Design and manufacturing method of polyamideimide composite coating gear

Through the design and manufacturing method of polyamide imide composite coating gear, the problems of poor wear resistance and insufficient corrosion resistance under complex working conditions are solved, and the effects of high wear resistance, vibration damping performance and long service life are achieved.

CN120105622AActive Publication Date: 2025-06-06CHONGQING UNIV +1

Patent Information

Application Number
CN202510234923.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-02-28
Publication Date
2025-06-06
Estimated Expiration
2045-02-28

AI Technical Summary

Technical Problem

Traditional metal gears are difficult to meet the needs of complex working conditions due to high surface friction coefficient, poor wear resistance and insufficient corrosion resistance under special operating conditions.

Method used

The design and manufacturing method of polyamide imide composite coated gears is adopted, and the precise coating composition design, coating thickness optimization, matrix tooth thickness thinning and automated spray curing processes are carried out through the IDDOV model Six Sigma design frame, which significantly improves the service performance and service life of the gears.

Benefits of technology

It significantly improves the wear resistance, vibration damping and fatigue resistance of the gear, extends the service life of the gear, and is suitable for high-performance mechanical transmission parts under complex working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120105622A_ABST
    Figure CN120105622A_ABST
Patent Text Reader

Abstract

The invention discloses a design and manufacturing method of a polyamideimide composite coating gear, which comprises the following steps: S1, collecting customer demands, sequencing the priorities of the customer demands, and establishing a quality house based on a quality function expansion method; s2, formulating a design project according to the priority of the customer demand; s3, preliminarily evaluating the feasibility of the design project through probability evaluation and risk analysis tools; s4, key quality characteristics are obtained, and a tolerance limit range is determined; s5, on the basis of a multi-objective optimization machining parameter reverse adjustment method, a parameter-driven input and output model is established; s6, inputting the key quality characteristics into the input and output model to obtain a design scheme; s7, inputting the design scheme into the multi-objective optimization model to obtain optimized key quality characteristics; s8, planning a manufacturing process based on customer requirements and optimized key quality characteristics; and S9, manufacturing a composite coating gear sample, testing the composite coating gear sample, and verifying the service performance of the composite coating gear sample.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of design and manufacture of composite coating gears, in particular to a design and manufacture method of polyamide-imide composite coating gears. Background Art

[0002] Using advanced design methods and manufacturing processes to optimize product features and production processes is a key strategy for modern manufacturing companies to improve product quality, reduce costs and enhance market competitiveness. However, product performance and quality are often determined in the design stage and early in the product development cycle.

[0003] Gears are core components in mechanical transmission, and their performance directly affects the operating efficiency and reliability of the equipment. Under special working conditions, traditional metal gears are difficult to meet the requirements of complex working conditions due to problems such as high surface friction coefficient, poor wear resistance, and insufficient corrosion resistance. Therefore, it is necessary to design the performance of gears during the design stage and product development cycle. Summary of the invention

[0004] The object of the present invention is to provide a method for designing and manufacturing a polyamide-imide composite coated gear, comprising the following steps:

[0005] S1. Collect customer needs and functional requirements, prioritize customer needs, and build a quality house based on the quality function deployment method;

[0006] S2. Develop design projects based on the priority of customer needs;

[0007] S3. Preliminarily evaluate the feasibility of the design project through probability assessment and risk analysis tools. If the design is feasible, proceed to step S4), otherwise, return to step S1);

[0008] S4. According to the quality house and functional requirements, obtain key quality characteristics and clarify the tolerance limit range of the amount of reinforcement material added to the polyamide-imide composite coating;

[0009] The key quality characteristics include the wear rate, decomposition temperature, vibration reduction amplitude, noise reduction amplitude, friction coefficient and service life of the coating;

[0010] S5. Establish a parameter-driven input-output model based on the multi-objective optimization processing parameter inversion method;

[0011] S6. Inputting the key quality characteristics into the input-output model to obtain a design scheme for the polyamide-imide composite coating gear; the design scheme includes the thickness, material composition and proportion of the polyamide-imide composite coating reinforcement material;

[0012] S7. Input the design solution into the multi-objective optimization model to obtain the optimized key quality characteristics;

[0013] S8. Based on customer needs and optimized key quality characteristics, plan the manufacturing process, which includes thinning the gear substrate, gear coating spraying, and gear coating processing;

[0014] S9. Manufacture polyamide-imide composite coated gear samples, and conduct wear resistance, heat resistance, vibration and noise reduction effect, friction coefficient and service life test and reliability test on the polyamide-imide composite coated gear samples to verify the service performance of the composite coated gear samples; the reliability test is to detect the mean time between failures of the composite coated gear samples;

[0015] If the verification result does not meet the key quality characteristic requirements and tolerance limit range, return to step S5), otherwise, deliver the polyamide-imide composite coated gear sample.

[0016] Further, in step S1), the customer requirements include gear wear resistance, heat resistance, vibration and noise reduction, friction coefficient and service life performance requirements.

[0017] The functional requirements include the requirements for the optimal ratio of each component in the coating material and the maximum error limit between the actual coating thickness and the designed coating thickness.

[0018] In step S4), the coating material of the coating layer comprises polyamideimide, reinforcing material, additives and coating solvent.

[0019] The additives include dispersants, leveling agents and defoamers.

[0020] The components of the reinforcing material need to undergo interface modification treatment.

