A method for preparing ruthenium oxide with a large specific surface area

By controlling the reaction temperature and rate of ruthenium trichloride with diluted diethanolamine solution, combined with rapid freezing with liquid nitrogen and freeze drying, high-purity ruthenium oxide powder with a large specific surface area was prepared. This solved the problems of easy agglomeration and high cost of powder in the existing technology, and achieved good performance and low-cost production of the water electrolysis hydrogen production catalyst.

CN120058010BActive Publication Date: 2026-11-17NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202510215965.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-02-26
Publication Date
2026-11-17
Estimated Expiration
2045-02-26

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare high-purity ruthenium oxide powder with a large specific surface area, and the preparation process is complex and costly, which is difficult to meet the requirements of catalysts for hydrogen production by water electrolysis.

Method used

Using ruthenium trichloride as raw material and diluted diethanolamine solution as precipitant, the reaction temperature and rate are controlled at low temperature to form nanocrystalline hydrated ruthenium oxide. Combined with rapid freezing with liquid nitrogen and freeze drying to prevent agglomeration, and then low-temperature annealing to remove impurities, high-purity ruthenium oxide powder with a large specific surface area is obtained.

Benefits of technology

The prepared ruthenium oxide powder has good dispersibility and high specific surface area, making it suitable for resistance slurry and hydrogen production catalysts via water electrolysis. This reduces ruthenium usage, lowers costs, and facilitates industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120058010B_ABST
    Figure CN120058010B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing ruthenium oxide with a large specific surface area. The method includes: 1. Slowly adding a diluted diethanolamine solution to a ruthenium trichloride solution under low temperature conditions and stirring to obtain a hydrated ruthenium oxide suspension; 2. Rapidly freezing and freeze-drying the hydrated ruthenium oxide suspension to obtain hydrated ruthenium oxide powder, followed by low-temperature annealing to obtain ruthenium oxide powder with a large specific surface area. This invention uses ruthenium trichloride as a raw material to prepare a solution and reacts it with a diluted diethanolamine solution as a precipitant, controlling the reaction temperature and rate to obtain nanocrystalline hydrated ruthenium oxide. Then, after rapid freeze-drying, well-dispersed hydrated ruthenium oxide nanoparticles are obtained. Low-temperature annealing is then used to remove impurities and prevent ruthenium oxide agglomeration, resulting in high-purity ruthenium oxide powder with a large specific surface area. This method is suitable for thick-film resistor slurries and water electrolysis hydrogen production catalysts, and is simple in process, has a high yield, and is easy to industrialize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of powder metallurgy technology, specifically relating to a method for preparing ruthenium oxide with a large specific surface area. Background Technology

[0002] Ruthenium oxide (RuO2) is widely used in resistive components and industrial water electrolysis for hydrogen production due to its excellent physicochemical properties, including a very stable structure, corrosion resistance, low temperature coefficient of resistance, and high catalytic performance in water electrolysis. With continuous technological advancements, there is an increasingly urgent demand for RuO2, especially for ruthenium oxide with a large specific surface area. A large specific surface area can significantly reduce the RuO2 content in RuO2 resistive slurries, while simultaneously improving resistor performance and saving costs. Furthermore, a large specific surface area of ​​RuO2 has always been an important indicator for water electrolysis catalysts; the larger the specific surface area of ​​the RuO2 powder during water electrolysis, the more RuO2 atoms are exposed, resulting in better catalytic performance. Currently, methods for preparing large specific surface area RuO2 mainly include liquid-phase chemical synthesis, sol-gel method, and direct calcination method. Although there are many methods for preparing RuO2, very few are suitable for use in high-performance resistive slurries. Therefore, developing a technology for preparing large specific surface area RuO2 is of great significance.

