Environment-friendly phase change energy storage type light thermal insulation mortar and preparation method thereof
By using particle-grade expanded perlite loaded paraffin in phase change energy storage materials and encapsulated with polymer shell, the phase separation and paraffin leakage problems of phase change energy storage materials under low temperature conditions were solved, and an environmentally friendly phase change energy storage lightweight insulation mortar with excellent frost resistance, mechanical properties and thermal properties was prepared.
Patent Information
- Application Number
- CN202510506298.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-22
- Publication Date
- 2025-07-25
- Estimated Expiration
- 2045-04-22
AI Technical Summary
Existing phase change energy storage materials are prone to phase separation or supercooling under low temperature conditions, which affects the use effect and has the risk of paraffin leakage, which may cause environmental pollution.
The particle-grade expanded perlite loaded with paraffin, and the phase change energy storage material is encapsulated using polymer shells, combined with raw materials such as aluminate cement, vitrified microbeads and boron nitride powder, an environmentally friendly phase change energy storage lightweight insulation mortar with low leakage rate is prepared.
It significantly reduces the leakage rate of paraffin, improves the thermal stability and compressive strength of the material, enhances the insulation effect, and is suitable for long-term use.
Smart Images

Figure BDA0005369884550000121
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermal insulation mortar, and in particular to an environmentally friendly phase change energy storage lightweight thermal insulation mortar and a preparation method thereof. Background Art
[0002] In the field of building thermal insulation, with the continuous improvement of people's requirements for energy conservation and environmental protection, the development of high-performance thermal insulation materials is crucial. Traditional thermal insulation materials have some deficiencies, such as limited thermal insulation performance and no energy storage function. Phase change energy storage materials can absorb and release heat within a certain temperature range, which can effectively regulate the indoor temperature fluctuation. However, when used alone, there are problems such as poor stability and easy leakage. Combining it with thermal insulation mortar to make a phase change energy storage lightweight thermal insulation mortar is expected to overcome the shortcomings of traditional materials and achieve good thermal insulation and energy storage effects, with broad application prospects.
[0003] Chinese Patent with Application No. 202010387914.3 discloses a phase change thermal insulation mortar and a preparation method thereof. This method uses natural inorganic porous materials to load hydrated salt phase change materials to form a hydrated salt-porous carrier composite. This composite is wrapped and dehydrated by water-soluble silicon or water glass to obtain a phase change energy storage material coated with hydrogel. Mixing this material with thermal insulation mortar realizes the effective isolation of the hydrated salt phase change material from the mortar and maintains its good heat storage and release performance. At the same time, the multi-layer hydrogel coating prevents the leakage and migration of hydrated salts during mixing and application, thus ensuring its effective application in thermal insulation mortar. However, under low-temperature conditions, hydrated salt substances such as calcium nitrate hexahydrate are prone to phase separation or supercooling phenomena, resulting in a decrease in latent heat and affecting the use effect. In addition, nitrate substances such as manganese nitrate hexahydrate will penetrate into the soil or water body, causing eutrophication or heavy metal pollution, which will have an adverse impact on the environment. Chinese Patent with Application No. 202010768144.7 discloses a phase change thermal insulation cement mortar material. The main body of this material is a cement mortar layer, and a waterproof glue layer is coated on the outside. The cement mortar layer is composed of 10-25% phase change composite material, 30-50% fine aggregate, and 25-40% cementitious material. This invention optimizes the ratio of the phase change composite material to the building mortar, tests the actual performance of the paraffin / SiO2 material to improve its deficiencies, and systematically sorts out and analyzes the preparation, technical indicators, and use effects of the paraffin / SiO2 phase change material to determine the best mixing ratio to achieve the best thermal insulation effect on the premise of ensuring the structural strength. However, in this invention, the paraffin and SiO2 are mainly physically coated, and the free SiO2 particles will reduce the structural stability of the material, and paraffin leakage problems may occur during long-term use, affecting the material performance.
[0004] Therefore, the development of a lightweight thermal insulation mortar with excellent frost resistance, mechanical properties, and thermal properties has become an urgent need in the industry. Summary of the Invention
[0005] To solve the above problems, the present invention provides an environmentally friendly phase change energy storage lightweight thermal insulation mortar and a preparation method thereof. First, expanded perlite with particle grading is used to load paraffin, and then a shell material is prepared by monomer polymerization reaction. A phase change energy storage material with a low leakage rate is prepared by coating the shell material on the phase change material. The environmentally friendly phase change energy storage lightweight thermal insulation mortar with excellent frost resistance, mechanical properties and thermal properties is obtained by compounding the phase change energy storage material with raw materials such as aluminate cement and vitrified microspheres.
[0006] The technical solution adopted by the present invention to achieve the above object is as follows:
[0007] An environmentally friendly phase change energy storage lightweight thermal insulation mortar, comprising the following raw materials in parts by weight: 160 - 190 parts of aluminate cement, 50 - 70 parts of vitrified microspheres, 12 - 18 parts of phase change energy storage material, 4 - 6 parts of boron nitride powder, 60 - 80 parts of auxiliary cementitious material, 2 - 3 parts of fiber reinforcing material, 0.5 - 1 part of retarder, 0.1 - 1 part of defoamer;
[0008] The preparation method of the phase change energy storage material is as follows:
[0009] Step S1: Mix molten paraffin with pretreated expanded perlite evenly, and vacuum impregnate for 20 - 30 min to obtain a primary phase change material;
[0010] Step S2: Add nano - silica and silane coupling agent KH - 550 to anhydrous ethanol and stir evenly, then add the primary phase change material, vacuum impregnate for 0.5 - 1.5 h, restore to normal pressure and dry, then add paraffin and vacuum impregnate for 30 - 40 min to obtain an intermediate phase change material;
[0011] Step S3: Add methyl methacrylate monomer and acrylic acid monomer to deionized water and mix evenly, then add the intermediate phase change material and sodium dodecyl sulfate, perform high - speed homogenization treatment for 10 - 15 min, then add ammonium persulfate, stir for 4 - 6 h under a nitrogen atmosphere at 70 - 80 °C, cool to room temperature, centrifuge, wash and dry to obtain the product.
