Preparation process of collection paper literature deacidification test paper

By preparing a deacid test paper for the collection of paper documents, the problem of lack of unified evaluation standards and irreversible damage in the prior art is solved, and a more reliable and economical deacidification effect evaluation is achieved, supporting the application of deacidification technology in the overall paper on a large scale.

CN120119491APending Publication Date: 2025-06-10NANJING FORESTRY UNIV

Patent Information

Application Number
CN202411425799.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2025-06-10

AI Technical Summary

Technical Problem

The existing technology lacks a unified standard system for evaluating deacidity effects. The existing detection methods require destructive testing directly using document entities, resulting in irreversible damage to precious documents, and existing industrial papers cannot accurately simulate the deacidity behavior of real documents.

Method used

A paper-based document deacidification test paper is developed in the library. By selecting bleached wood pulp and straw pulp as raw materials, rosin latex liquid, alum solution and saturated alum solution, it is prepared through beating, pulp preparation, pulp injection, whitening amount, adjusting pH value and adding retention aids, and finally drying under specific conditions to obtain a deacidification test paper that can replace the document entity.

Benefits of technology

It provides a more reliable, comprehensive and economical method for deacidification effect evaluation, which can replace precious literature for lossy testing, support the construction of a deacidification effect evaluation system, and promote the large-scale application of deacidification technology in this paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120119491A_ABST
    Figure CN120119491A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation technology of collection paper literature deacidification test paper, and belongs to the technical field of papermaking engineering. The method comprises the following steps: firstly, determining physicochemical indexes of the deacidification test paper according to ontology characteristics of precious ancient books and recent modern paper literatures, then taking saponified rosin size as an internal sizing agent, taking talcum powder as a filler, taking cationic polyacrylamide (CPAM) as a retention aid, and finally, carrying out papermaking and drying to obtain the deacidification test paper. The performance of the product prepared by the process is basically consistent with that of recent modern literature paper, the product has the capability of replacing a paper literature body to carry out lossy testing, and a more reliable, more comprehensive and more economical basis can be provided for constructing a deacidification effect evaluation system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of papermaking engineering, and particularly relates to a preparation process of a deacidification test paper for library paper documents. Background Art

[0002] At present, there is no unified deacidification effect evaluation standard system in China's industry. Existing detection methods require direct use of the literature entity for destructive testing, which causes irreversible damage to precious literature. Although a variety of industrial papers have been developed in China, such as wrapping paper (CN 117926636 A), coated paper (CN 102817277 A), etc., there are essential differences in key parameters such as fiber morphology and acid-base properties between these papers and literature papers, and the deacidification behavior of real literature cannot be accurately simulated. To address these problems, based on the physical and chemical properties of precious ancient books and modern paper documents, the present invention develops a special deacidification test paper to replace the literature entity for destructive testing, which will provide a more reliable, comprehensive and economical scientific basis for constructing a deacidification effect evaluation system. This is also a key issue that needs to be addressed for promoting the application of deacidification technology for large-scale integral literature. Summary of the Invention

[0004] Aiming at the problems existing in the prior art, the technical problem to be solved by the present invention is to provide a preparation technology for a deacidification test paper for library paper documents, and its product can replace the paper document body for destructive testing, and can bring a more reliable, comprehensive and economical basis for constructing a deacidification effect evaluation system.

[0005] To prepare this product, the following steps are included:

[0006] (1) Stock preparation: Select bleached wood pulp and straw pulp board as raw materials, and prepare 2wt% rosin emulsion, 4wt% alum solution and saturated alum solution for standby;

[0007] (2) Beating treatment: Weigh 400g (absolute dry) of the above-mentioned pulp board, dilute it with tap water to a pulp consistency of 2wt%, pour it into a Valley beater for beating, and set the beating degree to 30 - 42°SR;

[0008] (3) Pulp preparation: Take 1.32 - 1.42g (absolute dry) of the qualified treated pulp and defibrate it in a standard defibrator. Add 10 - 20% talc filler to the pulp dispersion and mix evenly, and then add aluminum sulfate and rosin emulsion and stir evenly for standby;

[0009] (4) When the white water injection volume reaches 4L, pour the pulp into a rapid sheet former. When the white water injection volume reaches 6L, adjust the pH to 3.8 - 4.2 with saturated alum solution, and add 100 - 200ppm of CPAM retention aid to the pulp stock, and dehydrate and form;

[0010] (5) The dry paper web is obtained by drying at 95 - 100 °C and 96 kPa for 5 - 7 min.