[0003] Patent CN 114105228 A discloses a method for preparing ruthenium oxide with a large specific surface area. The invention includes: 1. mixing ruthenium trichloride and ammonium chloride and then ball-milling to obtain a mixed powder; 2. calcining and reducing the mixed powder to obtain flake-shaped ruthenium powder; 3. ball-milling the flake-shaped ruthenium powder to obtain nano-ruthenium powder; 4. calcining the nano-ruthenium powder in air to obtain ruthenium oxide for thick-film resistors. This invention, by controlling the ball milling of the precursor ruthenium salt, combined with controlling the morphology of the ruthenium powder, and then calcining in air, obtains large-particle-size, near-spherical ruthenium oxide powder. This avoids the ruthenium oxide powder inheriting the morphology of the flake-shaped ruthenium powder, ensuring the near-spherical morphology of the ruthenium oxide powder, making it suitable for use in thick-film resistors. Furthermore, this preparation method is simple, has a high yield, large production volume, is environmentally friendly, and is easy to industrialize. Although the ruthenium oxide prepared by this method is suitable for some resistive slurries, the specific surface area of ​​the ruthenium oxide prepared by this method is very small, the cost of the prepared resistive slurry is very high, and the ruthenium oxide powder is not suitable for hydrogen production catalysts by water electrolysis.

[0004] Patent CN106587180A discloses a method for preparing ruthenium dioxide for resistive slurries. The method involves first preparing a 0.011 mol / L ruthenium trichloride solution and a 0.013 mol / L quaternary ammonium salt solution. Then, at a molar ratio of 1:35, the ruthenium trichloride solution is added dropwise to the quaternary ammonium salt solution under heating and magnetic stirring. Stirring is stopped when the pH of the solution reaches 7.8. The resulting black precipitate is washed with a centrifuge, filtered, and dried to obtain ruthenium dioxide powder, which can be used as a medium-to-low resistivity material. However, this method suffers from difficulties in controlling experimental conditions, a tendency for the prepared ruthenium dioxide to agglomerate, and numerous challenges in industrialization.

[0005] Patent CN115321616A discloses a low-cost, high-specific-surface-area ruthenium oxide nanoparticles preparation method with controllable particle size. The method includes: 1. Preparing ruthenium salt aqueous solution and weak alkali aqueous solution containing dispersant, respectively; 2. Using high-frequency electronic oscillation to convert ruthenium-containing micro / nano aerosols and weak alkali-containing micro / nano aerosols, respectively; 3. Performing a gas-phase confined micro-region mixing reaction on the ruthenium-containing micro / nano aerosols and weak alkali-containing micro / nano aerosols; 4. Sequentially performing solid-liquid separation, washing, drying, and topological oxidation calcination to obtain high-specific-surface-area ruthenium oxide nanoparticles. This invention uses common, low-cost soluble ruthenium salts as the ruthenium source and low-cost weak alkalis as the reaction control agent for nucleation and growth. By converting the ruthenium source and weak alkali into micro / nano aerosol morphology for reaction, constructing three-dimensional spatially confined micro-region reaction conditions, and controlling the reaction kinetics, the number of nuclei is increased, achieving controllable particle size preparation of high-specific-surface-area ruthenium oxide nanoparticles and reducing preparation costs. However, the process is complex, difficult to control, and it is unknown whether it can be mass-produced.

[0006] Therefore, there is an urgent need for a method to prepare ruthenium oxide with a large specific surface area. Summary of the Invention

[0007] The technical problem to be solved by this invention is to provide a method for preparing ruthenium oxide with a large specific surface area, addressing the shortcomings of the prior art. This method involves reacting a ruthenium trichloride solution with a diluted diethanolamine solution as a precipitant, controlling the reaction temperature and rate to obtain hydrated ruthenium oxide in nanocrystalline form. This is then rapidly freeze-dried to obtain well-dispersed hydrated ruthenium oxide nanoparticles. Finally, low-temperature annealing is used to remove impurities and prevent ruthenium oxide agglomeration, resulting in high-purity ruthenium oxide powder with a large specific surface area. This method solves the problems of small surface area, high cost, and complex and difficult-to-control process in the preparation of ruthenium oxide powder using existing techniques.

