A soft magnetic stainless steel wire rod with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness, and its preparation method.
By adjusting the chemical composition and processing flow of soft magnetic stainless steel, the contradiction between corrosion resistance, machinability, and toughness of the material was resolved, and a soft magnetic stainless steel with excellent properties was prepared, which is suitable for processing complex-shaped parts such as solenoid valves for intelligent control.
Patent Information
- Application Number
- CN202510215526.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-02-26
AI Technical Summary
There is a contradiction between improving machinability and corrosion resistance in existing soft magnetic stainless steel materials. It is difficult to simultaneously satisfy good plasticity, toughness and machinability, which affects subsequent processing and service performance.
By adjusting the chemical composition, increasing the Cr and Mo content, controlling the C, S, and Se content, and adding Nb, and combining specific smelting and heat treatment processes, the material microstructure and properties are optimized, including electric arc furnace smelting, AOD furnace refining, LF refining, die casting, and heat treatment, to prepare soft magnetic stainless steel with ultra-high corrosion resistance, good machinability, and excellent plasticity and toughness.
It achieves ultra-high corrosion resistance, excellent soft magnetic properties and good machinability of the material, while improving plasticity and toughness, making it suitable for large-scale industrial production and applicable to processing into complex-shaped parts such as solenoid valves for various intelligent control applications.
Smart Images

Figure CN120272818B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of soft magnetic stainless steel technology, and involves technical fields such as metal smelting, rolling, and heat treatment. Specifically, it relates to a soft magnetic stainless steel with ultra-high corrosion resistance, good machinability, and excellent plasticity and toughness, and its preparation method. Background Technology
[0002] Soft magnetic stainless steel wire rods are used to manufacture various intelligent control solenoid valves. First, the material must be drawn in multiple stages, requiring good plasticity and toughness to prevent cracking or breakage during the drawing process. Then, it needs to be processed into various complex shapes through grinding, turning, and drilling, requiring the material to have good machinability. At the same time, soft magnetic stainless steel must also adapt to the requirements of use in liquid media, chlorides, chemical reagents, and other harsh environments, and the requirements for the material's corrosion resistance are becoming increasingly stringent.
[0003] However, these properties are contradictory. For example, increasing the sulfur content in a material to improve machinability often sacrifices corrosion resistance; increasing the Cr and Mo content to improve corrosion resistance significantly reduces the material's ductility and toughness, which is detrimental to subsequent drawing processes. Therefore, obtaining soft magnetic stainless steel materials that combine ultra-high corrosion resistance, good machinability, and excellent ductility and toughness is a difficult and challenging issue in the industry, and it is also the fundamental reason for the gap between my country's soft magnetic stainless steel materials and those of foreign countries. Summary of the Invention
[0004] To address the problems existing in the prior art, this invention provides a soft magnetic stainless steel that combines ultra-high corrosion resistance, good machinability, and excellent ductility and toughness; it also provides a method for manufacturing the soft magnetic stainless steel. The method for preparing the stainless steel described in this invention is easy to operate and suitable for large-scale industrial production.
[0005] To achieve the above objectives, the present invention provides the following technical solution:
[0006] This invention provides a soft magnetic stainless steel that combines ultra-high corrosion resistance, good machinability, and excellent ductility and toughness. The chemical composition of the wire rod, by mass percentage, includes: C ≤ 0.020%, Si: 1.20~2.00%, Mn ≤ 0.50%, Cr: 18.0~20.0%, Ni: ≤ 0.30%, Mo: 2.50~3.00%, N ≤ 0.020%, P < 0.020%, S: 0.008~0.015%, Se: 0.030~0.050%, Nb: 0.20~0.30%, with the balance being Fe and unavoidable impurities. This invention improves the corrosion resistance of materials by reducing the C and Mn content while increasing the Cr (≥18%) and Mo (≥2.5%) content. By controlling the S (0.008-0.015%) and Se (0.030-0.050%) content, the turning performance is optimized while avoiding a significant decrease in corrosion resistance. The addition of Nb content refines the grain size of the material to improve plasticity and toughness, thereby obtaining a soft magnetic stainless steel material with ultra-high corrosion resistance, good machinability, and excellent plasticity and toughness.