[0012] Furthermore, in step S1, the mass ratio of the molten paraffin to the pretreated expanded perlite is 1:2 - 3, and the weight - fraction ratio of the expanded perlite according to particle grading is 100 mesh:120 - 300 mesh:325 mesh = 2:4 - 6:2 - 4.
[0013] Furthermore, in step S2, the mass ratio of the nano - silica, silane coupling agent KH - 550 and the primary phase change material is 0.1 - 0.2:0.01 - 0.03:1, and the addition amount of nano - silica in anhydrous ethanol is 0.1 - 0.15 g / mL.
[0014] Further, in step S3, the mass ratio of methyl methacrylate monomer, acrylic acid monomer, ammonium persulfate, sodium dodecyl sulfate, and the intermediate phase change material is 1:0.25 - 1:0.01 - 0.05:0.02 - 0.03:1 - 2, and the addition amount of methyl methacrylate monomer in deionized water is 0.1 - 0.2 g / mL.
[0015] Further, the fiber reinforcement material is one or more of basalt fiber, polypropylene fiber, glass fiber, and polyvinyl alcohol fiber.
[0016] Further, the retarder is one or more of tartaric acid, borax, sodium gluconate, and calcium lignosulfonate.
[0017] Further, the supplementary cementitious material is one or more of metakaolin, desulfurized gypsum, and redispersible latex powder.
[0018] Further, the defoamer is a polyether defoamer or a silicone defoamer.
[0019] The present invention also provides a preparation method of an environmentally friendly phase change energy storage lightweight thermal insulation mortar, comprising the following steps:
[0020] (1) Stir aluminate cement, boron nitride powder, supplementary cementitious material, fiber reinforcement material, retarder, and defoamer for 3 - 5 min to obtain a mixture.
[0021] (2) Add the phase change energy storage material and expanded perlite beads to the mixture obtained in step (1) and stir for 3 - 5 min to obtain the product.
[0022] The present invention has the following beneficial effects:
[0023] The present invention prepares a phase change energy storage material by combining the adsorption of expanded perlite loaded with paraffin with the encapsulation of a polymer shell layer, and then the phase change energy storage material is compounded with raw materials such as aluminate cement, vitrified microspheres, boron nitride powder, auxiliary cementitious materials, and fiber reinforcing materials. By optimizing the ratio and preparation process, an environmentally friendly phase change energy storage type lightweight thermal insulation mortar with excellent comprehensive performance is prepared. The dual effects of physical adsorption of paraffin by particle-sized expanded perlite and encapsulation of the polymer shell layer significantly reduce the leakage rate of paraffin. This dual effect not only improves the thermal stability of paraffin but also enhances the application effect of paraffin in building insulation. Using particle-sized expanded perlite to load paraffin and introducing nano-silica into the phase change material improves the compressive strength of the thermal insulation mortar. The porous structure of expanded perlite can disperse stress and prevent the expansion of cracks, while the particle grading of different particle sizes can form a more compact packing structure, effectively improving the compressive strength of the thermal insulation mortar. The shell layer structure formed by polymerizing methyl methacrylate monomer and acrylic monomer can also significantly improve the frost resistance of the thermal insulation mortar. In addition, by loading paraffin with particle-sized expanded perlite and the encapsulation of the polymer shell layer, the leakage rate of the phase change material paraffin is reduced, thereby increasing the phase change latent heat of the environmentally friendly phase change energy storage type lightweight thermal insulation mortar. The specific heat capacity of the environmentally friendly phase change energy storage type lightweight thermal insulation mortar is enhanced by the high heat capacity of lightweight aggregates such as vitrified microspheres and the energy storage effect of the phase change material paraffin. The thermal conductivity of the environmentally friendly phase change energy storage type lightweight thermal insulation mortar is reduced by the porous structure of particle-sized expanded perlite and the low thermal conductivity of boron nitride powder.
[0024] The present invention selects raw materials such as paraffin, expanded perlite, and nano-silica, adjusts the ratio, and then uses preparation processes such as vacuum impregnation method, nano-modification treatment, and cross-linking polymerization reaction to prepare a phase change energy storage material with a low leakage rate. Then, it is compounded with raw materials such as aluminate cement, vitrified microspheres, and boron nitride powder to prepare an environmentally friendly phase change energy storage type lightweight thermal insulation mortar. This environmentally friendly phase change energy storage type lightweight thermal insulation mortar has excellent compressive strength, frost resistance, phase change latent heat, specific heat capacity, and thermal conductivity performance, and also greatly reduces the leakage rate of the phase change material paraffin. These characteristics make the mortar have broad application prospects in the field of building energy conservation. Specific Embodiments
[0025] Next, the technical solutions in the embodiments of the present application will be clearly and completely described in conjunction with the embodiments of the present application. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without creative efforts shall fall within the protection scope of the present application.
