically more stable than the alpha nickelate from Example 4.
[0129] Example 6: β-Nickelate Synthesis
[0130] β-nickelate was synthesized based on the method described in US10,910,647B2 as follows. 8.6 g of finely ground LiOH·H2O and 20.9 g of Ni(OH)2 were mixed using a ball mill. The mixture was transferred to an alumina boat. The furnace was heated from room temperature to 800 °C at a rate of 5 °C / min under an O2 flow and held at 800 °C for 60 h. After cooling, the material was taken out of the furnace and ground in a Spex for 6 min. Then, at a temperature of 1 to 4 °C, the synthesized LiNiO2 powder was delithiated with 6 M H2SO4 at an electrolyte-to-powder weight ratio of 20:1 by continuous stirring for 20 h. The delithiated solid was washed with deionized (DI) water until the supernatant was nearly neutral (pH 6 - 7). The solid was collected by vacuum filtration and the material was dried at 60 °C overnight. To convert the material to β-nickelate, the powder was treated with a 36 wt% KOH solution at a powder-to-solution ratio of 3:1 at room temperature for 24 h. Then, the solid was washed with DI water and filtered until the filtrate was neutral. The collected solid was dried at 71 °C overnight. Based on the XRD spectrum in US10,910,647B2, the final material was confirmed to be β-nickelate.
[0131] Example 7: β-Nickelate pre-aged with LiOH
[0132] It has been shown that, compared with α-nickelate (US9,793,542B2), the stability of β-nickelate in a concentrated KOH electrolyte is improved. However, the stability of β-nickelate is still not as good as that of the conventional alkaline cathode material electrolytic manganese dioxide (EMD). In this application, it has been demonstrated that the stability of β-nickelate is improved by pre-aging with LiOH as follows: 40 mL of 1 M LiOH electrolyte was measured; and the LiOH solution was added to a vial containing 4 g of nickelate powder, and the vial was rotated to ensure that all the powder was coated. The powder was allowed to stand for 1 min, then the contents of the vial were poured into a filtering funnel, and DI water was used to transfer any remaining solid, and the product was washed with DI water until the filtrate pH was equal to 10. After filtration was completed, the solid product was placed in an oven at 71 °C and dried overnight.
[0133] As Figure 7 shown, in the XRD spectrum of β-nickelate, after pre-aging, in addition to β-nickelate at approximately 50.0 - 52.0, 53.6 - 56.8, 60.8 - 62.6, 66.4 - 67.5, and 67.4 - 68.6° 2θ, there are several additional characteristic peaks; and these peaks are related to lithium nickel oxides and sodium nickel oxides in the general form of M x Ni 1+y O2·nH2O (where M = Li or Na, 0 < x < 1, 0 < y < 0.2, 0 ≤ n ≤ 1).
[0134] Example 8: Half-cell test comparison between pre-aged and non-pre-aged β-nickelate at O / C ratio = 1
[0135] Both pre-aged and non-pre-aged β-nickelates were discharged in a cathode half-cell test apparatus to determine electrochemical discharge capacity as follows: 49 wt% of the active material was mixed with 49 wt% SFG 15 graphite (oxide to carbon ratio (O / C ratio) = 1) and 2 wt% coathylene binder to form a cathode mixture. 200 mg of the cathode mixture was pressed into a 357 coin cell can with a force of 5,000 lbf. The coin cell was placed in an acrylic plastic test fixture filled with 40 wt% KOH and 6 wt% ZnO; and the coin cell was discharged at a rate of 10 mA / g with a 1 hour rest for every 5 hours of discharge to observe voltage recovery. The discharge rate is based on the active material. Figure 8 The discharge curve of the material is shown. It can be seen from the figure that LiOH pre-aging has little effect on the cathode discharge energy.