[0007] Furthermore, the chemical composition of the aforementioned stainless steel wire rod, by mass percentage, includes C: 0.010–0.020%, Si: 1.6–1.7%, Mn: 0.2–0.4%, Cr: 18.50–19.00%, Ni: 0.1–0.3%, Mo: 2.55–2.65%, N: 0.010–0.020%, P: 0.010–0.020%, S: 0.008–0.015%, Se: 0.030–0.050%, Nb: 0.20–0.30%, with the balance being Fe and unavoidable impurities.
[0008] This invention provides a method for preparing soft magnetic stainless steel wire rods with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness. The method includes sequentially processing the furnace charge through electric arc furnace smelting, AOD furnace refining, LF refining furnace refining, die casting, ingot billet preparation, primary heat treatment, rolling, and secondary heat treatment to obtain soft magnetic stainless steel wire rods with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness. Furthermore, by using the above preparation method, the overall yield of the material is ≥85%.
[0009] Furthermore, in the electric arc furnace smelting process, the furnace charge is melted and the molten steel is initially smelted using an electric arc furnace, and the P content is controlled to be ≤0.020% when tapping the steel.
[0010] Furthermore, in the AOD furnace refining process, ferrosilicon, pure manganese, ferrochrome, and ferromolybdenum are added to fine-tune the content of Si, Mn, Cr, and Mo elements in the molten steel, so that the composition of the finished stainless steel wire rod meets the target mass percentage ratio requirements, and the carbon and nitrogen content in the molten steel is removed to C≤0.015% and N≤0.010%.
[0011] Furthermore, in the refining process of the LF refining furnace, by adding ferroniobium to the furnace, the Nb content in the molten steel is adjusted to 0.20-0.30%. At the same time, sulfur wire and Se wire are fed in to control the S and Se in the molten steel at S: 0.008-0.015% and Se: 0.030-0.050%, respectively. The steel is then tapped after stirring with soft argon gas for more than 10 minutes.
[0012] Furthermore, in the casting process, large-size steel ingot molds are used for pouring, and even more specifically, 17-20 inch steel ingot molds are used for pouring, with the ladle temperature controlled at 1500-1530℃.
[0013] Furthermore, in the steel ingot heating and billet opening process, the steel ingot is loaded into a heating furnace, heated to 1100-1150℃, and held for 1.5-2.5 hours.
[0014] Furthermore, the billet after roughing is subjected to a heat treatment annealing process at a temperature of 680–720℃ and a holding time of 4–6 hours.
[0015] Furthermore, in the wire rod rolling process, the billet after annealing is placed in a heating furnace and heated to 950–1000℃ for 1–2 hours. During rolling, the final rolling temperature is controlled to be ≤850℃. Even further, the wire rod specifications are φ5.5–30mm.
[0016] Furthermore, after the wire rod is rolled, it undergoes a secondary heat treatment. In the secondary heat treatment annealing process of the wire rod, the rolled wire rod is placed in a bell-type annealing furnace for heating. The annealing temperature is controlled at 800-880℃, and the holding time is more than 60 minutes. More preferably, the temperature is 780-860℃, and the holding time is ≥2 hours.
[0017] In summary, compared with the prior art, the technical solutions provided by this invention can achieve the following beneficial effects:
[0018] (1) This invention adds extremely high Cr (≥18%) and Mo (≥2.5%) content to steel, and at the same time uses AOD smelting to control the content of harmful elements C and P in steel to ≤0.02%, so that the material has extremely high corrosion resistance (no rust after salt spray test ≥1000 hours);
[0019] (2) This invention increases the ferrite-forming elements such as Si, Cr, Mo, and Nb, and decreases the austenite-forming elements such as C, N, Mn, and Ni. After rolling, a suitable heat treatment process is used to make the material structure a pure ferrite structure, thereby having excellent soft magnetic properties (saturation magnetic induction intensity ≥1.5T, coercivity ≤250A / m).
[0020] (3) Since the subsequent processing of soft magnetic stainless steel into parts requires turning, drilling, and other operations, the material must have good machinability. Therefore, this invention adds appropriate amounts of elements such as S and Se to the steel to improve machinability. To avoid excessive S content reducing the corrosion resistance of the material, the S content in the steel is controlled at 0.008-0.015%, and an appropriate amount of Se element that does not reduce corrosion resistance is added, with its content controlled at 0.030-0.050%, so that the material has good machinability while still ensuring excellent corrosion resistance.