[0011] Furthermore, it is characterized in that in step (1), bleached chemical hardwood pulp board and bleached chemical wheat straw pulp board are selected.

[0012] Furthermore, in step (1), 50 - 100 ml of deionized water is measured, stirred at a rotation speed of 60 - 100 r / min, and 1 - 2 g of alum powder is added simultaneously. After the powder is dissolved, this step is repeated until obvious alum crystals appear in the solution, which is a saturated alum solution.

[0013] Furthermore, in step (1), the concentration of rosin latex emulsion is 2%, and the concentration of aluminum sulfate solution is 4%.

[0014] Furthermore, in step (2), 400 g (bone dry) of pulp board is diluted with tap water to a pulp consistency of 2 wt%, poured into a Valley beater for beating, and the beating degree is set to 30 - 42 °SR.

[0015] Furthermore, in step (3), 1.32 - 1.42 g (bone dry) of qualified treated pulp is disintegrated in a standard disintegrator, and 1.47 - 1.58 g of 10 wt% talc filler is added to the pulp dispersion and mixed evenly for standby.

[0016] Furthermore, in step (3), 0.99 g - 2.13 g of 2 wt% rosin gum emulsion is added to the pulp - talc dispersion.

[0017] Furthermore, in step (3), 2.97 - 6.39 g of 4 wt% aluminum sulfate solution is added to the pulp - talc dispersion. In addition, the dosage ratio of rosin gum to aluminum sulfate is 1:6 (bone dry).

[0018] Furthermore, in step (4), the white water is the wastewater discharged from the rapid paper machine in this papermaking process stage, which contains fine fibers, fillers, coatings, and dissolved wood components.

[0019] Furthermore, in step (4), 100 - 200 ppm of cationic polyacrylamide (CPAM) is added to the stock before papermaking as a retention and drainage aid.

[0020] Furthermore, in step (4), when the white water injection volume is 4 L, the pulp is poured into the rapid paper machine. When the water injection volume reaches 6 L, the pH value of the pulp slurry is adjusted and controlled at 3.8 - 4.2 with the saturated alum solution for dehydration and forming.

[0021] Furthermore, in step (4), the wet paper web is dried at 95 - 100 °C and 96 kPa for 5 - 7 min to obtain the dry paper web, and the indexes of the dry paper web are shown in Table 1.

[0022] Compared with the prior art, the beneficial effects of the present invention are as follows: The acid deacidification test paper for library paper documents prepared by the production method of the present invention adopts the reverse sizing method, uses alum and rosin size to size the paper, and uses talcum powder as the paper filler at the same time. According to the physical properties of precious ancient books and modern paper documents, an acid deacidification test paper with performance similar to that of the existing library paper documents is prepared to replace the paper document body for destructive testing. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 It is a diagram of the degree of polymerization of cellulose in library paper documents of different ages; Figure 2 It is a diagram of the degree of polymerization of cellulose in the paper after aging treatment in Example 1; Figure 3 It is a diagram of the degree of polymerization of cellulose in the paper after aging treatment in Example 2.

[0023] Table 1 Physical and Chemical Indexes of Acid Deacidification Test Paper for Library Paper Documents

[0024] DETAILED DESCRIPTION OF THE INVENTION

[0025] The present invention will be further described below in conjunction with specific embodiments.