[0136] Example 9: Half-cell test comparison between pre-aged β-nickelate mixed with EMD and non-pre-aged β-nickelate mixed with EMD at O / C ratio = 14.5
[0137] To test the cathode at an O / C ratio that more closely approximates actual cell conditions, beta nickelate before and after pre-aging was compared with Borman HD EMD, MX15 graphite, and Binder mix. The Ni content relative to the total Ni and Mn was 40 wt%, the combined EMD and nickelate in the mix was 93.1 wt%, MX15 graphite was 6.4 wt%, and coathylene (binder) was 0.5 wt%. The half-cell fixture and discharge protocol in this test were the same as those in Example 8. However, the cathodes in the half-cell tests here were aged in an oven at 60°C for up to 4 weeks before discharge. Fig. 9The discharge curves at 10 mA / g are compared. It can be easily seen from the figure that when the half-cell is fresh (0 weeks of aging), the discharge energy of the pre-aged β-nickelate is equal to the discharge energy of the non-pre-aged β-nickelate. However, the discharge voltage and energy of the battery cell with the pre-aged nickelate are higher after both aging for 1 week and 4 weeks at 60°C during the entire discharge process. For example, after aging for 1 week at 60°C, the discharge energy density of the pre-aged nickelate to reach a 1.0V cutoff value is 394mWh / g, which is higher than the discharge energy density of the non-pre-aged nickelate (382mWh / g). Therefore, pre-aging improves the stability of β-nickelate under high temperature storage, and it is expected that the shelf life of the battery with LiOH pre-aged β-nickelate will be longer than that of β-nickelate without pre-aging.
[0138] Example 10: Half-cell discharge of sodium nickelate desodiumized and oxidized by sulfate (PS sodium nickelate) and comparison with β-nickelate
[0139] The cathode having the sodium nickelate desodiumed and oxidized by sulfate (PS sodium nickelate) was discharged under the same conditions as in Example 9 and mixed with Fig.10 β-nickelates in the Fig.10 It can be seen from the discharge curves in that when the cathode is fresh (without any high temperature aging), the discharge energy density (mWh / g) of β-nickelate is higher than that of PS sodium nickelate. However, after aging at 60°C, the energy density of PS sodium nickelate is always higher than that of β-nickelate. For example, when the cathode is fresh (without any high temperature aging), the energy density of PS sodium nickelate is 1.5% lower than that of β-nickelate at 1.0V. However, when the cathode is aged at 60°C for 1 week and 4 weeks, respectively, the energy density of PS sodium nickelate is 3.6% and 5.3% higher than that of β-nickelate at 1.0V. Therefore, it is believed that the service retention of PS sodium nickelate as an alkaline cathode material will be better than that of β-nickelate.
[0140] Example 11: Half-cell discharge of cathode with EMD / PS sodium nickelate mixture
[0141] As is well known, nickel-containing materials are much more expensive than EMD (MnO2), and it would make more sense if a mixture of EMD and PS sodium nickelate were used as cathode materials by taking advantage of the low-cost EMD and high-performance nickelates. In order to study the synergistic effect of EMD and nickelates, a series of EMD / PS sodium nickelate mixtures with different levels of Niwt% were evaluated in a half-cell test. The test equipment and cathode formulation were the same as above (e.g., O / C = 14.5, and the total active material was 93.1wt%, and the binder % was 0.6wt%), and Fig.11 The discharge curves are given. The discharge voltage of the cathode mixture with nickelate is higher than that of the cathode with EMD, and it is not surprising that the voltage is higher with more nickelate. However, the energy of cathodes with high nickelate levels is not always higher than that of cathodes with low nickelate levels. For example, Fig.11 It is shown that at a voltage of about 1.15 V, the discharge curves of cathodes with 80 wt% and 90 wt% nickel (relative to the total weight of nickel and manganese) intersect with the cathode with 40 wt% nickel. Fig.12 It is clearly seen in Figure 1 that the graph is a plot of energy density at 1.0 V versus Ni wt%. More importantly, Fig.12 It is shown that the discharge efficiency in the case of 20-40wt% Ni is greater than that in the case of 97% Ni, while the discharge efficiency in the case of 60-100wt% Ni is in the range of 70% to 87%. Therefore, cathodes with 40wt% or less Ni wt% are more cost-effective. The discharge efficiency is Fig.11 The ratio of the discharge capacity (mAh / g) to 1.0 V to the EMD discharge capacity (285 mAh / g) and PS sodium nickelate discharge capacity (340 mAh / g) calculated when discharged at a rate of 10 mA / g under conditions similar to Example 8 with O / C=1.