[0008] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a method for preparing ruthenium oxide with a large specific surface area, characterized in that the method includes the following steps:

[0009] Step 1: Prepare a ruthenium trichloride solution using ruthenium trichloride as the raw material. Then, under low temperature conditions, slowly add a diluted diethanolamine solution to the ruthenium trichloride solution and stir to react, thereby obtaining a hydrated ruthenium oxide suspension.

[0010] Step 2: The hydrated ruthenium oxide suspension obtained in Step 1 is rapidly frozen in liquid nitrogen, then freeze-dried in a freeze-drying device to obtain hydrated ruthenium oxide powder, which is then annealed at low temperature in a tube furnace to obtain ruthenium oxide powder with a large specific surface area.

[0011] Compared to traditional methods that react reducing agents or precipitants with ruthenium solutions to prepare ruthenium oxide with large specific surface area, this method involves the addition of dispersants, followed by filtration and drying to obtain ruthenium oxide powder. This results in drawbacks such as easy agglomeration, difficulty in cleaning the dispersant, poor control, and large waste volume. This invention first prepares a solution using ruthenium trichloride as a raw material, then slowly adds a diluted diethanolamine solution under low-temperature conditions with stirring to prepare a hydrated ruthenium oxide suspension. Using the diluted diethanolamine solution as a precipitant, the reaction temperature and rate are controlled to allow the hydrated ruthenium oxide to slowly crystallize and precipitate, preventing rapid growth of ruthenium oxide nanoparticles and effectively controlling the primary particle size of ruthenium oxide. To ensure that hydrated ruthenium oxide particles do not agglomerate and form nanocrystals, the ruthenium oxide suspension is rapidly frozen in liquid nitrogen to prevent particle sedimentation and aggregation during freezing. The frozen hydrated ruthenium oxide is then freeze-dried, avoiding the agglomeration and surface area reduction problems caused by traditional filtration and drying processes, resulting in well-dispersed hydrated ruthenium oxide nanoparticles. The hydrated ruthenium oxide nanoparticles are then low-temperature annealed in air to effectively remove moisture and residual organic matter, ensuring the purity of the ruthenium oxide product. Low-temperature annealing also prevents agglomeration, ensuring a large specific surface area of ​​the resulting nano-ruthenium oxide. Ultimately, the large-surface-area ruthenium oxide powder prepared by this invention has the advantages of high purity and large specific surface area. When applied to resistor slurries, it significantly reduces ruthenium usage while maintaining performance, thus lowering costs. When used as a catalyst for water electrolysis to produce hydrogen, it exhibits excellent catalytic activity. Therefore, the large-specific-surface-area ruthenium oxide powder prepared by this invention has broad application prospects.

[0012] The above-described method for preparing ruthenium oxide with a large specific surface area is characterized in that, in step one, the concentration of ruthenium in the ruthenium trichloride solution is 0.1wt% to 3wt%, the concentration of the diluted diethanolamine solution is 0.1wt% to 0.5wt%, and the volume ratio of the ruthenium trichloride solution to the diluted diethanolamine solution is 1:1 to 1:3; the stirring reaction temperature is 5°C, and the time is 0.5h to 4h. This invention effectively prepares a nano-hydrated ruthenium oxide suspension by controlling the concentrations and amounts of the raw material solution and precipitant solution, as well as the stirring reaction temperature and time, thus preventing the aggregation of hydrated ruthenium oxide.

