Silver-coated copper composite material and preparation method thereof, conductive paste and solar cell

By setting an intermediate layer containing nickel or cobalt and phosphorus between the copper core and the silver layer, the problem of insufficient conductivity and high temperature resistance of traditional silver-clad copper powder is solved, and low-cost application in the field of solar cells is achieved.

CN120388777APending Publication Date: 2025-07-29GUANGDONG SHENGYANG HUACHUANG TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510853738.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-24
Publication Date
2025-07-29

AI Technical Summary

Technical Problem

The conductivity and high temperature resistance of traditional silver-clad copper powder are poor, and the use of precious metal silver is high, which limits its large-scale application in the field of solar cells.

Method used

An intermediate layer is arranged between the copper core and the silver layer. The intermediate layer contains main metal elements such as nickel or cobalt and phosphorus elements. By controlling the doping content of the phosphorus element, the bonding force between the intermediate layer and the copper core and the silver layer is enhanced, preventing the mutual diffusion between silver and copper, and improving anti-oxidation performance.

Benefits of technology

While ensuring electrical conductivity, the anti-oxidation temperature and thermal stability of silver-clad copper composite materials are improved, the use of precious metal silver is reduced, and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120388777A_ABST
    Figure CN120388777A_ABST
Patent Text Reader

Abstract

The invention relates to a silver-coated copper composite material and a preparation method thereof, conductive paste and a solar cell. The silver-coated copper composite material comprises a copper core, a middle layer and a silver layer, the middle layer is arranged on the surface of the copper core, the silver layer is arranged on the surface, away from the copper core, of the middle layer, the middle layer comprises main metal elements and phosphorus elements, the main metal elements comprise at least one of nickel elements and cobalt elements, and the mass of the phosphorus elements accounts for 1%-4% of the total mass of the middle layer. By arranging the middle layer between the copper core and the silver layer, mutual diffusion between silver and copper can be effectively prevented, and the problem that traditional silver-coated copper powder is prone to oxidation is solved; according to the silver-coated copper composite material, the middle layer containing proper metal elements is doped with the phosphorus element, meanwhile, the doping content of the phosphorus element is controlled, the binding force between the middle layer and the copper core and the binding force between the middle layer and the silver layer can be effectively improved, the conductivity is guaranteed, meanwhile, the anti-oxidation temperature of the silver-coated copper composite material is effectively increased, and the thermal stability of the silver-coated copper composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a silver-coated copper composite material and a preparation method thereof, a conductive paste and a solar cell. Background Art

[0002] Silver powder is a common conductive filler in electronic pastes due to its high conductivity and chemical stability. However, the high price of silver has limited the large-scale application of pure silver-based conductive pastes in solar cells. Copper is inexpensive and has a similar conductivity to silver, but it easily oxidizes during preparation and use, forming cupric oxide or cuprous oxide, which affects conductivity. To address this problem, silver is plated on the surface of copper powder to create a core-shell structure of silver-coated copper powder, which prevents copper oxidation and significantly reduces costs. However, traditional silver-coated copper powder has poor high-temperature resistance.

[0003] Therefore, it is necessary to improve the traditional technology. Summary of the Invention

[0004] Based on this, the present application provides a silver-coated copper composite material having both good electrical conductivity and good high-temperature resistance, a preparation method thereof, a conductive paste, and a solar cell.

[0005] The technical solution of this application to solve the above technical problems is as follows.

[0006] In a first aspect, the present application provides a silver-clad copper composite material, comprising a copper core, an intermediate layer and a silver layer, wherein the intermediate layer is arranged on the surface of the copper core, and the silver layer is arranged on the surface of the intermediate layer away from the copper core. The intermediate layer comprises a main metal element and a phosphorus element, wherein the main metal element comprises at least one of nickel and cobalt, and the mass of the phosphorus element accounts for 1% to 5% of the total mass of the intermediate layer.

[0007] In some embodiments, in the silver-clad copper composite material, the mass of the intermediate layer accounts for 0.5% to 2% of the total mass of the intermediate layer and the copper core.

[0008] In some embodiments, in the silver-clad copper composite material, the copper core has voids, and the voids are filled with silver.

[0009] In some embodiments, the silver-clad copper composite material satisfies at least one of the following characteristics:

[0010] (1) The mass of the silver element accounts for 0.1% to 1% of the total mass of the copper core;

[0011] (2) The total mass proportion of silver element in the silver-clad copper composite material is 3% to 15%.

[0012] In some of these embodiments, in the silver-coated copper composite material, the average particle size of the silver-coated copper composite material is 3.5 μm to 6.5 μm.

