Solid composite electrolyte

By using fluoroelastomer and sulfide-based inorganic particles in the solid composite electrolyte of a solid state battery, combined with a slurry of a non-aqueous solvent, the problems of poor solvent compatibility, insufficient adhesion and insufficient flexibility of the solid state battery electrolyte in the prior art are solved, and the effects of high adhesion, flexibility and high ionic conductivity are achieved.

CN120113057APending Publication Date: 2025-06-06SOLVAY SPECIALTY POLYMERS ITALY SPA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380071904.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-08-10
Filing Date
2023-07-26
Publication Date
2025-06-06

AI Technical Summary

Technical Problem

The solid composite electrolytes of existing solid state batteries have problems such as poor solvent compatibility, insufficient adhesion to current collectors, complex manufacturing process and relatively weak flexibility.

Method used

A solid composite electrolyte containing fluoroelastomer and sulfide-based solid ion-conducting inorganic particles different from lithium salts is used to form a slurry in combination with a non-aqueous solvent to produce electrodes with excellent adhesion and better flexibility.

Benefits of technology

It achieves high adhesion characteristics and better flexibility to the current collector, while maintaining high ionic conductivity and good mechanical characteristics, improving the performance of solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120113057A_ABST
    Figure CN120113057A_ABST
Patent Text Reader

Abstract

The invention relates to a solid composite electrolyte comprising a) at least one fluoroelastomer and b) at least one sulfide-based solid ion-conducting inorganic particle different from a lithium salt, wherein the fluoroelastomer a) comprises repeating units derived from i) vinylidene fluoride and ii) 15.0 to 80.0 mol% of at least one C2-C8 chloro and / or bromo and / or iodo-fluoroolefin, the mol% being relative to the total moles of repeating units, and wherein the solid composite electrolyte does not contain a lithium salt; the present invention relates to a slurry for manufacturing a solid composite electrolyte, the slurry comprising a) a fluoroelastomer and b) sulfide-based solid ion conducting inorganic particles different from a lithium salt, and c) at least one non-aqueous solvent wherein the slurry does not contain a lithium salt; the present invention also relates to a solid-state battery comprising a positive electrode, a negative electrode, and a membrane, at least one of which comprises the solid composite electrolyte according to the present invention. The invention also relates to a binder solution for a solid state battery comprising a) at least one fluoroelastomer and c) at least one non-aqueous solvent.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority from European patent application No. 22189656.6 filed on August 10, 2022, the entire contents of which are incorporated by reference into this application for all purposes. Technical Field

[0003] The present invention relates to a solid composite electrolyte comprising a) at least one fluoroelastomer and b) at least one solid ion-conducting inorganic particle based on a sulfide other than a lithium salt, wherein the fluoroelastomer a) comprises repeating units derived from i) vinylidene fluoride and ii) 15.0 to 80.0 mol % of at least one C 2 -C 8 Chlorinated and / or brominated and / or iodinated fluoroolefins, the mol% is relative to the total molar number of repeating units, wherein the solid composite electrolyte does not contain a lithium salt; relates to a slurry for making a solid composite electrolyte, the slurry comprising a) a fluoroelastomer, b) solid ion-conducting inorganic particles based on sulfides other than lithium salts, and c) at least one non-aqueous solvent, wherein the slurry does not contain a lithium salt; relates to an electrode, the electrode comprising a solid composite electrolyte according to the present invention, d) at least one electroactive material, and optionally e) at least one conductive agent; and relates to a solid-state battery, the solid-state battery comprising a positive electrode, a negative electrode and a membrane, at least one of the positive electrode, the negative electrode and the membrane comprising a solid composite electrolyte according to the present invention. The present invention also relates to a binder solution for a solid-state battery, the binder solution comprising a) at least one fluoroelastomer according to the present invention and c) at least one non-aqueous solvent. Background Art

[0004] Lithium-ion batteries have maintained their dominance in the rechargeable energy storage device market for decades due to their multiple advantages such as light weight, reasonable energy density, and good cycle life. Nevertheless, with the development of high-power applications such as electric vehicles, hybrid electric vehicles, grid energy storage, etc., there is a continuous demand for better safety and higher energy density.

[0005] Therefore, solid-state battery is considered to be the energy storage device of next generation, and wherein highly combustible liquid electrolyte is replaced by solid electrolyte, thus can substantially eliminate the risk of ignition and / or explosion.As solid electrolyte, organic polymer, inorganic matter and composite material have been actively studied, and each of them has its own advantages and disadvantages.Especially, in view of the high ionic conductivity of solid electrolyte based on sulfide and good mechanical properties and easy processability of polymer, composite material (that is, inorganic electrolyte dispersed in polymer, for example comprising those of sulfide particles dispersed in polymer matrix) is considered to be the most promising solution on industrial scale.Nevertheless, there are also shortcomings to be solved, such as poor solvent compatibility of sulfide material, which limits the selection of polymer that can be used to manufacture electrolyte, insufficient adhesion of current collector to electrode, the process of manufacturing solid composite electrolyte is quite complicated, the flexibility of solid composite electrolyte is relatively weak etc.

[0006] US2015 / 096169 A1 (Kureha Corp. and Toyota) discloses that a positive electrode for a sulfide-based solid-state battery exhibits good adhesion to a current collector, the positive electrode being formed with a slurry containing a fluorine-based copolymer having a specific amount of VDF units (between 40 and 70 mol %).

[0007] WO 2021 / 039950 (Fujifilm) describes a composition containing an inorganic solid electrolyte, comprising an inorganic solid electrolyte, a polymer binder and a dispersion medium, wherein the polymer binder comprises a fluorine-based copolymer containing a VDF component and 21 to 65 mol% of a hexafluoropropylene (HFP) component, exhibits more than 60% adsorption to the inorganic solid electrolyte and effectively controls excessive viscosity increase, recondensation or sedimentation of inorganic particles, thereby achieving a solid-state battery with excellent cycle characteristics. In particular, the polymer binder exhibits a tensile fracture strain of 500% or more.

[0008] However, there remains a continuing need in this field for sulfide-based solid composite electrolytes that exhibit excellent adhesion to current collectors, and / or better flexibility while maintaining high ionic conductivity and good mechanical properties. Summary of the invention

[0009] A first object of the present invention is a solid composite electrolyte comprising a) at least one fluoroelastomer and b) at least one solid ion-conducting inorganic particle based on a sulfide other than a lithium salt, wherein the fluoroelastomer a) comprises repeating units derived from i) vinylidene fluoride (VDF) and ii) 15.0 to 80.0 mol % of at least one C2 -C 8 Chlorinated and / or brominated and / or iodinated fluoroolefins, the mol % is relative to the total molar number of the repeating units, wherein the solid composite electrolyte does not contain a lithium salt.

[0010] A second object of the present invention is a slurry for making a solid composite electrolyte, the slurry comprising a) a fluoroelastomer, b) solid ion-conducting inorganic particles based on sulfides other than lithium salts, and c) at least one non-aqueous solvent, wherein the slurry does not contain lithium salts.

[0011] A third object of the present invention is an electrode comprising a solid composite electrolyte according to the invention, d) at least one electroactive material and optionally e) at least one conducting agent.

[0012] A fourth object of the present invention is a solid-state battery comprising a positive electrode; a negative electrode; and a membrane located between the positive electrode and the negative electrode, wherein at least one of the positive electrode, the negative electrode and the membrane comprises a solid composite electrolyte according to the present invention, optionally d) at least one electroactive material and / or e) at least one conductive agent.

