Preparation process of PET (Polyethylene Terephthalate) film laser printing coating

By preparing a laser printing coating containing aqueous acrylic resin, polydimethylsiloxane and silicon-doped titanium dioxide on the PET film, the problems of insufficient heat resistance of the coating and poor adhesion of the toner are solved, and efficient graphic printing effect is achieved.

CN120173462AActive Publication Date: 2025-06-20NANYANG DAZZLE DIGITAL PRINTING MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202510506605.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-22
Publication Date
2025-06-20
Estimated Expiration
2045-04-22

AI Technical Summary

Technical Problem

The existing water-based acrylic resin coatings are insufficient in heat resistance during laser printing, which leads to softening, discoloration or bubbles of the coating, affecting the quality of the graphics and text. At the same time, the toner is not strong, resulting in spots or tailings of the graphics and text.

Method used

By adopting a preparation process for laser printing coating of PET film, the aqueous acrylic resin emulsion, polydimethylsiloxane, silicon-doped titanium dioxide, silane coupling agent, crosslinking agent, film forming additive, photoinitiator and defoaming agent are dispersed in a twin-screw high-speed disperser, and uniformly coated on the pretreated PET film, and heat curing and photocuring treatment are carried out.

Benefits of technology

The heat resistance of the coating and the adsorption ability of the toner are significantly improved, ensuring the stability of the coating and the clarity of the graphics and text during laser printing, the peeling strength reaches more than 5.2N/mm, and the adhesion of the toner reaches more than 99.0%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120173462A_ABST
    Figure CN120173462A_ABST
Patent Text Reader

Abstract

The invention provides a preparation process of a PET (Polyethylene Terephthalate) film laser printing coating, and belongs to the technical field of laser printing coatings. 72-75 parts of water-based acrylic resin emulsion, 2-2.5 parts of polydimethylsiloxane, 5-7 parts of silicon-doped titanium dioxide, 1-2 parts of a silane coupling agent KH-570, 2-3 parts of a cross-linking agent vinyltriethoxysilane, 2-4 parts of a coalescing agent propylene glycol phenyl ether, 0.6-0.8 part of a photoinitiator and 0.3-0.5 part of a defoaming agent are put into a double-screw high-speed dispersion machine to be dispersed and left to stand, and a mixture is obtained; s2, carrying out corona treatment on the PET film to obtain a pretreated PET film; and S3, uniformly coating the pretreated PET film obtained in S2 with the mixture obtained in S1, and performing curing treatment to obtain the PET film laser printing coating. The heat resistance of the prepared PET film laser printing coating and the adsorption capacity of the PET film laser printing coating to carbon powder can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of laser printing coatings, and particularly relates to a preparation process of a laser printing coating for PET films. Background Art

[0002] Polyethylene terephthalate (PET) films have the advantages of good mechanical strength, high transparency, high heat resistance temperature, and low price, and are increasingly used in fields such as medical films and advertising labels. The molecular chain structure of PET is regular and the crystallinity is relatively high, which is not conducive to the direct attachment of toner. In order to make the toner for laser printing present a better printing effect on the PET film, a coating is usually applied on the surface of the PET film to optimize the interfacial bonding. Since waterborne acrylic resin uses water as the dispersion medium, has a very low VOC content, meets international environmental protection standards, and has high coating transparency, it can present bright colors and clear patterns, and the existing coatings generally use waterborne acrylic resin.

[0003] However, the polarity matching degree between the waterborne acrylic resin and the laser printing toner is insufficient. The large polarity difference between the toner and the coating will weaken the intermolecular force and affect the effective attachment / adsorption of the toner, resulting in graphic spots or trailing. In addition, the toner for laser printing is fixed on the medium by heating, and the coating needs to withstand extremely short instantaneous high temperatures. However, the heat resistance temperature of conventional waterborne acrylic resin is usually lower than 120°C. During the laser printing process, the coating is prone to softening, discoloration or blistering, affecting the graphic quality. Summary of the Invention

[0004] In view of the above problems, the present invention proposes a preparation process of a laser printing coating for PET films, which can effectively improve the heat resistance performance of the prepared laser printing coating for PET films and its adsorption capacity for toner.