[0013] The second aspect of the present application provides a method for preparing a silver-coated copper composite material, comprising the following steps:

[0014] Perform a first reduction reaction on the copper core and the main metal precursor solution to form an intermediate layer on the surface of the copper core to prepare an intermediate; the main metal precursor solution includes a main metal source and a first reducing agent, the main metal source includes at least one of a nickel source and a cobalt source, the first reducing agent includes a phosphorus element, and the concentration of the first reducing agent in the main metal precursor solution is 100 g / L to 500 g / L;

[0015] Perform a second reduction reaction on the intermediate, the first silver precursor solution and the second reducing agent to form a silver layer on the surface of the intermediate layer away from the copper core.

[0016] In some of these embodiments, in the method for preparing a silver-coated copper composite material, the preparation method satisfies at least one of the following characteristics:

[0017] (1) The first reducing agent includes sodium hypophosphite;

[0018] (2) The nickel source includes nickel sulfate hexahydrate;

[0019] (3) The cobalt source includes at least one of cobalt nitrate hexahydrate, cobalt chloride hexahydrate and cobalt sulfate heptahydrate;

[0020] (4) The concentration of the main metal source is 300 g / L to 500 g / L;

[0021] (5) The main metal precursor solution includes a wetting agent, the wetting agent includes dodecylbenzenesulfonic acid, and the concentration of the wetting agent is 5 g / L to 10 g / L;

[0022] (6) The temperature of the first reduction reaction is 60°C to 80°C;

[0023] (7) The first silver precursor solution includes a silver source and a complexing agent, the silver source includes silver nitrate, and the complexing agent includes at least one of ethylenediaminetetraacetic acid, sodium ethylenediaminetetraacetate, potassium sodium tartrate and sodium citrate;

[0024] (8) The second reducing agent includes at least one of sodium hypophosphite, sodium borohydride, ascorbic acid, glucose and potassium sodium tartrate;

[0025] (9) The reaction solution of the second reduction reaction includes a dispersant, and the dispersant includes at least one of polyvinyl pyrrolidone, OP-10, Triton-100, sodium dodecylsulfonate, and sodium dodecylbenzenesulfonate.

[0026] In some embodiments, in the method for preparing the silver-coated copper composite material, the preparation of the copper core comprises the following steps:

[0027] The copper powder and the second silver precursor solution are subjected to a replacement reaction to replace part of the copper atoms in the copper powder with silver elements to prepare copper cores.

[0028] The third aspect of the present application provides a conductive paste, comprising the silver-clad copper composite material provided in the first aspect or the silver-clad copper composite material prepared by the preparation method of the silver-clad copper composite material provided in the second aspect.

[0029] The fourth aspect of the present application provides a solar cell, comprising the silver-coated copper composite material provided in the first aspect, the silver-coated copper composite material prepared by the preparation method of the silver-coated copper composite material provided in the second aspect, or an electrode formed using the conductive paste provided in the third aspect.

[0030] The silver-clad copper composite material of the present application includes a copper core, an intermediate layer and a silver layer. By arranging the intermediate layer between the copper core and the silver layer, the mutual diffusion between silver and copper can be effectively prevented, thereby solving the problem of easy oxidation of traditional silver-clad copper powder. In addition, phosphorus is doped into the intermediate layer containing suitable metal elements, and the doping content of phosphorus is controlled at the same time, which can effectively improve the bonding strength between the intermediate layer and the copper core and the silver layer. While ensuring conductivity, the oxidation resistance temperature of the silver-clad copper composite material is effectively increased, thereby improving the thermal stability of the silver-clad copper composite material.

[0031] The silver-clad copper composite material of the present application reduces the usage of precious metal silver, which is beneficial to reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0033] Figure 1 A scanning electron microscope image of a nickel-copper-phosphorus intermediate provided in one embodiment;

[0034] Figure 2 A surface scanning elemental analysis diagram of a nickel-copper-phosphorus intermediate provided in one embodiment;

[0035] Figure 3Test result graph of the mass proportion of phosphorus in the nickel-copper-phosphorus intermediate provided for an embodiment. Specific embodiments

[0036] The present application will be further described in detail below in combination with embodiments and examples. It should be understood that these embodiments and examples are only used to illustrate the present application and not to limit the scope of the present application. The purpose of providing these embodiments and examples is to make the understanding of the disclosed content of the present application more thorough and comprehensive.