[0013] A fifth object of the present invention is a binder solution for solid-state batteries comprising a) at least one fluoroelastomer according to the present invention and c) at least one non-aqueous solvent.

[0014] The inventors have surprisingly found that the solid composite electrolyte according to the present invention can provide a particularly advantageous combination of properties, such as excellent adhesion to the current collector, better flexibility, and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 Figure 1 is a cross-section of a pressure cell for AC impedance spectroscopy, developed in-house at Solvay to measure the ionic conductivity of membranes. In the pressure cell, the membrane is pressed between 2 stainless steel electrodes during impedance measurements.

[0016] Figure 2 represents the equivalent circuit used to simulate the conductivity behavior of the solid composite electrolyte, where R1 and R2 represent the bulk resistance and grain boundary resistance, respectively, and Q2 and Q3 represent the grain boundary and electrode contributions, respectively. DETAILED DESCRIPTION

[0017] Ratios, concentrations, amounts and other numerical data may be presented in the form of a range herein. It should be understood that the use of such a range format is only for convenience and brevity, and should be flexibly interpreted as including not only the numerical values ​​explicitly mentioned as range limits, but also all individual numerical values ​​or sub-ranges included within this range, as if each numerical value and sub-range were explicitly mentioned. In the context of the present invention, the term 'percent by weight' (wt%) indicates the content of a specific component in a mixture, which is calculated as the ratio between the weight of the component and the total weight of the mixture. As used herein, unless otherwise expressly stated, the concentration of repeating units in 'percent by mole' (mol%) refers to the concentration relative to the total number of repeating units in the polymer.

[0018] It should be understood that the foregoing general description and the following detailed description are exemplary and are intended to provide further explanation of the claimed invention. Therefore, various changes and modifications described herein will be apparent to those skilled in the art. In addition, for the sake of clarity and brevity, descriptions of well-known functions and configurations may be omitted.

[0019] The present invention provides a solid composite electrolyte, which comprises:

[0020] a) at least one fluoroelastomer; and

[0021] b) at least one sulfide-based solid ion-conducting inorganic particle other than a lithium salt;

[0022] wherein the fluoroelastomer a) comprises repeating units derived from

[0023] i) vinylidene fluoride (VDF); and

[0024] ii) 15.0 to 80.0 mol% of at least one C 2 -C 8 Chloro and / or brominated and / or iodinated fluoroolefins, the mol % being relative to the total molar number of the repeating units,

[0025] The solid composite electrolyte does not contain lithium salt.

[0026] In one embodiment, the C 2 -C 8 The chlorinated and / or brominated and / or iodinated fluoroolefins ii) account for 15.0 to 65.0 mol %, preferably 15.0 to 50.0 mol %, the mol % being relative to the total number of moles of repeating units.

[0027] In another embodiment, the C 2 -C 8The chlorinated and / or brominated and / or iodinated fluoroolefins ii) are selected from the group consisting of 1,1-chlorofluoroethylene (CFE), chlorodifluoroethylene (CDFE), bromotrifluoroethylene, chlorotrifluoroethylene (CTFE), 1,2-dichloro-1,2-difluoroethylene, iodotrifluoroethylene, and combinations thereof.

[0028] In a specific embodiment, the C 2 -C 8 The chlorinated and / or brominated and / or iodinated fluoroolefin ii) is cis-1,2-dichloro-1,2-difluoroethylene or trans-1,2-dichloro-1,2-difluoroethylene, preferably trans-1,2-dichloro-1,2-difluoroethylene.

[0029] In another specific embodiment, the C 2 -C 8 The chlorinated and / or brominated and / or iodinated fluoroolefin ii) is chlorotrifluoroethylene (CTFE).

[0030] In a preferred embodiment, the fluoroelastomer a) comprises repeating units derived from VDF and CTFE.

[0031] In a more preferred embodiment, the fluoroelastomer a) comprises repeating units derived from 80.0 mol% of VDF and 20.0 mol% of CTFE.

[0032] In another more preferred embodiment, the fluoroelastomer a) comprises repeating units derived from 70.0 mol % of VDF and 30.0 mol % of CTFE.

[0033] In another more preferred embodiment, the fluoroelastomer a) comprises repeating units derived from 60.0 mol% of VDF and 40.0 mol% of CTFE.

[0034] In one embodiment, the fluoroelastomer a) further comprises C derived from iii) at least one C different from i) and ii) 2 -C 8 Repeating units of fluoroolefins.

[0035] In the present invention, the C 2 -C 8 Fluoroolefin iii) is selected from the group consisting of:

[0036] -C 2 -C 8 Perfluoroolefins, such as tetrafluoroethylene (TFE) and hexafluoropropylene (HFP);

[0037] -Hydrogenated C 2 -C 8Fluoroolefins, such as vinyl fluoride (VF), trifluoroethylene (TrFE), hexafluoroisobutylene;

[0038] - having the formula CH 2 =CH-R f (per)fluoroalkylethylene, wherein R f It is C 1 -C 6 (Per)fluoroalkyl;

[0039] -With formula CF 2 =CFOR f (per)fluoroalkyl vinyl ether (PAVE), where R f It is C 1 -C 6 (Per)fluoroalkyl;

[0040] -With formula CF 2 = (per)fluorooxyalkyl vinyl ether of CFOX, wherein X is C 1 -C 12 ((Per)fluoro)oxyalkyl;

[0041] -With style (Per)fluorodioxole

[0042] Where R f3 , R f4 , R f5 and R f6 are identical or different from each other and are independently selected from fluorine atoms, and C optionally containing at least one oxygen atom 1 -C 6 (Per)fluoroalkyl;

[0043] -With CFX 2 =CX 2 OCF 2 OR" f (per)fluoroalkoxy vinyl ether (MOVE), where R" f Selected from linear or branched C 1 -C 6 (Per)fluoroalkyl; C 5 -C 6 Cyclic (per) fluoroalkyl; and a linear or branched C 2 -C 6 (per)fluorooxyalkyl, and X 2 is F or H; preferably, R" f Yes - CF 2 CF 3 (MOVE1), -CF 2 CF 2 OCF 3(MOVE2), or -CF 3 (MOVE3), and X 2 is F; and

[0044] - combinations thereof.

[0045] In a specific embodiment, the C 2 -C 8 The fluoroolefin iii) is selected from the group consisting of vinyl fluoride (VF), trifluoroethylene (TrFE), tetrafluoroethylene (TFE), hexafluoropropylene (HFP), hexafluoroisobutylene, and combinations thereof.

[0046] In the present invention, the fluoroelastomer can be produced by suspension or emulsion polymerization.

[0047] In the present invention, the term "fluoroelastomer" is intended to designate the fluoropolymer resins serving as the base component for obtaining true elastomers. True elastomers are defined by ASTM, Special Technical Bulletin, No. 184, as materials that can be stretched to twice their intrinsic length at room temperature and, after holding them under tension for 5 minutes, recover within the same time to within 10% of their initial length once they are released.

[0048] Fluoroelastomers are generally amorphous, exhibit low crystallinity (i.e., have less than 20 vol% crystalline phase), and have a glass transition temperature (T g In most cases, the fluoroelastomer advantageously has a T below 10°C, preferably below 5°C, more preferably below 0°C, and even more preferably below -5°C. g .

[0049] The term "amorphous" herein is intended to mean a polymer having a heat of fusion of less than 5.0 J / g, preferably less than 3.0 J / g, and more preferably less than 2.0 J / g, as measured by differential scanning calorimetry (DSC) according to ASTM D3418 at a heating rate of 10°C / min.