[0026] Example 1

[0027] A preparation process for an acid deacidification test paper for library paper documents specifically includes the following steps:

[0028] (1) Preparation of materials: Select bleached straw pulp board as the raw material, and prepare a rosin size emulsion with a concentration of 2wt%, an alum solution with a concentration of 4wt%, and a saturated alum solution for later use;

[0029] (2) Beating treatment: Weigh 400g (dry weight) of the above-mentioned pulp board, dilute it with tap water to a pulp consistency of 2wt%, pour it into a Valley beater for beating, and set the beating degree to 30-42°SR;

[0030] (3) Pulp preparation: Take 1.31g (dry weight) of the qualified treated pulp and defibrate it in a standard defibrator. Add 0.33g of talcum powder filler to the pulp dispersion and mix evenly. First add 18% (based on the dry fiber weight) of alum and then add 3% (based on the dry fiber weight) of rosin size and stir evenly for later use;

[0031] (4) When the white water injection volume reaches 4L, pour the pulp into a rapid sheet former (the diameter of the sheet forming bucket is 200mm). When the white water injection volume reaches 6L, adjust the pH to 3.8-4.2 with a saturated alum solution, and add 100-200ppm of CPAM retention aid to the paper stock for dehydration and forming;

[0032] (5) Dry the paper web at 95 - 100 °C and 96 kPa for 5 - 7 min to obtain a dry paper web.

[0033] Example 2

[0034] The preparation method of the deacidification test paper for library paper documents is the same as that in Example 1, where in step (1), the bleached straw pulp board is replaced by a bleached hardwood pulp board; in step (3), after adding 18% (based on the dry fiber content) of alum, adding 3% (based on the dry fiber content) of 2 wt% rosin size emulsion is replaced by adding 15% (based on the dry fiber content) of alum and then adding 2.5% (based on the dry fiber content) of 2 wt% rosin size emulsion.

[0035] Example 3

[0036] The preparation method of the deacidification test paper for library paper documents is the same as that in Example 1, where in step (1), the bleached wheat straw pulp board is replaced by a bleached hardwood pulp board and a bleached wheat straw pulp board; in step (3), taking 1.31 g (dry weight) of qualified pulp is replaced by taking 0.92 g and 0.31 g of qualified bleached wheat straw pulp and bleached hardwood pulp respectively.

[0037] Example 4

[0038] Taking the 7 representative literature book samples published from 1930 to 1995 in Table 2 and Examples 1 - 2 as examples, evaluate the basis weight of the paper of library paper documents. The determination of the basis weight of the paper of library paper documents is carried out in accordance with the national standard GB / T 451.2 - 2002.

[0039] Table 2 Library paper document samples

[0040] Number Book Title Publisher Publication Date 1# Deacidification Test Paper for Straw Pulp-based Library Paper Documents (Example 1) - 2024 2# Deacidification Test Paper for Wood Pulp-based Library Paper Documents (Example 2) - 2024 3# Deacidification Test Paper for Mixed Pulp-based Library Paper Documents (Example 3) - 2024 4# Collection of Evidences of Solar Eclipses in Spring and Autumn Period The Commercial Press 1930 5# Investigation and Research on Vegetable Tanning Materials in Hebei and Sichuan Light Industry Press 1959 6# Song of Ouyang Hai People's Literature Publishing House 1966 7# Modern English Expressions China and Foreign Publishing House 1975 8# Dream of the Red Chamber People's Literature Publishing House 1979 9# Xinhua Dictionary The Commercial Press 1982 10# Introduction to Antiseptic, Mold-proof and Bactericidal Shaanxi Science and Technology Press 1995

[0041] Example 5

[0042] Taking the 7 representative literature book samples published from 1930 to 1995 in Table 2 and Examples 1 - 2 as examples, evaluate the tightness of the paper of library paper documents. The determination of the tightness of the paper of library paper documents is carried out in accordance with the national standards GB / T 451.2 - 2002 and GB / T 451.3 - 2002.