[0005] To achieve the above object, the technical solution adopted by the present invention is as follows: A preparation process of a laser printing coating for PET films, comprising the following steps:

[0006] S1. By weight, 72 - 75 parts of a waterborne acrylic resin emulsion, 2 - 2.5 parts of polydimethylsiloxane, 5 - 7 parts of silicon-doped titanium dioxide, 1 - 2 parts of silane coupling agent KH-570, 2 - 3 parts of crosslinking agent vinyltriethoxysilane, 2 - 4 parts of film-forming auxiliary propylene glycol phenyl ether, 0.6 - 0.8 parts of photoinitiator, and 0.3 - 0.5 parts of defoamer are put into a twin-screw high-speed disperser, dispersed, and left standing to obtain a mixed material;

[0007] S2. After the PET film is subjected to corona treatment, a pretreated PET film is obtained;

[0008] S3. Uniformly coat the mixture obtained in S1 on the pretreated PET film obtained in S2, and perform curing treatment to obtain a PET film laser printing coating.

[0009] Further, in S1, the specific operation of dispersion is as follows: First, disperse at a rotation speed of 480 - 520 rpm for 4 - 5 min, then disperse at a rotation speed of 1150 - 1200 rpm for 6 - 8 min, and then disperse at a rotation speed of 1800 - 2000 rpm for 2.5 - 3.5 min.

[0010] Further, in S3, the curing treatment includes thermal curing and photocuring.

[0011] Further, the thickness of the PET film laser printing coating is 5 ± 0.5 μm.

[0012] Further, the preparation method of the silicon-doped titanium dioxide is as follows:

[0013] A1. At room temperature, divide ethanol into two parts, namely the first part of ethanol and the second part of ethanol, and the molar amounts of the first part of ethanol and the second part of ethanol are equal; mix and stir tetrabutyl titanate, tetraethyl orthosilicate and the first part of ethanol to obtain a first mixed solution; mix and stir water, nitric acid and the second part of ethanol to obtain a second mixed solution;

[0014] A2. Dropwise add the second mixed solution obtained in A1 into the first mixed solution, and continue to stir to obtain a uniform and transparent sol;

[0015] A3. After standing and aging the sol obtained in A2 at room temperature for 24 h, dry it at 55 - 75 °C for 12 h to obtain a dry gel;

[0016] A4. Put the dry gel obtained in A3 into a muffle furnace, heat it up, after heat treatment, naturally cool it to room temperature to obtain silicon-doped titanium dioxide powder.

[0017] Further, in A1, the molar ratio of tetrabutyl titanate, tetraethyl orthosilicate, ethanol, water and nitric acid is 1:(0.3 - 0.4):25:4:0.2.

[0018] Further, in A2, the dropping rate of the second mixed solution dropwise added into the first mixed solution is 1 - 1.5 mL / min.

[0019] Further, in A4, the heating rate is 3 - 5 °C / min, the temperature of the heat treatment is 490 - 510 °C, and the time of the heat treatment is 68 - 80 min.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] In the present invention, silicon-doped titanium dioxide forms micron-scale composite protrusions in the coating through controllable agglomeration or interaction with the resin matrix, enhancing the mechanical anchoring of toner by physical embedding; the high specific surface area and surface residual hydroxyl groups (-OH) of silicon-doped titanium dioxide form hydrogen bonds or covalent bonds with carboxyl groups (-COOH) in the toner, improving the chemical adsorption strength. The reflectivity of silicon-doped titanium dioxide in the near-infrared band (700 - 2500 nm) is ≥ 75%, which can reflect external thermal radiation, reduce the internal temperature gradient of the coating, reduce the molecular chain breakage caused by heat accumulation, and improve the heat resistance of the coating.