[0021] The components of the reinforcement material include at least graphene, boron nitride BN, aluminum oxide Al 2 O 3 、ZrO 2 , one of the polytetrafluoroethylene (PTFE) particles.

[0022] When the component of the reinforcing material is graphene, the amount of graphene used is 0.5-3.0% of the total mass of the coating.

[0023] When the component of the reinforcing material is boron nitride BN, the amount of boron nitride BN used is 1-5% of the total mass of the coating.

[0024] When the reinforcing material is aluminum oxide Al 2 O 3 When Al2O3 2 O 3 The dosage is 5-10% of the total mass of the coating.

[0025] When the reinforcing material is zirconium oxide ZrO 2 When ZrO 2 The dosage is 5-10% of the total mass of the coating.

[0026] When the component of the reinforcing material is polytetrafluoroethylene (PTFE) particles, the amount of the polytetrafluoroethylene (PTFE) particles used is 2-8% of the total mass of the coating.

[0027] Further, in step S4), the coating thickness t is calculated by the following formula:

[0028]

[0029] Where: F load Indicates the maximum working load on the gear surface;

[0030] σ coating Indicates the maximum allowable stress of the coating.

[0031] Further, in step S5), the multi-objective function of the multi-objective optimization processing parameter inversion method is expressed as:

[0032]

[0033] Quantify customer needs, and the multi-objective function after quantification is as follows:

[0034]

[0035] Where: κ i represents the weight factor, i=1,2,…,N;

[0036] ω i The coefficient representing the design target, i = 1, 2, ..., N;

[0037] N is the number of targets;

[0038] R is the range of the design variable;

[0039] X represents the design factor, X = {W, T, V, N, μ, L};

[0040] W is the wear rate, W MAX is the maximum wear rate; T is the decomposition temperature, T MIN is the minimum decomposition temperature; V is the vibration reduction amplitude, V MIN is the minimum vibration reduction amplitude; N is the noise reduction amplitude, N MIN is the minimum noise reduction amplitude; μ is the friction coefficient, μ MAX is the maximum friction coefficient; L is the service life, L MIN Minimum service life increase

[0041] Further, in step S5), the regression formula of the input-output model is as follows:

[0042]

[0043] Where: t is the coating thickness;

[0044] x graphene ,x hBN , x PTFE They are graphene ratio, boron nitride ratio, aluminum oxide ratio, zirconium oxide ratio, and PTFE particle ratio respectively.

[0045] Further, in step S7), the optimization objective function of the multi-objective optimization model is as follows:

[0046] f = a 1 W+a 2 T+a 3 V+a 4 N+a 5 μ+a 6 L(5)

[0047] In the formula, a 1 、a 2 、a 3 、a 4 、a 5 、a 6 are the weight coefficients of W, T, V, N, μ, and L.

[0048] Further, in step S8), the method for thinning the gear base includes the following steps:

[0049] 1) Calculate the target value Ra of tooth surface roughness

[0050]

[0051] Where: k represents the proportionality coefficient;

[0052] γ represents the surface tension between the coating and the air;

[0053] θ represents the contact angle of the coating on the gear substrate;

[0054] σ represents the target bonding strength between the coating and the gear substrate;

[0055] 2) Use gear hobbing technology to thin the gear base;

[0056] During gear hobbing, the gear base is thinned by controlling the modification coefficient to perform negative modification. The calculation formula of the negative modification coefficient x is as follows:

[0057]

[0058] Where: Δt represents the service thickness of the coating; m represents the module of the gear.

[0059] 3) Determine whether the tooth surface roughness after thinning reaches the target value of the tooth surface roughness. If it reaches the target value, the thinning of the gear matrix is ​​completed, otherwise, sand blasting is required.

[0060] Further, in step S8), the gear coating spraying method comprises the following steps:

[0061] 1) Clean the gear surface thoroughly;

[0062] 2) Preheat the gear base;

[0063] 3) Use automated spray gun equipment to air spray the gear substrate;

[0064] 4) Send the gear into the oven for curing;

[0065] 5) After curing is completed, use a gear micrometer to check the coating thickness to determine whether the coating thickness meets the thickness requirements. If it meets the requirements, the gear coating spraying is completed, otherwise, return to step 3).

[0066] Further, in step S8), whether gear coating processing is required is determined in the following manner: determine whether the surface accuracy of the coating after spraying meets the requirements. If so, the gear can be put into use directly after spraying. Otherwise, processing allowance should be prepared when spraying the gear, and the coating should be thinned after spraying and curing to make its surface accuracy meet the requirements.

[0067] 1. The present invention adopts the IDDOV model of Six Sigma Design (DFSS) framework to develop a design method for polyamide-imide composite coated gears, which significantly improves the service performance and service life of the gears through precise coating composition design, coating thickness optimization design, substrate tooth thickness thinning treatment and automated spray curing process.

[0068] 2. The present invention proposes for the first time to use polyamide-imide (PAI) as a coating material for gears, which significantly improves the wear resistance, vibration reduction performance and fatigue resistance of the gears. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1 A Six Sigma Design Implementation Roadmap using the IDDOV Framework as described in Example 11;

[0070] Figure 2 This is a flow chart of the design phase of the polyamide-imide composite coated gear involved in Example 11;

[0071] Figure 3 This is a flow chart of the use phases of the polyamide-imide composite coated gear involved in Example 11. DETAILED DESCRIPTION

[0072] The present invention is further described below in conjunction with the embodiments, but it should not be understood that the above subject matter of the present invention is limited to the following embodiments. Without departing from the above technical ideas of the present invention, various substitutions and changes are made according to the common technical knowledge and customary means in the art, which should all be included in the protection scope of the present invention.