[0013] The above-described method for preparing ruthenium oxide with a large specific surface area is characterized in that the freeze-drying time in step two is 12h to 24h, and the low-temperature annealing temperature is 100℃ to 250℃ for 0.5h to 4h. Typically, the volume of the hydrated ruthenium oxide suspension rapidly cooled in liquid nitrogen in a single step is 500mL to ensure rapid freezing effect; the freeze-drying power used is 1kW. This invention effectively prevents the agglomeration of the obtained nano-ruthenium oxide powder by controlling the process parameters of freeze-drying and low-temperature annealing, ensuring that the product ruthenium oxide powder has a high specific surface area.

[0014] The above-described method for preparing ruthenium oxide with a large specific surface area is characterized in that the specific surface area of ​​the ruthenium oxide powder in step two is 30 m². 2 / g~80m 2 The ruthenium oxide powder prepared by this invention has the advantages of high purity and large specific surface area. When used in resistive slurries, it can ensure performance while greatly reducing the amount of ruthenium used and reducing costs. It can also be used as a catalyst for hydrogen production by water electrolysis and exhibits good catalytic activity.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] 1. This invention uses ruthenium trichloride as raw material and diluted diethanolamine solution as precipitant. By controlling the reaction temperature and rate of both, the prepared hydrated ruthenium oxide slowly crystallizes to form nanocrystals. Then, combined with rapid freezing with liquid nitrogen and freeze-drying, the dispersibility of the hydrated ruthenium oxide nanoparticles is improved. Finally, low-temperature annealing removes residual organic matter and moisture, improving the purity of ruthenium oxide and effectively preventing ruthenium oxide agglomeration. This results in high-purity ruthenium oxide powder with a large specific surface area, which is suitable for thick film resistor slurries and electrolytic hydrogen production catalysts.

[0017] 2. The preparation process of this invention is simple, effectively controls the specific surface area of ​​ruthenium oxide, has a high yield, is easy to industrialize, and has broad application prospects.

[0018] 3. The specific surface area of ​​the ruthenium oxide powder prepared by this invention is 30 m². 2 / g~80m 2 With a particle size of less than 100 nm and a ruthenium content of 75%–76%, it can simultaneously meet the requirements of thick film resistive slurry and electrolytic water hydrogen production catalyst.

[0019] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0020] Figure 1 This is a flowchart of the preparation method of ruthenium oxide with large specific surface area according to the present invention.

[0021] Figure 2 This is a SEM image of the ruthenium oxide powder with a large specific surface area prepared in Example 1 of the present invention.

[0022] Figure 3 The image shows the XRD pattern of the large specific surface area ruthenium oxide powder prepared in Example 1 of this invention. Detailed Implementation

[0023] Example 1

[0024] like Figure 1 As shown, this embodiment includes the following steps:

[0025] Step 1: Prepare a ruthenium trichloride solution with a ruthenium element concentration of 3wt% by adding ruthenium trichloride to deionized water. Then, under low temperature conditions, slowly add a 0.3wt% diluted diethanolamine solution to the ruthenium trichloride solution and stir the reaction. The volume ratio of the ruthenium trichloride solution to the diluted diethanolamine solution is 1:2. The stirring reaction temperature is controlled at 5℃ and the time is 2h to obtain a hydrated ruthenium oxide suspension.

[0026] Step 2: Place 500 mL of the hydrated ruthenium oxide suspension obtained in Step 1 into liquid nitrogen for rapid freezing, then place it in a freeze dryer for freeze drying at a power of 1 kW for 18 hours to obtain hydrated ruthenium oxide powder. Then place it in a tube furnace for low-temperature annealing at 100°C for 4 hours to obtain ruthenium oxide powder with a large specific surface area.

[0027] Figure 2 This is a SEM image of the large specific surface area ruthenium oxide powder prepared in this embodiment. Figure 2 It can be seen that the ruthenium oxide powder is nanoscale in size, has good dispersibility, and a specific surface area of ​​50 m². 2 / g~70m 2 / g, particle size less than 100nm, ruthenium content of 75% to 76% by mass.