[0022] Polydimethylsiloxane forms Si-O-Ti bonds through the condensation reaction of silanol groups (-Si-OH) and surface hydroxyl groups (-OH) of silicon-doped titanium dioxide under the catalysis of high temperature (service temperature) of 150 °C, constructing a continuous three-dimensional crosslinked network to synergistically inhibit the thermal movement of resin molecular chains; at the same time, it improves the compatibility of the two-phase interface and reduces the defects caused by phase separation. In addition, this structure will also increase the nano-scale roughness of the coating surface, increase the physical contact area between the toner and the coating, enhance the van der Waals force by increasing the specific surface area, and synergistically improve the adhesion. The high-polarity surface of silicon-doped titanium dioxide can partially compensate for the polarity loss in the low-surface-energy region of polydimethylsiloxane, alleviating the overall phase separation through local chemical bonding (Si-O-Ti); at the same time, the low-surface-energy region of polydimethylsiloxane and the high-polarity surface of silicon-doped titanium dioxide form a gradient distribution, balancing the polarity difference of the toner and improving the adsorption uniformity. Brief Description of the Drawings

[0023] Figure 1 It is a comparative trend chart of the peel strength test data of the laser printing coatings on PET films prepared in Examples 1 - 3 and Comparative Examples 1 - 3 in the test examples of the present invention after maintaining at a constant temperature of 150 °C for 10 min;

[0024] Figure 2 It is a comparative trend chart of the adhesion test data of the laser printing toner (graphic) on the laser printing coatings on PET films prepared in Examples 1 - 3 and Comparative Examples 1 - 3 in the test examples of the present invention. Detailed Description of the Invention

[0025] Next, the technical solutions in the embodiments of the present invention will be clearly and completely described in conjunction with the drawings of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts shall fall within the protection scope of the present invention.

[0026] Example 1: (1) The preparation method of silicon-doped titanium dioxide is as follows:

[0027] A1. At room temperature, divide ethanol into two portions, namely the first portion of ethanol and the second portion of ethanol, and the molar amounts of the first portion of ethanol and the second portion of ethanol are equal; mix and stir tetrabutyl titanate, tetraethyl orthosilicate and the first portion of ethanol to obtain a first mixed solution; mix and stir water, nitric acid and the second portion of ethanol to obtain a second mixed solution. Among them, the molar ratio of tetrabutyl titanate, tetraethyl orthosilicate, ethanol, water and nitric acid is 1:0.35:25:4:0.2.

[0028] A2. Slowly add the second mixed solution obtained in A1 drop by drop to the first mixed solution at a dropping rate of 1.2 mL / min, and continue to stir (magnetic stirring at 800 rpm) to obtain a uniform and transparent sol.

[0029] A3. After standing and aging the sol obtained in A2 at room temperature for 24 h, first dry it at 50 °C for 6 h, and then dry it at 70 °C for 6 h to obtain a xerogel.

[0030] A4. Put the xerogel obtained in A3 into a muffle furnace, heat it to 500 °C at a heating rate of 4 °C / min, keep it for heat treatment for 75 min, and then naturally cool it to room temperature to obtain silicon-doped titanium dioxide powder.

[0031] (2) A preparation process of a PET film laser printing coating, comprising the following steps:

[0032] S1. By weight, put 74 parts of aqueous acrylic resin emulsion, 2.2 parts of polydimethylsiloxane, 6 parts of silicon-doped titanium dioxide, 1.5 parts of silane coupling agent KH-570, 2.5 parts of cross-linking agent vinyltriethoxysilane, 3 parts of film-forming aid propylene glycol phenyl ether, 0.7 part of photoinitiator Irgacure 819 and 0.4 part of defoamer BYK-024 into a twin-screw high-speed disperser, first disperse at a speed of 500 rpm for 4.5 min (temperature < 30 °C), then disperse at a speed of 1180 rpm for 7 min (circulating water cooling to maintain 35 ± 2 °C), and then disperse at a speed of 1900 rpm for 3 min (nitrogen protection, temperature < 40 °C), and stand for 35 min at 25 °C and humidity ≤ 30% to eliminate internal stress and stabilize viscosity to obtain a mixed material.

[0033] S2. After corona treatment of the PET film, a pretreated PET film is obtained. Corona treatment parameters: the corona power is set to 42 kW, and the treatment speed is 12 m / min linear speed; after corona treatment, it is cleaned with 0.5% fluorocarbon surfactant (Capstone FS-63) aerosol to remove impurities while maintaining the surface energy.

