Electronic component

By introducing the interface between alkali metal and alkaline earth metal oxides into the glass film of electronic components, the problems of increased melting point of conductive paste and insufficient flux resistance are solved, and higher flux resistance is achieved.

CN119096311APending Publication Date: 2024-12-06MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036449.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-10-28
Filing Date
2023-07-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When the amount of silicon dioxide is increased, the melting point of the conductive paste becomes high, which easily leads to cracks, and the flux resistance is insufficient, making it difficult to improve.

Method used

A glass film with alkali metal and alkaline earth metal oxide is used to prevent the water-soluble flux from entering, thereby improving flux resistance by introducing an interface into the glass film.

Benefits of technology

By introducing an interface into the glass film, the water-soluble flux is effectively prevented from immersing, the flux resistance of electronic components is improved, and the limitation of increasing the amount of silica in the conductive paste is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096311A_ABST
    Figure CN119096311A_ABST
Patent Text Reader

Abstract

A glass film (50) has a base part (51) and a specific part (52). The base portion (51) contains, in addition to a silicon oxide, an oxide of one or more metal elements selected from among an alkali metal and an alkaline earth metal. In addition to silicon oxide, the specific part (52) contains an oxide of the same metal element as the base part (51). The content ratio of the metal element in the specific part (52) is smaller than the content ratio of the metal element in the base part (51).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electronic component. Background Art

[0002] Patent Document 1 describes an electronic component. The electronic component includes a main body and an external electrode laminated on the surface of the main body. The external electrode is formed by firing a conductive paste. The conductive paste contains conductive powder, borosilicate glass, silica powder, and an organic vehicle.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent No. 5765041 Summary of the invention

[0006] The electronic component described in Patent Document 1 contains silicon dioxide powder in the external electrode. Therefore, the resistance to the surface treatment agent during welding, that is, the water-soluble flux, can be improved, that is, the so-called flux resistance can be improved. On the other hand, in the electronic component described in Patent Document 1, since the conductive paste contains silicon dioxide at a high concentration, the melting point of the conductive paste becomes high. Therefore, when the conductive paste is fired, cracks are easily generated in the main body, etc. Therefore, there is also a limit on increasing the amount of silicon dioxide. Therefore, in addition to adding silicon dioxide, a technology for improving flux resistance is also required.

[0007] In order to solve the above-mentioned problems, one method of the present invention is an electronic component, which has a main body, a glass film covering the outer surface of the above-mentioned main body, and an external electrode arranged on the outer surface of the above-mentioned glass film and having at least a base electrode, the above-mentioned glass film has a base part containing an oxide of one or more metal elements of alkali metals and alkaline earth metals in addition to silicon oxide, and a specific part containing an oxide of the same metal element as the above-mentioned base part in addition to silicon oxide, and the content ratio of the above-mentioned metal element in the above-mentioned specific part is smaller than the content ratio of the above-mentioned metal element in the above-mentioned base part.

[0008] According to the above configuration, the interface between the base and the specific portion can be present in the glass film. If the interface exists in the glass film, even if the water-soluble flux penetrates into the glass film, the water-soluble flux will extend to the interface and will be difficult to penetrate into deeper parts. Therefore, it is possible to further prevent corrosion from the outside to the main body.

[0009] The present invention has the effect of improving flux resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 This is a perspective view of an electronic component according to one embodiment.

[0011] Figure 2 This is a side view of an electronic component according to one embodiment.

[0012] Figure 3 It is along Figure 2 Cross-sectional view of line 3-3 in .

[0013] Figure 4 is included Figure 3 An enlarged cross-sectional view of the location of the glass membrane.

[0014] Figure 5 This is a flowchart illustrating a method for manufacturing an electronic component.

[0015] Figure 6 This is an explanatory diagram for explaining a method for manufacturing an electronic component.

[0016] Figure 7 This is an explanatory diagram for explaining a method for manufacturing an electronic component.

[0017] Figure 8 This is an explanatory diagram for explaining a method for manufacturing an electronic component.

[0018] Fig. 9 This is an explanatory diagram for explaining a method for manufacturing an electronic component.

[0019] Fig.10 This is an explanatory diagram for explaining a method for manufacturing an electronic component.

[0020] Fig.11 This is an explanatory diagram for explaining a method for manufacturing an electronic component.

[0021] Fig.12 This is an enlarged cross-sectional view including the position of the glass film of the electronic component according to the modification example. DETAILED DESCRIPTION

[0022] (One embodiment)

[0023] Hereinafter, one embodiment of the electronic component will be described with reference to the drawings. It should be noted that the drawings may enlarge the components for easier understanding. The dimensional ratios of the components may be different from the actual dimensions or dimensions in other drawings.

[0024] <Brief structure of electronic components>

[0025] like Figure 1 As shown, the electronic component 10 is, for example, a surface-mounted negative characteristic thermistor component mounted on a circuit board, etc. It should be noted that the negative characteristic thermistor component is a component having a characteristic that the resistance value decreases as the temperature rises.

[0026] The electronic component 10 includes a main body 20. The main body 20 is roughly quadrangular and has a central axis CA. It should be noted that, hereinafter, an axis extending along the central axis CA is set as the first axis X. In addition, an axis orthogonal to the first axis X is set as the second axis Y. Then, an axis orthogonal to the first axis X and the second axis Y is set as the third axis Z. Furthermore, one direction along the first axis X is set as the first positive direction X1, and the direction opposite to the first positive direction X1 in the direction along the first axis X is set as the first negative direction X2. In addition, one direction along the second axis Y is set as the second positive direction Y1, and the direction opposite to the second positive direction Y1 in the direction along the second axis Y is set as the second negative direction Y2. Furthermore, one direction along the third axis Z is set as the third positive direction Z1, and the direction opposite to the third positive direction Z1 in the direction along the third axis Z is set as the third negative direction Z2.