[0073] Embodiment 1:

[0074] The design and manufacturing method of a polyamide-imide composite coated gear comprises the following steps:

[0075] S1. Collect customer needs and functional requirements, prioritize customer needs, and build a quality house based on the quality function deployment method;

[0076] S2. Develop design projects based on the priority of customer needs;

[0077] S3. Preliminarily evaluate the feasibility of the design project through probability assessment and risk analysis tools. If the design is feasible, proceed to step S4), otherwise, return to step S1);

[0078] S4. According to the quality house and functional requirements, obtain key quality characteristics and clarify the tolerance limit range of the addition amount of polyamide-imide composite coating reinforcement materials (see GB / T 10095.1-2022 and GB / T 10095.2-2023 for specific requirements and parameters);

[0079] The key quality characteristics include the wear rate, decomposition temperature, vibration reduction amplitude, noise reduction amplitude, friction coefficient and service life of the coating;

[0080] S5. Establish a parameter-driven input-output model based on the multi-objective optimization processing parameter inversion method;

[0081] S6. Inputting the key quality characteristics into the input-output model to obtain a design scheme for the polyamide-imide composite coating gear; the design scheme includes the thickness, material composition and proportion of the polyamide-imide composite coating reinforcement material;

[0082] S7. Input the design solution into the multi-objective optimization model to obtain the optimized key quality characteristics;

[0083] S8. Based on customer needs and optimized key quality characteristics, plan the manufacturing process, which includes thinning the gear substrate, gear coating spraying, and gear coating processing;

[0084] S9. Manufacture polyamide-imide composite coated gear samples, and conduct wear resistance, heat resistance, vibration and noise reduction effect, friction coefficient and service life test and reliability test on the polyamide-imide composite coated gear samples to verify the service performance of the composite coated gear samples; the reliability test is to detect the mean time between failures of the composite coated gear samples;

[0085] If the verification result does not meet the key quality characteristic requirements and tolerance limit range, return to step S5), otherwise, deliver the polyamide-imide composite coated gear sample.

[0086] Embodiment 2:

[0087] The main structure of this embodiment is the same as that of Embodiment 1. Furthermore, in step S1), the customer requirements include gear wear resistance, heat resistance, vibration and noise reduction, friction coefficient, and service life performance requirements.

[0088] The functional requirements include the requirements for the optimal ratio of each component in the coating material and the maximum error limit between the actual coating thickness and the designed coating thickness.

[0089] Embodiment 3:

[0090] The main structure of this embodiment is the same as any one of Embodiments 1 to 2. Further, in step S4), the coating material of the coating comprises polyamide-imide, reinforcing material, additives and coating solvent.

[0091] The additives include dispersants, leveling agents and defoamers.

[0092] The components of the reinforcing material need to undergo interface modification treatment.

[0093] The components of the reinforcement material include at least graphene, boron nitride BN, aluminum oxide Al 2 O 3 、ZrO 2 , one of the polytetrafluoroethylene (PTFE) particles.

[0094] When the component of the reinforcing material is graphene, the amount of graphene used is 0.5-3.0% of the total mass of the coating.

[0095] When the component of the reinforcing material is boron nitride BN, the amount of boron nitride BN used is 1-5% of the total mass of the coating.

[0096] When the reinforcing material is aluminum oxide Al 2 O 3 When Al2O3 2 O 3 The dosage is 5-10% of the total mass of the coating.

[0097] When the reinforcing material is zirconium oxide ZrO 2 When ZrO 2 The dosage is 5-10% of the total mass of the coating.

[0098] When the component of the reinforcing material is polytetrafluoroethylene (PTFE) particles, the amount of the polytetrafluoroethylene (PTFE) particles used is 2-8% of the total mass of the coating.

[0099] When the reinforcing material is a two-component composite or a multi-component composite, the recommended dosage can be reduced.

[0100] Embodiment 4:

[0101] The main structure of this embodiment is the same as any one of Embodiments 1 to 3. Further, in step S4), the coating thickness t is calculated by the following formula:

[0102]

[0103] Where: F load Indicates the maximum working load on the gear surface;

[0104] σ coating Indicates the maximum allowable stress of the coating.

[0105] Embodiment 5:

[0106] The main structure of this embodiment is the same as any one of Embodiments 1 to 4. Further, in step S5), the multi-objective function of the multi-objective optimization processing parameter inversion method is expressed as:

[0107]

[0108] Quantify customer needs, and the multi-objective function after quantification is as follows:

[0109]

[0110] Where: κ i represents the weight factor, o=1,2,…,N;

[0111] ω i The coefficient representing the design target, which represents the contribution of different design targets (wear resistance, heat resistance, etc.) to the performance of the final product, i = 1, 2, ..., N;

[0112] N is the number of targets;

[0113] R is the range of the design variable, which represents the set of all possible design parameters and defines the range of variables that can be adjusted during the design process;

[0114] X represents the design factor, X = {W, T, V, N, μ, L};

[0115] W is the wear rate, W MAX is the maximum wear rate; T is the decomposition temperature, T MIN is the minimum decomposition temperature; V is the vibration reduction amplitude, V mIN is the minimum vibration reduction amplitude; N is the noise reduction amplitude, N MIN is the minimum noise reduction amplitude; μ is the friction coefficient, μ MAX is the maximum friction coefficient; L is the service life, L MIN This is the minimum service life increase.