[0050] In the present invention, the term "sulfide-based solid ion-conductive inorganic particle" is not particularly limited as long as it is a solid electrolyte material containing one or more sulfur atoms in the molecular structure or composition.

[0051] The sulfide-based solid ion-conductive inorganic particles preferably contain Li, S, and an element of Groups 13 to 15 (e.g., P, Si, Sn, Ge, Al, As, Sb, or B) to increase Li ion conductivity.

[0052] The sulfide-based solid ion-conducting inorganic particles according to the present invention are preferably selected from the group consisting of:

[0053] - Lithium tin phosphide ("LSPS") materials, such as Li 10 SnP 2 S 12 ;

[0054] - lithium phosphosulfide ("LPS") materials, such as glasses, crystals or glass-ceramics having the following formula: (Li 2 S) x -(P 2 S 5 ) y , where x+y=1 and 0≤x≤1; Li 7 P 3 S 11 ;Li 7 PS 6 ;Li 4 P 2 S 6 ;Li 9.6 P 3 S 12 and Li 3 PS 4 ;

[0055] - doped LPS, such as Li 2 CuPS 4 ;Li 1+2x Zn 1-x PS 4 , where 0≤x≤1; Li 3.33 Mg 0.33 P 2 S 6 and Li 4- 3x Sc x P 2 S 6 , where 0≤x≤1;

[0056] -With formula Li x P y S z A lithium phosphorus sulfide oxygen ("LPSO") material of O, wherein 0.33≤x≤0.67, 0.07≤y≤0.2, 0.4≤z≤0.55;

[0057] - Lithium phosphide materials containing X ("LXPS"), wherein X is Si, Ge, Sn, As, or Al, such as Li 10 SnP 2 S 12 , Li 10 G2 S 12 , Li 10 SiP 2 S 12 , and Li 2 SP 2 S 5 -SnS;

[0058] - lithium phosphorus oxysulfide containing X ("LXPSO"), wherein X is Si, Ge, Sn, As or Al;

[0059] - Lithium Silicon Sulfide ("LSS") materials, such as Li 2 SiS 3 , Li 2 SP 2 S 5 -SiS 2 , Li 2 SP 2 S 5 -SiS 2 -LiCl, Li 2 S-SiS 2 -P 2 S 5 , Li 2 S-SiS 2 -P 2 S 5 -LiI, Li 2 S-SiS 2 -LiI, Li 2 S-SiS 2 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , and Li 2 S-SiS 2 -Al 2 S 3 ;

[0060] -Lithium boron sulfide materials, such as Li 3 BS 3 and Li 2 SB 2 S 3 -LiI;

[0061] -Lithium tin sulfide materials and lithium arsenide materials, such as Li 0.8 Sn 0.8 S 2 , Li 4 S N 4 , Li 3.833 Sn 0.833 As0.166 S 4 , Li 3 AsS 4 -Li 4 S N 4 , and Ge substituted Li 3 AsS 4 ;

[0062] -Has the general formula Li a PS b X c A lithium phosphosulfide material, wherein X represents at least one halogen element selected from the group consisting of Cl, Br and I or a combination thereof; and a represents a number from 2.0 to 7.0, b represents a number from 3.5 to 6.0, and c represents a number from 0 to 3.0, such as Li 4 PS 4 Cl, Li 7 P 2 S 8 Cl, and Li 7 P 2 S 8 I; and

[0063] - combinations thereof.

[0064] In a more preferred embodiment, the sulfide-based solid ion-conducting inorganic particles are of the general formula Li a PS b X c Lithium phosphide materials, more particularly having the formula Li 6 PS 5 An argyrodite-type sulfide material of X, wherein X is Cl, Br, or I.

[0065] In another preferred embodiment, having the formula Li 6 PS 5 Argentatite-type sulfide materials of Y lack sulfur and / or lithium, such as Li 6-x PS 5-x Cl 1+x (where 0≤x≤0.5), or doped with heteroatoms.

[0066] Particularly preferred sulfide-based solid ion-conducting particles are lithium tin phosphide ("LSPS") materials (e.g., Li 10 SnP 2 S 12 ) and argyrodite-type sulfide materials (such as Li 6 PS 5 Cl).

[0067] In one embodiment, the amount of the sulfide-based solid ion-conducting inorganic particles b) is at least 40.0 wt%, preferably at least 60.0 wt%, more preferably at least 70.0 wt%, even more preferably at least 80.0 wt% and most preferably at least 90.0 wt%, and / or at most 99.8 wt%, preferably at most 99.5 wt%, more preferably at most 99.0 wt% and most preferably at most 98.0 wt%, based on the total weight of the solid composite electrolyte.

[0068] In a specific embodiment, the amount of the sulfide-based solid ion-conductive inorganic particles b) is 40.0 to 99.8 wt%, preferably 60.0 to 99.5 wt%, more preferably 70.0 to 99.0 wt%, even more preferably 80.0 to 99.0 wt%, and most preferably 90.0 to 99.0 wt%, based on the total weight of the solid composite electrolyte.

[0069] In a more specific embodiment, the amount of the sulfide-based solid ion-conductive inorganic particles b) is 95.0 to 99.0 wt % based on the total weight of the solid composite electrolyte.

[0070] In the present invention, b) at least one sulfide-based solid ion-conductive inorganic particle is different from a lithium salt conventionally used as an essential element of a lithium secondary battery.

[0071] The term "lithium salt" is intended herein to mean a substance that needs to be dissolved in a solvent to ensure ion conduction.

[0072] In lithium secondary batteries, the liquid electrolyte is mainly composed of lithium salts in non-aqueous organic solvents, in which lithium ions (i.e., Li + cations) act as charge carriers, so that the liquid electrolyte acts as a cation (i.e., Li + The conductive pathway for the movement of cations from the cathode to the anode during discharge. The dissolution of lithium salts is through the solvent - Li + The interaction is carried out, that is, Li + The dissociation of cation-(counter) anion interactions is critical. Therefore, many simple lithium salts are excluded from use in electrolytes because their strong cation-anion interactions lead to high lattice energies and thus poor stability in relevant aprotic solvents (e.g., LiCl, LiF, Li 2 O, etc. Non-limiting examples of lithium salts notably include lithium hexafluorophosphate (LiPF 6 ), lithium perchlorate (LiClO 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium hexafluoroantimonate (LiSbF 6 ), lithium hexafluorotantalate (LiTaF 6), lithium tetrachloroaluminate (LiAlCl 4 ), lithium tetrafluoroborate (LiBF 4 ), lithium chloroborate (Li 2 B 10 Cl 10 ), lithium fluoroborate (Li 2 B 10 F 10 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), Lithium Bis(FSO 2 ) 2 N(LiFSI), Lithium Bis(trifluoromethanesulfonyl)imide Li(SO 2 CF 3 ) 2 N(LiTFSI), and mixtures thereof.

[0073] Li + Cationic conductivity is derived from both the total ionic conductivity and the cation transfer number. Considering that the cation transfer number in non-aqueous organic solvents is low, for example, typically less than 0.5, ionic conductivity plays a key role in battery performance.

[0074] In short, a liquid electrolyte in which at least one lithium salt is dissolved in at least one non-aqueous organic solvent plays a key role as one of the main components of a conventional lithium secondary battery.