[0027] The outer surface 21 of the main body 20 has six planes 22. It should be noted that the "plane" of the main body 20 mentioned here refers to the plane that can be observed as a plane when observing the entire main body 20. In other words, even if there are tiny bumps and steps that can only be seen by magnifying and observing a part of the main body 20 with a microscope, etc., they are also expressed as planes or curved surfaces. The six planes 22 extend in different directions. The six planes 22 are roughly divided into a first end face 22A facing the first positive direction X1, a second end face 22B facing the first negative direction X2, and four side faces 22C. The four side faces 22C are respectively a face facing the third positive direction Z1, a face facing the third negative direction Z2, a face facing the second positive direction Y1, and a face facing the second negative direction Y2.

[0028] The outer surface 21 of the main body 20 has 12 boundary surfaces 23. The boundary surfaces 23 include curved surfaces existing at the boundaries between adjacent flat surfaces 22. That is, the boundary surfaces 23 include curved surfaces formed by, for example, rounding the corners of the adjacent flat surfaces 22.

[0029] In addition, the outer surface 21 of the main body 20 has eight spherical corner surfaces 24. The corner surface 24 is a boundary portion between three adjacent planes 22. In other words, the corner surface 24 includes a curved surface at a portion where three boundary surfaces 23 intersect. That is, the corner surface 24 includes, for example, a curved surface formed by rounding the corner formed by the three adjacent planes 22.

[0030] It should be noted that Figure 1 and Figure 2 In the figure, the surface of the glass film 50 described later is regarded as the same as the outer surface 21 of the main body 20 and is denoted by a reference numeral.

[0031] like Figure 2 As shown in FIG. 1 , the dimension of the main body 20 along the first axis X is larger than the dimension along the third axis Z. Figure 1 As shown, the dimension of the body 20 along the first axis X is larger than the dimension along the second axis Y. The body 20 is made of ceramics fired from a metal oxide containing at least one of Mn, Fe, Ni, Co, Ti, Ba, Al and Zn as a component.

[0032] like Figure 3 As shown, the electronic component 10 includes two first internal electrodes 41 and two second internal electrodes 42 . The first internal electrodes 41 and the second internal electrodes 42 are buried inside the body 20 .

[0033] The first internal electrode 41 is made of a conductive material. For example, the first internal electrode 41 is made of silver and palladium. The second internal electrode 42 is made of the same silver and palladium as the first internal electrode 41 .

[0034] The first internal electrode 41 has a rectangular plate shape. The main surface of the first internal electrode 41 is perpendicular to the second axis Y. The second internal electrode 42 has the same rectangular plate shape as the first internal electrode 41. The main surface of the second internal electrode 42 is perpendicular to the second axis Y as the first internal electrode 41.

[0035] The dimension of the first internal electrode 41 along the first axis X is smaller than the dimension of the main body 20 along the first axis X. Figure 1 As shown, the dimension of the first inner electrode 41 along the third axis Z is approximately two thirds of the dimension of the body 20 along the third axis Z. The dimensions of the second inner electrode 42 in each direction are the same as those of the first inner electrode 41 .

[0036] like Figure 3 As shown in FIG. 2 , the first internal electrode 41 and the second internal electrode 42 are located at different positions in the direction along the second axis Y. That is, from the side surface 22C facing the second positive direction Y1 to the second negative direction Y2, the first internal electrode 41, the second internal electrode 42, the first internal electrode 41, and the second internal electrode 42 are arranged in this order. In the present embodiment, the distances between the internal electrodes in the direction along the second axis Y are equal.

[0037] like Figure 1 As shown in FIG. 1 , the two first internal electrodes 41 and the two second internal electrodes 42 are both located at the center of the body 20 in the direction along the third axis Z. Figure 3 As shown in FIG. 1 , the first inner electrode 41 is located closer to the first positive direction X1 , and the second inner electrode 42 is located closer to the first negative direction X2 .

[0038] Specifically, the end of the first inner electrode 41 on the first positive direction X1 side coincides with the end of the body 20 on the first positive direction X1 side. The end of the first inner electrode 41 on the first negative direction X2 side is located inside the body 20 and does not reach the end of the body 20 on the first negative direction X2 side. On the other hand, the end of the second inner electrode 42 on the first negative direction X2 side coincides with the end of the body 20 on the first negative direction X2 side. The end of the second inner electrode 42 on the first positive direction X1 side is located inside the body 20 and does not reach the end of the body 20 on the first positive direction X1 side.

[0039] The electronic component 10 includes a glass film 50. The glass film 50 covers the outer surface 21 of the main body 20. In the present embodiment, the glass film 50 covers almost all of the outer surface 21 of the main body 20. The main material of the glass film 50 is insulating glass. Therefore, the glass film 50 contains silicon oxide, specifically silicon dioxide.

[0040] like Figure 3 As shown, the electronic component 10 includes a first external electrode 61 and a second external electrode 62. The first external electrode 61 includes a first base electrode 61A and a first metal layer 61B. The first base electrode 61A is laminated on a portion of the outer surface 21 of the main body 20 including the first end surface 22A from the glass film 50. Specifically, the first base electrode 61A is a five-sided electrode covering a portion of the first end surface 22A and four side surfaces 22C of the main body 20 on the first positive direction X1 side. In the present embodiment, the material of the first base electrode 61A is copper.

[0041] The first metal layer 61B covers the first base electrode 61A from the outside. Therefore, the first metal layer 61B is stacked on the first base electrode 61A. Specifically, Figure 4 As shown in FIG. 1 , the first metal layer 61B is a double-layer structure of a nickel layer 61C and a tin layer 61D. Figure 3 As shown, the outer edge of the first metal layer 61B is located outside the outer edge of the first base electrode 61A. Also, the outer edge of the first metal layer 61B is located on the surface of the glass film 50. Therefore, a portion of the first metal layer 61B is located on the surface of the glass film 50.