Claims
1. A nickelate material having an X-ray diffraction (XRD) pattern, wherein the XRD pattern includes a first peak at about 12°-14° 2θ, a second peak at about 18°-21° 2θ, a third peak at about 24°-25° 2θ, and a fourth peak set at about 36°-43° 2θ. 2 . The nickelate material according to claim 1 , wherein the nickelate material is a desodiumated and oxidized sodium nickelate material.
3. The nickelate material according to any one of claims 1 to 2, wherein the desodiumed nickelate material is a desodiumed and oxidized nickelate hydride comprising the following phases: i) 40-90 wt% of a compound having the formula (Na x NiO2·nH2O), wherein 0.2≤x<1, and 0 <n<2; ii) nickel oxide (NiO2) in an amount of 5-40 wt%; and iii) β-nickel hydroxide (NiOOH) in an amount of 5-20 wt%.
4. A method for preparing a sulfate-treated, desodiumed, oxidized nickelate, the method comprising contacting sodium nickelate with a persulfate solution to produce the sulfate-treated, desodiumed, oxidized nickelate.
5. The method of claim 4, wherein the sulfate-treated, desodiumated and oxidized nickelate is a mixture of nickel oxide, sodium nickel oxide hydrate and / or nickel oxide hydroxide.
6. The method according to any one of claims 4 to 5, wherein the sulfate-treated, desodiumated, oxidized nickelate comprises the following phases: i) 40-90 wt% of a compound having the formula (Na x NiO2·nH2O), wherein 0.2≤x<1, and 0 <n<2; ii) nickel oxide (NiO2) in an amount of 5-40 wt%; and iii) β-nickel hydroxide (NiOOH) in an amount of 5-20 wt%.
7. The method of any one of claims 4 to 6, wherein the molar ratio of persulfate to nickel is about 2-4.
8. The method of any one of claims 4 to 7, wherein the sodium nickelate is contacted with the persulfate solution for a period of about 1-72 hours.
9. The process according to any one of claims 4 to 8, wherein the process is carried out at a temperature less than or equal to 50°C.
10. The method of any one of claims 4 to 9, wherein the pH of the persulfate solution is about 12-14.
11. The method according to any one of claims 4 to 10, wherein the persulfate solution comprises a persulfate selected from the group consisting of potassium persulfate and sodium persulfate.
12. A nickelate material prepared by the method according to any one of claims 4 to 11.
13. An alkaline cathode composition comprising the nickelate material according to any one of claims 1 to 3 and 12 and electrolytic manganese dioxide (EMD).
14. The composition of claim 13, wherein the ratio of nickel to manganese is about 99:1 to 1:99 by weight.
15. The composition of claim 14, wherein the ratio of nickel to manganese is about 10:90 to 50:50 by weight.
16. The composition of any one of claims 13 to 15, further comprising graphite and a binder.
17. The composition of claim 16, wherein the nickelate material is present in an amount of about 8.8-45.1 wt.%, the EMD is present in an amount of about 48-84.3 wt.%, the graphite is present in an amount of about 3-8 wt.%, and the binder is present in an amount of about 0.1-5 wt.%, relative to the total weight of the nickelate, the EMD, the graphite, and the binder.
18. The composition of claim 16, wherein the total weight percentage of the nickelate material and the EMD material combination is about 92-97 wt.%, the graphite is present in an amount of about 2-7 wt.%, and the binder is present in an amount of about 0.1-1.0 wt.%.