[0075] In this regard, recent advances in the field of batteries involve the use of solid substances as electrolyte materials, and among others, solid ion-conducting inorganic particles based on sulfides are promising materials. In such solid-state batteries, the solid electrolyte replaces the function / role of the liquid electrolyte. Although many efforts have been made to understand the ion transport mechanism in solid electrolytes, the Li+ transport mechanism within the solid electrolyte (i.e., the interface between the electrode and the electrolyte (electrode / solid electrolyte interface and the active material / solid electrolyte interface within the electrode)) is still unclear. + The cation diffusion behavior still lacks a deep understanding.

[0076] Like liquid electrolytes, solid electrolytes are ionic conductors that deliver ions between two electrodes. However, unlike liquid electrolytes, solid electrolytes do not need to dissociate / dissolve into Li + Cations make solid electrolytes conductive. For example, in lithium germanium sulfide Li 6 PS 5 The lithium cation in X (X = Cl, Br or I) is in Li + The cation diffusion mechanism plays a role as Li + However, it dissociates into Li in the non-aqueous solvent that constitutes the liquid electrolyte.+ The lithium salts of cations and corresponding counter anions are different. It should be understood that Li 6 PS 5 The lithium sites in X form local cages, in which multiple hopping processes may occur, namely bimodal hopping, intracage hopping, and intercage hopping, thereby generating Li + Cation diffusion / transport (Reddy et al., Sulfide and oxide inorganic solid electrolytes for All-Solid-State LiBatteries: Nanomaterials 2020, 10, 1606; doi: 10.3390 / nano10081606). That is, unlike liquid electrolytes, only one species in solid electrolytes is mobile and these structures have the mobile species (i.e., Li + cations), corresponding to a cooperative conduction mechanism.

[0077] In view of the above, lithium salts are significantly different from sulfide-based solid ion-conducting inorganic particles containing lithium species in their inorganic structure, because lithium salts need to be dissolved in a solvent to ensure ion conduction, while sulfide-based solid ion-conducting inorganic particles have an intrinsic ionic conductivity higher than 0.1 mS / cm at room temperature, which is due to the diffusion of sublattices of mobile lithium species in their inorganic skeletons.

[0078] In the present invention, the solid composite electrolyte does not contain a lithium salt.

[0079] EP 3940846 A1 (Solvay SA) discloses a solid composite electrolyte comprising at least one polymer, at least one sulfide-based solid ion-conducting inorganic particle, and at least one lithium salt, which exhibits excellent ionic conductivity.

[0080] In this respect, the solid composite electrolyte according to the present invention differs from the solid composite electrolyte of EA'846A1 in that the solid composite electrolyte of EA'846A1 comprises at least one solid ion-conducting inorganic particle based on sulfide and a "conductive" polymer, wherein the conductive polymer requires the presence of a lithium salt, whereas the solid composite electrolyte according to the present invention does not require the presence of a lithium salt. It is also believed that there may be two conductive pathways for the movement of cations from the cathode to the anode during discharge, namely one is a solid electrolyte and the other is a so-called (solid) polymer electrolyte. In the latter, the conduction of the cations is achieved by interaction with the substituent groups of the polymer chain.

[0081] The solid composite electrolyte of the present invention is characterized by high adhesion properties to a current collector when it is used to manufacture an electrode (eg, a positive electrode) of a solid-state battery.

[0082] In the present invention, the nature of the "current collector" depends on whether the electrode provided thereby is a positive electrode or a negative electrode. If the electrode of the present invention is a positive electrode, the current collector typically comprises, preferably consists of, at least one metal selected from the group consisting of aluminum (Al), nickel (Ni), titanium (Ti) and alloys thereof, preferably Al. If the electrode of the present invention is a negative electrode, the current collector typically comprises, preferably consists of, at least one metal selected from the group consisting of lithium (Li), sodium (Na), zinc (Zn), magnesium (Mg), copper (Cu) and alloys thereof, preferably Cu.

[0083] A second object of the present invention is a slurry for making a solid composite electrolyte, the slurry comprising a) at least one fluoroelastomer, b) at least one sulfide-based solid ion-conducting inorganic particle different from a lithium salt, and c) at least one non-aqueous solvent, wherein the slurry does not contain a lithium salt.

[0084] The fluoroelastomer is as defined in the present invention.

[0085] There is no particular limitation on the non-aqueous solvent, as long as the non-aqueous solvent c) is able to dissolve the fluoroelastomer a) and is compatible with the sulfide-based solid ion-conductive inorganic particles b), which means that the solvent has no negative impact on the ionic conductivity of the resulting solid composite electrolyte.

[0086] In one embodiment, the non-aqueous solvent c) is selected from the group consisting of nitrile-containing solvents, ethers, esters, thiols, thioethers, ketones and tertiary amines.

[0087] In a preferred embodiment, the non-aqueous solvent c) is a nitrile-containing solvent having the general formula R-CN, wherein R represents an alkyl group. Non-limiting examples of nitrile-containing solvents are acetonitrile, butyronitrile, valeronitrile, isobutyronitrile, and the like.

[0088] In another preferred embodiment, the non-aqueous solvent c) is a solvent having the general formula R 1 -OR 2 Ether, where R 1 and R 2 The alkyl radicals are independently represented by alkyl radicals. Ether solvents include cyclic ethers based on 3, 5 or 6 rings. Cyclic ethers may be substituted by alkyl radicals, may have unsaturation and may have additional functional elements such as nitrogen or oxygen atoms inside the ring. Non-limiting examples of (cyclic) ether solvents are diethyl ether, 1,2-dimethoxy ether, cyclopentyl methyl ether, diethyl ether, dibutyl ether, 1,3-dioxolane, anisole, tetrahydrofuran, methyltetrahydrofuran, tetrahydropyran, etc.

[0089] In another preferred embodiment, the non-aqueous solvent c) is a solvent having the general formula R 3 -COO-R 4 Esters, where R 3 and R 4 Independently represents an alkyl group. Non-limiting examples of ester solvents are butyl butyrate, ethyl benzoate, and the like.

[0090] In another preferred embodiment, the non-aqueous solvent c) is a solvent having the general formula R 5 =SH or a thiol having the general formula R 6 -SR 7 sulfide, where R 5 , R 6 and R 7 The thioether solvents include cyclic thioethers based on 3, 5 or 6 rings. The cyclic thioethers can be substituted by alkyl, can have unsaturation and can have additional functional elements such as nitrogen or oxygen atoms in the ring. The non-limiting examples of mercaptan solvents are ethanethiol, tert-dodecyl mercaptan, thiophenol, tert-butyl mercaptan, octanethiol, dimethyl sulfide, ethyl methyl sulfide, methyl benzyl sulfide etc.

[0091] In another preferred embodiment, the non-aqueous solvent c) is a solvent having the general formula R 8 R 9 Ketone with C=O, where R 8 and R 9 Independently represents an alkyl group. Non-limiting examples of ketone solvents are methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, acetophenone, benzophenone, and the like, preferably methyl isobutyl ketone.

[0092] In another preferred embodiment, the non-aqueous solvent c) is a solvent having the general formula R 10 R 11 R 12 N tertiary amine, where R 10 , R 11 and R 12 and independently represent an alkyl group. The N atom of the tertiary amine may be embedded in a 3-, 5-, or 6-membered ring. Non-limiting examples of tertiary amine solvents are triethylamine, dimethylbutylamine, tributylamine, cyclohexyldimethylamine, N-ethylpiperidine, and the like.