[0034] S3. Use a gravure coating head (150 lines / cm ceramic anilox roll + 65 Shore A rubber roller), with a coating speed of 10 m / min, and evenly coat the mixture obtained in S1 on the pretreated PET film obtained in S2, followed by curing treatment. The curing treatment specifically includes thermal curing and light curing. The specific operation of thermal curing is as follows: First, pre-bake at a temperature of about 80 °C for 2.5 min (pre-crosslinking), then cure at a temperature of about 120 °C for 2 min (main crosslinking), and then cure at a temperature of about 135 °C for 1 min (post-curing); meanwhile, the specific operation of light curing is: UV-LED irradiation (395 nm, 600 mJ / cm 2 ). After curing, the film is naturally cooled to below 40 °C, and the winding tension ≤ 5 N / m to prevent the coating from cracking due to thermal shrinkage, thus obtaining the PET film laser printing coating with a thickness of 4.9 μm.

[0035] Example 2: The difference between this example and Example 1 lies in: A preparation process of a PET film laser printing coating, including the following steps:

[0036] S1. By weight, put 72 parts of aqueous acrylic resin emulsion, 2 parts of polydimethylsiloxane, 5 parts of silicon-doped titanium dioxide, 1 part of silane coupling agent KH-570, 2 parts of crosslinking agent vinyltriethoxysilane, 2 parts of film-forming aid propylene glycol phenyl ether, 0.6 part of photoinitiator Irgacure 819, and 0.3 part of defoamer BYK-024 into a twin-screw high-speed disperser. First, disperse at a speed of 480 rpm for 5 min, then disperse at a speed of 1150 rpm for 8 min, and then disperse at a speed of 1800 rpm for 3.5 min, and let it stand to obtain a mixture.

[0037] S2. After corona treatment of the PET film, a pretreated PET film is obtained.

[0038] S3. Evenly coat the mixture obtained in S1 on the pretreated PET film obtained in S2, followed by curing treatment, thus obtaining the PET film laser printing coating with a thickness of 4.8 μm.

[0039] Example 3: The difference between this example and Example 1 lies in: A preparation process of a PET film laser printing coating, including the following steps:

[0040] S1. By weight, put 75 parts of aqueous acrylic resin emulsion, 2.5 parts of polydimethylsiloxane, 7 parts of silicon-doped titanium dioxide, 2 parts of silane coupling agent KH-570, 3 parts of crosslinking agent vinyltriethoxysilane, 4 parts of film-forming aid propylene glycol phenyl ether, 0.8 part of photoinitiator Irgacure 819 and 0.5 part of defoamer BYK-024 into a twin-screw high-speed disperser. First, disperse at a speed of 520 rpm for 4 min, then disperse at a speed of 1200 rpm for 6 min, and then disperse at a speed of 2000 rpm for 2.5 min. Let it stand to obtain a mixed material.

[0041] S2. After corona treatment of the PET film, a pretreated PET film is obtained.

[0042] S3. Uniformly coat the mixed material obtained in S1 on the pretreated PET film obtained in S2, and perform curing treatment to obtain a PET film laser printing coating with a thickness of 5.2 μm.

[0043] Comparative Example 1: The difference between this comparative example and Example 1 is that polydimethylsiloxane and silicon-doped titanium dioxide are deleted.

[0044] Specifically, a preparation process of a PET film laser printing coating includes the following steps:

[0045] S1. By weight, put 74 parts of aqueous acrylic resin emulsion, 1.5 parts of silane coupling agent KH-570, 2.5 parts of crosslinking agent vinyltriethoxysilane, 3 parts of film-forming aid propylene glycol phenyl ether, 0.7 part of photoinitiator Irgacure 819 and 0.4 part of defoamer BYK-024 into a twin-screw high-speed disperser. First, disperse at a speed of 500 rpm for 4.5 min (temperature < 30 °C), then disperse at a speed of 1180 rpm for 7 min (circulating water cooling to maintain 35 ± 2 °C), and then disperse at a speed of 1900 rpm for 3 min (under nitrogen protection, temperature < 40 °C). Let it stand for 35 min at 25 °C and humidity ≤ 30% to eliminate internal stress and stabilize viscosity, and obtain a mixed material.

[0046] S2. After corona treatment of the PET film, a pretreated PET film is obtained. Corona treatment parameters: The corona power is set to 42 kW, and the treatment speed is 12 m / min linear speed; after corona treatment, it is cleaned with 0.5% fluorocarbon surfactant (Capstone FS-63) aerosol to remove impurities while maintaining the surface energy.