[0116] Embodiment 6:

[0117] The main structure of this embodiment is the same as any one of Embodiments 1 to 5. Further, in step S5), the regression formula of the input-output model is as follows:

[0118]

[0119] Where: t is the coating thickness;

[0120] x graphene ,x hBN , x PTFE They are graphene ratio, boron nitride ratio, aluminum oxide ratio, zirconium oxide ratio, and PTFE particle ratio respectively.

[0121] When a component is not included in the design combination, the proportion of the combination is 0.

[0122] Embodiment 7:

[0123] The main structure of this embodiment is the same as any one of Embodiments 1 to 6. Further, in step S7), the optimization objective function of the multi-objective optimization model is as follows:

[0124] f = a 1 W+a 2 T+a 3 V+a 4 N+a 5 μ+a 6 L(5)

[0125] In the formula, a 1 、a 2 、a 3 、a 4 、a 5 、a 6 are the weight coefficients of W, T, V, N, μ, and L.

[0126] Embodiment 8:

[0127] The main structure of this embodiment is the same as any one of Embodiments 1 to 7. Further, in step S8), the method for thinning the gear base includes the following steps:

[0128] 1) Calculate the target value Ra of tooth surface roughness

[0129] Method 1: Determine the target value of tooth surface roughness (Ra range is 2-8μm) based on the particle size and adhesion performance requirements of PAI coating and composite reinforcement materials.

[0130] Method 2: According to the principle of mechanical bonding of coating, the target value of tooth surface roughness is calculated. The calculation formula is as follows:

[0131]

[0132] Where: k represents the proportionality coefficient, which is determined by empirical value or pre-experimental regression fitting;

[0133] γ represents the surface tension between the coating and the air;

[0134] θ represents the contact angle of the coating on the gear substrate;

[0135] σ represents the target bonding strength between the coating and the gear substrate;

[0136] 2) Use gear hobbing technology to thin the gear base;

[0137] The tooth thickness reduction must be strictly controlled during the processing, and the tolerance range should be less than ±0.001mm to ensure accurate matching of the subsequent coating thickness.

[0138] During gear hobbing, the gear base is thinned by controlling the modification coefficient to perform negative modification. The calculation formula of the negative modification coefficient x is as follows:

[0139]

[0140] Where: Δt represents the service thickness of the coating; m represents the module of the gear.

[0141] 3) Determine whether the tooth surface roughness after thinning reaches the target value of the tooth surface roughness. If it reaches the target value, the thinning of the gear matrix is ​​completed, otherwise, sand blasting is required.

[0142] Sandblasting process parameters include:

[0143] Sandblasting particle size: 40-60μm;

[0144] Spray angle: 30°-45°;

[0145] Injection pressure: 0.6-0.8MPa.

[0146] The surface should be cleaned after sandblasting to ensure that there are no residual particles or oil stains on the tooth surface.

[0147] Embodiment 9:

[0148] The main structure of this embodiment is the same as any one of Embodiments 1 to 8. Further, in step S8), the gear coating spraying method includes the following steps:

[0149] 1) Thoroughly clean the gear surface to remove oil, oxides and other impurities to ensure good adhesion between the coating and the substrate;

[0150] 2) Preheat the gear substrate at a temperature range of 100-130°C for 10-15 minutes to enhance the adhesion and uniformity of the coating.

[0151] 3) Use automated spray gun equipment to air spray the gear substrate;

[0152] During the spraying process, the spraying speed is controlled at 10-15mm / s to ensure uniform distribution of the coating, and the deviation of the spraying thickness is controlled within ±0.02mm;

[0153] 4) Send the gear into the oven for curing at a temperature of 210-280°C for 0.5-1 hour;

[0154] 5) After curing is completed, use a gear micrometer to check the coating thickness to determine whether the coating thickness meets the thickness requirements. If it meets the requirements, the gear coating spraying is completed, otherwise, return to step 3).

[0155] Thickness requirements that should be achieved during the spraying stage:

[0156] The deviation of spraying thickness is controlled within ±0.02mm.

[0157] Method for determining spraying thickness:

[0158] If the coating accuracy of the tooth surface meets the requirements after spraying, the spraying thickness = the service thickness of the coating;

[0159] If the tooth surface coating accuracy after spraying does not meet the requirements, the spraying thickness = coating service thickness + coating processing allowance.

[0160] Wherein, the sprayed coating includes PAI material and reinforcing material.

[0161] In the process of preparing the PAI coating matrix, the components of the reinforcing material need to be added gradually, and the reinforcing material is dispersed by ultrasonic dispersion, mechanical stirring or high-energy ball milling.

[0162] Embodiment 10:

[0163] The main structure of this embodiment is the same as any one of Embodiments 1 to 9. Furthermore, in step S8), whether gear coating processing is required is determined by the following method: judging whether the surface accuracy of the coating after spraying meets the requirements. If so, the gear can be put into use directly after spraying. Otherwise, processing allowance should be prepared when spraying the gear, and the coating should be thinned after spraying and curing to make its surface accuracy meet the requirements.

[0164] For specific requirements and parameters, please refer to GB / T 10095.1-2022 and GB / T 10095.2-2023.