[0093] In the present invention, R 1 To R 12The alkyl groups of the present invention refer to "alkyl" including saturated hydrocarbons having one or more carbon atoms, including: straight chain alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, cyclic alkyl groups (or "cycloalkyl" or "alicyclic" or "carbocyclyl") such as cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl and cyclooctyl, branched alkyl groups such as isopropyl, tert-butyl, sec-butyl and isobutyl, and alkyl-substituted alkyl groups such as alkyl-substituted cycloalkyl and cycloalkyl-substituted alkyl groups, as defined above. In addition, the alkyl group may include functional groups such as one or more unsaturated, ether, carbonyl, carboxyl, hydroxyl, sulfhydryl, thiol, sulfoxyl, sulfonic acid, nitrile, nitro, nitroso, azo, amide, imide, amino, imine or halogen.

[0094] In a preferred embodiment, the non-aqueous solvent c) includes nitrile-containing solvents, such as acetonitrile; ethers, such as tetrahydrofuran, 2-methyl-tetrahydrofuran, 2,5-dimethyl-tetrahydrofuran, 1,3-dioxolane, diethyl ether and 1,2-dimethoxy ether; esters, such as butyl butyrate; and ketones, such as methyl isobutyl ketone.

[0095] In a more preferred embodiment, the non-aqueous solvent c) is an ester, such as butyl butyrate.

[0096] In another more preferred embodiment, the non-aqueous solvent c) is a ketone, such as methyl isobutyl ketone.

[0097] In one embodiment, the slurry may further comprise a second solvent, such as saturated and aromatic hydrocarbons, such as, but not limited to, linear and branched alkanes (eg, heptane), cyclic alkanes (eg, cyclohexane), and aromatic compounds (eg, xylene and toluene).

[0098] In the present invention, the slurry can be suitably prepared by a method comprising mixing the following by any method known to those skilled in the art: a) fluoroelastomer, b) sulfide-based solid ion-conductive inorganic particles, and c) non-aqueous solvent. In a preferred embodiment, the slurry is prepared by a method comprising dissolving a) fluoroelastomer in c) non-aqueous solvent, then adding b) sulfide-based solid ion-conductive inorganic particles, and mixing the resulting mixture.

[0099] In the present invention, the amount of a) fluoroelastomer in the slurry is such as to provide a solid composite electrolyte comprising an amount of the fluoroelastomer a) in the range of at least 1.0 wt%, preferably at least 1.5 wt%, more preferably 2.0 wt%, and / or at most 20.0 wt%, preferably at most 15.0 wt%, more preferably at most 10.0 wt%, most preferably at most 5.0 wt%, relative to the total weight of the fluoroelastomer a) and the sulfide-based solid ion-conductive inorganic particles b).

[0100] In a specific embodiment, the amount of a) fluoroelastomer in the slurry is such as to provide a solid composite electrolyte comprising an amount of the fluoroelastomer a) ranging from 1.0 to 20.0 wt%, preferably 1.5 to 15.0 wt%, more preferably 2.0 to 10.0 wt%, and most preferably 2.0 to 5.0 wt%, relative to the total weight of the fluoroelastomer a) and the sulfide-based solid ion-conducting inorganic particles b). Thus, the resulting solid composite electrolyte exhibits good cohesion between the fluoroelastomer a) and the sulfide-based solid ion-conducting inorganic particles b) while maintaining good ionic conductivity.

[0101] The slurry according to the present invention is typically applied to the foil of at least one inert flexible carrier by a technique selected from the following: casting, spraying, spin spraying, roller coating, blade coating, slot coating, gravure coating, inkjet printing, spin coating and screen printing. In one embodiment, the wet film thus obtained typically has a thickness of 10 to 400 μm, preferably 50 to 200 μm. The wet film is then dried at a temperature between 10°C and 200°C, preferably between 20°C and 80°C. An additional drying step can be suitably performed in an oven under vacuum at a temperature between 20°C and 150°C, preferably between 50°C and 80°C, to completely remove the solvent. Those skilled in the art can select the optimal duration and temperature of the drying step according to the boiling point of the solvent. The dry film thus obtained can be further subjected to an additional compression step, such as calendaring, uniaxial or isostatic compression method, to reduce porosity and increase the density of the solid composite electrolyte.

[0102] In another embodiment, the slurry may further comprise d) at least one electroactive material, and optionally e) at least one conductive agent.

[0103] In a preferred embodiment, the electroactive material d) is used in a positive electrode.

[0104] In the present invention, the term "positive electrode" is intended to denote in particular an electrode of an electrochemical cell, wherein reduction occurs during discharge, whereas the term "negative electrode" is intended to denote in particular an electrode of an electrochemical cell, wherein oxidation occurs during discharge.

[0105] In the present invention, the term "electroactive material" is intended to mean a material that is capable of incorporating or inserting lithium ions into its structure and releasing lithium ions therefrom in large quantities during the charging and discharging phases of the battery.

[0106] In the case of forming a positive electrode for a solid-state battery, the electroactive material for the positive electrode is not particularly limited. It may include a LiMQ 2Composite metal chalcogenides, where M is at least one metal selected from transition metals such as Co, Ni, Fe, Mn, Cr, and V, and Q is a chalcogen element such as O and S. Among these, it is preferred to use those having the formula LiMO 2 Based lithium composite metal oxides, where M is the same as defined above. Preferred examples thereof may include LiCoO 2 , LiNiO 2 , LiNi x Co 1-x O 2 (0 < x < 1) and spinel-structured LiMn 2 O 4 . Another preferred example thereof may include metal oxides based on lithium-nickel-manganese-cobalt having the formula LiNi x Mn y Co z O 2 (x + y + z = 1, referred to as NMC), such as LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O 2 , LiNi 0.6 Mn 0.2 Co 0.2 O 2 , and metal oxides based on lithium-nickel-cobalt-aluminum having the formula LiNi x Co y Al z O 2 (x + y + z = 1, referred to as NCA), such as LiNi 0.8 Co 0.15 Al 0.05 O 2 .

[0107] As an alternative, still in the case of forming a positive electrode for a lithium metal battery, the electroactive material of the positive electrode may include electroactive materials based on lithiated or partially lithiated transition metal oxyanions having the formula M 1 M 2 (JO 4 ) f E 1-f , where M 1 is lithium, which may be partially replaced by another alkali metal less than 20% of the M 1 metal; M 2 is a transition metal selected from Fe, Mn, Ni, or a mixture thereof at an oxidation level of +2, which may be partially replaced by one or more additional metals that are at an oxidation level between +1 and +5 and account for M 2Less than 35% of metal, including 0; JO 4 is any oxygen anion, where J is P, S, V, Si, Nb, Mo, or a combination thereof; E is a fluoride anion, a hydroxide anion, or a chloride anion; f is JO 4 The mole fraction of the oxygen anion, generally included between 0.75 and 1.

[0108] M as defined above 1 M 2 (JO 4 ) f E 1-f The electroactive material is preferably phosphate-based and may have an ordered or modified olivine structure.

[0109] More preferably, the electroactive material of the positive electrode has the formula Li 3-x M’ y M” 2-y (JO 4 ) 3 , where 0 ≤ x ≤ 3, 0 ≤ y ≤ 2, M’ and M” are the same or different metals, at least one of which is a transition metal; JO 4 is preferably PO 4 , which may be partially replaced by another oxygen anion, where J is S, V, Si, Nb, Mo, or a combination thereof. Even more preferably, the electroactive material is a phosphate-based electroactive material having the formula Li(Fe x Mn 1-x )PO 4 , where 0 ≤ x ≤ 1, preferably x = 1, that is, lithium iron phosphate having the formula LiFePO 4 .