[0042] like Figure 3 As shown, the second external electrode 62 includes a second base electrode 62A and a second metal layer 62B. The second base electrode 62A is laminated on a portion of the outer surface 21 of the body 20 including the second end surface 22B from the glass film 50. Specifically, the second base electrode 62A is a five-sided electrode covering a portion of the second end surface 22B and four side surfaces 22C of the body 20 on the first negative direction X2 side. In the present embodiment, the material of the second base electrode 62A is the same as that of the first external electrode 61, that is, copper.

[0043] The second metal layer 62B covers the second base electrode 62A from the outside. Therefore, the second metal layer 62B is stacked on the second base electrode 62A. Specifically, although the second metal layer 62B is not shown in the figure, it has a double-layer structure of a nickel layer and a tin layer like the first metal layer 61B. Figure 3 As shown, the outer edge of the second metal layer 62B is located outside the outer edge of the second base electrode 62A. Furthermore, the outer edge of the second metal layer 62B is located on the surface of the glass film 50. Therefore, a part of the second metal layer 62B is located on the surface of the glass film 50.

[0044] The second external electrode 62 does not reach the first external electrode 61 on the side surface 22C, but is arranged separately from the first external electrode 61 in the direction along the first axis X. Moreover, on the side surface 22C of the body 20, the first external electrode 61 and the second external electrode 62 are not stacked in the central portion along the direction of the first axis X, and the glass film 50 is exposed. Figure 1 to Figure 3 In FIG. 6 , the first external electrode 61 and the second external electrode 62 are indicated by two-dot chain lines.

[0045] like Figure 3 As shown, the first external electrode 61 and the end of the first internal electrode 41 on the first positive direction X1 side are connected via a first through portion 71 that penetrates the glass film 50. It should be noted that, although the details will be described later, the first through portion 71 is formed by extending the silver and palladium constituting the first internal electrode 41 toward the first external electrode 61 side during the manufacturing process of the electronic component 10.

[0046] In addition, the second external electrode 62 and the end of the second internal electrode 42 on the first negative direction X2 side are connected via a second through portion 72 that penetrates the glass film 50. The second through portion 72 is also formed by extending the silver and palladium constituting the second internal electrode 42 toward the second external electrode 62 side during the manufacturing process of the electronic component 10, similarly to the first through portion 71. Figure 3 In the figure, the first internal electrode 41 and the first through-hole 71 are shown as other components having a boundary, but in reality, there is no clear boundary between the two. This is also true for the second through-hole 72. Figure 1 and Figure 2 In the figure, the first through portion 71 and the second through portion 72 are omitted.

[0047] <About glass film>

[0048] The portion of the glass film 50 not covered by both the first and second base electrodes 61A and 62A is a substantially uniform silicon dioxide glass layer. On the other hand, the portion of the glass film 50 covered by either the first and second base electrodes 61A and 62A is a mixture of two glass layers having different compositions.

[0049] Specifically, if Figure 4 As shown, the glass film 50 has a base portion 51 and a specific portion 52. Most of the base portion 51 and the specific portion 52 are located between the first base electrode 61A in the glass film 50 and the outer surface 21 of the main body 20, and between the second base electrode 62A and the outer surface 21 of the main body 20. In addition to silicon oxide, the base portion 51 also contains oxides of one or more metal elements among alkali metals and alkaline earth metals. In this embodiment, the metal element is barium. In this embodiment, the base portion 51 contains oxides of barium and calcium among alkaline earth metals. In addition, the base portion 51 contains zinc oxide. Furthermore, the base portion 51 contains aluminum oxide.

[0050] When observed in cross section, the specific portion 52 is in a flat layer shape. The specific portion 52 contains an oxide of the same metal element as the base portion 51 in addition to silicon oxide. That is, in the present embodiment, the specific portion 52 contains an oxide of barium among alkaline earth metals. On the other hand, the specific portion 52 contains an oxide of calcium. In addition, the specific portion 52 contains an oxide of zinc. On the other hand, the specific portion 52 contains an oxide of aluminum.

[0051] Furthermore, the content ratio of the metal element, that is, barium, in the specific portion 52 is lower than the content ratio of the metal element, that is, barium, in the base portion 51. Furthermore, the content ratio of silicon in the specific portion 52 is higher than the content ratio of silicon in the base portion 51. In addition, the content ratio of zinc in the specific portion 52 is higher than the content ratio of zinc in the base portion 51.

[0052] <Method for manufacturing electronic components>

[0053] Next, a method for manufacturing the electronic component 10 will be described.

[0054] like Figure 5 As shown, the method for manufacturing the electronic component 10 includes a laminate preparation step S11, a rounding processing step S12, a solvent introduction step S13, a catalyst introduction step S14, a main body introduction step S15, a polymer introduction step S16, and a metal alkoxide introduction step S17. In addition, the method for manufacturing the electronic component 10 further includes a film forming step S18, a drying step S19, a firing step S20, a conductor coating step S21, a curing step S22, and a plating step S23.

[0055] First, when forming the main body 20, in the laminate preparation step S11, a laminate is prepared as the main body 20 without the boundary surface 23 and the corner surface 24. That is, the laminate is in a state before rounding, and is a rectangular parallelepiped with 6 planes 22. For example, first, a plurality of ceramic sheets forming the main body 20 are prepared. The sheet is in the shape of a thin plate. A conductive paste for forming the first internal electrode 41 is stacked on the sheet. A ceramic sheet for forming the main body 20 is stacked on the laminate paste. A conductive paste for forming the second internal electrode 42 is stacked on the sheet. Thus, ceramic sheets and conductive paste are stacked. Then, an unfired laminate is formed by cutting into a specified size. Then, the unfired laminate is fired at a high temperature to prepare the laminate.

[0056] Next, a chamfering process S12 is performed. In the chamfering process S12, a boundary surface 23 and a corner surface 24 are formed with respect to the laminated body prepared in the laminated body preparation process S11. For example, the corners of the laminated body are chamfered by roller grinding, thereby forming a boundary surface 23 having a curved surface and a corner surface 24 having a curved surface. Thus, the main body 20 is formed.

