Perovskite cell and preparation method thereof, laminated cell and photovoltaic module
By using vinyl dithiophenetopyrrole (DTP) as the hole transport material, the problems of high material cost and insufficient stability in existing perovskite batteries are solved, and low-cost and high-performance perovskite battery applications are realized, with long-term stability and high mobility, and are suitable for large-area trans perovskite batteries.
Patent Information
- Application Number
- CN202510384278.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-03-27
- Publication Date
- 2025-07-04
AI Technical Summary
The commonly used organic hole transport materials in existing perovskite batteries have problems such as high material synthesis cost, mismatch in energy levels and dopant hygroscopy affecting device stability. The existing polymer hole transport materials are insufficient in the passivation of interface defects, which affects the photoelectric conversion performance and stability of solar cells.
Using vinyl dithiopheneopyrrole (DTP) as the core of the hole transport material, a multifunctional electron-rich thiophene fused heterocyclic unit is developed by chemical modification at the thiophene site and combining the electron-donating group of aniline fluorene, which has high mobility, low cost and high stability, can match the energy level of the perovskite material and passivate interface defects.
It realizes low-cost, high-performance and stable perovskite battery application, with long-term operation stability and high thermal stability, is suitable for industrial production, and is suitable for large-area trans perovskite batteries.
Smart Images

Figure CN120265006A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar energy, and particularly to perovskite solar cells, their preparation methods, tandem solar cells, and photovoltaic modules. Background Art
[0002] In the past decade or so, perovskite solar cells (PSCs) have emerged as a rising star in the photovoltaic field due to their unique optoelectronic performance advantages. In a p-i-n perovskite solar cell, the hole transport layer located below the perovskite absorption layer not only plays a role in carrier transport but also serves as a growth substrate for perovskite, affecting the crystallization growth of perovskite. Therefore, the structural design and performance of hole transport materials (HTMs) play a crucial role in the performance of p-i-n perovskite solar cells.
[0003] Currently, the commonly used organic hole transport materials in p-i-n perovskite solar cells mainly include PTAA, P3HT, and PEDOT:PSS. However, they have problems such as high material synthesis cost, energy level mismatch, and the hygroscopicity of dopants affecting device stability. Therefore, it is urgent to develop alternative hole transport materials. Most of the polymer hole transport materials developed currently have complex synthesis steps, and their functional design mainly focuses on improving the hole mobility of the materials, ignoring their passivation effect on perovskite interface defects. Interface defects will cause serious charge non-radiative recombination, thereby affecting the photoelectric conversion performance and stability of solar cells.
[0004] Therefore, the development of hole transport materials with low cost, no doping, and interface passivation effect is of great significance for promoting the further development of high-performance perovskite solar cells. Summary of the Invention
[0005] The present application provides a perovskite solar cell, its preparation method, a tandem solar cell, and a photovoltaic module. The hole transport material has the advantages of low cost, high performance, and high stability, and can realize the application of large-area p-i-n perovskite solar cells with low cost, high performance, and stability.
[0006] In a first aspect, an embodiment of the present application provides a perovskite solar cell, including a hole transport layer, a perovskite absorption layer, and an electron transport layer sequentially arranged on one surface of a conductive substrate from near to far. The hole transport layer includes a hole transport material, and the structure of the hole transport material is shown in the following formula (1):
[0007] Wherein, 10 < n < 1000, and R1 and R2 are independently selected from any one of the following structures (1-1) or (1-2):
[0008]
[0009] Second aspect, an embodiment of the present application provides a method for preparing a perovskite battery, including preparing a hole transport material, and the preparation steps of the hole transport material include:
[0010] Providing raw material 1, preparing intermediate 1 from the raw material 1, and the structural formula of the raw material 1 is: The structural formula of the intermediate 1 is:
[0011] Reacting the intermediate 1 with N-bromosuccinimide to obtain intermediate 2, and the structural formula of the intermediate 2 is:
[0012] Preparing intermediate 4, and the structural formula of the intermediate 4 is:
[0013]
[0014] Reacting the intermediate 2 and the intermediate 4 to obtain intermediate 5, and the structural formula of the intermediate 5 is: R1 and R2 are independently selected from any one of the following structures (1-1) or (1-2):
[0015]
[0016] Performing an elimination reaction on the intermediate 5 to obtain intermediate 6, and the structural formula of the intermediate 6 is:
[0017]
[0018] Mixing the intermediate 6 with an initiator to carry out a polymerization reaction to obtain the hole transport material, and the structure of the hole transport material is shown in the following formula (1):
[0019] 10 < n < 1000.
[0020] Third aspect, an embodiment of the present application further provides a tandem battery, including:
[0021] A bottom cell, the bottom cell includes at least one crystalline silicon cell and / or amorphous silicon cell;
[0022] A top cell, stacked on the bottom cell, the top cell includes one or more perovskite cells, wherein at least one perovskite cell is the perovskite cell as described in the first aspect, or at least one perovskite cell is prepared by the preparation method as described in the second aspect.
[0023] Fourth aspect, an embodiment of the present application further provides a photovoltaic module, including the tandem battery as described in the third aspect.