[0021] (4) Currently, ultrapure ferritic stainless steel is prone to forming coarse grain structure during hot working, which reduces the plasticity and toughness of the material and leads to brittle fracture and central cracking during subsequent drawing processes. This invention increases the rolling compression ratio by using large ingots for billet preparation, with the cross-sectional area of the original billet / the cross-sectional area of the final product ≥20. At the same time, it adds 0.20-0.40% Nb to refine the grains and uses ultra-low temperature rolling (final rolling temperature ≤850℃) to control the grain size of the material to be finer than level 4, thereby improving the plasticity and toughness of the material.
[0022] This invention produces a material that simultaneously possesses extremely high corrosion resistance, excellent soft magnetic properties, good machinability, and good ductility and toughness, making it suitable for subsequent drawing and turning processes and possessing broad market application prospects. Furthermore, the preparation method provided by this invention has a high yield rate and is suitable for large-scale industrial production. Attached Figure Description
[0023] Appendix Figure 1 This is a flowchart of the manufacturing process of the soft magnetic stainless steel wire rod of the present invention;
[0024] Appendix Figure 2 This is a metallographic diagram of the soft magnetic stainless steel wire rod of Embodiment 1 of the present invention;
[0025] Appendix Figure 3 This is the hysteresis loop (soft magnetic property data) measured by the soft magnetic stainless steel bar in Embodiment 1 of the present invention. Detailed Implementation
[0026] To better clarify and understand the objectives, process solutions, and advantages of this invention, the technical solutions and implementation methods of this invention will be further described clearly, completely, and in detail below through specific embodiments and in conjunction with the accompanying drawings. It should be understood that the embodiments described in this invention are implemented under the premise of the technical solutions of this invention, providing detailed implementation methods and specific operating procedures, but are only some embodiments of this invention, not all embodiments. The specific implementation methods described are limited to illustrating and explaining this invention and do not limit this invention. Based on the embodiments of this invention, all other implementation methods obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0027] Unless otherwise specified, the experimental methods and conditions used in the embodiments of this invention are conventional methods and conditions. The materials, reagents, and instruments used in the embodiments, unless otherwise specified, can be obtained commercially or prepared by conventional methods. The reaction conditions described in the invention can all achieve the reactions and obtain the desired products. Due to space limitations, some embodiments are listed below to further illustrate the advantages of the technical solution of this invention.
[0028] Example 1
[0029] This embodiment provides a soft magnetic stainless steel wire rod with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness, as well as its preparation method. The composition of the soft magnetic stainless steel wire rod is shown in Table 1 below:
[0030] Table 1. Schematic diagram of the composition of stainless steel wire rod in Example 1
[0031]
[0032] The preparation method of the soft magnetic stainless steel wire rod includes the following steps: the furnace charge is successively processed through electric arc furnace smelting, AOD furnace refining, LF refining furnace refining, die casting, steel ingot billet opening, primary heat treatment, rolling, secondary heat treatment and other processes to obtain soft magnetic stainless steel wire rod with ultra-high corrosion resistance, good machinability and excellent plasticity and toughness. Moreover, by adopting the preparation method, the overall yield of the material is ≥85%.
[0033] In the electric arc furnace smelting process, the furnace charge is melted and the molten steel is initially smelted using an electric arc furnace, and the P content is controlled to be ≤0.020% when tapping the steel.
[0034] In the AOD furnace refining process, ferrosilicon, pure manganese, ferrochrome, and ferromolybdenum are added to fine-tune the content of Si, Mn, Cr, and Mo elements in the molten steel, so that the composition of the finished stainless steel wire rod meets the target mass percentage ratio requirements, and the carbon and nitrogen content in the molten steel is removed to C≤0.015% and N≤0.010%.
[0035] In the LF furnace refining process, by adding ferroniobium to the furnace, the Nb content in the molten steel is adjusted to 0.20-0.30%. At the same time, sulfur wire and se wire are fed in to control the S and Se in the molten steel at S: 0.008-0.015% and Se: 0.030-0.050%, respectively. The steel is then tapped after stirring with soft argon gas for more than 10 minutes.
[0036] The composition of the molten steel after LF refining is shown in Table 1; using the chemical composition of Example 1 described in Table 1, the subsequent wire rod manufacturing process is as follows:
[0037] In the die casting process, the larger the steel ingot size, the greater the forging compression ratio, which is beneficial to grain refinement. If the steel ingot size is too large, the time required for billet opening is too long, and the risk of cracking in the first-fire billet opening is very high. It is preferable to use 17-inch to 20-inch steel ingot molds for casting. In this embodiment, a 17-inch steel ingot mold is used, and the ladle temperature is controlled at 1500 to 1530℃.