[0037] It should also be understood that the present application can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various changes or modifications without departing from the connotation of the present application, and the equivalent forms obtained also fall within the protection scope of the present application. For example, features described or illustrated as part of one embodiment can be combined in a suitable manner with another embodiment to produce a new embodiment. In addition, in the following description, a large number of specific details are given to provide a more thorough understanding of the present application. It should be understood that the present application can be implemented without one or more of these details.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the technical field to which this application belongs. The terms used in the description of the present application herein are only for the purpose of describing embodiments and examples and are not intended to limit the present application.

[0039] Unless otherwise stated or there is a contradiction, the terms or phrases used herein have the following meanings:

[0040] In the present application, the terms "a plurality of", "a variety of", "multiple times", etc., unless otherwise specified, mean greater than 2 or equal to 2 in quantity. For example, "one or more" means one or greater than or equal to two.

[0041] As used herein, "combinations thereof", "any combinations thereof", "any combination manners thereof", etc. include all suitable combination manners of any two or more of the listed items.

[0042] In this document, the "suitable" in "suitable combination manners", "suitable manners", "any suitable manners", etc. is subject to being able to implement the technical solution of the present application, solve the technical problems of the present application, and achieve the expected technical effects of the present application.

[0043] In this text, "preferred", "better", "more preferred", and "preferably" are only used to describe embodiments or examples with better effects. It should be understood that they do not constitute a limitation on the protection scope of this application. If "preferred" appears multiple times in a technical solution, without special instructions and without contradictions or mutual restrictions, each "preferred" is independent of each other.

[0044] In this application, "further", "even further", "especially", etc. are used for descriptive purposes, indicating differences in content, but should not be construed as a limitation on the protection scope of this application.

[0045] In this application, "optionally", "optional", and "option" mean that it can be either present or absent, that is, it refers to any one of two alternative options: "present" or "absent". If "optional" appears multiple times in a technical solution, without special instructions and without contradictions or mutual restrictions, each "optional" is independent of each other.

[0046] In this application, in "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are only used for descriptive purposes and cannot be construed as indicating or implying relative importance or quantity, nor can it be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive listing and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0047] In this application, for technical features described in an open-ended manner, it includes a closed technical solution composed of the listed features, as well as an open technical solution containing the listed features.

[0048] In this application, when it comes to a numerical interval (i.e., a numerical range), without special instructions, the distribution of the optional numerical values within this numerical interval is considered continuous, and it includes the two numerical endpoints of this numerical interval (i.e., the minimum value and the maximum value), as well as each numerical value between these two numerical endpoints. Without special instructions, when the numerical interval only refers to the integers within this numerical interval, it includes the two endpoint integers of this numerical range, as well as each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all sub-ranges subsumed therein. The "numerical value" in this numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. The "numerical interval" allows for a broad inclusion of numerical interval types such as percentage intervals, ratio intervals, and ratio value intervals.

[0049] Unless otherwise specified, the temperature parameters in this application allow for both constant temperature treatment and temperature fluctuations within a certain temperature range. It should be understood that the constant temperature treatment allows for temperature fluctuations within the accuracy range of instrument control. Fluctuations within ranges such as ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are permitted.

[0050] In this application, the term "room temperature" or "normal temperature" generally refers to 4°C to 35°C, for example, 20°C ± 5°C. In some embodiments of this application, "room temperature" or "normal temperature" refers to 10°C to 30°C. In some embodiments of this application, "room temperature" or "normal temperature" refers to 20°C to 30°C.

[0051] In this application, when referring to a range of units, if the unit is only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 3~5h means that the units of the left endpoint "3" and the right endpoint "5" are both hours.

[0052] All documents mentioned in this application are cited as references in this application, just as each document is cited as a reference individually. Unless they conflict with the invention purpose and / or technical solution of this application, the cited documents involved in this application are cited in their entirety and for all purposes. When cited documents are involved in this application, the definitions of relevant technical features, terms, nouns, phrases, etc. in the cited documents are also cited. When cited documents are involved in this application, the examples and preferred embodiments of the cited relevant technical features may also be incorporated into this application as references, but are limited to the ability to implement this application. It should be understood that when the cited content conflicts with the description in this application, the present application shall prevail or be adaptively amended according to the description in this application.

[0053] The mass or weight of the relevant components mentioned in the examples of this application may not only refer to the specific content of each component, but also represent the proportional relationship of the mass or weight of each component. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the examples of this application, it is within the scope disclosed in the examples of this application. Specifically, the mass or weight described in the examples of this application may be units known in the chemical industry such as μg, mg, g, and kg.