[0057] Next, the solvent adding step S13 is performed. Figure 6 As shown, in the solvent adding step S13 , 2-propanol is added as the solvent 82 into the reaction container 81 .

[0058] Then, if Figure 5 As shown, the catalyst adding step S14 is performed. Figure 7 As shown, in the catalyst introduction step S14, first, stirring of the solvent 82 in the reaction container 81 is started. Then, ammonia water is introduced into the reaction container 81 as an aqueous solution 83 containing a catalyst. The catalyst in this embodiment is a hydroxide ion, which functions as a catalyst for promoting hydrolysis of a metal alkoxide 85 described later.

[0059] Then, if Figure 5 As shown, the main body input process S15 is performed. Figure 8 As shown, in the main body loading step S15 , the plurality of main bodies 20 formed in advance in the chamfering step S12 as described above are loaded into the reaction container 81 .

[0060] Then, if Figure 5 As shown, the polymer feeding step S16 is performed. Fig. 9 As shown, in the polymer introduction step S16 , polyvinyl pyrrolidone is introduced into the reaction container 81 as the polymer 84 . Thus, the polymer 84 introduced into the reaction container 81 is adsorbed on the outer surface 21 of the main body 20 .

[0061] Then, if Figure 5 As shown, the metal alkoxide adding step S17 is performed. Fig.10 As shown, in the metal alkoxide feeding step S17, liquid tetraethyl orthosilicate is fed into the reaction vessel 81 as the metal alkoxide 85. It should be noted that tetraethyl orthosilicate is sometimes also referred to as tetraethoxysilane. In the present embodiment, the amount of the metal alkoxide 85 fed in the metal alkoxide feeding step S17 is calculated based on the area of ​​the outer surface 21 of the main body 20 fed in the main body feeding step S15. Specifically, the amount of the metal alkoxide 85 of each main body 20 required to form the pre-diffusion glass film 50A covering the outer surface 21 of the main body 20 is calculated. As described later, the pre-diffusion glass film 50A is a film in a state before the metal elements contained in the glass of the conductor paste are diffused. That is, the pre-diffusion glass film 50A is in a state without containing the metal elements from the conductor paste.

[0062] Then, if Figure 5 As shown, the film forming step S18 is performed. Fig.11 As shown, in the film forming step S18, after the metal alkoxide 85 is introduced into the reaction vessel 81 in the metal alkoxide introduction step S17, the stirring of the solvent 82 started in the solvent introduction step S13 is continued for a predetermined time. In the film forming step S18, the pre-diffusion glass film 50A is formed by a liquid phase reaction in the reaction vessel 81.

[0063] Then, if Figure 5 In the drying step S19, after stirring is continued for a predetermined time in the film forming step S18, the main body 20 is taken out from the reaction container 81 and dried. Thus, the sol-like pre-diffusion glass film 50A is dried to become a gel-like pre-diffusion glass film 50A.

[0064] Next, a firing step S20 is performed. In the firing step S20, the main body 20 covered with the gel-like pre-diffusion glass film 50A is heated. Thus, water and polymer 84 are vaporized from the gel-like pre-diffusion glass film 50A. As a result, the pre-diffusion glass film 50A made of silicon dioxide is formed.

[0065] Next, the conductor coating step S21 is performed. In the conductor coating step S21, a conductor paste is applied to two locations on the surface of the pre-diffusion glass film 50A, including a portion of the portion covering the first end face 22A of the main body 20 and a portion of the portion covering the second end face 22B of the main body 20. Specifically, the conductor paste is applied so as to cover the entire area of ​​the first end face 22A and a portion of the glass film 50 on the four side faces 22C. In addition, the conductor paste is applied so as to cover the entire area of ​​the second end face 22B and a portion of the pre-diffusion glass film 50A on the four side faces 22C. The conductor paste contains copper powder, glass, and an organic medium. The copper powder of the conductor paste becomes the first base electrode 61A and the second base electrode 62A through the subsequent curing step S22. The glass of the conductor paste has an additive containing one or more metal elements of alkali metals and alkaline earth metals. More specifically, the metal element is barium. Furthermore, the conductor paste contains calcium, aluminum, and zinc as an additive.

[0066] Next, the curing step S22 is performed. Specifically, in the curing step S22, the pre-diffusion glass film 50A and the main body 20 coated with the conductive paste are heated. As a result, the organic medium in the conductive paste is vaporized. Then, the copper powder in the conductive paste is integrated to form the first base electrode 61A and the second base electrode 62A. In other words, the material of the first base electrode 61A and the second base electrode 62A is copper. It should be noted that the first base electrode 61A and the second base electrode 62A may also not contain impurities.

[0067] At the same time, the glass in the conductor paste melts and becomes one with a part of the front-diffusion glass film 50A. However, the front-diffusion glass film 50A is basically composed of only silicon oxide at the start of the curing step S22. Therefore, the melting point of the front-diffusion glass film 50A is high. Therefore, a part of the front-diffusion glass film 50A does not become one with the glass of the conductor paste and remains. However, at this time, the metal elements contained in the additives of the glass in the conductor paste diffuse into the front-diffusion glass film 50A composed of silicon dioxide. As a result, the metal elements enter the front-diffusion glass film 50A covering the outer surface 21 of the main body 20. Then, if the main body 20 is fired, the mixture of the glass from the conductor paste and the front-diffusion glass film 50A becomes the base 51. On the other hand, the front-diffusion glass film 50A that does not become one with the glass of the conductor paste and remains becomes a specific part 52. As described above, the metal elements also diffuse into the front-diffusion glass film 50A that does not become one with the glass of the conductor paste and remains. Therefore, the specific portion 52 contains the metal element, although in a smaller amount than the base portion 51 .

[0068] The metal element hardly diffuses in the portion of the pre-diffusion glass film 50A not covered with the conductive paste. Therefore, the portion of the pre-diffusion glass film 50A not covered with the conductive paste is a substantially uniform glass layer without distinction between the base portion 51 and the specific portion 52 .