[0026] The raw materials used in the following examples are all ordinary commercially available products. The aluminate cement has a compressive strength of 55 MPa and is purchased from Zhengzhou Kanghui Refractory Co., Ltd.; the vitrified microspheres have a particle size of 30 mesh, a silicon content of 56-62%, and an aluminum content of 33-38%, and are purchased from Hebei Jiyan Mineral Products Co., Ltd.; the boron nitride powder has an active ingredient content of 99.9% and a particle size of 10 μm, and is purchased from Qinghe Ruijiang Metal Materials Co., Ltd.; the paraffin wax is 60# solid paraffin wax and is purchased from Shandong Zhuoxuan New Materials Co., Ltd.; the nano-silica has a model of PST-S05, a particle size of 20 nm, and an SiO2 content of 99%, and is purchased from Nanjing Baokete New Materials Co., Ltd.; the basalt fiber has a length of 6 mm, an active ingredient content of 90%, and a compressive strength of 1600 MPa, and is purchased from Tai'an Haosong Fiber Co., Ltd.; the polypropylene fiber has a length of 6 mm, an active ingredient content of 90%, and a breaking strength of ≥560 MPa, and is purchased from Tai'an Haosong Fiber Co., Ltd.; the glass fiber has a length of 3 mm, an active ingredient content of 90%, and a compressive strength of 1700 MPa, and is purchased from Tai'an Haosong Fiber Co., Ltd.; the polyvinyl alcohol fiber has a length of 6 mm, an active ingredient content of 98%, and a compressive strength of ≥1200 MPa, and is purchased from Tai'an Haosong Fiber Co., Ltd.; the borax is sodium borate decahydrate, with an active ingredient content of 99% and a density of 1.73 g / cm 3 , and is purchased from Guangdong Qiming Chemical Technology Co., Ltd.; the calcium lignosulfonate has an active ingredient content of 99% and a density of 0.5 g / cm 3 , and is purchased from Wuhan Jixin Yibang Biotechnology Co., Ltd.; the metakaolin has a silicon dioxide content of 70%, a particle size of 1250 mesh, and a water-soluble matter (W%) ≤ 0.5%, and is purchased from Hebei Jiegui Mineral Products Co., Ltd.; the desulfurized gypsum has a density of 2.3 g / cm 3 , a purity of 85%, and is from Shijiazhuang Lincheng Mineral Products Trading Co., Ltd.; the redispersible latex powder has an average particle size of 80 μm and a viscosity of ≥10.0 pas for a 50% aqueous solution, and is purchased from Chengdu Junxinpeng New Materials Technology Co., Ltd.; the polyether defoamer is the D-50 type polyether industrial defoamer purchased from Fujian Chilong Chemical Materials Co., Ltd., with an active ingredient content of 99%; the silicone defoamer is the FD-930 silicone defoamer purchased from Xiangyang Fuding Environmental Protection Technology Co., Ltd., with an active ingredient content of 99%; the expanded perlite, with a particle size of 325 mesh, is purchased from Puyang Xianda New Materials Co., Ltd., with an SiO2 content of 56.5%, the one with a particle size of 100 mesh is purchased from Shijiazhuang Jinli Mining Co., Ltd., with an SiO2 content of 78%, and the one with a particle size of 120-300 mesh is purchased from Xinyang Houpu Mining Co., Ltd., with an SiO2 content of 75%;
[0027] Example 1
[0028] An environmentally friendly phase change energy storage type lightweight thermal insulation mortar, comprising raw materials in the following parts by weight: 160 parts of aluminate cement, 50 parts of vitrified microspheres, 12 parts of phase change energy storage material, 4 parts of boron nitride powder, 60 parts of auxiliary cementitious material, 2 parts of fiber reinforcing material, 0.5 part of retarder, 0.1 part of defoamer, and 130 parts of deionized water;
[0029] Wherein the auxiliary cementitious material is metakaolin, the fiber reinforcing material is basalt fiber, the retarder is tartaric acid, and the defoamer is a polyether defoamer;
[0030] The preparation method of the phase change energy storage material is as follows:
[0031] Step S1: Mix molten paraffin with expanded perlite having a particle size grading after being dried at 105 °C for 4 h evenly, and then place it in a vacuum container under a vacuum of 0.05 - 0.1 MPa and at 70 °C for impregnation for 25 min. Open the vacuum valve to naturally restore to normal pressure and naturally cool to room temperature to obtain a primary phase change material. The mass ratio of molten paraffin to the pretreated expanded perlite with particle size grading is 1:2.5. The expanded perlite with particle size grading is composed of expanded perlite particles with different particle sizes, and the mass ratio is 100 mesh:120 - 300 mesh:325 mesh = 2:5:3;
[0032] Step S2: Add nano-silica and silane coupling agent KH-550 to anhydrous ethanol and stir evenly, then immerse it together with the primary phase change material in a vacuum container under a vacuum of 0.05 - 0.08 MPa for impregnation for 1 h. Open the vacuum valve to naturally restore to normal pressure, filter and vacuum dry to constant weight at 50 °C, and then add it together with molten paraffin to a vacuum container under a vacuum of 0.05 - 0.1 MPa and at 70 °C for impregnation for 35 min. Then open the vacuum valve to naturally restore to normal pressure and naturally cool to room temperature to obtain an intermediate phase change material. The mass ratio of nano-silica, silane coupling agent KH-550, and the primary phase change material is 0.15:0.02:1, and the addition amount of nano-silica in anhydrous ethanol is 0.12 g / mL;
[0033] Step S3: Add methyl methacrylate monomer and acrylic acid monomer into deionized water and mix evenly. Then add the intermediate phase change material and sodium dodecyl sulfate. Use a high-speed homogenizer to homogenize and disperse at a rotational speed of 9000 rpm for 13 minutes. Then add ammonium persulfate and stir under a nitrogen atmosphere at 75 °C and 400 rpm for 5 hours. Finally, cool naturally to room temperature, centrifuge three times at 2000 rpm for 5 minutes each time, then place in a vacuum drying oven at 80 °C and dry for 5 hours. Finally, perform ball milling. Select zirconia balls with large, medium, and small ball diameters of 10 mm, 5 mm, and 3 mm respectively, with a large, medium, and small ball ratio of 2:5:3, a rotational speed of 400 r / min, a ball-to-material ratio of 10:1, and a ball milling time of 10 h. Pass through a 200-mesh sieve to obtain the product. The mass ratio of methyl methacrylate monomer, acrylic acid monomer, ammonium persulfate, sodium dodecyl sulfate, and intermediate phase change material is 1:0.6:0.03:0.025:1.5, and the addition amount of methyl methacrylate monomer in deionized water is 0.15 g / mL.