[0110] In a preferred embodiment, the electroactive material of the positive electrode is selected from the group consisting of: LiMQ 2 , where M is at least one metal selected from Co, Ni, Fe, Mn, Cr, and V and Q is O or S; LiNi x Co 1-x O 2 (0 < x < 1); spinel-structured LiMn 2 O 4 ; lithium-nickel-manganese-cobalt-based metal oxide (NMC) having the formula LiNi x Mn y Co z O 2 (x + y + z = 1), lithium-nickel-cobalt-aluminum-based metal oxide having the formula LiNi x Co y Al z O 2(x+y+z=1) based on lithium-nickel-cobalt-aluminum metal oxide (NCA), lithium-cobalt metal oxide (LCO), lithium-nickel-manganese metal oxide (LNMO) and LiFePO 4 .

[0111] In a more preferred embodiment, the electroactive material of the positive electrode is selected from the group consisting of NMC, NCA, LCO, and LNMO.

[0112] In the present invention, the term "conductive agent" is intended to specifically refer to a material for ensuring that the electrode has good charge and discharge properties and provides additional conductivity. Non-limiting examples of conductive agents are carbonaceous materials and metal powders or fibers, such as carbon black, carbon nanotubes (CNTs), vapor-grown carbon fibers (VGCFs), graphite, graphene, graphite fibers, etc. Examples of carbon black include Ketjen black and acetylene black. Metal powders or fibers include nickel and aluminum powders or fibers.

[0113] In a specific embodiment, the amount of a) fluoroelastomer in the slurry is such as to provide a solid composite electrolyte comprising an amount of the fluoroelastomer a) in the range of 1.0 to 20.0 wt%, preferably 1.5 to 15.0 wt%, more preferably 2.0 to 10.0 wt%, and most preferably 2.0 to 5.0 wt% relative to the total weight of the fluoroelastomer a), the sulfide-based solid ion-conducting inorganic particles b), the electroactive material c), and optionally e) at least one conductive agent. Thus, the resulting electrode exhibits excellent adhesion to the current collector.

[0114] A third object of the present invention is an electrode comprising a solid composite electrolyte according to the invention, d) at least one electroactive material and optionally e) at least one conducting agent.

[0115] In one embodiment, the electroactive material d) is used in a positive electrode.

[0116] In one embodiment, the positive electrode comprises a solid composite electrolyte according to the present invention, d) at least one electroactive material, and optionally e) at least one conductive agent.

[0117] In a specific embodiment, the positive electrode comprises a solid composite electrolyte comprising a) a VDF-CTFE copolymer as a fluoroelastomer, b) a Li+ as a sulfide-based solid ion-conducting inorganic particle, 6 PS 5 Cl, LiNi as d) electroactive material for the positive electrode 0.6 Mn 0.2 Co 0.2 O 2 , and optionally carbon black as e) a conductive agent.

[0118] In a more specific embodiment, the VDF-CTFE copolymer as the fluoroelastomer a) comprises repeating units derived from CTFE in an amount of 15.0 to 50.0 mol %, the mol % being relative to the total moles of repeating units.

[0119] A fourth object of the present invention is a solid-state battery comprising a positive electrode; a negative electrode; and a membrane located between the positive electrode and the negative electrode, wherein at least one of the positive electrode, the negative electrode and the membrane comprises a solid composite electrolyte according to the present invention, optionally d) at least one electroactive material and / or e) at least one conductive agent.

[0120] In the present invention, the term "membrane" is intended to mean in particular an ion-permeable membrane placed between the positive electrode and the negative electrode. Its function is to allow lithium ions to pass through while blocking electrons and ensuring physical isolation between the electrodes.

[0121] A fifth object of the present invention is a binder solution for solid-state batteries comprising a) at least one fluoroelastomer according to the present invention and c) at least one non-aqueous solvent.

[0122] The non-aqueous solvent is as defined in the present invention.

[0123] When the binder solution according to the present invention is used to prepare a solid composite electrolyte, a person skilled in the art can easily select an appropriate amount of the non-aqueous solvent c) to achieve uniform dissolution of the fluoroelastomer a) and proper evaporation thereof. This solid composite electrolyte can be used as a membrane between a positive electrode and a negative electrode or as an electrode of a solid-state battery.

[0124] Should the disclosure of any patents, patent applications, and publications incorporated herein by reference conflict with the description of the present application to the extent that it might render a term unclear, the present invention shall take precedence.

[0125] The present invention will now be described in more detail with reference to the following examples, which are for illustrative purposes only and are not intended to limit the scope of the present invention.

[0126] Examples

[0127] raw materials

[0128] -Crystallized sulfide-based solid ion-conducting inorganic particles LPSCl (Li 6 PS 5 Cl), commercially available from NEI Corporation;

[0129] -NMC622( NMC KHX12), commercially available from Umicore;

[0130] -Conductive carbon black (C-NERGY TM SUPER C65T), commercially available from Imerys;

[0131] - butyl butyrate (BB), commercially available from Sigma Aldrich; and

[0132] -Methyl isobutyl ketone (MIBK), commercially available from Sigma-Aldrich Fluoroelastomers

[0133] -Polymer 1: VDF-CTFE (80 / 20 in mol%), synthesized in-house at Solvay Specialty Polymers Italy SpA

[0134] -Polymer 2: VDF-CTFE (70 / 30 in mol%), synthesized in-house at Solvay Specialty Polymers Italy

[0135] - Polymer 3: VDF-CTFE (60 / 40 in mol %), G150M, commercially available from Arkema (T g =-16℃)

[0136] -Polymer 4: VDF-CTFE (86 / 14 in mol%), synthesized in-house at Solvay Specialty Polymers Italy

[0137] - Polymer 5: VDF-HFP (78.5 / 21.5 mol%), N935, commercially available from Solvay Specialty Polymers Italy (T g =-19°C).

[0138] Synthesis of polymers 1, 2 and 4

[0139] Polymer 1:

[0140] In a steel vertical autoclave equipped with baffles and a stirrer operating at 550 rpm, 1.3 L of demineralized water were introduced. The temperature was then brought to a reaction temperature of 75° C. and 3.5×10 5 Pa (absolute pressure) of VDF. A gaseous mixture of VDF-CTFE with a nominal molar ratio of 80 / 20 was added by using a compressor until a pressure of 20.0×10 5 The pressure is Pa (absolute pressure).

[0141] Before starting the reaction, the composition of the gaseous mixture present in the head of the autoclave was analyzed by gas chromatography: 83.5 mol% of VDF and 16.5 mol% of CTFE. Subsequently, 45.0 cc of ammonium persulfate (NH 4 ) 2 S 2 O 8 ) in ethyl acetate solution (3% w / w) and 2 ml of pure ethyl acetate were fed into the autoclave.

[0142] The polymerization pressure was maintained constant by feeding the monomer mixture, and when 300.0 g of the mixture had been fed, the feed was stopped, the reactor was cooled to room temperature and then degassed to remove residual (i.e., unreacted) monomers. The latex as produced was discharged and further degassed with nitrogen for 24 hours. The resulting polymer was then separated by using standard separation procedures with aluminum sulfate (Al 2 (SO 4 ) 3 ) and then dried in a ventilated oven at 90° C. for 24 hours.

[0143] Polymer 2:

[0144] Polymer 2 was synthesized in the same manner as Polymer 1 except that a gaseous mixture of VDF-CTFE with a nominal molar ratio of 70 / 30 was mixed with 3.3 × 10 5 Pa (absolute pressure) of VDF were added together. Before the start of the reaction, the composition of the gaseous mixture present in the head of the autoclave was analyzed by gas chromatography: 73.8 mol% of VDF and 26.2 mol% of CTFE.