[0024] Compared with the prior art, the technical solution of the present invention has at least the following technical effects:
[0025] The hole transport material of the perovskite battery of the present application has vinyl dithienopyrrole as the core. The electron-rich N atom in dithienopyrrole (DTP) can improve the stability of the organic semiconductor material in the oxidized state, enabling the optoelectronic device to have long-term operational stability. The S atom can interact with metal ions (such as Pb 2+ ) in the perovskite absorption layer, thereby passivating the interface defects on the perovskite surface. At the same time, DTP, as a multifunctional electron-rich thiophene-fused heterocyclic unit, has unique characteristics such as small reorganization energy, high mobility, chemical modification of N and thiophene sites, and interaction with metal ions. By chemically modifying the thiophene sites in DTP with an electron-donating group containing aniline fluorene, the hole transport material has a deeper HOMO energy level, better matches the energy level of the perovskite material, achieves better mobility, and is more conducive to the extraction and transport of holes. The hole transport material of the perovskite battery of the present application has a relatively high decomposition temperature and good thermal stability. It has good solubility in solvents such as dimethyl sulfoxide, N,N'-dimethylformamide, toluene, chlorobenzene, and dichloromethane, has good film-forming properties, and has good wettability with the perovskite precursor solvent, which helps the crystallization and film formation of perovskite. In addition, it also has the advantages of low raw material cost, simple preparation process, high reproducibility, and can be used in inverted perovskite batteries without doping any additives, is suitable for industrial production, and has good application prospects.
[0026] In summary, the hole transport material of the perovskite battery of the present application combines the advantages of low cost, high performance, and high stability, and can realize the application of low-cost, high-performance, and stable perovskite batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The present invention will be further described below in conjunction with the drawings and embodiments.
[0028] Figure 1 1H NMR spectrum of Compound 9 in Example 1 of the present application;
[0029] Figure 2 1H NMR spectrum of Compound 14 in Example 2 of the present application. DETAILED DESCRIPTION OF THE EMBODIMENTS
[0030] The raw materials and equipment used in the present invention are all common raw materials and equipment in the art without special instructions. The methods used in the present invention are all conventional methods in the art without special instructions.
[0031] Unless otherwise specified, the meanings of the terms in this specification are the same as those generally understood by those skilled in the art. However, if there is a conflict, the definition in this specification shall prevail.
[0032] In this text, "including", "comprising", "containing", "having" or other variants are intended to cover non-closed inclusion, and no distinction is made among these terms. The term "comprising" means that other steps and components can be added without affecting the final result. The term "comprising" also includes the terms "consisting of" and "consisting essentially of". The compositions and methods / processes of the present invention comprise, consist of, and consist essentially of the essential elements and limitations described herein, as well as any additional or optional ingredients, components, steps, or limitations described herein.
[0033] All numerical values or statements relating to component amounts, process conditions, etc. used in the specification and claims should be understood to be modified by "about" in all cases. All ranges relating to the same component or property include the endpoints, and these endpoints can be combined independently. Since these ranges are continuous, they include every numerical value between the minimum and maximum values. It should also be understood that any numerical range cited in this application is expected to include all sub-ranges within that range.
[0034] It should be understood that the term "and / or" used in the present invention is merely a correlative relationship describing related objects, indicating that three relationships can exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. Additionally, the character " / " in this text generally represents an "or" relationship between the related objects before and after.
[0035] In a first aspect, the present application provides a perovskite solar cell, comprising a hole transport layer, a perovskite absorption layer, and an electron transport layer sequentially arranged on one surface of a conductive substrate from near to far, and the hole transport layer comprises a hole transport material.
[0036] In the embodiments of the present application, the structure of the hole transport material is shown in the following formula (1):
[0037] Wherein, 10 < n < 1000, and R1 and R2 are independently selected from any one of the following structures (1-1) or (1-2):
[0038]
[0039] The hole transport material of the perovskite solar cell of the present application has vinyl dithienopyrrole as the core. The electron-rich N atom in dithienopyrrole (DTP) can improve the stability of the organic semiconductor material in the oxidized state, enabling the optoelectronic device to have long-term operational stability. The S atom can bond with metal ions (such as Pb) in the perovskite absorption layer 2+) Interact to passivate the interfacial defects on the perovskite surface. Meanwhile, as a multifunctional electron-rich thiophene-fused heterocyclic unit, DTP has unique characteristics such as small reorganization energy, high mobility, chemical modification possible at N and thiophene sites, and the ability to interact with metal ions. By chemically modifying the thiophene sites in DTP with an electron-donating group containing aniline fluorene, the hole transport material has a deeper HOMO energy level, which is more matched with the energy level of the perovskite material, achieving better mobility and being more conducive to the extraction and transport of holes. The hole transport material of the perovskite battery in this application has a relatively high decomposition temperature and good thermal stability. It has good solubility in solvents such as dimethyl sulfoxide, N,N'-dimethylformamide, toluene, chlorobenzene, and dichloromethane, good film-forming properties, and good wettability with the perovskite precursor solvent, which helps the crystallization and film formation of perovskite. In addition, it also has the advantages of low raw material cost, simple preparation process, high repeatability, and can be used in inverted perovskite batteries without doping any additives, being suitable for industrial production and having good application prospects.
[0040] In summary, the hole transport material of the perovskite battery in this application combines the advantages of low cost, high performance, and high stability, and can realize the application of low-cost, high-performance, and stable large-area inverted perovskite batteries.
[0041] In the embodiments of this application, the conductive substrate can be an ITO glass substrate, a silicon substrate, or other common conductive substrates in the art. This application does not make special limitations on this, and those skilled in the art can select according to specific application scenarios.
[0042] In the embodiments of this application, the thicknesses of the hole transport layer, the perovskite absorption layer, and the electron transport layer can all be adjusted according to specific application scenarios.
[0043] In some embodiments, the thickness of the hole transport layer is 10 - 30 nm, specifically it can be 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, or any value between them. Those skilled in the art can adjust according to actual application requirements.
[0044] In some embodiments, the thickness of the perovskite absorption layer is 500 - 700 mn, specifically it can be 500 nm, 550 nm, 600 nm, 650 nm, 700 mn, or any value between them. Those skilled in the art can adjust according to actual application requirements.
[0045] In some embodiments, the thickness of the electron transport layer is 80 - 120 nm, specifically it can be 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, or any value between them. Those skilled in the art can adjust according to actual application requirements.