[0047] S3. Use a gravure coating head (150 - line / cm ceramic anilox roll + 65 Shore A rubber roll), with a coating speed of 10 m / min, to uniformly coat the mixture obtained in S1 onto the pretreated PET film obtained in S2, and then perform a curing treatment. The curing treatment specifically includes thermal curing and light curing. The specific operation of thermal curing is as follows: First, pre - bake at a temperature of about 80 °C for 2.5 min (pre - crosslinking), then cure at a temperature of about 120 °C for 2 min (main crosslinking), and then cure at a temperature of about 135 °C for 1 min (post - curing); meanwhile, the specific operation of light curing is: UV - LED irradiation (395 nm, 600 mJ / cm 2 ). After curing, the film is naturally cooled to below 40 °C, and the winding tension ≤ 5 N / m to prevent the coating from cracking due to thermal shrinkage, thus obtaining the PET film laser - printing coating with a thickness of 4.9 μm.

[0048] Comparative Example 2: The difference between this comparative example and Example 1 is that silicon - doped titanium dioxide is deleted.

[0049] Comparative Example 3: The difference between this comparative example and Example 1 is that polydimethylsiloxane is deleted.

[0050] Test Example: Test items and methods: 1. Respectively place the specimens prepared in Examples 1 - 3 and Comparative Examples 1 - 3 in a high - temperature oven, heat them at a rate of 5 °C / min to 150 °C, and keep them at a constant temperature for 10 min. After the coating and the PET film substrate are fully heated, refer to the standard ASTM D3330 to test the peel strength. The unit is N / mm.

[0051] 2. Respectively perform laser printing on the surfaces of the PET film laser - printing coatings prepared in Examples 1 - 3 and Comparative Examples 1 - 3. After the toner is fixed to the medium (coating) through instantaneous heating (150 - 180 °C), refer to the standard ASTM D3359 (cross - hatch method) to test the adhesion. Adhesion (%) = (total number of squares - number of peeled - off squares) / total number of squares × 100%.

[0052] Test results: See Table 1.

[0053] Table 1. Test data of the test example

[0054] Peeling strength (N / mm) Adhesion (%) Example 1 5.2 99.1 Example 2 5.2 99.3 Example 3 5.4 99.4 Comparative Example 1 3.8 96.9 Comparative Example 2 3.3 96.0 Comparative Example 3 4.7 98.3

[0055] Result analysis: Analyzing Examples 1 - 3 and combining the data in Table 1 and Figure 1 - Figure 2 , it can be seen that for the PET film laser - printing coatings of the present invention (Examples 1 - 3), the peel strength after keeping at a constant temperature of 150 °C for 10 min reaches above 5.2 N / mm, and the adhesion of the laser - printed toner (graphic) reaches above 99.0%.

[0056] Analyze Example 1 and Comparative Examples 1-3 and combine the data in Table 1 and Figure 1 - Figure 2 , by comparing Comparative Example 1 and Comparative Example 2, it can be seen that adding polydimethylsiloxane alone will cause the peel strength of the laser printing coating of the prepared PET film to decrease after being kept at a constant temperature of 150 °C for 10 min, resulting in a decrease in the adhesion of the laser printing toner (graphic). This is because polydimethylsiloxane migrates to the surface of the coating to form a low surface energy region, increasing the polarity difference from the toner, weakening the electrostatic adsorption and van der Waals forces; at the same time, polydimethylsiloxane covers the carboxyl groups (-COOH) and hydroxyl groups (-OH) in the waterborne acrylic resin, reducing the hydrogen bond binding sites with the toner, resulting in a decrease in the physical adsorption strength of the coating to the toner. The waterborne acrylic resin is a polar system, while polydimethylsiloxane belongs to a non-polar silicone material. Phase separation is likely to occur when the two are mixed, forming interface defects, accelerating the cracking or peeling of the coating at 150 °C.