[0145] Polymer 4:

[0146] Polymer 4 was synthesized in the same manner as Polymer 1 except that a gaseous mixture of VDF-CTFE with a nominal molar ratio of 86 / 14 was mixed with 3.8 × 10 5 Pa (absolute pressure) of VDF were added together. Before the start of the reaction, the composition of the gaseous mixture present in the head of the autoclave was analyzed by gas chromatography: 88.8 mol% of VDF and 11.2 mol% of CTFE.

[0147] Preparation of solid composite electrolytes

[0148] Example 1 (E1) of the present invention

[0149] A solid composite electrolyte composed of 95.0 parts by weight (pbw) of LPSCl and 5.0 pbw of polymer 1 was produced in the form of a film as follows:

[0150] A 10.0 wt% polymer solution was prepared by weighing 1.0 g of polymer 1 and 9.0 g of BB. Subsequently, 3.705 g of LPSCl, 1.95 g of the 10.0 wt% polymer solution and 0.345 g of BB were mixed with 4 glass balls under magnetic stirring at 400 rpm for a minimum of 6 hours. The solid content of the slurry and the casting speed were adjusted so that the slurry viscosity was maintained between 2.0 and 10.0 Pa.s during casting. The obtained slurry was cast on a flexible support ( FN). The wet film was dried on a hot plate at 50°C for one hour and then placed in an oven under vacuum at 80°C during the night. The samples were stored in mini grip bags and then placed in sealed bags. All experiments were performed in an argon-filled glove box.

[0151] Inventive Example 2 (E2) and Inventive Example 3 (E3)

[0152] The solid composite electrolytes of E2 and E3 were prepared in the same manner as E1, except that polymer 2 and polymer 3 were used instead of polymer 1, respectively.

[0153] Example 4 (E4) of the present invention

[0154] The solid composite electrolyte of E4 was prepared in the same manner as E1, except that MIBK was used instead of BB as the solvent.

[0155] Comparative Example 1 (CE1)

[0156] CE1 was prepared in the same manner as E1, except that polymer 4 was used instead of polymer 1. For CE1, both BB and MIBK were tried as solvents, respectively. However, polymer 4 was not soluble in either BB or MIBK, making it impossible to form a solid composite electrolyte in the form of a film.

[0157] Comparative Example 2 (CE2)

[0158] The solid composite electrolyte of CE2 was prepared in the same manner as E1, except that polymer 5 was used instead of polymer 1.

[0159] Comparative Example 3 (CE3)

[0160] The solid composite electrolyte of CE3 was prepared in the same manner as CE2, except that MIBK was used instead of BB as the solvent.

[0161] Preparation of positive electrode

[0162] The positive electrodes of E1-E3 and CE2 composed of 74.0 pbw NMC622, 20.0 pbw LPSCl, 2.0 pbw conductive carbon black, and 4.0 pbw fluoroelastomer (selected from polymers 1 to 3 and polymer 5, respectively) were produced as follows:

[0163] A 10.0 wt% binder solution was prepared by weighing 1.0 g of fluoroelastomer and 9.0 g of BB. Subsequently, 1.0 g of LPSCl, 0.1 g of conductive carbon, 3.7 g of NMC622 and 2.0 g of 10.0 wt% binder solution were mixed with 4 glass balls under magnetic stirring at 400 rpm for at least 6 hours. The slurry obtained was cast on an aluminum (Al) current collector using an automatic film applicator from ECO. The solid content and casting speed of the slurry were adjusted so that the slurry viscosity was maintained between 2.0 and 10.0 Pa.s during casting and so as to obtain 25.0 to 30.0 mg / cm 2 The wet film was dried on a hot plate at 50°C for one hour, placed in an oven under vacuum at 80°C during the night, stored in a mini grip bag, and then placed in a sealed bag. The experiments were performed in an argon-filled glove box.

[0164] The cathodes of E4 and CE3 were produced in the same manner as described above, except that MIBK was used instead of BB as the solvent.

[0165] Adhesion of positive electrode to Al current collector (peel test)

[0166] The adhesion strength of the positive electrode to the Al current collector is evaluated using a 180° peel test. The electrode strips (2cm*10cm) of the dried electrode are fixed on a rigid Al plate (2.6cm*10cm) with the electrode facing down and the current collector facing up using double-sided tape (width 25mm; thickness 0.24mm). Using an electric tension / compression tester (ESM303, from Mark-10 Corporation), an angle of 180° is maintained and the Al current collector is peeled off from the electrode at a constant speed of 300mm / min. The force required to remove the Al current collector from the electrode is recorded in Table 1, which is the average value of 3 independent strips generated by 3 independent electrodes using 3 independent slurries with the same composition. The peel test was carried out in a dry room with a dew point of -40°C.

[0167] In all cathodes from E1 to E4, significant adhesion properties to the Al current collector are clearly observed, unlike those of CE2 and CE3.

[0168] Bending test of solid composite electrolytes E1, E3 and CE2

[0169] By using a cylindrical mandrel bend tester ( 1506) implements a bending test to measure the flexibility / elongation properties of solid composite electrolytes. The tester has a bending bar with height-adjustable rollers and a sliding vise for clamping the sample so that the test piece is perfectly and regularly bent on a decreasing mandrel until the desired effect can be observed.

[0170] The solid composite electrolytes of E1, E3 and CE2 in the form of self-supporting films were bent on different cylinders varying from large diameter to small diameter. The diameter of the first cylinder when cracks began to appear when the film was bent on the cylinder was observed. The results are recorded in Table 1. For the solid composite electrolytes of E1 and E3, the first cracks were observed when bent on a cylinder with a diameter of 2 mm, while the solid composite electrolyte of CE2 began to crack earlier when bent on a cylinder with a diameter of 3 mm.

[0171] Ionic conductivity of solid composite electrolytes E1, E3 and CE2

[0172] The ionic conductivity of the solid composite electrolytes of E1, E3 and CE2 in membrane form was measured by AC impedance spectroscopy using an in-house developed pressure cell, where the membrane was pressed between two stainless steel electrodes during the impedance measurement. The cross section of the pressure cell is Figure 1 Shown in.

[0173] The impedance spectrum was measured at a pressure of 370 MPa and a temperature of 20° C. AC impedance measurements were performed with a potentiostat (VMP-300, BioLogic Science Instruments SAS, France) in the frequency range of 1000 Hz to 4.7 MHz.

[0174] The Nyquist plot of solid composite electrolytes shows the typical behavior of solid electrolytes (inorganic, polymer or composite materials) with semicircular and Warburg type impedances in the high frequency region and low frequency region, respectively. According to the equivalent circuit R1(R2 / Q2)Q3 (see Figure 2 ) is used to simulate the conductive behavior of the composite electrolyte, where R is the resistance and Q is the constant phase element, where R1 and R2 represent the bulk resistance and grain boundary resistance, respectively, and Q2 and Q3 represent the grain boundary and electrode contributions, respectively.

[0175] The intercept of the semicircle with the real axis at high frequencies is attributed to the bulk resistance (R1), while the intercept with the real axis at low frequencies is attributed to the total resistance of the membrane (R1+R2). This total resistance R is conventionally used to calculate the conductivity of solid composite electrolytes. Therefore, the ionic conductivity σ is obtained using the equation σ=d / (R x A), where d is the thickness of the membrane and A is the area of ​​the stainless steel electrode. The SI unit of ionic conductivity is Siemens / meter (S / m), where S is ohm -1 , and 1 millisiemens / centimeter (mS / cm) is the decimal part of the SI unit, that is, 1 mS / cm=0.1 S / m.