[0046] In the embodiments of the present application, the material of the perovskite light-absorbing layer can be a three-dimensional perovskite material or a quasi-two-dimensional perovskite material. The embodiments of the present application do not make specific limitations in this regard, and those skilled in the art can select according to actual needs.
[0047] In the embodiments of the present application, the material of the electron transport layer can be selected from conventional materials in the art, such as C60, C70, PCBM, etc. The embodiments of the present application do not make specific limitations in this regard, and those skilled in the art can select according to actual needs.
[0048] In some embodiments, an electrode is further provided on the side of the electron transport layer facing away from the perovskite absorption layer. The material of the electrode can be selected from conventional materials in the art, such as Au, Ag, Al, Cu, etc. The embodiments of the present application do not make specific limitations in this regard, and those skilled in the art can select according to actual needs.
[0049] In a second aspect, the present application also proposes a preparation method of a perovskite battery, and this preparation method can be used to prepare the perovskite battery described in the first aspect.
[0050] In the embodiments of the present application, the preparation method of the perovskite battery includes the steps of:
[0051] Provide a conductive substrate;
[0052] Successively arrange a hole transport layer, a perovskite absorption layer, an electron transport layer, and an electrode on one side of the conductive substrate.
[0053] In the embodiments of the present application, the hole transport layer includes the hole transport material shown in the above structure (1).
[0054] In the embodiments of the present application, the preparation method of the hole transport material includes the following steps:
[0055] Provide raw material 1, and prepare intermediate 1 from raw material 1. The structural formula of raw material 1 is: The structural formula of intermediate 1 is:
[0056] React intermediate 1 with N-bromosuccinimide to obtain intermediate 2. The structural formula of intermediate 2 is:
[0057]
[0058] Prepare intermediate 4, and intermediate 4 includes at least one of the following structural compounds:
[0059]
[0060] React intermediate 2 and intermediate 4 to obtain intermediate 5. The structural formula of intermediate 5 is:
[0061]
[0062] The elimination reaction is carried out on intermediate 5 to obtain intermediate 6, and the structural formula of intermediate 6 is:
[0063]
[0064] Intermediate 6 is mixed with an initiator to carry out a polymerization reaction to obtain a hole transport material.
[0065] In this application, the synthesis route of the hole transport layer is as follows:
[0066]
[0067] The preparation method of the hole transport material is described in more detail below:
[0068] In some embodiments, the preparation method of intermediate 4 includes the following steps:
[0069] Provide raw material 2 and raw material 3, and mix and react raw material 2 and raw material 3 to obtain intermediate 3. Among them, the structural formula of raw material 2 is: The structural formula of raw material 3 is: The structural formula of intermediate 3 is:
[0070]
[0071] Intermediate 3 is mixed and reacted with tert-butylpinacol borate to obtain intermediate 4.
[0072] In some embodiments, the specific preparation steps of intermediate 3 include: dissolving raw material 2, raw material 3, sodium tert-butoxide, tris(dibenzylideneacetone)dipalladium(0), and 2-(dicyclohexylphosphino)-2',4',6'-triisopropylbiphenyl in toluene, heating to 100 °C to 120 °C under a nitrogen atmosphere, stirring and reacting for 8 h to 10 h to obtain crude product 3, and purifying crude product 3 to obtain intermediate 3.
[0073] In some embodiments, the specific preparation steps of intermediate 4 include: reacting intermediate 3 with tert-butylpinacol borate to obtain intermediate 4. More specifically: weigh intermediate 3, tert-butylpinacol borate, and n-butyllithium according to an appropriate ratio. First, dissolve intermediate 3, and then gradually add n-butyllithium dropwise to the solution of intermediate 3, react at -70 °C to -85 °C for 1 to 1.5 h, then continue to add tert-butylpinacol borate, continue to react at -70 °C to -85 °C for 1 to 1.5 h, then transfer to room temperature and continue to react for 10 to 15 h, add deionized water to quench the reaction to obtain crude product 4, and purify crude product 4 to obtain intermediate 4.
[0074] In some embodiments, the specific preparation steps of intermediate 1 include: mixing raw material 1 with potassium carbonate, potassium hydroxide, tetrabutylammonium bromide and 1,2-dichloroethane according to a molar ratio of 1:(5 - 20):(2 - 10):(0.05 - 0.1):(30 - 50), reacting at a reaction temperature of 50°C to 60°C for a reaction time of 6 h to 8 h to obtain crude product 1, and purifying crude product 1 to obtain intermediate 1.
[0075] In some embodiments, the specific preparation steps of intermediate 2 include: dropwise adding N-bromosuccinimide (NBS) to intermediate 1 for reaction under the protection of an inert gas. Among them, the molar ratio of intermediate 1 to N-bromosuccinimide is 1:(2 - 3), the reaction temperature is -5°C to 5°C, and the reaction time is 3 h to 5 h to obtain crude product 2, and purifying crude product 2 to obtain intermediate 2.
[0076] In some embodiments, the specific preparation steps of intermediate 5 include: reacting intermediate 2 with intermediate 4 and a catalyst under an alkaline environment. Among them, the molar ratio of intermediate 2, intermediate 4 and the catalyst is 1:(2.2 - 3):(0.05 - 0.15):(5 - 7), and the reaction temperature is 80°C to 90°C to obtain crude product 5, and purifying crude product 5 to obtain intermediate 5.
[0077] In some embodiments, in the polymerization reaction, the concentration of intermediate 6 is 0.1 mol / L to 1.0 mol / L, and the initiator is azobisisobutyronitrile, and the concentration of the initiator is (1.0 - 10.0)×10 -3 mol / L.