[0165] Embodiment 11:

[0166] The main structure of this embodiment is the same as any one of the embodiments 1 to 10. Furthermore, a design method for polyamide-imide composite coated gears is developed by using the IDDOV model's Six Sigma Design (DFSS) framework. The gear's service performance and service life are significantly improved through precise substrate tooth thickness thinning, coating thickness optimization design, and automated spray curing process. It is mainly divided into the design stage and the manufacturing application stage:

[0167] 1. Design stage of composite coated gears

[0168] 1. Design of composite coated gears

[0169] A design methodology for polyamide-imide composite coated gears was developed using the Design for Six Sigma (DFSS) framework of the IDDOV model, which included the following stages:

[0170] (S1) Identification

[0171] Objective: Identify project Needs of the Customer (VOC), clarify design challenges and priorities.

[0172] Design process:

[0173] 1. Determine the project to be implemented: polyamide-imide composite coated gear design optimization.

[0174] 2. Identify customer needs and functional requirements

[0175] Customer requirements: high wear resistance, high heat resistance, vibration and noise reduction, low friction coefficient, and long service life.

[0176] Functional requirements: optimal ratio of coating materials and various reinforcing components, precise control of coating thickness.

[0177] 3. Prioritization

[0178] Use QFD (Quality Function Deployment) to build the House of Quality (HOQ), prioritize performance indicators, and sort customer needs.

[0179] 4. Conduct DFSS project demonstration

[0180] Use probability assessment and risk analysis tools to preliminarily assess design feasibility.

[0181] (S2) Define

[0182] Objective: Define critical quality characteristics (CTQ), select conceptual design solutions, and convert VOCs into CTQs.

[0183] In view of the large number of fuzzy, uncertain and even contradictory VOCs in the market, it is necessary to first optimize and screen them, and transform them into important, accurate and useful information through precise processing and fuzzy optimization methods. Subsequently, QFD is used to refine the VOCs layer by layer, clarify the design, process flow and production requirements of the composite gear, and extract CTQs. Finally, the product design and process requirements of the composite gear are determined by accurately identifying and quantifying customer needs. Combined with the comprehensive analysis of VOCs and CTQs, the geometric and physical properties of the gear are used as design factors for collaborative optimization and integrated into the design scheme. It is worth emphasizing that the evaluation criteria for the optimal CTQs items are proposed to determine the final performance evaluation items. These evaluation items can be expressed as functions of the input processing parameters throughout the entire product development process. Therefore, the design scheme based on CTQs is novel and challenging in the design of composite gears, and also represents an advanced improvement method for process and performance optimization.

[0184] Design Process

[0185] 1. Determine technical requirements (CTQ variables and tolerance limits)

[0186] Design basis:

[0187] According to the service requirements of composite coated gears, select appropriate reinforcement materials according to the following table:

[0188]

[0189]

[0190] Design variables: coating thickness S, graphene ratio x graphene , Boron Nitride Ratio x hBN , Alumina ratio x Al2O3 、Zirconium oxide ratio x ZrO2 , PTFE particle ratio x PTFE .

[0191] Tolerance range: Control the errors of each variable to meet the design goals.

[0192] 2. Concept design selection, simulation and review

[0193] TRIZ (Theory of Inventive Problem Solving) and fuzzy information processing were used to simulate and evaluate different design solutions and select the best concept. Based on the specific description of the composite coated gear in HOQ, the research objectives and design purposes were clarified, and customer needs were clearly defined. A multi-objective optimization (MOO) processing parameter back-adjustment method integrating customer needs was proposed as the core solution of the collaborative optimization system. On this basis, the multi-objective function of the design factor X was expressed as:

[0194]

[0195] In the formula, κ i (i=1,2,...,N) represents the weight factor, which is generally set to ±1.

[0196] When setting HOQ, customer needs (maximum wear rate W MAX , minimum decomposition temperature T MIN , Small vibration reduction amplitude V MIN , minimum noise reduction amplitude N MIN , Maximum friction coefficient μ MAX 、Minimum service life improvement L MIN ) is quantified, we have:

[0197]

[0198] wxya MAX ≤5;

[0199] 200℃≤T MIN

[0200] 20%≤V MIN

[0201] 20%≤N MIN

[0202] μ MAX ≤0.2

[0203] 30%≤L MIN

[0204] The amount of reinforcement material added can be optimized according to the process requirements to ensure a balance between the mechanical properties and process properties of the coating.

[0205] In order to achieve multi-performance synergistic optimization, composite reinforcement materials are designed in the following ways:

[0206] a. Two-component composite: such as graphene + boron nitride combination, which takes into account both lubricity and heat resistance.

[0207] b. Multi-component composite: such as the combination of alumina + graphene + PTFE particles, which has the characteristics of wear resistance, corrosion resistance and low friction.

[0208] c. Interface modification: Chemical or physical modification (such as acidification, coupling agent treatment) of the surface of the reinforcing material to improve its bonding strength and dispersibility with the PAI coating.

[0209] Addition sequence: Reinforcement materials should be added gradually during the preparation of the PAI coating matrix to avoid agglomeration.

[0210] Dispersion technology: Ultrasonic dispersion, mechanical stirring or high-energy ball milling are used to ensure that the reinforcing materials are evenly distributed in the coating.

[0211] (S3) Development stage (D:Develop)

[0212] Objective: Identify design parameters, model inputs and outputs, and develop manufacturing plans.

[0213] Design Process

[0214] 1. Use FMEA (Failure Mode and Effects Analysis) to identify potential defects

[0215] Analyze the potential failure modes of each design variable (coating thickness and material ratio) and develop risk avoidance measures.