[0176] Table 1

[0177]

[0178] *NA: Not available

Claims

1. A solid composite electrolyte comprising: a) at least one fluoroelastomer; and b) at least one sulfide-based solid ion-conducting inorganic particle other than a lithium salt; wherein the fluoroelastomer a) comprises repeating units derived from i) vinylidene fluoride (VDF); and ii) 15.0 to 80.0 mol% (mol%) of at least one C 2 -C 8 Chloro and / or brominated and / or iodinated fluoroolefins, the mol % being relative to the total molar number of the repeating units, The solid composite electrolyte does not contain lithium salt.

2. The solid composite electrolyte according to claim 1, in, The C 2 -C 8 The chlorinated and / or brominated and / or iodinated fluoroolefins ii) account for 15.0 to 65.0 mol %, preferably 15.0 to 50.0 mol %, the mol % being relative to the total number of moles of repeating units.

3. The solid composite electrolyte according to claim 1 or 2, in, These C 2 -C 8 The chlorinated and / or brominated and / or iodinated fluoroolefins ii) are selected from the group consisting of 1,1-chlorofluoroethylene (CFE), chlorodifluoroethylene (CDFE), bromotrifluoroethylene, chlorotrifluoroethylene (CTFE), 1,2-dichloro-1,2-difluoroethylene, iodotrifluoroethylene, and combinations thereof.

4. The solid composite electrolyte according to any one of claims 1 to 3, in, The fluoroelastomer a) further comprises C derived from iii) at least one compound different from i) and ii) 2 -C 8 Repeating units of fluoroolefins.

5. The solid composite electrolyte according to claim 4, in, The C 2 -C 8 The fluoroolefin iii) is selected from the group consisting of vinyl fluoride (VF), trifluoroethylene (TrFE), tetrafluoroethylene (TFE), hexafluoropropylene (HFP), hexafluoroisobutylene, and combinations thereof.

6. The solid composite electrolyte according to any one of claims 1 to 5, in, The fluoroelastomer a) has a heat of fusion as measured according to ASTM D3418 of less than 5.0 J / g, preferably less than 3.0 J / g, more preferably less than 2.0 J / g.

7. The solid composite electrolyte according to any one of claims 1 to 6, in, The sulfide-based solid ion-conducting inorganic particles b) are selected from the group consisting of: -Lithium tin phosphide ("LSPS") materials, such as Li 10 SnP 2 S 12 ; - lithium phosphosulfide ("LPS") materials, such as glasses, crystals or glass ceramics having the following formula: (Li 2 S) x -(P 2 S 5 ) y , where x+y=1 and 0≤x≤1; Li 7 P 3 S 11 ;Li 7 PS 6 ;Li 4 P 2 S 6 ;Li 9.6 P 3 S 12 and Li 3 PS 4 ; - doped LPS, such as Li 2 CuPS 4 ;Li Li 1+2x Zn 1-x PS 4 , where 0≤x≤1; Li 3.33 Mg 0.33 P 2 S 6 and Li 4- 3x Sc x P 2 S 6 , where 0≤x≤1; - a lithium phosphorus oxysulfide ("LPSO") material having the formula LixPySzO, wherein 0.33≤x≤0.67, 0.07≤y≤0.2, 0.4≤z≤0.55, 0≤w≤0.15; - Lithium phosphide materials containing X ("LXPS"), where X is Si, Ge, Sn, As, Al, such as Li 10 G 2 S 12 and Li 10 SiP 2 S 12 ; - lithium phosphorus oxysulfide containing X ("LXPSO"), wherein X is Si, Ge, Sn, As, Al; - lithium silicon sulfide ("LSS") materials; -Lithium boron sulfide materials, such as Li 3 BS 3 and Li 2 SB 2 S 3 -LiI; -Lithium tin sulfide materials and lithium arsenide materials, such as Li 0.8 Sn 0.8 S 2 , Li 4 S N 4 , Li 3.833 Sn 0.833 As 0.166 S 4 , Li 3 AsS 4 -Li 4 S N 4 , Ge substituted Li 3 AsS 4 ; as well as -Has the general formula Li a PS b X c A lithium phosphorus sulfide material, wherein X represents at least one halogen element selected from the group consisting of Cl, Br and I or a combination thereof; and a represents a number from 2.0 to 7.0, b represents a number from 3.5 to 6.0, and c represents a number from 0 to 3.

0.

8. A slurry for making a solid composite electrolyte according to any one of claims 1 to 7, comprising a) at least one fluoroelastomer, b) at least one sulfide-based solid ion-conductive inorganic particle other than a lithium salt, and c) at least one non-aqueous solvent, wherein the slurry does not contain a lithium salt.

9. The slurry according to claim 8, in, The non-aqueous solvent c) is selected from the group consisting of nitrile-containing solvents, ethers, esters, thiols, thioethers, ketones, tertiary amines, and cyclic carbonates, preferably butyl butyrate and / or methyl isobutyl ketone.

10. The slurry according to claim 8 or 9, further comprising d) at least one electroactive material and optionally e) at least one conductive agent.

11. The slurry according to claim 10, in, The electroactive material d) is for the positive electrode and is selected from the group consisting of: having the formula LiNi x Mn y Co z O 2 (x+y+z=1) based lithium-nickel-manganese-cobalt metal oxide having the formula LiNi x Co y Al z O 2 (x+y+z=1) lithium-nickel-cobalt-aluminum-based metal oxide, lithium-cobalt-based metal oxide, and lithium-nickel-manganese-based metal oxide.

12. An electrode comprising the solid composite electrolyte according to any one of claims 1 to 7, d) at least one electroactive material, and optionally e) at least one conductive agent.

13. The electrode according to claim 12, in, The electroactive material d) is for the positive electrode and is selected from the group consisting of: having the formula LiNi x Mn y Co z O 2 (x+y+z=1) based lithium-nickel-manganese-cobalt metal oxide having the formula LiNi x Co y Al z O 2 (x+y+z=1) lithium-nickel-cobalt-aluminum-based metal oxide, lithium-cobalt-based metal oxide, and lithium-nickel-manganese-based metal oxide.

14. A solid-state battery comprising a positive electrode, a negative electrode, and a membrane located between the positive electrode and the negative electrode, wherein at least one of the positive electrode, the negative electrode and the membrane comprises a solid composite electrolyte according to any one of claims 1 to 7, optionally further comprising d) at least one electroactive material and / or e) at least one conductive agent.

15. A binder solution for a solid-state battery comprising a) at least one fluoroelastomer and c) at least one non-aqueous solvent, wherein the fluoroelastomer a) comprises repeating units derived from: i) vinylidene fluoride (VDF); and ii) 15.0 to 80.0 mol% of at least one C 2 -C 8 For chlorinated and / or brominated and / or iodinated fluoroolefins, the mol % is relative to the total molar number of repeating units.

Citation Information

Patent Citations

  • Solid composite electrolyte

    EP3940846A1

  • Slurry for positive electrode for sulfide-based solid-state battery, positive electrode for sulfide-based solid-state battery and method for manufacturing the same, and sulfide-based solid-state battery and method for manufacturing the same

    US20150096169A1

  • Inorganic solid electrolyte-containing composition, sheet for solid-state secondary batteries, solid-state secondary battery, and methods for producing solid-state secondary battery and sheet for solid-state secondary batteries