[0078] In the above embodiments, the specific steps of mixing intermediate 6 and the initiator for the polymerization reaction include: adding intermediate 6 and azobisisobutyronitrile to a solvent (such as toluene, tetrahydrofuran, N-methylpyrrolidone, etc.) according to an appropriate ratio, freeze-drying with liquid nitrogen and evacuating for 1 minute and then filling with nitrogen, repeating three times and then sealing, initiating at 60°C to 70°C for 3 h to 3.5 h, reacting at 80°C to 90°C for 3 days, cooling to room temperature after the reaction ends to obtain crude product 7, and purifying crude product 7 to obtain the final product.
[0079] The synthesis route of the hole transport material provided by the embodiments of the present application is simple and the synthesis cost is low. By controlling conditions such as the raw materials and their feeding amounts, reaction temperature, and reaction time in each reaction step, the yield of the product is increased to a relatively high level.
[0080] In some embodiments, the preparation method of the perovskite battery includes the following steps:
[0081] (1) Cleaning: The ITO glass substrate (transparent conductive substrate) was ultrasonically cleaned successively with deionized water, acetone, and ethanol for 15 - 20 minutes, then the residual solvent on the surface of the ITO glass substrate was blown dry using an N2 gas gun, followed by oxygen plasma treatment for 10 - 15 minutes, and subsequently the ITO glass substrate was transferred to a nitrogen glove box.
[0082] (2) Preparation of the hole - transporting layer: Weigh 3 - 15 mg of the hole - transporting material and dissolve it completely in 1 mL of chlorobenzene solution. Take an appropriate amount of the solution and uniformly drop it onto the ITO glass substrate, spin - coat it at 4000 - 5000 rpm for 20 - 30 seconds, and then anneal it at 90 - 110 °C for 10 - 15 minutes to obtain the composite structure of ITO / hole - transporting layer.
[0083] (3) Preparation of the perovskite absorption layer: Cool the composite structure obtained in step (2) above to room temperature, pre - heat it at 130 - 140 °C for 3 - 5 minutes, take an appropriate amount (for example, 50 μL) of the perovskite solution and spread it evenly on the surface of the hole - transporting layer, spin - coat it at 3000 - 5000 rpm for 20 - 30 seconds, and then anneal it at 90 - 100 °C for 10 - 15 minutes to obtain the composite structure of ITO / hole - transporting layer / perovskite absorption layer. Among them, the perovskite solution is prepared by mixing one or more of 3 - bromo - benzylammonium iodide, 3 - chlorobenzylammonium iodide, methylammonium chloride, and lead iodide in a certain molar ratio in DMF or DMSO. For example, it is prepared by dissolving 3 - fluoro - benzylammonium iodide (3FBAI), methylammonium chloride (MACl), and lead iodide (PbI2) in DMF in a ratio of 2.2:3.5:4.
[0084] (4) Preparation of the electron - transporting layer: Cool the composite structure obtained in step (3) above to room temperature, prepare a solution of PC61 BM at 15 mg / mL, then take an appropriate amount (for example, 40 μL) of the solution and spread it evenly on the surface of the perovskite, spin - coat it at 1000 rpm for 30 - 50 seconds, and anneal it at 70 °C for 10 - 15 minutes to obtain the composite structure of ITO / hole - transporting layer / perovskite absorption layer / electron - transporting layer.
[0085] (5) Preparation of the electrode: Place the composite structure obtained in step (4) above in a vacuum evaporation chamber, and evaporate Cr (6 nm) and Au (80 nm) respectively on the PC61 BM layer (electron - transporting layer) to fabricate a tandem perovskite solar cell. Define the area overlapping with the electrode on the ITO glass substrate as the effective area, and the effective area is 0.03 cm 2 .
[0086] In the third aspect, the present application proposes a tandem cell.
[0087] In the embodiments of the present application, the tandem cell includes a bottom cell and a top cell; wherein, the bottom cell includes at least one silicon cell, and the silicon cell is selected from any one of crystalline silicon cells and amorphous silicon cells. If the bottom cell includes multiple silicon cells, the multiple silicon cells are stacked; the top cell is stacked on the bottom cell, and the top cell includes one or more perovskite cells, wherein at least one perovskite cell is the perovskite cell described in the above first aspect or is prepared by the preparation method described in the above second aspect, and the top cell includes multiple perovskite cells, and the multiple perovskite cells are stacked.
[0088] In the embodiments of the present application, the crystalline silicon cell can be selected from any one of TOPCon (Tunnel Oxide Passivated Contact cell), HJT (Heterojunction cell), IBC (Interdigitated Back Contact cell), PERC (Passivated Emitter and Rear Contact cell) or other common crystalline silicon cells in the art. The embodiments of the present application do not make special limitations in this regard, and those skilled in the art can adjust according to the actual application scenario.
[0089] It should be noted that when the top cell includes multiple crystalline silicon cells, the types of the multiple crystalline silicon cells can be the same or different.
[0090] In the embodiments of the present application, the amorphous silicon cell can be selected from any one of single-junction amorphous silicon cells, amorphous silicon tandem cells (such as: double-junction / triple-junction tandem cells) or other common amorphous silicon cells in the art. The embodiments of the present application do not make special limitations in this regard, and those skilled in the art can adjust according to the actual application scenario.
[0091] Fourthly, the present application also proposes a photovoltaic module, which includes a laminate and a frame, and the frame is installed at the edge of the laminate. Specifically, the laminate includes a photovoltaic glass, a first encapsulation film, a cell layer, a second encapsulation film and a backsheet stacked in sequence, or the laminate includes a first photovoltaic glass, a first encapsulation film, a cell layer, a second encapsulation film and a second photovoltaic glass stacked in sequence; wherein, the cell layer includes multiple cell strings connected in parallel, and each cell string includes multiple cells connected in series, and the cell is a whole cell or a cut piece that is 1 / N of the whole cell, and at least part of the cells are the tandem cells described in the third aspect.