[0054] One embodiment of the present application provides a silver-clad copper composite material, including a copper core, an intermediate layer and a silver layer, the intermediate layer is arranged on the surface of the copper core, the silver layer is arranged on the surface of the intermediate layer away from the copper core, the copper core has a gap, the gap is filled with silver, the intermediate layer includes a main metal element and a phosphorus element, the main metal element includes at least one of nickel and cobalt, and the mass of the phosphorus element accounts for 1% to 5% of the total mass of the intermediate layer.

[0055] By setting an intermediate layer between the copper core and the silver layer, the mutual diffusion between silver and copper can be effectively prevented, solving the problem of easy oxidation of traditional silver-coated copper powder; and by doping phosphorus elements in the intermediate layer containing suitable metal elements and controlling the doping content of phosphorus elements, the bonding strength between the intermediate layer and the copper core and the silver layer can be effectively improved. While ensuring conductivity, the oxidation resistance temperature of the silver-coated copper composite material is effectively increased, thereby improving the thermal stability of the silver-coated copper composite material.

[0056] The silver-clad copper composite material of the present application reduces the usage of precious metal silver, which is beneficial to reducing costs.

[0057] It can be understood that the intermediate layer includes a nickel-phosphorus layer, a cobalt-phosphorus layer or a nickel-cobalt-phosphorus alloy layer.

[0058] It can be understood that the percentage of the mass of the phosphorus element to the total mass of the intermediate layer includes but is not limited to 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, and 5%; in some examples, it can be within the range consisting of any two of these point values as end values, the same below; for example, the mass of the phosphorus element accounts for 1%~2%, 2%~5%, 2%~4%, 2%~3% of the total mass of the intermediate layer, etc.

[0059] In some of these examples, in silver-clad copper composites, the mass of the intermediate layer accounts for 0.5% to 2% of the total mass of the intermediate layer and the copper core.

[0060] It can be understood that the percentage of the mass of the intermediate layer to the total mass of the intermediate layer and the copper core includes but is not limited to 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, and 2%; for example, the mass of the intermediate layer accounts for 0.8%~1.5% of the total mass of the intermediate layer and the copper core.

[0061] In some examples, the silver-coated copper composite material has a copper core with voids filled with elemental silver.

[0062] In some examples, the mass of silver in the silver-clad copper composite material accounts for 0.1%~1% of the total mass of the copper core.

[0063] It can be understood that the total mass of the copper core includes the mass of the silver element; further, the percentage of the mass of the silver element to the total mass of the copper core includes but is not limited to 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, and 1.0%; for example, the mass of the silver element accounts for 0.2%~0.8% of the total mass of the copper core.

[0064] In some of these examples, in the silver-clad copper composite material, the total mass proportion of the silver element in the silver-clad copper composite material is 3%~15%.

[0065] It can be understood that the total mass proportion of silver elements in the silver-clad copper composite material includes but is not limited to 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, and 15%. For example, the total mass proportion of silver elements in the silver-clad copper composite material is 3%~10%, 5%~15%.

[0066] By controlling the total mass proportion of silver elements in the silver-clad copper composite material, the conductivity is guaranteed on the basis of reducing the silver usage rate. The copper core, intermediate layer and silver layer cooperate with each other to effectively improve the oxidation resistance temperature of the silver-clad copper composite material while ensuring conductivity and conversion efficiency.

[0067] In some of the examples, in the silver-clad copper composite material, the average particle size of the silver-clad copper composite material is 3.5 μm to 6.5 μm.

[0068] Traditional methods for preparing silver-coated copper powder mainly include the replacement method and the reduction method. The replacement method uses copper powder as a reducing agent. The copper powder surface loses electrons to form copper ions that enter the solution, and the silver ions gain electrons to form silver particles that are deposited on the copper powder surface. When the thickness of the surface silver layer reaches a certain level, the reaction basically stops, resulting in a thin silver layer and loose coating. The reduction method adds a reducing agent to the reaction system, prompting the silver ions to gain electrons to form silver particles that are deposited on the copper powder surface. The copper powder only serves as a substrate and does not participate in the reaction. The reduction method can obtain a thicker silver layer, but the coating uniformity is insufficient. Regardless of whether it is the replacement method or the reduction method, silver and copper metals easily diffuse into each other, and copper easily migrates to the surface of the silver layer, resulting in oxidation discoloration and affecting the conductivity of the silver-coated copper powder.