[0034] The present invention also provides a preparation method for an environmentally friendly phase change energy storage lightweight thermal insulation mortar, comprising the following steps:
[0035] (1) Stir aluminate cement, boron nitride powder, auxiliary cementitious material, fiber reinforcing material, retarder, and defoamer at 100 rpm for 3 minutes to obtain a mixture;
[0036] (2) Add the phase change energy storage material and expanded perlite beads to the mixture obtained in step (1) and stir at a rotational speed of 100 rpm for 3 minutes to obtain the product.
[0037] Example 2
[0038] An environmentally friendly phase change energy storage lightweight thermal insulation mortar, comprising the following raw materials in parts by weight: 190 parts of aluminate cement, 70 parts of expanded perlite beads, 18 parts of phase change energy storage material, 6 parts of boron nitride powder, 80 parts of auxiliary cementitious material, 3 parts of fiber reinforcing material, 1 part of retarder, 1 part of defoamer, and 150 parts of deionized water;
[0039] The auxiliary cementitious material is desulfurized gypsum, the fiber reinforcing material is polypropylene fiber, the retarder is borax, and the defoamer is a polyether defoamer;
[0040] The preparation method of the phase change energy storage material is the same as that in the example;
[0041] The present invention also provides a preparation method for an environmentally friendly phase change energy storage lightweight thermal insulation mortar, comprising the following steps:
[0042] (1) Stir aluminate cement, boron nitride powder, auxiliary cementitious material, fiber reinforcing material, retarder, and defoamer at 100 rpm for 5 minutes to obtain a mixture;
[0043] (2) Add the phase change energy storage material and the vitrified microspheres to the mixture obtained in step (1), and stir at a speed of 100 rpm for 5 min to obtain the product.
[0044] Example 3
[0045] An environmentally friendly phase change energy storage type lightweight thermal insulation mortar, comprising the following raw materials in parts by weight: 180 parts of aluminate cement, 60 parts of vitrified microspheres, 15 parts of phase change energy storage material, 5 parts of boron nitride powder, 70 parts of auxiliary cementitious material, 2.5 parts of fiber reinforcing material, 0.8 part of retarder, 0.5 part of defoamer, and 140 parts of deionized water;
[0046] Among them, the auxiliary cementitious material is desulfurized gypsum, the fiber reinforcing material is glass fiber, the retarder is sodium gluconate, and the defoamer is an organosilicon defoamer;
[0047] Among them, the preparation method of the phase change energy storage material is the same as that of the example;
[0048] The present invention also provides a preparation method of an environmentally friendly phase change energy storage type lightweight thermal insulation mortar, comprising the following steps:
[0049] (1) Stir aluminate cement, boron nitride powder, auxiliary cementitious material, fiber reinforcing material, retarder, and defoamer at 100 rpm for 4 min to obtain a mixture;
[0050] (2) Add the phase change energy storage material and the vitrified microspheres to the mixture obtained in step (1), and stir at a speed of 100 rpm for 4 min to obtain the product.