[0092] In some embodiments, adjacent cells in the present application are connected in series through a conductive connection member (such as a wire or a solder strip) or a conductive adhesive, that is, one end of the conductive connection member is welded to the back electrode of one cell, and the other end of the conductive connection member is welded to the front electrode of another cell.
[0093] In some embodiments, adjacent cells can also form a photovoltaic module string by using high-density module technology, that is, the shingle technology, the stacked welding technology or the diced cell technology, which greatly reduces or eliminates the gap between cells.
[0094] Overlap technology: The whole piece of battery is cut into several small battery strips by laser slicing technology, and the small battery strips are stacked and flexibly connected with conductive adhesive. This connection method optimizes the structure of the photovoltaic module string, realizes zero gap between battery cells, makes full use of the limited area of the photovoltaic module, and can place more battery cells of the same version than other types of modules, effectively increasing the light-receiving area of the module.
[0095] Overlap welding technology: Adjacent half-cell battery slices are'micro-overlapped' and welded through special round wire solder tapes. This connection method greatly reduces the gap between battery cells in the traditional welding process and realizes high energy density. Compared with ordinary flat solder tapes, the round wire solder tapes have a narrower cross-section, reducing the light-shielding effect of the solder tapes on the battery cells. In addition, the round side of the solder tape enhances the reflection of incident light and the secondary refractive index of light on the front plate glass. The introduction of round solder tapes effectively solves the inherent contradiction between main grid occlusion and increasing current collection ability, improves the light absorption and utilization of battery cells, and increases the power of the module.
[0096] Chip-splicing technology: Triangular solder tapes are used on the front of the battery cell, and ultra-flexible flat solder tapes are used on the back. Adjacent half-cell battery slices are welded with a micro-gap through double solder tape technology, realizing high energy density. The triangular solder tapes used in the chip-splicing technology are welded three-dimensionally on the front of the battery. The reflection ability of the nearly 45° side angle to incident light is further improved compared with round solder tapes, and the reflection can be more fully utilized to increase the light absorption ability of the battery and the power of the module.
[0097] In the embodiments of the present application, preferably, the frame is made of high-strength lightweight materials, such as: steel, aluminum, or composite materials made of resin and reinforcing materials. Among them, the resin includes polyurethane, polyester, polycarbonate, etc., and the reinforcing materials include glass fiber, aluminum, steel, etc.
[0098] In the embodiments of the present application, the first encapsulant film and the second encapsulant film can independently be ethylene-vinyl acetate copolymer (EVA) encapsulant film, polyethylene octene co-elastic body (POE) encapsulant film, polyethylene terephthalate (PET) encapsulant film, PVB encapsulant film, EPE encapsulant film (EVA and POE three-layer co-extruded encapsulant film), EP encapsulant film (EVA and POE two-layer co-extruded encapsulant film), or other types of encapsulant films. Those skilled in the art can choose according to the actual situation and are not limited herein.
[0099] The present invention will be further described below through more specific embodiments.
[0100] Embodiment 1
[0101] The synthesis route of PVDTP-1 is as follows:
[0102]
[0103] The specific preparation steps of PVDTP-1 are as follows:
[0104] Synthesis of Compound 3: The raw material 2 (Compound 1, 1.61 g, 5.11 mmol), raw material 3 (Compound 2, 1.02 g, 4.26 mmol), sodium tert-butoxide (0.61 g, 6.35 mmol), tris(dibenzylideneacetone)dipalladium(0) (0.077 mg, 0.085 mmol), and 2-(dicyclohexylphosphino)-2′,4′,6′-triisopropylbiphenyl (0.081 g, 0.169 mmol) were mixed and dissolved in toluene (30 mL), and then put into a two-necked round-bottom flask. Under a nitrogen atmosphere, it was heated to 110 °C, stirred and reacted for 8 h, then cooled to room temperature, and then extracted with ethyl acetate. The organic layer was washed with brine (100 mL × 3). After that, the organic layer was successively dried over anhydrous sodium sulfate, filtered, and subjected to vacuum distillation. Finally, the vacuum-distilled product was purified by silica gel column chromatography (DCM / PE with a volume ratio of 1:4) to obtain 1.48 g of yellow solid Compound 3, that is, Intermediate 3, with a yield of 73.2%.
[0105] Synthesis of Compound 4: Weighed Compound 3 (4.74 g, 10 mmol) and added it to a 500 mL three-necked flask. Then 30 mL of dry THF was added. Under N2 conditions, it was cooled to -78 °C and stirred for 10 min. Then n-butyllithium (3.75 mL, 1.00 equiv, 1.6 M in n-hexane) was slowly added dropwise. The reaction was carried out at -78 °C for 1 h. Then tert-butylpinacol borate (2.75 mL, 15 mmol) was added, and the reaction was continued at -78 °C for 1 h. Finally, it was transferred to room temperature and reacted for 12 h. The reaction was quenched with 50 mL of deionized water. First, it was extracted with saturated NaCl solution and DCM. Then the organic phase was successively dried over anhydrous Mg2SO4, filtered. Finally, it was purified by column chromatography (PE:DCM = 15:1) to obtain 4.8 g of Compound 4 (Intermediate 4), with a yield of 80%.
[0106] Synthesis of Compound 6: The raw material 1 (Compound 5, 1.79 g, 10 mmol), potassium carbonate (10.35 g, 75 mmol), potassium hydroxide (1.70 g, 30 mmol), and tetrabutylammonium bromide (0.24 g, 0.75 mmol) were added to 30 mL of 1,2-dichloroethane solution. After reacting at 50 °C for 6 h and then cooling to room temperature, it was extracted with saturated sodium chloride solution and dichloromethane. After that, the organic phase was successively dried over anhydrous magnesium sulfate, filtered, and subjected to vacuum distillation. Finally, the vacuum-distilled product was purified by silica gel chromatography to obtain 2.1 g of Compound 6 (Intermediate 1), with a yield of 87%.