[0043] Example 6

[0044] Taking the 7 representative literature book samples published from 1930 to 1995 in Table 2 and Examples 1 - 2 as examples, evaluate the whiteness of the paper of library paper documents. The determination of the whiteness of the paper is carried out using a reflectance photometer, a standard working white board, a standard black cylinder and in accordance with the national standard GB / T 7974 - 2013.

[0045] Example 7

[0046] Taking the 7 representative literature book samples published from 1930 to 1995 in Table 2 and Examples 1-2 as examples, the ash content of the paper of the library's paper-based literature was evaluated. The determination of the ash content of the paper of the library's paper-based literature was carried out in accordance with the national standard GB / T 742-2018.

[0047] Example 8

[0048] Taking the 7 representative literature book samples published from 1930 to 1995 in Table 2 and Examples 1-2 as examples, the pH value of the paper of the library's paper-based literature was evaluated. The determination of the pH of the paper of the library's paper-based literature was carried out using the cold water extraction method and in accordance with the national standard GB / T 1545-2008.

[0049] Example 9

[0050] Taking the 7 representative literature book samples published from 1930 to 1995 in Table 2 and Examples 1-2 as examples, the breaking length of the paper of the library's paper-based literature was evaluated. The determination of the breaking length of the paper of the library's paper-based literature was carried out using a tensile strength tester. It was carried out in accordance with the national standard GB / T 12914-2008. The following are the experimental steps.

[0051] Example 10

[0052] Taking the 7 representative literature book samples published from 1930 to 1995 in Table 2 and Examples 1-2 as examples, the folding endurance of the paper of the library's paper-based literature was evaluated. The determination of the folding endurance of the paper of the library's paper-based literature was carried out using a Schopper folding endurance tester and in accordance with the national standard GB / T 457-2002.

[0053] Example 11

[0054] Taking the 7 representative literature book samples published from 1930 to 1995 in Table 2 and Examples 1-2 as examples, the sizing degree value of the paper of the library's paper-based literature was evaluated. The determination of the sizing degree of the paper of the library's paper-based literature was carried out using the Cobb value method and in accordance with the national standard GB / T 1540-2002.

[0055] Example 12

[0056] Taking Examples 1-2 as examples, the deacidification test paper of the library's paper-based literature was simulated for aging, carried out in accordance with the national standard GB / T 464-2008, to compare the aging degradation performance.

[0057] It can be seen from Table 3 that the basis weight of the library's paper-based literature is 49.2-54 g / m 2 , the tightness is 0.50-0.85 g / cm 3 , the ash content is 2.2-15.6%, the pH value is 3.98-5.60, the breaking length is 1.2-31 km, the folding endurance is 2, and the water absorbency is 23-46 g / m2 , and both Example 1 and Example 2 are within the range. Therefore, it is considered that the deacidification test paper for library paper documents has similar physical and chemical properties to library paper documents.

[0058] From Figure 1 it can be seen that the trend of the degree of polymerization of cellulose in the papers of Example 1 and Example 2 decreasing with the increase of aging time is consistent with the trend of the degree of polymerization of cellulose decreasing in library paper documents of different ages. Therefore, it can be considered that the deacidification test paper for library paper documents has similar aging laws to library paper documents.

[0059] The above are only the preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention shall be included within the protection scope of the present invention. Table 3 Comparison between Examples 1-2 and Library Paper Document Samples

[0060]