[0057] , by comparing Comparative Example 1 and Comparative Example 3, it can be seen that adding silicon-doped titanium dioxide alone can increase the peel strength of the laser printing coating of the prepared PET film after being kept at a constant temperature of 150 °C for 10 min, and increase the adhesion of the laser printing toner (graphic). By comparing with Example 1, it can be seen that when polydimethylsiloxane and silicon-doped titanium dioxide are added simultaneously, the two can produce a synergistic effect, synergistically increasing the peel strength of the laser printing coating of the prepared PET film after being kept at a constant temperature of 150 °C for 10 min, and synergistically increasing the adhesion of the laser printing toner (graphic).

[0058] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments, or perform equivalent replacements for some of the technical features. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention shall be included within the protection scope of the present invention.

Claims

1. A process for preparing a PET film laser printing coating, characterized in that: The following steps are involved: S1. By weight, 72-75 parts of aqueous acrylic resin emulsion, 2-2.5 parts of polydimethylsiloxane, 5-7 parts of silicon-doped titanium dioxide, 1-2 parts of silane coupling agent KH-570, 2-3 parts of cross-linking agent vinyl triethoxysilane, 2-4 parts of film-forming aid propylene glycol phenyl ether, 0.6-0.8 parts of photoinitiator and 0.3-0.5 parts of defoamer are put into a twin-screw high-speed disperser, dispersed, and allowed to stand to obtain a mixture; S2, subjecting the PET film to corona treatment to obtain a pretreated PET film; S3, evenly coating the mixture obtained in S1 on the pre-treated PET film obtained in S2, and curing the mixture to obtain a PET film laser printing coating.

2. The process for preparing the PET film laser printing coating according to claim 1, characterized in that: In S1, the specific operation of dispersion is: first disperse at a rotation speed of 480-520 rpm for 4-5 min, then disperse at a rotation speed of 1150-1200 rpm for 6-8 min, and then disperse at a rotation speed of 1800-2000 rpm for 2.5-3.5 min.

3. The process for preparing the PET film laser printing coating according to claim 1, characterized in that: In S3, the curing process includes thermal curing and photocuring.

4. The process for preparing the PET film laser printing coating according to claim 1, characterized in that: The thickness of the PET film laser printing coating is 5±0.5 μm.

5. The process for preparing the PET film laser printing coating according to claim 1, characterized in that: The preparation method of the silicon-doped titanium dioxide is as follows: A1. At room temperature, ethanol is divided into two parts, namely a first part of ethanol and a second part of ethanol, and the molar amounts of the first part of ethanol and the second part of ethanol are equal; tetrabutyl titanate, ethyl orthosilicate and the first part of ethanol are mixed and stirred to obtain a first mixed solution; water, nitric acid and the second part of ethanol are mixed and stirred to obtain a second mixed solution; A2, adding the second mixed solution obtained in A1 dropwise into the first mixed solution, and continuing stirring to obtain a uniform and transparent sol; A3, the sol obtained in A2 was aged at room temperature for 24 hours, and then dried at 55-75°C for 12 hours to obtain a dry gel; A4. Place the dry gel obtained in A3 into a muffle furnace, heat it, and after heat treatment, naturally cool it to room temperature to obtain silicon-doped titanium dioxide powder.

6. The process for preparing the PET film laser printing coating according to claim 5, characterized in that: In A1, the molar ratio of tetrabutyl titanate, ethyl orthosilicate, ethanol, water and nitric acid is 1:(0.3-0.4):25:4:0.

2.

7. The process for preparing the PET film laser printing coating according to claim 5, characterized in that: In A2, the second mixed solution is added dropwise to the first mixed solution at a dropping speed of 1-1.5 mL / min.

8. The process for preparing the PET film laser printing coating according to claim 5, characterized in that: In A4, the heating rate is 3-5°C / min, the heat treatment temperature is 490-510°C, and the heat treatment time is 68-80min.

Citation Information

Patent Citations

  • Preparation method of functional waterborne multicolored basic paint for multicolored coating for external wall

    CN107603484A

  • Formula of antifog pad pasting for automobile glass and preparation process thereof

    CN108329856A

  • Titanium dioxide material and preparation method thereof

    CN109678204A

  • Antibacterial material for cookware and preparation method of antibacterial material

    CN119463595A

  • Super-hydrophilic antifouling paint for concrete surface

    CN119799042A