[0107] Synthesis of Compound 7: Compound 6 (725 mg, 3 mmol) was added to a 100 mL flask, and 15 mL of tetrahydrofuran solution was added. The reaction was carried out at 0 °C for 10 minutes under nitrogen protection. Then, NBS (1.1 g, 6 mmol) was dissolved in 25 mL of tetrahydrofuran solution and added to the tetrahydrofuran mixed solution of Compound 6 in several portions. The reaction continued at 0 °C for 3 hours and then cooled to room temperature. Then, extraction was carried out using saturated sodium chloride solution and dichloromethane. After that, the organic phase was successively dried over anhydrous magnesium sulfate, filtered, and distilled under reduced pressure. Finally, the product obtained by distillation under reduced pressure was purified by silica gel chromatography to obtain 940 mg of Compound 7 (Intermediate 2) with a yield of 78%.
[0108] Synthesis of Compound 8: Compound 7 (0.4 g, 1.0 mmol), Compound 4 (1.38 mg, 2.3 mmol), tetrakis(triphenylphosphine)palladium (69.4 mg, 0.06 mmol), and potassium carbonate (973 mg, 7 mmol) were added to a 100 mL flask. After evacuation, nitrogen was filled. 25 mL of toluene, 12.5 mL of ethanol, and 12.5 mL of deionized water were added as solvents. The reaction was carried out at 85 °C for 6 hours and then cooled to room temperature. Then, extraction was carried out using saturated sodium chloride solution and dichloromethane. After that, the organic phase was dried over anhydrous magnesium sulfate, filtered, and distilled under reduced pressure. Finally, 0.88 g of yellow powder of Compound 8 (Intermediate 5) was obtained by column chromatography purification with a yield of 75%.
[0109] Synthesis of Compound 9: Compound 8 (0.58 g, 0.5 mmol), potassium hydroxide (0.898 g, 16 mmol), and p-diphenol (22 mg, 0.2 mmol) were dissolved in a toluene:isopropanol (1:8) mixed solution. The reaction was carried out at 85 °C for 48 hours and then cooled to room temperature. First, the isopropanol-toluene mixed solution was rotary evaporated under reduced pressure, and then washed and extracted using saturated sodium chloride solution and dichloromethane. After that, the organic phase was successively dried over anhydrous magnesium sulfate, filtered, and distilled under reduced pressure. Recrystallization of the product obtained by distillation under reduced pressure was carried out using n-hexane (methanol) / dichloromethane to obtain 400 mg of Compound 9 (Intermediate 6) with a yield of 69%. For the ¹H NMR spectrum of Compound 9, please refer to Figure 1 。
[0110] Synthesis of PVDTP-1: 300 mg of Compound 9 and 1% by mass of azobisisobutyronitrile (previously recrystallized from ethanol; 3 mg) were weighed and added to a solution of toluene (or tetrahydrofuran, N-methylpyrrolidone). After freeze-drying with liquid nitrogen and evacuating for 1 minute, nitrogen was filled. This process was repeated three times and then sealed. After initiation at 65 °C for 3 hours, the temperature was raised to 85 °C and the reaction was carried out for 3 days. After the reaction ended and cooled to room temperature, crystallization was carried out using n-hexane (ethanol) / dichloromethane. After suction filtration and drying, extraction was carried out using acetone as a solvent in a Soxhlet extractor for three days to obtain 140 mg of the product PVDTP-1.
[0111] Example 2
[0112] Synthesis route of PVDTP-2:
[0113]
[0114] The specific preparation steps of PVDTP-2 are as follows:
[0115] Synthesis of compound 11: Compound 10 (1.69 g, 5.11 mmol), compound 2 (1.02 g, 4.26 mmol), sodium tert-butoxide (0.61 g, 6.35 mmol), tris(dibenzylideneacetone)dipalladium(0) (0.077 mg, 0.085 mmol) and 2-dicyclohexylphosphino-2′,4′,6′-triisopropylbiphenyl (0.081 g, 0.169 mmol) were mixed and dissolved in toluene (30 mL), and put into a two-necked round-bottom flask. Under a nitrogen atmosphere, it was heated to 110 °C and stirred for 8 h. After the reaction was completed, it was cooled to room temperature, extracted with ethyl acetate, and the organic layer was washed with brine (100 mL × 3). Then, the organic layer was successively dried over anhydrous sodium sulfate, filtered, and subjected to vacuum distillation. The vacuum distillation product was purified by silica gel column chromatography (DCM / PE with a volume ratio of 1:4) to obtain 1.4 g of compound 12 (intermediate 3) with a yield of 70%.
[0116] Synthesis of compound 12: Weigh compound 10 (4.89 g, 10 mmol) and add it to a 500 mL three-necked flask. Then add 30 mL of dry THF. Cool it to -78 °C under N2 conditions and stir for 10 min. Then slowly dropwise add n-butyllithium (3.75 mL, 1.00 equiv, 1.6 M in n-hexane). After reacting at -78 °C for 1 h, add tert-butylpinacol borate (2.75 mL, 15 mmol). Continue to react at -78 °C for 1 h and then transfer it to room temperature and react for 12 h. Quench the reaction with 50 mL of deionized water, then extract with saturated NaCl solution and DCM. Then, the organic phase was successively dried over anhydrous Mg2SO4 and filtered. Finally, it was purified by column chromatography (PE:DCM = 15:1) to obtain 5.0 g of compound 12 (intermediate 4) with a yield of 82%.