[0216] According to the working load, rotation speed and tribological characteristics of the gear, the service thickness of the coating is determined by a theoretical calculation formula, and the thickness design is optimized in combination with the actual working conditions to ensure that the strength, transmission accuracy and lubrication requirements of the gear are met.

[0217] The coating service thickness is calculated by the following formula:

[0218]

[0219] Among them, F load Indicates the maximum working load on the gear surface; σ coating Maximum allowable stress in the coating.

[0220] 2. Use engineering analysis methods to identify design parameters

[0221] The experimental design (DOE) was used to generate the experimental matrix and collect data on the impact of design variables on performance indicators (wear resistance, heat resistance, vibration and noise reduction effect, friction coefficient, and service life).

[0222] 3. Build an input-output model

[0223] Regression Modeling:

[0224]

[0225] Goal: high wear resistance, high heat resistance, vibration and noise reduction, low friction coefficient, and long service life.

[0226] 4. Determine the manufacturing plan

[0227] Planning of manufacturing processes, including spraying technology, coating curing, inspection and precision control.

[0228] (S4) Optimize (O)

[0229] Goal: Optimize design parameters, ensure design robustness, and reduce process variability.

[0230] Design Process

[0231] 1. Determine process capability

[0232] Determine whether the design parameters (coating thickness, material ratio) meet the CTQ requirements and tolerance limits.

[0233] 2. Optimize design

[0234] Use multi-objective optimization (Monte Carlo method, robust design):

[0235] Maximize wear resistance, maximize heat resistance, maximize vibration and noise reduction, minimize friction coefficient, and maximize service life

[0236] Optimization objective function:

[0237] In step S7), the optimization objective function of the multi-objective optimization model is as follows:

[0238] f = a 1 W+a 2 T+a 3 V+a 4 N+a 5 μ+a 6 L(5)

[0239] 3. Robust design

[0240] Consider the noise factor (coating thickness deviation) to improve the robustness of the design.

[0241] 4. Statistical Tolerance Optimization

[0242] Optimize standard deviation and reduce manufacturing costs and precision requirements.

[0243] (S5) Verification phase (V)

[0244] Objective: To verify the design results and ensure that the design meets Six Sigma quality standards.

[0245] Design Process

[0246] 1. Prototype testing and verification

[0247] Composite coating gear specimens were manufactured and tested for friction coefficient, wear resistance and service life.

[0248] 2. Evaluate design performance

[0249] Reliability test: Mean time between failures (MTBF)

[0250] Life testing and failure mode analysis.

[0251] 3. Repeat design

[0252] If the verification results do not meet the CTQ requirements, return to the optimization stage to readjust the design parameters.

[0253] 4. Final Review

[0254] Conduct comprehensive review, complete design delivery and project summary.

[0255] 2. Thinning of the gear base

[0256] (1) Determination of tooth surface roughness requirements

[0257] According to the particle size and adhesion performance requirements of PAI coating and composite reinforcement materials, the target value of tooth surface roughness (Ra range is 2-8μm) is determined.

[0258] According to the principle of mechanical bonding of coating, the target value of tooth surface roughness is calculated by combining the formula:

[0259]

[0260] Wherein, k represents the proportionality coefficient, which is determined by empirical value or pre-experimental regression fitting;

[0261] γ represents the surface tension between the coating and the air;

[0262] θ represents the contact angle of the coating on the gear substrate;

[0263] σ represents the target bonding strength between the coating and the gear substrate;

[0264] (2) Matrix thinning process selection

[0265] The gear hobbing process is used to thin the gear matrix. During the process, the tooth thickness reduction must be strictly controlled, and the tolerance range should be less than ±0.001mm to ensure the precise matching of the subsequent coating thickness. During the gear hobbing process, the gear matrix is ​​thinned by controlling the displacement coefficient to perform negative displacement. The negative displacement coefficient is determined by the following formula:

[0266]

[0267] Where x represents the negative displacement coefficient; Δt represents the service thickness of the coating; and m represents the module of the composite gear.

[0268] (3) Sand blasting

[0269] If the tooth surface roughness still does not meet the design requirements after thinning, sandblasting is required. The sandblasting process parameters include:

[0270] Sandblasting particle size: 40-60μm;

[0271] Spray angle: 30°-45°;

[0272] Injection pressure: 0.6-0.8MPa.

[0273] The surface should be cleaned after sandblasting to ensure that there are no residual particles or oil stains on the tooth surface.

[0274] 3. Gear coating spraying

[0275] (1) Cleaning pretreatment

[0276] The gear surface is thoroughly cleaned by chemical or physical methods to remove oil, oxides and other impurities to ensure good adhesion between the coating and the substrate.

[0277] (2) Substrate preheating

[0278] According to the characteristics of PAI coating and composite reinforcement materials, the substrate preheating process is optimized. The preheating temperature range is 100-130℃ and the preheating time is 10-15 minutes to enhance the adhesion and uniformity of the coating.

[0279] (3) Spraying process

[0280] Use automated spray gun equipment to air spray PAI coatings. During the spraying process, control the spraying speed (10-15mm / s) to ensure that the coating is evenly distributed and the deviation of the spraying thickness is controlled within ±0.02mm.

[0281] Method for determining spraying thickness:

[0282] If the coating accuracy of the tooth surface meets the requirements after spraying, the spraying thickness = the service thickness of the coating;

[0283] If the tooth surface coating accuracy after spraying does not meet the requirements, the spraying thickness = coating service thickness + coating processing allowance.