[0028] Figure 3 The XRD pattern of the large specific surface area ruthenium oxide powder prepared in this embodiment is shown below. Figure 3 As can be seen from the comparison with the standard card, the ruthenium oxide powder product is a simple ruthenium oxide phase.

[0029] Example 2

[0030] like Figure 1 As shown, this embodiment includes the following steps:

[0031] Step 1: Prepare a ruthenium trichloride solution with a ruthenium element concentration of 0.3 wt% by adding ruthenium trichloride to deionized water. Then, under low temperature conditions, slowly add a 0.2 wt% diluted diethanolamine solution to the ruthenium trichloride solution and stir the reaction. The volume ratio of ruthenium trichloride solution to diluted diethanolamine solution is 1:1. The stirring reaction temperature is controlled at 5℃ and the time is 2 hours to obtain a hydrated ruthenium oxide suspension.

[0032] Step 2: Place 500 mL of the hydrated ruthenium oxide suspension obtained in Step 1 into liquid nitrogen for rapid freezing, then place it in a freeze dryer for freeze drying at a power of 1 kW for 24 h to obtain hydrated ruthenium oxide powder. Then place it in a tube furnace for low-temperature annealing at 100 °C for 0.5 h to obtain ruthenium oxide powder with a large specific surface area.

[0033] Testing revealed that the ruthenium oxide powder prepared in this embodiment is nanoscale in size, exhibits good dispersibility, and has a specific surface area of ​​60 m². 2 / g~80m 2 / g, particle size less than 100nm, ruthenium content of 75% to 76% by mass.

[0034] Example 3

[0035] like Figure 1 As shown, this embodiment includes the following steps:

[0036] Step 1: Prepare a ruthenium trichloride solution with a ruthenium element concentration of 0.1 wt% by adding ruthenium trichloride to deionized water. Then, under low temperature conditions, slowly add a 0.5 wt% diluted diethanolamine solution to the ruthenium trichloride solution and stir the reaction. The volume ratio of the ruthenium trichloride solution to the diluted diethanolamine solution is 1:2. The stirring reaction temperature is controlled at 5℃ and the time is 0.5 h to obtain a hydrated ruthenium oxide suspension.

[0037] Step 2: Place 500 mL of the hydrated ruthenium oxide suspension obtained in Step 1 into liquid nitrogen for rapid freezing, then place it in a freeze dryer for freeze drying at a power of 1 kW for 12 hours to obtain hydrated ruthenium oxide powder. Then place it in a tube furnace for low-temperature annealing at a temperature of 200°C for 2 hours to obtain ruthenium oxide powder with a large specific surface area.

[0038] Testing revealed that the ruthenium oxide powder prepared in this embodiment is nanoscale in size, exhibits good dispersibility, and has a specific surface area of ​​40 m². 2 / g~60m 2 / g, particle size less than 100nm, ruthenium content of 75% to 76% by mass.

[0039] Example 4

[0040] like Figure 1 As shown, this embodiment includes the following steps:

[0041] Step 1: Prepare a ruthenium trichloride solution with a ruthenium element concentration of 2wt% by adding ruthenium trichloride to deionized water. Then, under low temperature conditions, slowly add a 0.1wt% diluted diethanolamine solution to the ruthenium trichloride solution and stir the reaction. The volume ratio of the ruthenium trichloride solution to the diluted diethanolamine solution is 1:3. The stirring reaction temperature is controlled at 5℃ and the time is 4h to obtain a hydrated ruthenium oxide suspension.

[0042] Step 2: Place 500 mL of the hydrated ruthenium oxide suspension obtained in Step 1 into liquid nitrogen for rapid freezing, then place it in a freeze dryer for freeze drying at a power of 1 kW for 16 h to obtain hydrated ruthenium oxide powder. Then place it in a tube furnace for low-temperature annealing at a temperature of 250 °C for 4 h to obtain ruthenium oxide powder with a large specific surface area.