[0038] In the steel ingot heating and billet-making process, the steel ingot is placed in a heating furnace and heated to a temperature of 1100–1150℃ for a holding time of 1.5–2.5 hours. In this embodiment, the heating temperature is 1140℃ and the holding time is 2.0 hours. After billet-making, the billet undergoes a first annealing treatment at a temperature of 680–720℃ for a holding time of 4–6 hours. In this embodiment, the annealing temperature is 720℃ and the holding time is 6 hours.
[0039] In the wire rod rolling process (specifications φ5.5~30mm), the billet after annealing is placed in a heating furnace, heated to 950~1000℃, held for 1~2 hours, and the final rolling temperature is controlled to ≤850℃. In this embodiment, the heating temperature is 980℃, the holding time is 1.5 hours, and the final rolling temperature is controlled to 800~820℃.
[0040] The rolled wire rod is placed into a bell-type annealing furnace for secondary annealing heat treatment. The annealing temperature is controlled at 800-880℃ and the holding time is more than 60 minutes. In this embodiment, the annealing temperature is 860℃ and the holding time is 2 hours.
[0041] The soft magnetic stainless steel prepared in this embodiment possesses excellent corrosion resistance, machinability, and ductility. It does not rust after 1000 hours of salt spray testing, exhibits excellent machinability, and has a surface roughness of ≤1.0μm after turning. It also shows minimal tool wear and excellent magnetic properties, with a saturation magnetic induction intensity Bs >1.50T and coercivity <250A / m. Grain size testing shows an external grade of 6-7 and an internal grade of 4-5. Tensile properties testing shows a tensile strength of 530MPa, an elongation after fracture of 35%, and a reduction of area of 72%. The material also demonstrates excellent ductility and toughness.
[0042] The salt spray test method is GB / T10125-2021 Artificial Atmosphere Corrosion Test + Salt Spray Test;
[0043] The magnetic property testing method is GB / T13012-2008 Measurement method of DC magnetic properties of soft magnetic materials;
[0044] The grain size determination method is GB / T6394-2017 Method for Determination of Average Grain Size of Metals;
[0045] The tensile property test method is GB / T228.1-2021 Metallic materials, tensile testing—Part 1: Test at room temperature;
[0046] The evaluation of turning performance involves testing the surface roughness and tool wear of the sample after turning. The roughness testing method is based on the product geometry specification (GPS) in GB / T6062-2009, which includes surface structure, profile method, and nominal characteristics of contact (stylus) instruments.
[0047] Examples 2-6
[0048] Based on Example 1, by changing the composition ratio and process parameters of the stainless steel material, a corresponding soft magnetic stainless steel wire rod was obtained. The composition of the soft magnetic stainless steel wire rod is shown in Table 2 below.
[0049] Table 2. Schematic diagram of stainless steel wire rod composition for each embodiment.
[0050]
[0051] The process parameters for preparing the soft magnetic stainless steel wire rod are shown in Table 3 below:
[0052] Table 3. Schematic diagram of stainless steel wire rod preparation process parameters for each embodiment.
[0053]
[0054] Examples 2-6 yielded soft magnetic stainless steels with excellent corrosion resistance, machinability, and ductility. The performance of the soft magnetic stainless steels was basically equivalent to that of Example 1, with the soft magnetic stainless steels of Examples 5 and 6 showing even better performance.
[0055] Comparative Examples 1-4
[0056] Meanwhile, based on Example 1, the stainless steel formula and production process were changed as a comparative example to further demonstrate the advantages of the present invention.
[0057] The compositions of the soft magnetic stainless steel wire rods of Comparative Examples 1-4 are shown in Table 4 below:
[0058] Table 4. Schematic diagram of the composition of stainless steel wire rods in Example 1 and Comparative Examples 1-4.
[0059]
[0060] The performance of the stainless steel samples in each comparative example was tested, and the test results and effects are shown in Table 5 below:
[0061] Table 5. Summary of performance tests of stainless steel wire rods in Examples 1 and Comparative Examples 1-4
[0062]
[0063]
[0064] Based on the preparation method steps of Example 1, the specific process parameters and implementation effect test descriptions for each comparative example are shown in Table 6 below:
[0065] Table 6 Summary of Stainless Steel Wire Rod Production Process and Effect Tests in Examples 1 and Comparative Examples 1-4
[0066]
[0067]
[0068] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the present invention in any way. Other variations and modifications may be made without departing from the technical solutions described in the claims.