[0117] Synthesis of Compound 6: Raw material 1 (Compound 5, 1.79 g, 10 mmol), potassium carbonate (10.35 g, 75 mmol), potassium hydroxide (1.70 g, 30 mmol), and tetrabutylammonium bromide (0.24 g, 0.75 mmol) were added to a 30 mL 1,2-dichloroethane solution. After reacting at 50 °C for 6 hours and cooling to room temperature, extraction was carried out using saturated sodium chloride solution and dichloromethane. Then, the organic phase was successively dried over anhydrous magnesium sulfate, filtered, and distilled under reduced pressure. Finally, the product obtained by distillation under reduced pressure was purified by silica gel chromatography to obtain 2.1 g of Compound 6 (Intermediate 1) with a yield of 87%.
[0118] Synthesis of Compound 7: Compound 6 (725 mg, 3 mmol) was added to a 100 mL flask, and 15 mL of tetrahydrofuran solution was added. The reaction was carried out at 0 °C for 10 minutes under nitrogen protection. Then, NBS (1.1 g, 6 mmol) was dissolved in 25 mL of tetrahydrofuran solution and added to the tetrahydrofuran mixed solution of Compound 6 in several portions. The reaction continued at 0 °C for 3 hours and then cooled to room temperature. Extraction was carried out using saturated sodium chloride solution and dichloromethane. Then, the organic phase was successively dried over anhydrous magnesium sulfate, filtered, and distilled under reduced pressure. Finally, the product obtained by distillation under reduced pressure was purified by silica gel chromatography to obtain 940 mg of Compound 7 (Intermediate 2) with a yield of 78%.
[0119] Synthesis of Compound 13: Compound 7 (0.4 g, 1.0 mmol), Compound 12 (1.5 mg, 2.3 mmol), tetrakis(triphenylphosphine)palladium (69.4 mg, 0.06 mmol), and potassium carbonate (973 mg, 7 mmol) were added to a 100 mL flask. After evacuating and filling with nitrogen, 25 mL of toluene, 12.5 mL of ethanol, and 12.5 mL of deionized water were added as solvents. The reaction was carried out at 85 °C for 6 hours and then cooled to room temperature. First, extraction was carried out using saturated sodium chloride solution and dichloromethane, and then the organic phase was successively dried over anhydrous magnesium sulfate, filtered, and distilled under reduced pressure. Finally, the product obtained by distillation under reduced pressure was purified by column chromatography to obtain 0.8 g of yellow powder of Compound 13 (Intermediate 5) with a yield of 66%.
[0120] Synthesis of Compound 14: Dissolve Compound 13 (0.59 g, 0.5 mmol), potassium hydroxide (0.898 g, 16 mmol), and p-diphenol (22 mg, 0.2 mmol) in a mixed solution of toluene:isopropanol (1:8). After reacting at 85 °C for 48 hours, cool to room temperature. First, rotary evaporate the isopropanol-toluene mixed solution under reduced pressure, then wash and extract with saturated sodium chloride solution and dichloromethane. After that, dry the organic phase with anhydrous magnesium sulfate, filter, and distill under reduced pressure. Finally, recrystallize the product obtained by distillation under reduced pressure with n-hexane (methanol) / dichloromethane to obtain 370 mg of Compound 14 (Intermediate 6) with a yield of 64%. For the 1H NMR spectrum of Compound 14, please refer to Figure 2 。
[0121] Synthesis of PVDTP-2: Weigh 300 mg of Compound 14 and 1% by mass of azobisisobutyronitrile (previously recrystallized from ethanol; 3 mg), add them to a solution of toluene (or tetrahydrofuran, N-methylpyrrolidone). After freeze-drying with liquid nitrogen and evacuating for 1 minute, refill with nitrogen, repeat three times and then seal. After initiating the reaction at 65 °C for 3 hours, raise the temperature to 85 °C and react for 3 days. After the reaction is completed, cool to room temperature, then crystallize with n-hexane (ethanol) / dichloromethane, filter and dry by suction. Then, use acetone as the solvent and extract with a Soxhlet extractor for three days to obtain 152 mg of PVDTP-2.
[0122] Performance Testing
[0123] 1. HOMO Energy Level Testing:
[0124] To study the energy level matching between PVDTP-1 and PVDTP-2 materials as HTMs and the energy level of perovskite, a three-electrode test system was used to measure the cyclic voltammograms (C-V) of these two polymer HTMs. A three-electrode test system was adopted. Using ferrocene as an external standard, the working electrode was a glassy carbon electrode, the counter electrode was a platinum wire electrode, and the reference electrode was an Ag / AgCl electrode. First, prepare PVDTP-1 and PVDTP-2 solutions with a concentration of 5 mg / mL in dichloromethane as the solvent, and then use the thin-film method to drop-coat them on the glassy carbon electrode and test in an acetonitrile solution of 0.1 M Bu4NPF6 with a scanning rate of 50 mV·s –1 , at room temperature, the C-V curve was obtained through multiple scans, and then the oxidation-reduction potential of the curve was analyzed, and the HOMO energy level of the material was calculated according to the formula.
[0125] 2. Hole Mobility Testing:
[0126] The space charge limited current method was used for testing. A single-hole device of ITO / PEDOT:PSS / HTMs to be tested / MoO3 / Ag was fabricated. The film thickness of each layer was determined by a profilometer. Under dark conditions, the J-V characteristic curve of the device was obtained by a Keithley 2450 Source-Measure instrument, and the curve was analyzed by non-linear fitting to obtain the hole mobility of the sample.
[0127] 3. Film formation performance test:
[0128] AFM was used to study the crystallization growth of quasi-two-dimensional perovskite films (perovskite absorption layer) on different polymer HTMs, and the RMS roughness on different polymer HTMs was measured.
[0129] 4. Photovoltaic and stability test:
[0130] Trans-type quasi-two-dimensional perovskite solar cell devices using PVDTP-1 and PVDTP-2 as hole transport materials were fabricated respectively by the same preparation method. The specific preparation method refers to the preparation method of the perovskite solar cell above.