[0069] In the present embodiment, during heating in the curing step S22, due to the Kirkendall effect caused by the difference in diffusion speed between the first internal electrode 41 and the first base electrode 61A, silver and palladium contained in the first internal electrode 41 side are attracted to the first base electrode 61A side which is copper. As a result, the first through-portion 71 extends from the first internal electrode 41 toward the first base electrode 61A to penetrate the glass film 50, and the first internal electrode 41 is connected to the first base electrode 61A. This is also the case with the second through-portion 72 connecting the second internal electrode 42 to the second base electrode 62A.

[0070] Next, a plating step S23 is performed. In the plating step S23, the first base electrode 61A and the second base electrode 62A are electroplated. Thus, the first metal layer 61B is formed on the surface of the first base electrode 61A. In addition, the second metal layer 62B is formed on the surface of the second base electrode 62A. Figure 4 As shown, the first metal layer 61B is electroplated with nickel and tin to form a double-layer structure having a nickel layer 61C and a tin layer 61D. Although not shown in the figure, similarly to the first metal layer 61B, the second metal layer 62B is electroplated with nickel and tin in sequence to form a double-layer structure of a nickel layer and a tin layer. Thus, the electronic component 10 is formed.

[0071] (Effects of Implementation Methods)

[0072] The electronic component 10 of the above embodiment is surface treated with a water-soluble flux when soldered to a substrate, etc. At this time, the water-soluble flux penetrates into the glass film 50 from the interface between the first external electrode 61 and the glass film 50 , and may further penetrate into the body 20 .

[0073] (Effects of Embodiments)

[0074] (1) According to the above embodiment, the glass film 50 has a base 51 and a specific portion 52. Furthermore, the specific portion 52 contains silicon oxide and an oxide of a metal element. Furthermore, the content ratio of the metal element in the specific portion 52 is smaller than the content ratio of the metal element in the base 51. Therefore, in the glass film 50, there can be an interface between the base 51 and the specific portion 52. If an interface also exists in the glass film like this, even if it is assumed that the water-soluble flux is impregnated into the glass film, the water-soluble flux will extend to the interface. Therefore, it is difficult for the impregnated water-soluble flux to penetrate deeper into the interface between the base 51 and the specific portion 52. Thus, erosion from the outside to the main body 20 is further prevented. Therefore, according to the above embodiment, it is not necessary to add silica powder to improve flux resistance.

[0075] (2) According to the above embodiment, the silicon content of the specific portion 52 is greater than that of the base portion 51. Thus, the composition of the specific portion 52 is different from that of the base portion 51. Thus, the interface between the base portion 51 and the specific portion 52 becomes clearer.

[0076] (3) According to the above embodiment, the metal element is barium among alkaline earth metals. Barium is relatively easy to obtain among alkaline earth metals. Therefore, it is not necessary to prepare an element that is difficult to obtain.

[0077] (4) According to the above embodiment, the specific portion 52 contains zinc oxide. Therefore, the inclusion of zinc makes it easier to obtain a stable composition containing barium which is an alkaline earth metal.

[0078] (5) According to the above embodiment, the zinc content of the specific portion 52 is greater than the zinc content of the base portion 51. Therefore, the composition of the specific portion 52 is different from that of the base portion 51. As a result, the interface between the base portion 51 and the specific portion 52 becomes clearer.

[0079] (6) According to the above embodiment, the first external electrode 61 has the first metal layer 61B. Therefore, the electronic component 10 is likely to be mounted on a substrate or the like by soldering for use. In other words, the electronic component 10 is likely to be exposed to the water-soluble flux. Therefore, the effect of preventing the infiltration of the water-soluble flux is significant.

[0080] (7) According to the above embodiment, the first metal layer 61B extends over a wider range than the first base electrode 61A. Therefore, a portion of the first metal layer 61B is also located on the surface of the glass film 50. Thus, when the outer edge of the first metal layer 61B is located outside the outer edge of the first base electrode 61A, it is possible to prevent a gap from being generated between the first external electrode 61 and the glass film 50. By preventing the generation of such a gap, it is easy to prevent the water-soluble flux from infiltrating from between the first external electrode 61 and the glass film 50.

[0081] (Other embodiments)

[0082] The above-mentioned embodiment can be implemented by making the following modifications. The above-mentioned embodiment and the following modifications can be implemented in combination within the scope of no technical contradiction.

[0083] In the above embodiment, the electronic component 10 is not limited to a negative characteristic thermistor component. For example, as long as some wiring is provided inside the body 20, the electronic component 10 may be a thermistor component other than a negative characteristic component, a multilayer capacitor component, or an inductor component.

[0084] The material of the main body 20 is not limited to the example of the above embodiment. The material of the main body 20 may be a composite of resin and metal powder.

[0085] The shape of the main body 20 is not limited to the example of the above-mentioned embodiment. For example, the main body 20 may be a polygonal prism other than a quadrangular prism having a central axis CA. In addition, the main body 20 may be a core of a winding type inductor component. For example, the core may be a so-called drum core shape. Specifically, the core may also have a columnar winding core portion and flange portions provided at each end of the winding core portion.

[0086] The outer surface 21 of the main body 20 may not have the boundary surface 23 and the corner surface 24. For example, when the boundary between adjacent planes 22 in the outer surface 21 of the main body 20 is not chamfered, there is no curved surface on the boundary. Therefore, in this case, the boundary surface 23 and the corner surface 24 may not exist.

[0087] In the above embodiment, the shapes of the first internal electrode 41 and the second internal electrode 42 can be any shapes as long as they can ensure electrical conduction with the corresponding first external electrode 61 and the second external electrode 62. In addition, regardless of the number of the first internal electrodes 41 and the second internal electrodes 42, the number of internal electrodes may be one or three or more.