[0043] Testing revealed that the ruthenium oxide powder prepared in this embodiment is nanoscale in size, exhibits good dispersibility, and has a specific surface area of ​​30 m². 2 / g~50m 2 / g, particle size less than 100nm, ruthenium content of 75% to 76% by mass.

[0044] Example 5

[0045] like Figure 1 As shown, this embodiment includes the following steps:

[0046] Step 1: Prepare a ruthenium trichloride solution with a ruthenium element concentration of 0.1 wt% by adding ruthenium trichloride to deionized water. Then, under low temperature conditions, slowly add a 0.4 wt% diluted diethanolamine solution to the ruthenium trichloride solution and stir the reaction. The volume ratio of the ruthenium trichloride solution to the diluted diethanolamine solution is 1:1. The stirring reaction temperature is controlled at 5℃ and the time is 3 hours to obtain a hydrated ruthenium oxide suspension.

[0047] Step 2: Place 500 mL of the hydrated ruthenium oxide suspension obtained in Step 1 into liquid nitrogen for rapid freezing, then place it in a freeze dryer for freeze drying at a power of 1 kW for 24 hours to obtain hydrated ruthenium oxide powder. Then place it in a tube furnace for low-temperature annealing at a temperature of 150°C for 3 hours to obtain ruthenium oxide powder with a large specific surface area.

[0048] Testing revealed that the ruthenium oxide powder prepared in this embodiment is nanoscale in size, exhibits good dispersibility, and has a specific surface area of ​​50 m². 2 / g~70m 2 / g, particle size less than 100nm, ruthenium content of 75% to 76% by mass.

[0049] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention in any way. Any simple modifications, alterations, and equivalent changes made to the above embodiments based on the inventive essence shall still fall within the protection scope of the present invention.

Claims

1. A method for preparing ruthenium oxide with a large specific surface area, characterized in that, The method includes the following steps: Step 1: Prepare a ruthenium trichloride solution using ruthenium trichloride as the raw material. Then, under low temperature conditions, slowly add a diluted diethanolamine solution to the ruthenium trichloride solution and stir to react, thereby obtaining a hydrated ruthenium oxide suspension. The stirring reaction is carried out at a temperature of 5°C for 0.5 h to 4 h. Step 2: The hydrated ruthenium oxide suspension obtained in Step 1 is rapidly frozen in liquid nitrogen, then freeze-dried in a freeze-drying device to obtain hydrated ruthenium oxide powder, which is then annealed at low temperature in a tube furnace to obtain ruthenium oxide powder with a large specific surface area.

2. The method for preparing ruthenium oxide with a large specific surface area according to claim 1, characterized in that, In step one, the concentration of ruthenium in the ruthenium trichloride solution is 0.1wt%~3wt%, the concentration of the diluted diethanolamine solution is 0.1wt%~0.5wt%, and the volume ratio of the ruthenium trichloride solution to the diluted diethanolamine solution is 1:1~1:

3.

3. The method for preparing ruthenium oxide with a large specific surface area according to claim 1, characterized in that, The freeze-drying time in step two is 12h~24h, and the low-temperature annealing temperature is 100℃~250℃, and the time is 0.5h~4h.

4. The method for preparing ruthenium oxide with a large specific surface area according to claim 1, characterized in that, The specific surface area of ​​the ruthenium oxide powder with large specific surface area mentioned in step two is 30 m². 2 / g~80m 2 / g, with a particle size of less than 100nm and a ruthenium content of 75%~76%.

Citation Information

Patent Citations

  • Method for preparing ruthenium dioxide for resistance paste

    CN106587180A

  • Preparation method of ruthenium oxide for thick-film resistor

    CN114105228A

  • Preparation method of nano ruthenium oxide with low cost, controllable granularity and high specific surface area

    CN115321616A

  • Preparation method of ruthenium oxide electrode material

    CN102169759A

  • Preparation method of ruthenium dioxide for resistance paste

    CN107758751A