[0051] Example 4
[0052] An environmentally friendly phase change energy storage type lightweight thermal insulation mortar, comprising the following raw materials in parts by weight: 180 parts of aluminate cement, 60 parts of vitrified microspheres, 15 parts of phase change energy storage material, 5 parts of boron nitride powder, 70 parts of auxiliary cementitious material, 2.5 parts of fiber reinforcing material, 0.8 part of retarder, 0.5 part of defoamer, and 140 parts of deionized water;
[0053] Among them, the auxiliary cementitious material is redispersible latex powder, the fiber reinforcing material is polyvinyl alcohol fiber, the retarder is calcium lignosulfonate, and the defoamer is a polyether defoamer;
[0054] The preparation method of the phase change energy storage material is as follows:
[0055] Step S1: Mix the molten paraffin wax evenly with the particle-sized expanded perlite that has been dried at 105°C for 4 h, and then place it in a vacuum container with a vacuum degree of 0.05 - 0.1 MPa and a temperature of 70°C for impregnation for 30 min. Open the vacuum valve to naturally restore to normal pressure and naturally cool to room temperature to obtain the primary phase change material. The mass ratio of the molten paraffin wax to the pretreated particle-sized expanded perlite is 1:3. The particle-sized expanded perlite is composed of expanded perlite particles with different particle sizes, and the mass ratio is 100 mesh: 120 - 300 mesh: 325 mesh = 2:6:4;
[0056] Step S2: Add nano-silica and silane coupling agent KH-550 to anhydrous ethanol and stir evenly. Then immerse it together with the primary phase change material in a vacuum container with a vacuum degree of 0.05 - 0.08 MPa for impregnation for 1.5 h. Open the vacuum valve to naturally restore to normal pressure, filter, and vacuum dry to constant weight at 50°C. Then add it together with the molten paraffin wax to a vacuum container with a vacuum degree of 0.05 - 0.1 MPa and a temperature of 70°C for impregnation for 40 min. Then open the vacuum valve to naturally restore to normal pressure, and after naturally cooling to room temperature, obtain the intermediate phase change material. The mass ratio of nano-silica, silane coupling agent KH-550, and the primary phase change material is 0.2:0.03:1, and the addition amount of nano-silica in anhydrous ethanol is 0.15 g / mL;
[0057] Step S3: Add methyl methacrylate monomer and acrylic acid monomer to deionized water and mix evenly. Then add the intermediate phase change material and sodium dodecyl sulfate, and use a high-speed homogenizer to homogenize and disperse at a rotation speed of 9000 rpm for 15 minutes. Then add ammonium persulfate and stir for 6 hours under a nitrogen atmosphere, at 80°C, and 400 rpm. Finally, naturally cool to room temperature, centrifuge three times at 2000 rpm for 10 min each time, then place it in a vacuum drying oven at 80°C for drying for 5 hours, and finally ball mill. Select zirconia balls, with the diameters of large, medium, and small balls being 10 mm, 5 mm, and 3 mm respectively, the ratio of large, medium, and small balls being 2:5:3, the rotation speed being 400 r / min, the ball-to-material ratio being 10:1, the ball milling time being 10 h, and pass through a 200-mesh sieve to obtain it. The mass ratio of methyl methacrylate monomer, acrylic acid monomer, ammonium persulfate, sodium dodecyl sulfate, and the intermediate phase change material is 1:1:0.05:0.03:2, and the addition amount of methyl methacrylate monomer in deionized water is 0.2 g / mL.
[0058] The present invention also provides a preparation method of an environmentally friendly phase change energy storage lightweight thermal insulation mortar, and the preparation method of this environmentally friendly phase change energy storage lightweight thermal insulation mortar is the same as that in Example 3.
[0059] Comparative Example 1
[0060] An environmentally friendly phase change energy storage type lightweight thermal insulation mortar, comprising raw materials in the following parts by weight: 150 parts of aluminate cement, 40 parts of vitrified microspheres, 10 parts of phase change energy storage material, 5 parts of boron nitride powder, 70 parts of auxiliary cementitious material, 1 part of fiber reinforcing material, 0.1 part of retarder, 1 part of defoamer, and 100 parts of deionized water;
[0061] Wherein the auxiliary cementitious material is desulfurized gypsum, the fiber reinforcing material is glass fiber, the retarder is sodium gluconate, and the defoamer is an organosilicon defoamer;
[0062] Step S1: Mix molten paraffin with expanded perlite of graded particles after drying treatment at 105°C for 4 hours, then place it in a vacuum container at a vacuum degree of 0.05 - 0.1 MPa and 70°C for impregnation for 10 minutes. Open the vacuum valve to naturally restore to normal pressure and naturally cool to room temperature to obtain a primary phase change material. The mass ratio of molten paraffin to pretreated graded expanded perlite is 1:1. The graded expanded perlite is composed of expanded perlite particles with different particle sizes, and the mass ratio is 100 mesh:120 - 300 mesh:325 mesh = 2:5:3;
[0063] Step S2: Add nano-silica and silane coupling agent KH-550 to anhydrous ethanol and stir evenly, then immerse it together with the primary phase change material in a vacuum container with a vacuum degree of 0.05 - 0.08 MPa for impregnation for 10 minutes. Open the vacuum valve to naturally restore to normal pressure, filter and vacuum dry to constant weight at 50°C, and then add it together with molten paraffin to a vacuum container at a vacuum degree of 0.05 - 0.1 MPa and 70°C for impregnation for 60 minutes. Then open the vacuum valve to naturally restore to normal pressure, and after naturally cooling to room temperature, obtain an intermediate phase change material. The mass ratio of nano-silica, silane coupling agent KH-550, and primary phase change material is 0.15:0.1:1, and the addition amount of nano-silica in anhydrous ethanol is 0.12 g / mL;
[0064] Step S3: Add methyl methacrylate monomer and acrylic acid monomer into deionized water and mix evenly. Then add the intermediate phase change material and sodium dodecyl sulfate. Use a high-speed homogenizer to homogenize and disperse at a rotation speed of 9000 rpm for 10 minutes. Then add ammonium persulfate and stir for 1 hour under a nitrogen atmosphere at 75 °C and 400 rpm. Finally, cool naturally to room temperature, centrifuge three times at 2000 rpm for 10 minutes each time, then place it in a vacuum drying oven at 80 °C and dry for 5 hours. Finally, ball mill it. Select zirconia balls, with the diameters of large, medium, and small balls being 10 mm, 5 mm, and 3 mm respectively, the ratio of large, medium, and small balls being 2:5:3, the rotation speed being 400 r / min, the ball-to-material ratio being 10:1, and the ball milling time being 10 h. Sieve through a 200-mesh sieve to obtain it. The mass ratio of methyl methacrylate monomer, acrylic acid monomer, ammonium persulfate, sodium dodecyl sulfate, and intermediate phase change material is 1:0.6:0.03:0.025:1.5, and the addition amount of methyl methacrylate monomer in deionized water is 0.15 g / mL.