[0088] The structure of the first external electrode 61 is not limited to the above-described embodiment. For example, the first external electrode 61 may be composed of only the first base electrode 61A, or the first metal layer 61B may not be a double-layer structure. The second external electrode 62 is also similar in this regard.

[0089] In the above embodiment, the combination of the materials of the first internal electrode 41 and the first base electrode 61A is not limited to the combination of copper on one side and silver and palladium on the other side. For example, it may be a combination of palladium and silver, copper and nickel, copper and silver, copper and palladium, silver and gold, nickel and cobalt, or nickel and gold. Another example is a combination of copper on one side and copper and nickel on the other side. Another example is a combination of nickel on one side and copper and nickel on the other side. Another example is a combination of gold on one side and silver and palladium on the other side.

[0090] ·It should be noted that the Kirkendall effect may not be obtained depending on the combination of the first internal electrode 41 and the first base electrode 61A. In this case, processing may be performed before the external electrode forming step to expose the first internal electrode 41. For example, the first end surface 22A side of the main body 20 may be polished to physically remove a portion of the glass film 50. Then, by performing the base electrode forming step, the first internal electrode 41 and the first base electrode 61A can be connected. For example, after the first base electrode 61A is formed, the glass film 50 including the surface of the first base electrode 61A is formed, and then the glass film 50 covering the surface of the first base electrode 61A is removed. This is also the same in the combination of the materials of the second internal electrode 42 and the second base electrode 62A.

[0091] The arrangement position of the first external electrode 61 is not limited to the example in the above embodiment. For example, the first external electrode 61 may be arranged only on the first end surface 22A and one side surface 22C. The second external electrode 62 is also similar in this regard.

[0092] <About glass film>

[0093] The glass film 50 does not have to cover the entire area of ​​the outer surface 21 of the main body 20. The range covered by the glass film 50 can be appropriately changed along with the shape of the main body 20, the positions of the first external electrode 61 and the second external electrode 62, and the like.

[0094] The metal element contained in the glass film 50 may also be an alkali metal. In addition, the metal element contained in the glass film 50 may also be any one of lithium, sodium, and potassium among alkali metals. It should be noted that lithium, sodium, and potassium are relatively easy to obtain among alkali metals. Therefore, it is not necessary to prepare an element that is difficult to obtain.

[0095] The metal element contained in the glass film 50 may be calcium among alkaline earth metals. In addition, the metal contained in the glass film 50 may be other metals among alkaline earth metals.

[0096] The specific portion 52 may also contain aluminum oxide. The specific portion 52 may also contain zinc oxide. In addition, the base portion 51 and the specific portion 52 may also contain additives of other elements. Depending on the content ratio of other elements, the content ratio of silicon in the specific portion 52 may be lower than the content ratio of silicon in the base portion 51.

[0097] The base portion 51 may not contain aluminum oxide. The base portion 51 may not contain zinc oxide. Furthermore, the zinc content of the specific portion 52 may be lower than the zinc content of the base portion 51 .

[0098] The material of the glass film 50 is not limited to the examples of the above-mentioned embodiments. For example, the glass is not limited to silicon dioxide, but may be a multi-component oxide containing Si, such as B-Si, Si-Zn, Zr-Si, and Al-Si oxides. In addition, the glass may be a multi-component oxide containing alkali metals and Si, such as Al-Si, Na-Si, K-Si, and Li-Si oxides. Furthermore, the glass may be a multi-component oxide containing alkaline earth metals and Si, such as Mg-Si, Ca-Si, Ba-Si, and Sr-Si. In addition, the glass may not contain Si, or may be a mixture thereof. When the material of the glass film 50 contains boron, the specific portion 52 may also contain boron oxide. In addition, in this case, the base portion 51 may also contain boron oxide.

[0099] In addition, the material of the glass film 50 may contain a pigment, a silicone-based flame retardant, a silane coupling material, a titanate coupling agent, or a surface treatment agent or an antistatic agent in addition to glass.

[0100] More specifically, the glass film 50 may contain, in addition to glass, additives such as organic acid salts, oxides, inorganic salts, organic salts, and fine particles and nanoparticles of other metal oxides.

[0101] Examples of the organic acid salt include salts of oxo acids such as soda ash, sodium carbonate, sodium bicarbonate, sodium percarbonate, sodium sulfite, sodium bisulfite, sodium sulfate, sodium thiosulfate, sodium nitrate, and sodium sulfite; and halogen compounds such as sodium fluoride, sodium chloride, sodium bromide, and sodium iodide.

[0102] In addition, examples of oxides include sodium peroxide, and examples of hydroxides include sodium hydroxide.

[0103] Examples of the inorganic salt include sodium hydride, sodium sulfide, sodium hydrogen sulfide, sodium silicate, trisodium phosphate, sodium borate, sodium borohydride, sodium cyanide, sodium cyanate, and sodium tetrachloroaurate.

[0104] Examples of the inorganic salt include calcium peroxide, calcium hydroxide, calcium fluoride, calcium chloride, calcium bromide, calcium iodide, calcium hydride, calcium carbide, and calcium phosphide.

[0105] In addition, the additive may be calcium carbonate, calcium hydrogen carbonate, calcium nitrate, calcium sulfate, calcium sulfite, calcium silicate, calcium phosphate, calcium pyrophosphate, calcium hypochlorite, calcium chlorate, calcium perchlorate, calcium bromate, calcium iodate, calcium arsenite, calcium chromate, calcium tungstate, calcium molybdate, calcium magnesium carbonate, hydroxyapatite and the like oxoacid salts. In addition, the additive may include calcium acetate, calcium gluconate, calcium citrate, calcium malate, calcium lactate, calcium benzoate, calcium stearate, calcium aspartate.

[0106] For example, the additive can also be lithium carbonate, lithium chloride, lithium titanate, lithium nitride, lithium peroxide, lithium citrate, lithium fluoride, lithium hexafluorophosphate, lithium acetate, lithium iodide, lithium hypochlorite, lithium tetraborate, lithium bromide, lithium nitrate, lithium hydroxide, lithium aluminum hydride, lithium triethylborohydride, lithium hydride, lithium amide, lithium imide, lithium diisopropylamide, lithium tetramethylpiperidinium, lithium sulfide, lithium sulfate, lithium thiophenol, and lithium phenol.