Claims
1. A soft magnetic stainless steel wire rod possessing ultra-high corrosion resistance, good machinability, and excellent ductility and toughness, characterized in that, The chemical composition of the wire rod, by mass percentage, includes: C ≤ 0.020%, Si: 1.20–2.00%, Mn ≤ 0.50%, Cr: 18.0–20.0%, Ni: ≤ 0.30%, Mo: 2.50–3.00%, N ≤ 0.020%, P < 0.020%, S: 0.008–0.015%, Se: 0.030–0.050%, Nb: 0.20–0.30%, with the balance being Fe and unavoidable impurities; the preparation method of the soft magnetic stainless steel wire rod includes sequentially smelting the furnace charge in an electric arc furnace, refining it in an AOD furnace, and refining it in an LF refining furnace. The process involves ingot casting, ingot blanking, primary heat treatment, rolling, and secondary heat treatment to obtain soft magnetic stainless steel wire rods with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness. In the ingot casting process, 17-20 inch ingot molds are used for casting. The primary heat treatment annealing temperature is 680-720℃, with a holding time of 4-6 hours. During rolling, the final rolling temperature is controlled to be ≤850℃. The secondary heat treatment annealing temperature is 800-880℃, with a time controlled to be at least 60 minutes. The soft magnetic stainless steel exhibits rust-free performance after ≥1000 hours of salt spray testing, saturation magnetic induction intensity ≥1.5T, coercivity ≤250A / m, and grain size finer than grade 4.
2. The soft magnetic stainless steel wire rod with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness according to claim 1, characterized in that, The chemical composition of the wire rod, by mass percentage, includes: C: 0.010–0.020%, Si: 1.6–1.7%, Mn: 0.2–0.4%, Cr: 18.50–19.00%, Ni: 0.1–0.3%, Mo: 2.55–2.65%, N: 0.010–0.020%, P < 0.020%, S: 0.008–0.015%, Se: 0.030–0.050%, Nb: 0.20–0.30%, with the balance being Fe and unavoidable impurities.
3. A method for preparing a soft magnetic stainless steel with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness as described in claim 1 or 2, characterized in that, The preparation method includes sequentially processing the furnace charge in an electric arc furnace, refining it in an AOD furnace, refining it in an LF furnace, casting it in a die, billeting it into steel ingots, performing a first heat treatment, rolling it, and performing a second heat treatment to obtain soft magnetic stainless steel wire rods with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness. In the die casting process, 17-20 inch steel ingot molds are used for casting. The annealing temperature for the first heat treatment is 680-720℃, and the holding time is 4-6 hours. During rolling, the final rolling temperature is controlled to be ≤850℃. The annealing temperature for the second heat treatment is 800-880℃, and the time is controlled to be more than 60 minutes.
4. The method for preparing a soft magnetic stainless steel with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness according to claim 3, characterized in that, In the refining process of the LF refining furnace, ferroniobium is added, and S-line and Se-line are fed in to control the composition of the molten steel to be: S: 0.008~0.015%, Se: 0.030~0.050%, Nb: 0.20~0.30%.
5. The method for preparing a soft magnetic stainless steel with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness according to claim 3, characterized in that, During the die casting process, the ladle temperature is controlled at 1500–1530℃.
6. The method for preparing a soft magnetic stainless steel with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness according to claim 3, characterized in that, In the steel ingot billeting process, the steel ingot is loaded into a heating furnace and heated to a temperature of 1100-1150℃ for 1.5-2.5 hours.
7. The method for preparing a soft magnetic stainless steel with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness according to claim 3, characterized in that, In the rolling process, the billet after annealing is loaded into a heating furnace and heated to 950-1000℃ for 1-2 hours.
8. The method for preparing a soft magnetic stainless steel with ultra-high corrosion resistance, good machinability, and excellent ductility and toughness according to claim 3, characterized in that, The specifications for rolled wire rods are φ5.5~30mm.
Citation Information
Patent Citations
High-corrosion-resistance super-free-cutting soft magnetic ferrite stainless steel wire rod and preparation method thereof