19. A pre-aged beta nickelate material, the pre-aged beta nickelate material having an X-ray diffraction (XRD) pattern, the XRD pattern comprising a first peak at about 50.0°-52.0°2θ, a second peak at about 53.6°-56.8°2θ, a third peak at about 60.8°-62.6°2θ, a fourth peak at about 66.4°-67.5°2θ, and a fifth peak at about 67.4°-68.6°2θ.
20. The pre-aged beta nickelate material of claim 19, wherein the beta nickelate material has been prepared by pre-aging the beta nickelate in a pre-aging solution comprising a hydroxide.
21. The pre-aged beta nickelate material of claim 20, wherein the pre-aging solution comprises a hydroxide selected from the group consisting of LiOH, NaOH, and KOH.
22. The pre-aged beta nickelate material of any one of claims 19 to 21, wherein the pre-aging solution has a hydroxide concentration of about 0.005 M to about 1 M.
23. The pre-aged beta nickelate material of any one of claims 19 to 22, wherein the ratio of the pre-aging solution to the beta nickelate is from about 1 mL / g to about 200 mL / g.
24. The pre-aged beta nickelate material of any one of claims 19 to 23, wherein the pre-aged beta nickelate has been pre-aged for a period of about 1-60 minutes.
25. The pre-aged beta nickelate material of any one of claims 19 to 24, wherein the pre-aging solution is at a temperature of about 0°C to about 40°C.
26. The pre-aged beta nickelate material of any one of claims 19 to 25, wherein the pre-aged beta nickelate comprises beta nickelate, nickel oxide, beta nickel oxyhydroxide, or a combination thereof.
27. A method of preparing a pre-aged beta nickelate material, the method comprising contacting a beta nickelate with a pre-aging solution comprising a hydroxide to produce the pre-aged nickelate material.
28. The method of claim 27, wherein the pre-aging solution comprises a hydroxide selected from the group consisting of LiOH, NaOH, and KOH.
29. The method of any one of claims 27 to 28, wherein the pre-aging solution has a hydroxide concentration of about 0.005 M to about 1 M.
30. The method of any one of claims 27 to 29, wherein the ratio of the pre-aging solution to the beta nickelate is from about 1 mL / g to about 200 mL / g.
31. The method of any one of claims 27 to 30, wherein the beta nickelate is contacted with the pre-aging solution for a period of time of about 1-60 minutes.
32. The method of any one of claims 27 to 31, wherein the pre-aging solution is at a temperature of about 0°C to about 40°C.
33. A beta nickelate material prepared by the method of any one of claims 27 to 32.
34. An alkaline cathode composition comprising the beta nickelate material of any one of claims 19 to 26 and 33 and electrolytic manganese dioxide (EMD).
35. The composition of claim 34, wherein the ratio of nickel to manganese is about 99:1 to 1:99 by weight.
36. The composition of claim 35, wherein the ratio of nickel to manganese is about 10:90 to 50:50 by weight.
37. The composition of any one of claims 34 to 36, further comprising graphite and a binder.
38. A composition according to claim 37, wherein the nickelate material is present in an amount of about 8.8-45.1 wt.%, the EMD is present in an amount of about 48-84.3 wt.%, the graphite is present in an amount of about 3-8 wt.%, and the binder is present in an amount of about 0.1-5 wt.%, relative to the total weight of the nickelate, the EMD, the graphite and the binder.
39. The composition of claim 37, wherein the total weight percentage of the nickelate material and the EMD material combination is about 92-97 wt.%, the graphite is present in an amount of about 2-7 wt.%, and the binder is present in an amount of about 0.1-1.0 wt.%.
40. An alkaline electrochemical cell comprising the nickelate material of any one of claims 1 to 3, 12, 19 to 26 or 33 or the composition of any one of claims 13 to 18 or 34 to 39.