[0107] For example, the additive may be boron triiodide, sodium cyanoborohydride, sodium borohydride, tetrafluoroboric acid, triethylborane, borax or boric acid.

[0108] For example, the additive may be potassium arsenide, potassium bromide, potassium carbide, potassium chloride, potassium fluoride, potassium hydride, potassium iodide, potassium triiodide, potassium azide, potassium nitride, potassium superoxide, potassium ozonide, potassium peroxide, potassium phosphide, potassium sulfide, potassium selenide, potassium telluride, potassium tetrafluoroaluminate, potassium tetrafluoroborate, potassium tetrahydroborate, potassium methanide, potassium cyanide, potassium formate, potassium hydrogen fluoride, potassium tetraiodomercurate (II), potassium hydrogen sulfide, potassium octachlorodimolybdate (II), potassium amide, potassium hydroxide, potassium hexafluorophosphate, potassium carbonate, potassium tetrachloroplatinate (II), potassium hexachloroplatinate (IV), potassium nonahydrorhenate (VII), potassium sulfate, potassium acetate, potassium cyanide gold (I), potassium hexanitrocobalt (III), potassium hexacyanoferrate (III), hexacyanoferrate (II) ), potassium methoxide, potassium ethoxide, potassium tert-butoxide, potassium cyanate, potassium fulminate, potassium thiocyanate, potassium aluminum sulfate, potassium aluminate, potassium arsenate, potassium bromate, potassium hypochlorite, potassium chlorite, potassium chlorate, potassium perchlorate, potassium carbonate, potassium chromate, potassium dichromate, potassium tetra(peroxy)chromate(V), potassium cuprate(III), potassium ferrate, potassium iodate, potassium periodate, potassium permanganate, potassium manganate, potassium hypomanganate, potassium molybdate, potassium nitrite, potassium nitrate, tripotassium phosphate, potassium perrhenate, potassium selenate, potassium silicate, potassium sulfite, potassium sulfate, potassium thiosulfate, potassium pyrosulfite, potassium dithionate, potassium disulfate, potassium peroxydisulfate, potassium dihydrogen arsenate, dipotassium hydrogen arsenate, potassium bicarbonate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, potassium hydrogen selenate, potassium bisulfite, potassium hydrogen sulfate, potassium persulfate.

[0109] For example, the additive may be barium sulfite, barium chloride, barium chlorate, barium perchlorate, barium peroxide, barium chromate, barium acetate, barium cyanide, barium bromide, barium oxalate, barium nitrate, barium hydroxide, barium hydride, barium carbonate, barium iodide, barium sulfide, barium sulfate. Other additives may be sodium acetate and sodium citrate.

[0110] In addition, the additive may be fine particles or nanoparticles of metal oxides. For example, the metal oxides include sodium oxide, calcium oxide, lithium oxide, boron oxide, potassium oxide, barium oxide, silicon oxide, titanium oxide, zirconium oxide, aluminum oxide, zinc oxide, and magnesium oxide.

[0111] The specific part 52 is not limited to one layer. The number of the specific part 52 may be multiple. In addition, the shape of the specific part 52 may not be layered. For example, in Fig.12 In the variation shown, the glass film 50 has a plurality of specific portions 52. Furthermore, when viewed in section on a plane perpendicular to the outer surface 21 of the main body 20, the major diameter of the specific portion 52 is at least three times the minor diameter. The major diameter is the longest length of a line segment extending from the outer edge to the outer edge through the geometric center of a specific portion 52 when viewed in section. In addition, the minor diameter is the length of a line segment extending from the outer edge to the outer edge that passes through the geometric center of the same specific portion 52 and is perpendicular to the major diameter when viewed in section. That is, according to the above Fig.12 In the modification shown, due to the plurality of specific portions 52, the number of interfaces between the base portion 51 and the specific portion 52 becomes greater. In addition, the major diameter of one specific portion 52 is more than three times the minor diameter, that is, it is plate-shaped or needle-shaped in cross-sectional observation. Therefore, the passage from the outside of the glass film 50 to the body 20 through the base portion 51 can be complicated. In addition, the possibility of arranging more interfaces in a direction orthogonal to the outer surface 21 of the body 20 can be increased.

[0112] In the method for manufacturing the electronic component 10, the metal alkoxide 85 may be sodium methoxide, sodium ethoxide, calcium diethoxide, lithium isopropoxide, lithium ethoxide, lithium tert-butoxide, lithium methoxide, boric alcohol, potassium tert-butoxide, tetraethyl orthosilicate, allyl trimethoxysilane, isobutyl (trimethoxy) silane, tetrapropyl orthosilicate, tetramethyl orthosilicate, [3-(diethylamino)propyl]trimethoxysilane, triethoxy (octyl) silane, triethoxyvinyl silane, triethoxyphenyl silane, trimethoxyphenyl silane, trimethoxymethyl silane, butyl trichlorosilane, n-propyl triethoxysilane, methyl trichlorosilane, dimethoxy (methyl) octyl silane, dimethoxydimethyl silane, tri (tert-butoxy) silanol, tri (tert-pentyloxy) silanol, hexadecyl trimethoxy silane, tri(1,2-phthalate-O,O')dipotassium silicate, tetrabutyl orthosilicate, aluminum silicate, calcium silicate, tetramethylammonium silicate solution, chlorotriisopropoxytitanium(IV), titanium(IV) isopropoxide, 2-ethylhexyltitanium(IV), titanium(IV) ethoxide, titanium(IV) butoxide, titanium(IV) tert-butoxide, titanium(IV) propoxide, titanium(IV) methoxide, zirconium(IV) dipropoxide bis(diethyl citrate), zirconium(IV) dibutoxide (bis-2,4-pentanedionate), 2-ethyl zirconium(IV) acetate, zirconium(IV) isopropoxide isopropanol complex, zirconium(IV) ethoxide, zirconium(IV) butoxide, zirconium(IV) tert-butoxide, zirconium(IV) propoxide, aluminum(tert-butoxide, aluminum(isopropoxide), aluminum(ethoxide), aluminum(tri-sec-butoxide, aluminum(phenol), etc.