[0284] (4) Curing process

[0285] After spraying, the gear is sent to the oven for curing. The curing temperature is 210-280℃ and the time is 0.5-1 hour. After curing, ensure that the wear resistance and heat resistance of the coating meet the design standards.

[0286] (5) Thickness detection and adjustment

[0287] The coating thickness is measured using a gear micrometer.

[0288] If the thickness does not meet the requirements, adjustments can be made by optimizing the spraying parameters (such as spraying pressure, spraying time, etc.), or multiple spraying can be used to achieve the required thickness.

[0289] 4. Gear coating processing

[0290] (1) When the accuracy is met:

[0291] If the thickness and precision of the coating after spraying meet the service requirements, it can be put into use directly.

[0292] (2) When the accuracy is not satisfied:

[0293] If the test result after spraying does not meet the accuracy requirements, the coating needs to be thinned. The processing method can be selected by precision grinding process to achieve the required tooth surface accuracy.

[0294] 5. Service data collection

[0295] (1) Tooth thickness monitoring

[0296] During the use of gears, measuring equipment should be used regularly to detect tooth thickness, determine the degree of coating wear and whether it meets service requirements.

[0297] (2) Data feedback and re-spraying

[0298] If the coating is worn to the design threshold (thickness reduced to 60% of the original design value), the relevant service data is recorded and re-spraying is performed. Through data analysis, the re-spraying process parameters are optimized to further extend the service life of the gear.

[0299] 2. Manufacturing and application stage of composite coated gears

[0300] Based on the data from the preliminary design stage and service conditions, dynamic monitoring and maintenance management of gears throughout their life cycle are carried out. Specifically, it includes:

[0301] 1. Gear surface maintenance

[0302] Clean the tooth surface regularly during service to ensure the operating performance of the gear.

[0303] 2. Re-spraying of coating

[0304] Re-spray the coating according to the degree of coating wear. The spraying thickness is designed based on the remaining service thickness of the coating and the target thickness.

[0305] 3. Matrix scrapping judgment

[0306] If the gear matrix no longer meets the manufacturing standards due to repeated thinning or structural fatigue, it will be terminated and converted to scrap or remanufacturing.

[0307] Embodiment 12:

[0308] The main structure of this embodiment is the same as any one of Embodiments 1 to 11. Furthermore, the present invention relates to a design and manufacturing method for a polyamide-imide (PAI) composite coated gear. By adopting the IDDOV model of Six Sigma Design (DFSS) framework, a full-process optimization scheme from design to manufacturing is developed to meet the requirements of high wear resistance, high heat resistance, vibration and noise reduction, low friction coefficient and long service life in the gear service environment. The design stage includes the precise ratio optimization of reinforcing materials (graphene, boron nitride, aluminum oxide, etc.). Combining QFD and TRIZ methods, a coating processing parameter design method based on multi-objective optimization (MOO) is proposed. In the manufacturing stage, key processes such as substrate thinning, sandblasting, spray curing and thickness detection are adopted to ensure the uniformity and service performance of the coating. In the service stage, the coating wear data is dynamically monitored and a re-spraying process plan is formulated to achieve the full life cycle management of the gear. The present invention significantly improves the service reliability and service life of the gear, and is suitable for high-performance mechanical transmission components under complex working conditions.

Claims

1. A method for designing and manufacturing a polyamide-imide composite coated gear, characterized in that: The following steps are involved: S1. Collect customer needs and functional requirements, prioritize customer needs, and build a quality house based on the quality function deployment method; S2. Develop design projects based on the priority of customer needs; S3. Preliminarily evaluate the feasibility of the design project through probability assessment and risk analysis tools. If the design is feasible, proceed to step S4), otherwise, return to step S1); S4. According to the quality house and functional requirements, obtain key quality characteristics and clarify the tolerance limit range of the amount of reinforcement material added to the polyamide-imide composite coating; The key quality characteristics include the wear rate, decomposition temperature, vibration reduction amplitude, noise reduction amplitude, friction coefficient and service life of the coating; S5. Establish a parameter-driven input-output model based on the multi-objective optimization processing parameter inversion method; S6. Inputting the key quality characteristics into the input-output model to obtain a design scheme for the polyamide-imide composite coating gear; the design scheme includes the thickness, material composition and proportion of the polyamide-imide composite coating reinforcement material; S7. Input the design solution into the multi-objective optimization model to obtain the optimized key quality characteristics; S8. Based on customer needs and optimized key quality characteristics, plan the manufacturing process, which includes thinning the gear substrate, gear coating spraying, and gear coating processing; S9. Manufacture polyamide-imide composite coated gear samples, and conduct wear resistance, heat resistance, vibration and noise reduction effect, friction coefficient and service life test and reliability test on the polyamide-imide composite coated gear samples to verify the service performance of the composite coated gear samples; the reliability test is to detect the mean time between failures of the composite coated gear samples; If the verification result does not meet the key quality characteristic requirements and tolerance limit range, return to step S5), otherwise, deliver the polyamide-imide composite coated gear sample.

2. The design and manufacturing method of the polyamide-imide composite coated gear according to claim 1 is characterized in that: In step S1), the customer requirements include gear wear resistance, heat resistance, vibration and noise reduction, friction coefficient, and service life performance requirements; The functional requirements include the requirements for the optimal ratio of each component in the coating material and the maximum error limit between the actual coating thickness and the designed coating thickness.