[0065] The present invention also provides a preparation method of an environmentally friendly phase change energy storage type lightweight thermal insulation mortar, including the following steps:
[0066] (1) Stir aluminate cement, boron nitride powder, auxiliary cementitious material, fiber reinforcing material, retarder, and defoamer at 100 rpm for 1 minute to obtain a mixture.
[0067] (2) Add the phase change energy storage material and expanded perlite beads to the mixture obtained in step (1) and stir at a rotation speed of 100 rpm for 1 minute to obtain it.
[0068] Comparative Example 2
[0069] An environmentally friendly phase change energy storage type lightweight thermal insulation mortar, including the following raw materials in parts by weight: 180 parts of aluminate cement, 60 parts of expanded perlite beads, 15 parts of phase change energy storage material, 5 parts of boron nitride powder, 70 parts of auxiliary cementitious material, 2.5 parts of fiber reinforcing material, 0.8 part of retarder, 0.5 part of defoamer, and 140 parts of deionized water;
[0070] The auxiliary cementitious material is desulfurized gypsum, the fiber reinforcing material is glass fiber, the retarder is sodium gluconate, and the defoamer is an organosilicon defoamer;
[0071] The preparation method of the phase change energy storage material is as follows:
[0072] Step S1: Mix the molten paraffin wax evenly with the graded expanded perlite that has been dried at 105°C for 4 hours, and then place it in a vacuum container under a vacuum of 0.05 - 0.1 MPa and at 70°C for impregnation for 25 minutes. Open the vacuum valve to naturally return to normal pressure and cool naturally to room temperature to obtain the primary phase change material. The mass ratio of the molten paraffin wax to the pre-treated graded expanded perlite is 1:2.5. The graded expanded perlite consists of expanded perlite particles with different particle sizes, and the mass ratio is 100 mesh:120 - 300 mesh:325 mesh = 2:5:3;
[0073] Step S2: Add nano-silica and silane coupling agent KH-550 to anhydrous ethanol and stir evenly, then immerse it together with the primary phase change material in a vacuum container under a vacuum of 0.05 - 0.08 MPa for impregnation for 1 hour. Open the vacuum valve to naturally return to normal pressure, filter and vacuum dry at 50°C until constant weight, and then add it together with the molten paraffin wax to a vacuum container under a vacuum of 0.05 - 0.1 MPa and at 70°C for impregnation for 35 minutes. Then open the vacuum valve to naturally return to normal pressure, and cool naturally to room temperature to obtain the phase change energy storage material. The mass ratio of nano-silica, silane coupling agent KH-550, and the primary phase change material is 0.15:0.02:1, and the addition amount of nano-silica in anhydrous ethanol is 0.12 g / mL.
[0074] The present invention also provides a preparation method of an environmentally friendly phase change energy storage type lightweight thermal insulation mortar, including the following steps:
[0075] (1) Stir aluminous cement, boron nitride powder, auxiliary cementitious material, fiber reinforcing material, retarder, and defoamer at 100 rpm for 4 minutes to obtain a mixture;
[0076] (2) Add the phase change energy storage material and vitrified microspheres to the mixture obtained in step (1) and stir at a speed of 100 rpm for 4 minutes to obtain the product.
[0077] Comparative Example 3
[0078] An environmentally friendly phase change energy storage type lightweight thermal insulation mortar, including the following raw materials in parts by weight: 180 parts of aluminous cement, 60 parts of vitrified microspheres, 15 parts of phase change energy storage material, 5 parts of boron nitride powder, 70 parts of auxiliary cementitious material, 2.5 parts of fiber reinforcing material, 0.8 part of retarder, 0.5 part of defoamer, and 140 parts of deionized water;
[0079] Among them, the auxiliary cementitious material is desulfurized gypsum, the fiber reinforcing material is glass fiber, the retarder is sodium gluconate, and the defoamer is an organosilicon defoamer;
[0080] The preparation method of the phase change energy storage material is as follows: The molten paraffin is mixed evenly with the graded expanded perlite that has been dried at 105°C for 4 hours, and then placed in a vacuum container at a vacuum degree of 0.05 - 0.1 MPa and a temperature of 70°C for impregnation for 25 minutes. Then, the vacuum valve is opened to naturally return to normal pressure, and it is naturally cooled to room temperature to obtain the phase change energy storage material. The mass ratio of the molten paraffin to the pretreated graded expanded perlite is 1:2.5. The graded expanded perlite is composed of expanded perlite particles with different particle sizes, and the mass ratio is 100 mesh:120 - 300 mesh:325 mesh = 2:5:3.
[0081] The present invention also provides a preparation method of an environmentally friendly phase change energy storage type lightweight thermal insulation mortar, which includes the following steps:
[0082] (1) Mix aluminate cement, boron nitride powder, auxiliary cementitious material, fiber reinforcing material, retarder, and defoaming agent at 100 rpm for 4 minutes to obtain a mixture.
[0083] (2) Add the phase change energy storage material and vitrified microspheres to the mixture obtained in step (1) and stir at a speed of 100 rpm for 4 minutes to obtain the product.
[0084] The environmentally friendly phase change energy storage type lightweight thermal insulation mortar prepared in Examples 1 - 4 and Comparative Examples 1 - 3 is stirred with water for 2 minutes to prepare a mixture with a consistency of (50 ± 5) mm. The test method for consistency is carried out in accordance with the provisions of JGJ / T 70 - 2009 "Standard for Test Methods of Basic Properties of Building Mortars", and then it is cured under standard conditions for 28 days and dried to a constant weight at (105 ± 5)°C to prepare the sample sizes required for testing respectively.