Claims

1. A preparation process for a deacidification test paper for paper documents in a library, characterized in that: Firstly, the physical and chemical indicators of the deacidification test paper are determined according to the characteristics of precious ancient books and modern paper documents, saponified rosin glue is used as the sizing agent in the pulp, talcum powder is used as the filler, and cationic polyacrylamide (CPAM) is used as the retention and drainage aid. Finally, the deacidification test paper is obtained through papermaking and drying, which specifically includes the following steps: (1) Material preparation: bleached wood pulp and straw pulp board are selected as raw materials, and saturated alum solution is prepared for standby use; (2) Pulping treatment: weigh the above pulp board, dilute it with tap water, and pulp it; (3) Preparation of pulp and additives: 1.32-1.42 g (absolutely dry) qualified pulp is taken for delamination, 10-20% (based on the paper quantity) of talcum powder filler is added to the pulp dispersion and mixed evenly, then alum is first added and then rosin glue is added by reverse sizing process and stirred evenly; (4) After injecting white water to 6L, add saturated alum solution to adjust the pH to 3.8-4.2, and add 100-200ppm retention aid to the paper stock for dehydration and forming; (5) Drying.

2. The preparation technology of deacidification test paper for paper documents in library collection according to claim 1, characterized in that: In step (1), bleached chemical hardwood pulp board and bleached chemical wheat straw pulp board are selected.

3. The preparation technology of deacidification test paper for library paper documents according to claim 1, characterized in that: In step (1), 50-100 mL of deionized water is measured and stirred at a speed of 60-100 r / min, and 1-2 g of alum powder is added at the same time. After the powder is dissolved, this step is repeated until obvious alum crystals appear in the solution, which is a saturated alum solution.

4. The preparation technology of deacidification test paper for library paper documents according to claim 1, characterized in that: In step (2), about 400 g (absolutely dry) pulp is weighed and diluted with tap water to a pulp concentration of 2 wt %, and then poured into a Valley beater for pulping, with the beating degree set to 30-42° SR.

5. The preparation technology of deacidification test paper for library paper documents according to claim 1, characterized in that: In step (3), 1.32-1.42 g (absolutely dry) of qualified pulp is deflagrated in a standard deflagrator, and 1.47-1.58 g of 10 wt% talcum powder filler is added to the pulp dispersion and mixed evenly for use.

6. The preparation technology of deacidification test paper for library paper documents according to claim 1, characterized in that: In step (3), the concentrations of the rosin latex and the alum solution are 2wt% and 4wt%, respectively.

7. The preparation technology of deacidification test paper for paper documents in library collection according to claim 1, characterized in that: In step (3), 0.99 g to 2.13 g of 2 wt % rosin latex is added to the pulp-talcum powder dispersion.

8. The preparation technology of deacidification test paper for library paper documents according to claim 1, characterized in that: In step (3), 2.97 g to 6.39 g of a 4 wt% alum solution is added to the pulp-talcum powder dispersion. In addition, the amount of rosin glue: the amount of alum = 1:6 (absolute dry).

9. The preparation technology of deacidification test paper for paper documents in library collection according to claim 1, characterized in that: In step (4), the wastewater discharged from the fast sheet making machine contains fine fibers, fillers, coatings and dissolved wood components.

10. The preparation technology for deacidification test paper for paper documents in library collection according to claim 1, characterized in that: In step (4), 100-200 ppm of cationic polyacrylamide (CPAM) is added to the paper stock as a retention and drainage aid before papermaking.

11. The preparation technology of deacidification test paper for paper documents in library collection according to claim 1, characterized in that: In step (4), when the amount of white water injected is 4 L, the pulp is poured into a fast sheet making machine, and when the amount of water injected is 6 L, a saturated alum solution is used to adjust the pH value of the pulp liquid to 3.8-4.2, and dehydrate to form.

12. The preparation technology for deacidification test paper for paper documents in library collection according to claim 1, characterized in that: In step (4), the wet paper web is dried at 95-100°C and 96 kPa for 5-7 min to obtain a dry paper web, wherein the dry paper web has a basis weight of 50-54 g / m 2 、Ash content is 11-13%, cobb 60 20-30g / m 2 .

Citation Information

Patent Citations

  • Body paper, making method of body paper, coated paper, making method of coated paper

    CN102817277A

  • Packaging paper and preparation method thereof

    CN117926636A

Cited By

  • Nondestructive testing method for structural characteristics and adsorption and permeability of paper

    CN121164144A