[0131] Under the illumination condition of AM 1.5G, the J-V curves of the devices were measured at a forward and reverse scanning speed of 0.02 V·s -1 . From the analysis of the J-V curves, the photovoltaic parameters of the samples measured, such as open-circuit voltage (Voc), short-circuit current density (Jsc), fill factor (FF), and power conversion efficiency (PCE), could be obtained.
[0132] After storing the devices in an inert environment for 1200 hours, the retention efficiency of the devices (relative to the initial power conversion efficiency) was measured.
[0133] Table 1. Performance test results of the hole transport materials prepared in Example 1 and Example 2
[0134]
[0135] The test results shown in Table 1 can prove that: the designed and synthesized polyethylene-based hole transport materials in this application have excellent film-forming properties (the prepared quasi-two-dimensional perovskite films all exhibit low RMS roughness), which is beneficial to the diffusion and growth of perovskite as the HTL substrate, thus obtaining a dense, uniform, and smooth perovskite film. Moreover, it also has energy levels matching with perovskite and excellent hole mobility. These characteristics enable the trans-type perovskite solar cell devices prepared based on the hole transport materials provided in this application to have excellent power conversion efficiency; in addition, it can also be seen from Table 1 above that the structural stability of the trans-type perovskite solar cell devices prepared based on the hole transport materials provided in this application is also good.
[0136] The above are only the preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.
Claims
1. A perovskite solar cell, comprising a hole transport layer, a perovskite absorption layer, and an electron transport layer that are sequentially disposed on one surface of a conductive substrate from near to far, wherein the hole transport layer comprises a hole transport material, and is characterized in that, The structure of the hole transport material is shown in the following formula (1): Among them, 10 < n < 1000, and R1 and R2 are independently selected from any one of the following structures (1-1) or (1-2):
2. The perovskite cell according to claim 1, wherein The thickness of the hole transport layer is 10 - 30 nm; and / or, The thickness of the perovskite absorption layer is 500 - 700 nm; and / or, The thickness of the electron transport layer is 80 - 120 nm.
3. A method for preparing a perovskite solar cell, characterized in that, It includes the preparation of a hole transport material, and the preparation steps of the hole transport material include: Provide raw material 1, prepare intermediate 1 from the raw material 1, and the structural formula of the raw material 1 is: The structural formula of the intermediate 1 is: React the intermediate 1 with N-bromosuccinimide to obtain intermediate 2, and the structural formula of the intermediate 2 is: Prepare intermediate 4, the structural formula of which is: React the intermediate 2 with the intermediate 4 to obtain intermediate 5, and the structural formula of the intermediate 5 is: R1 and R2 are independently selected from any one of the following structures (1-1) or (1-2): The elimination reaction is carried out on the intermediate 5 to obtain an intermediate 6, and the structural formula of the intermediate 6 is as follows: Mixing the intermediate 6 with an initiator for a polymerization reaction to obtain the hole transport material, and the structure of the hole transport material is shown in the following formula (1):
4. The preparation method of the perovskite battery according to claim 3, characterized in that, The preparation method of the intermediate 4 includes the following steps: Provide raw material 2 and raw material 3, and react the raw material 2 and the raw material 3 to obtain intermediate 3. The structural formula of the raw material 2 is: The structural formula of the raw material 3 is: The structural formula of the intermediate 3 is: Reacting the intermediate 3 with tert-butylpinacol borate to obtain the intermediate 4.
5. The method for preparing a perovskite solar cell according to claim 3 or 4, characterized in that, The specific preparation steps of the intermediate 1 include: mixing the raw material 1 with potassium carbonate, potassium hydroxide, tetrabutylammonium bromide and 1,2-dichloroethane for a reaction, wherein the molar ratio of the raw material 1, potassium carbonate, potassium hydroxide, tetrabutylammonium bromide and 1,2-dichloroethane is 1:(5 - 20):(2 - 10):(0.05 - 0.1):(100 - 500), and the reaction temperature is 50°C - 60°C.
6. The preparation method of the perovskite battery according to claim 3 or 4, characterized in that The specific preparation steps of the intermediate 2 include: dropwise adding N-bromosuccinimide to the intermediate 1 for a reaction, wherein the molar ratio of the intermediate 1 to N-bromosuccinimide is 1:(2 - 3), the reaction temperature is -5°C - 5°C, and the reaction time is 3 h - 5 h.
7. The preparation method of the perovskite battery according to claim 3 or 4, characterized in that, The specific preparation steps of the intermediate 5 include: mixing the intermediate 2 with the intermediate 4, the catalyst tetrakis(triphenylphosphine)palladium and potassium carbonate for a reaction, wherein the molar ratio of the intermediate 2, the intermediate 4 and the catalyst is 1:(2.2 - 3):(0.05 - 0.15), and the reaction temperature is 80°C - 90°C.
8. The preparation method of the perovskite battery according to claim 3 or 4, characterized in that, In the polymerization reaction, the concentration of the intermediate 6 is 0.1 mol / L to 1.0 mol / L, and the concentration of the initiator is (1.0 to 10.0)×10 -3 mol / L.
9. A stacked battery, characterized in that, It includes: A bottom cell, the bottom cell includes at least one crystalline silicon cell and / or amorphous silicon cell; A top cell, stacked on the bottom cell, the top cell includes one or more perovskite cells, wherein at least one perovskite cell is the perovskite cell as described in claim 1 or 2, or at least one perovskite cell is prepared by the preparation method of the perovskite cell as described in any one of claims 3 - 8.
10. A photovoltaic module, characterized in that, It includes the tandem cell as described in claim 9.
Citation Information
Cited By
Perovskite solar cell for regulating and controlling interface residual strain and preparation method thereof
CN121099824A