[0085] The leakage rate test is to place a sample of 50mm×50mm×20mm in a thermostatic and humid cabinet at 60°C and a relative humidity of 90% for 20 minutes, then lower the temperature to 20°C and the relative humidity to 50% and keep it for 20 minutes, which is one cycle. Repeat this cycle 100 times. Then put the sample into a high-temperature furnace, heat it up to 80°C, keep it for 2 hours, weigh the change in the mass of the sample before and after, and calculate the leakage rate of the material. The leakage rate = (m1 - m2) / m1, where m1 is the mass of the sample before the leakage rate test and m2 is the mass of the sample after the leakage rate test; The compressive strength test is carried out in accordance with the provisions of GB / T 5486-2008 "Test Methods for Inorganic Rigid Thermal Insulation Products" based on GB / T 20473-2021 "Building Thermal Insulation Mortar". 6 specimens are required for each example and comparative example, and the final result is the arithmetic mean of the test values of the 6 specimens; The frost resistance test is carried out in accordance with the requirements in JGJ / T70-2009 "Standard for Test Methods of Basic Properties of Building Mortars", and the compressive strength after the freeze-thaw test is tested; The thermal performance test, including latent heat of phase change and specific heat capacity, is carried out in accordance with the requirements in JC / T 2111-2012 "Test Methods for Phase Change and Temperature Regulation Performance of Building Materials"; The thermal conductivity test is carried out in accordance with the provisions of GB / T10297-2015 "Hot Wire Method for Determining Thermal Conductivity of Non-Metallic Solid Materials" based on GB / T 20473-2021 "Building Thermal Insulation Mortar".
[0086] As can be seen from Table 1 for the specific test data.
[0087] Table 1 Performance Test Results
[0088]
[0089] It can be seen from the performance test data in Table 1 that the environmentally friendly phase change energy storage lightweight thermal insulation mortar prepared in Examples 1-4 is significantly superior to Comparative Examples 1-3 in terms of various performance indicators. The performance of the environmentally friendly phase change energy storage lightweight thermal insulation mortar prepared in Examples 1-4 is better than that of Comparative Example 1, which indicates that the raw material ratio and preparation conditions set in the present invention have obvious advantages. The compressive strength of the environmentally friendly phase change energy storage lightweight thermal insulation mortar prepared in Examples 1-4 is more excellent than that prepared in Comparative Examples 2-3. One of the reasons is that when preparing the phase change energy storage material, graded expanded perlite is used to load paraffin. Expanded perlite itself has a rich pore structure, and graded expanded perlite has a particle distribution with different particle sizes, which can form a more compact packing structure in the material system, provide a skeleton support for the material, enhance the overall mechanical properties of the phase change material, and thus improve the compressive strength of the mortar. Another reason is that the particle size of nano-silica is much smaller than the pore size of expanded perlite, and it can fill into the tiny pores of expanded perlite and the gaps between paraffin and expanded perlite. This filling effect makes the internal structure of the material more dense, reduces pore defects, and improves the density of the material. In the thermal insulation mortar, the densification of the phase change energy storage material structure helps to enhance the overall compressive strength of the mortar, making it less likely to be damaged when subjected to external forces.
[0090] The leakage rate of the thermal insulation mortar prepared in Examples 1-4 is also relatively low, indicating that the thermal insulation effect of this thermal insulation mortar is relatively stable and suitable for long-term use. On the one hand, the low leakage rate of the thermal insulation mortar prepared by this invention is because by loading paraffin on graded expanded perlite, the physical adsorption and encapsulation effects of expanded perlite are utilized to effectively limit the fluidity and migration of paraffin. On the other hand, it is because in the subsequent preparation process of the phase change energy storage material, a shell layer is prepared by the polymerization reaction of monomers to encapsulate the phase change material that has been loaded onto graded expanded perlite, forming a dense protective layer. Paraffin originally has a risk of leaking from the pores of expanded perlite, but after being encapsulated by the polymer shell layer, the leakage path is blocked, greatly limiting its outward migration, thereby reducing the leakage rate. Through the dual effects of porous material loading and shell layer encapsulation, synergistic effects are achieved, significantly reducing the leakage rate of paraffin. The adsorption of the porous material provides initial adsorption and fixation ability, while the shell layer encapsulation further blocks the leakage path by forming a dense protective layer. This synergistic effect not only reduces the leakage rate of the phase change material, but also enhances the application effect of the thermal insulation mortar in building thermal insulation. Compared with Example 2, Comparative Example 2 reduces the step of shell layer encapsulation. It can be seen from the data of Example 2 and Comparative Example 2 that the leakage rate of the thermal insulation mortar is greatly reduced, indicating that the encapsulation effect of the shell layer has a good anti-leakage effect. And Comparative Example 3 reduces the steps of loading paraffin on expanded perlite and shell layer encapsulation, and the leakage rate is significantly lower than the data obtained in Example 2, indicating that the adsorption effect of graded expanded perlite loaded with paraffin can also effectively reduce the leakage rate of the mortar.
[0091] The frost resistance of the environmentally friendly phase-change energy storage lightweight thermal insulation mortar prepared in Example 1 is also significantly better than that of Comparative Example 2, which lacks the shell encapsulation step. When used in a low-temperature environment, the water in the mortar will freeze and expand in volume, generating a large ice crystal expansion stress, which is one of the main reasons for the destruction of the mortar structure and the reduction of frost resistance. The shell structure formed by the polymerization of methyl methacrylate monomer and acrylic acid monomer has certain strength and elasticity. When the water freezes and expands, the shell layer can rely on its own mechanical properties to support and restrain the internal paraffin and expanded perlite. The shell layer can act like an elastic "protective cover" to buffer the stress generated by the expansion of ice crystals and avoid stress concentration from damaging the internal structure of the mortar, thereby maintaining the integrity of the mortar structure and improving its frost resistance.