3. The design and manufacturing method of the polyamide-imide composite coated gear according to claim 1 is characterized in that: In step S4), the coating material of the coating layer comprises polyamideimide, reinforcing material, additives and coating solvent. The additives include dispersants, leveling agents and defoamers; The components of the reinforcing material need to undergo interface modification treatment; The components of the reinforcing material include at least one of graphene, boron nitride BN, aluminum oxide Al2O3, zirconium oxide ZrO2, and polytetrafluoroethylene PTFE particles. When the component of the reinforcing material is graphene, the amount of graphene used is 0.5-3.0% of the total mass of the coating; When the component of the reinforcing material is boron nitride BN, the amount of boron nitride BN is 1-5% of the total mass of the coating; When the component of the reinforcing material is aluminum oxide Al2O3, the amount of aluminum oxide Al2O3 used is 5-10% of the total mass of the coating; When the component of the reinforcing material is zirconium oxide ZrO2, the amount of zirconium oxide ZrO2 is 5-10% of the total mass of the coating; When the component of the reinforcing material is polytetrafluoroethylene (PTFE) particles, the amount of the polytetrafluoroethylene (PTFE) particles used is 2-8% of the total mass of the coating.

4. The design and manufacturing method of the polyamide-imide composite coated gear according to claim 1 is characterized in that: In step S4), the coating thickness t is calculated by the following formula: Where: F load Indicates the maximum working load on the gear surface; σ coating Indicates the maximum allowable stress of the coating.

5. The design and manufacturing method of the polyamide-imide composite coated gear according to claim 1, characterized in that: In step S5), the multi-objective function of the multi-objective optimization processing parameter inversion method is expressed as: Quantify customer needs, and the multi-objective function after quantification is as follows: Where: κ i represents the weight factor, i = 1, 2, ..., N; ω i The coefficient representing the design target, i = 1, 2, ..., N; N is the number of targets; R is the value range of the design variable; X represents the design factor, X = {W, T, V, N, μ, L}; W is the wear rate, W MAX is the maximum wear rate; T is the decomposition temperature, T MIN is the minimum decomposition temperature; V is the vibration reduction amplitude, V MIN is the minimum vibration reduction amplitude; N is the noise reduction amplitude, N MIN is the minimum noise reduction amplitude; μ is the friction coefficient, μ MAX is the maximum friction coefficient; L is the service life, L MIN This is the minimum service life increase.

6. The design and manufacturing method of the polyamide-imide composite coated gear according to claim 1, characterized in that: In step S5), the regression formula of the input-output model is as follows: Where: t is the coating thickness; x graphene ,x hBN , x PTFE They are graphene ratio, boron nitride ratio, aluminum oxide ratio, zirconium oxide ratio, and PTFE particle ratio respectively.

7. The design and manufacturing method of the polyamide-imide composite coated gear according to claim 1, characterized in that: In step S7), the optimization objective function of the multi-objective optimization model is as follows: f=a1W+a2T+a3V+a4N+a5μ+a6L (5) Wherein, a1, a2, a3, a4, a5, and a6 are weight coefficients of W, T, V, N, μ, and L.

8. The design and manufacturing method of the polyamide-imide composite coated gear according to claim 1, characterized in that: In step S8), the method for thinning the gear base includes the following steps: 1) Calculate the target value Ra of tooth surface roughness Where: k represents the proportionality coefficient; γ represents the surface tension between the coating and the air; θ represents the contact angle of the coating on the gear substrate; σ represents the target bonding strength between the coating and the gear substrate; 2) Use gear hobbing technology to thin the gear base; During gear hobbing, the gear base is thinned by controlling the modification coefficient to perform negative modification. The calculation formula of the negative modification coefficient x is as follows: Where: Δt represents the service thickness of the coating; m represents the module of the gear. 3) Determine whether the tooth surface roughness after thinning reaches the target value of the tooth surface roughness. If it reaches the target value, the thinning of the gear matrix is ​​completed, otherwise, sand blasting is required.

9. The design and manufacturing method of the polyamide-imide composite coated gear according to claim 1, characterized in that: In step S8), the gear coating spraying method comprises the following steps: 1) Clean the gear surface thoroughly; 2) Preheat the gear base; 3) Use automated spray gun equipment to air spray the gear substrate; 4) Send the gear into the oven for curing; 5) After curing is completed, use a gear micrometer to check the coating thickness to determine whether the coating thickness meets the thickness requirements. If it meets the requirements, the gear coating spraying is completed, otherwise, return to step 3).

10. The design and manufacturing method of the polyamide-imide composite coated gear according to claim 9, characterized in that: In step S8), whether gear coating processing is required is determined by the following method: determine whether the surface accuracy of the coating after spraying meets the requirements. If so, the gear can be put into use directly after spraying. Otherwise, processing allowance should be prepared when spraying the gear, and the coating should be thinned after spraying and curing to make its surface accuracy meet the requirements.

Citation Information

Patent Citations

  • Six sigma design method for spiral bevel gear shape co-manufacturing

    CN109408860A

  • Preparation method of gear coating

    CN115595407A

  • Anti-fatigue and safety regulation and control method for service structure having ultra-long service life in extreme environment

    WO2024055271A1

Cited By

  • Wear-resistant coating, preparation method thereof and application of wear-resistant coating in gear manufacturing

    CN120888234A

  • Wear-resistant coating for automobile balance shaft gear set and preparation method of wear-resistant coating

    CN120966361A