[0113] In the manufacturing method of the electronic component 10, a metal complex or acetate, which is a precursor of the metal alkoxide 85, may be used instead of the metal alkoxide 85. In this case, in the metal alkoxide feeding step S17, a metal complex or acetate, which is a precursor of the metal alkoxide, may be fed. Examples of the metal complex include lithium acetylacetonate, titanium (IV) acetylacetonate, titanium diisopropoxide bis(acetylacetone), zirconium (IV) trifluoroacetylacetonate, zirconium (IV) acetylacetonate, aluminum acetylacetonate, aluminum (III) acetylacetonate, calcium (II) acetylacetonate, and acetylacetone such as zinc (II) acetylacetonate. In addition, examples of the acetate include zirconium acetate, zirconium (IV) acetate hydroxide, and basic aluminum acetate.

[0114] The method for manufacturing the electronic component 10 is not limited to the example of the above embodiment. For example, the solvent feeding step S13 may be performed after the catalyst feeding step S14 and the main body feeding step S15. In addition, the solvent 82 is not limited to 2-propanol. The solvent 82 may be appropriately changed as long as the metal alkoxide 85 can be sufficiently dispersed.

[0115] The following describes technical ideas derived from the above-mentioned embodiments and modified examples.

[0116] <1> An electronic component comprising: a body, a glass film covering an outer surface of the body, and an external electrode laminated on the outer surface of the glass film and having at least a base electrode.

[0117] The glass film comprises: a base portion containing an oxide of one or more metal elements selected from alkali metals and alkaline earth metals in addition to silicon oxide, and a specific portion containing an oxide of the same metal element as the base portion in addition to silicon oxide.

[0118] The content ratio of the metal element in the specific portion is lower than the content ratio of the metal element in the base portion.

[0119] <2>

[0120] The electronic component according to <1>, wherein the content ratio of silicon in the specific portion is greater than the content ratio of silicon in the base portion.

[0121] <3>

[0122] The electronic component according to <1> or <2>, wherein the metal element is any one of lithium, sodium and potassium among alkali metals.

[0123] <4>

[0124] The electronic component according to <1> or <2>, wherein the metal element is either calcium or barium among alkaline earth metals.

[0125] <5>

[0126] The electronic component according to any one of <1> to <4>, wherein the specific portion contains an oxide of any one of zinc, boron and aluminum.

[0127] <6>

[0128] The electronic component according to <5>, wherein:

[0129] The above base contains zinc oxide,

[0130] The specific portion contains zinc oxide,

[0131] The specific portion has a higher zinc content than the base portion.

[0132] <7>

[0133] The electronic component according to any one of <1> to <6>,

[0134] The glass film has a plurality of the specific portions.

[0135] In cross-section, the longest length of the line segments passing through the geometric center of the specific portion and extending from the outer edge to the outer edge is the major diameter.

[0136] In cross-section, the length of a line segment extending from the outer edge to the outer edge that passes through the geometric center of the specific portion and is orthogonal to the major axis is the minor axis. In this case,

[0137] The major diameter is at least 3 times the minor diameter.

[0138] <8>

[0139] The electronic component according to any one of <1> to <7>,

[0140] The external electrode further comprises a metal layer,

[0141] The metal layer is disposed on the surface of the base electrode.

[0142] <9>

[0143] The electronic component according to <8>, wherein a portion of the metal layer is located on the surface of the glass film.

[0144] Explanation of symbols

[0145] 10…Electronic components

[0146] 20…Main body

[0147] 21…External surface

[0148] 50…Glass film

[0149] 51…base

[0150] 52…Specified Department

[0151] 61…1st external electrode

[0152] 61A…1st base electrode

[0153] 61B…1st metal layer

Claims

1. An electronic component comprising: a main body, a glass film covering an outer surface of the main body, and an external electrode laminated on the outer surface of the glass film and having at least a base electrode, The glass film comprises a base portion and a specific portion, wherein the base portion contains an oxide of one or more metal elements selected from alkali metals and alkaline earth metals in addition to silicon oxide, and the specific portion contains an oxide of the same metal element as the base portion in addition to silicon oxide. Furthermore, the content ratio of the metal element in the specific portion is smaller than the content ratio of the metal element in the base portion.

2. The electronic component according to claim 1, in, The content ratio of silicon in the specific portion is greater than the content ratio of silicon in the base portion.

3. The electronic component according to claim 1 or 2, in, The metal element is any one of lithium, sodium and potassium among alkali metals.

4. The electronic component according to claim 1 or 2, in, The metal element is either calcium or barium among alkaline earth metals.

5. The electronic component according to any one of claims 1 to 4, in, The specific portion contains an oxide of any one element of zinc, boron, and aluminum.

6. The electronic component according to claim 5, in, The base contains zinc oxide, The specific portion contains zinc oxide, The specific portion has a higher zinc content than the base portion.

7. The electronic component according to any one of claims 1 to 6, in, The glass film has a plurality of the specific portions. When viewed in section, the longest length of the line segments passing through the geometric center of the specific part and drawn from the outer edge to the outer edge is set as the major diameter, and when viewed in section, the length of the line segments passing through the geometric center of the specific part and drawn from the outer edge to the outer edge orthogonal to the major diameter is set as the minor diameter. The major diameter is more than 3 times the minor diameter.

8. The electronic component according to any one of claims 1 to 7, in, The external electrode further has a metal layer, The metal layer is disposed on a surface of the base electrode.

9. The electronic component according to claim 8, in, A portion of the metal layer is located on the surface of the glass film.