[0092] The key thermal properties such as phase change latent heat, specific heat capacity and thermal conductivity of the environmentally friendly phase change energy storage lightweight thermal insulation mortar prepared in Examples 1-4 are greatly superior to those of Comparative Examples 2-3. Paraffin is a typical phase change material that can absorb and release a large amount of heat during its melting and solidification process and has a high phase change latent heat. Adding paraffin to the thermal insulation mortar can absorb and release heat within a certain temperature range, effectively adjust indoor temperature fluctuations, and reduce heat transfer. The synergistic effect of the load of the particle-graded expanded perlite and the shell encapsulation reduces the risk of paraffin leakage, improves the stability of paraffin, and can improve its effective utilization rate in the thermal insulation mortar, thereby improving the phase change latent heat of the thermal insulation mortar. Through the introduction of nano-silicon dioxide and the encapsulation of the polymer shell layer, the thermal stability of the phase change material is significantly improved, and this thermal stability enables the phase change material to maintain structural stability over a wide temperature range, thereby improving the specific heat capacity of the thermal insulation mortar. Boron nitride powder is a highly efficient thermal insulation material. Its low thermal conductivity and high thermal stability can significantly reduce the thermal conductivity of thermal insulation mortar. Boron nitride powder is evenly distributed in thermal insulation mortar to form a thermal insulation network, effectively blocking the transfer of heat. The particle-graded expanded perlite in the phase change energy storage material also has a low thermal conductivity and is a good thermal insulation material. After loading paraffin, the paraffin fills the pores of the expanded perlite, further reducing the heat conduction caused by air convection.
[0093] Although the embodiments of the present application have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. An environmentally friendly phase change energy storage type lightweight thermal insulation mortar, characterized in that, It includes the following raw materials in parts by weight: 160 - 190 parts of aluminate cement, 50 - 70 parts of vitrified microspheres, 12 - 18 parts of phase change energy storage material, 4 - 6 parts of boron nitride powder, 60 - 80 parts of auxiliary cementitious material, 2 - 3 parts of fiber reinforcing material, 0.5 - 1 part of retarder, and 0.1 - 1 part of defoamer; The preparation method of the phase change energy storage material is as follows: Step S1: Mix molten paraffin with pretreated expanded perlite evenly, and carry out vacuum impregnation for 20 - 30 min to obtain a primary phase change material; Step S2: Add nano - silica and silane coupling agent KH - 550 into anhydrous ethanol and stir evenly, then add the primary phase change material, carry out vacuum impregnation for 0.5 - 1.5 h, dry after restoring to normal pressure, then add paraffin, and carry out vacuum impregnation for 30 - 40 min to obtain an intermediate phase change material; Step S3: Add methyl methacrylate monomer and acrylic acid monomer into deionized water and mix evenly, then add the intermediate phase change material and sodium dodecyl sulfate, disperse for 10 - 15 min, then add ammonium persulfate, stir for 4 - 6 h under the condition of nitrogen atmosphere and 70 - 80 °C, cool to room temperature, carry out centrifugal washing and drying to obtain the product.
2. The environmentally friendly phase change energy storage type lightweight thermal insulation mortar according to claim 1, characterized in that, In step S1, the mass ratio of the molten paraffin to the pretreated expanded perlite is 1:2 - 3, and the weight - fraction ratio of the expanded perlite according to particle size distribution is 100 mesh:120 - 300 mesh:325 mesh = 2:4 - 6:2 - 4.
3. The environmentally friendly phase change energy storage type lightweight thermal insulation mortar according to claim 1, wherein In step S2, the mass ratio of the nano - silica, silane coupling agent KH - 550, and the primary phase change material is 0.1 - 0.2:0.01 - 0.03:1, and the addition amount of nano - silica in anhydrous ethanol is 0.1 - 0.15 g / mL.
4. The environmentally friendly phase change energy storage type lightweight thermal insulation mortar according to claim 1, characterized in that In step S3, the mass ratio of the methyl methacrylate monomer, acrylic acid monomer, ammonium persulfate, sodium dodecyl sulfate, and the intermediate phase change material is 1:0.25 - 1:0.01 - 0.05:0.02 - 0.03:1 - 2, and the addition amount of the methyl methacrylate monomer in deionized water is 0.1 - 0.2 g / mL.
5. The environmentally friendly phase change energy storage type lightweight thermal insulation mortar according to claim 1, wherein The fiber reinforcing material is one or more of basalt fiber, polypropylene fiber, glass fiber, and polyvinyl alcohol fiber.
6. The environmentally friendly phase change energy storage type lightweight thermal insulation mortar according to claim 1, characterized in that, The retarder is one or more of tartaric acid, borax, sodium gluconate, and calcium lignosulfonate.
Citation Information
Patent Citations
A phase change thermal insulation cement mortar material
CN111689725B
A phase change thermal insulation mortar and its preparation method
CN113173740B
Phase change thermal insulation mortar and preparation method thereof
CN113173740A
Phase-change energy-storage plastering mortar and preparation method thereof
CN115724630A
Low-temperature early-strength cement paste system based on cellulose-based composite phase change material
CN119410345A