[0069] One embodiment of the present application provides a method for preparing a silver-clad copper composite material, comprising the following steps:

[0070] Step S100: subjecting the copper core and the bulk metal precursor solution to a first reduction reaction to form an intermediate layer on the surface of the copper core to prepare an intermediate; the bulk metal precursor solution includes a bulk metal source and a first reducing agent, the bulk metal source includes a nickel source and a cobalt source, the first reducing agent includes phosphorus, and the concentration of the first reducing agent in the bulk metal precursor solution is 100 g / L~500 g / L.

[0071] It can be understood that the intermediate prepared in step S100 includes a copper core and an intermediate layer disposed on the surface of the copper core. The intermediate layer includes a main metal element and a doped phosphorus element. The percentage of the mass of the doped phosphorus element in the total mass of the intermediate layer is controlled by controlling the concentration of the first reducing agent in the nickel precursor solution. By controlling the percentage of the mass of the doped phosphorus element in the total mass of the intermediate layer, the bonding strength between the intermediate layer and the copper core and the silver layer can be effectively improved. While ensuring conductivity and conversion efficiency, the oxidation resistance temperature of the silver-clad copper composite material is effectively increased, thereby improving the reliability of the silver-clad copper composite material. Furthermore, the concentration of the first reducing agent in the main metal precursor solution includes, but is not limited to, 100 g / L, 200 g / L, 300 g / L, 400 g / L, and 500 g / L.

[0072] In some examples, in step S100 , the first reducing agent includes sodium hypophosphite.

[0073] In some examples, in step S100 , the cobalt source includes at least one of cobalt nitrate hexahydrate, cobalt chloride hexahydrate, and cobalt sulfate heptahydrate.

[0074] In some examples, in step S100 , the nickel source includes nickel sulfate hexahydrate.

[0075] In some examples, in step S100 , the concentration of the host metal source in the host metal precursor solution is 300 g / L to 500 g / L.

[0076] By controlling the concentration of the bulk metal source in the bulk metal precursor solution, the density of the intermediate layer can be effectively improved. It is understood that the concentration of the bulk metal source includes, but is not limited to, 300 g / L, 400 g / L, and 500 g / L. Furthermore, the nickel content in the intermediate layer can be controlled by controlling the concentration of the bulk metal source in the bulk metal precursor solution and the reaction time.

[0077] In some examples, in step S100, the bulk metal precursor solution includes a wetting agent. Furthermore, the wetting agent includes dodecylbenzenesulfonic acid. Furthermore, the concentration of the wetting agent in the bulk metal precursor solution is 5 g / L to 10 g / L. It is understood that the concentration of the wetting agent includes, but is not limited to, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 9 g / L, and 10 g / L.

[0078] In some examples, in step S100, the temperature of the first reduction reaction is 60°C to 80°C. Furthermore, the first reduction reaction lasts for 5 minutes to 10 minutes. It is understood that the temperature of the first reduction reaction includes, but is not limited to, 60°C, 70°C, and 80°C. Furthermore, the first reduction reaction lasts for, but is not limited to, 5 minutes, 8 minutes, and 10 minutes.

[0079] In some examples, in step S100, the preparation of the copper core includes:

[0080] Step S110 : performing a replacement reaction between the copper powder and the second silver precursor solution to replace a portion of the copper atoms in the copper powder with silver atoms to prepare copper cores.

[0081] By performing a replacement reaction between the copper powder and the second silver precursor solution, some of the copper atoms in the copper powder are replaced with silver elements with a dotted structure, providing catalytic sites for the first reduction reaction in step S100, thereby promoting the bonding force between the formed intermediate layer and the copper core, effectively improving the oxidation resistance temperature of the silver-clad copper composite material, and improving the reliability of the silver-clad copper composite material.

[0082] In some examples, in step S110, the second silver precursor solution includes a silver source and a complexing agent. Furthermore, the silver source includes silver nitrate. Furthermore, the complexing agent includes at least one of ethylenediaminetetraacetic acid, ethylenediaminetetraacetic acid sodium salt, potassium sodium tartrate, and sodium citrate. It is understood that ethylenediaminetetraacetic acid sodium salt includes but is not limited to at least one of ethylenediaminetetraacetic acid disodium salt and ethylenediaminetetraacetic acid trisodium salt. Furthermore, the mass ratio of the silver source to the copper powder is 0.1-0.5:10-50; further, the mass ratio of the complexing agent to the silver source is 1-10:0.1-0.5.

[0083] In some examples, in step S110, the reaction solution of the displacement reaction includes a dispersant. Furthermore, the dispersant includes at least one of polyvinyl pyrrolidone, OP-10, Triton-100, sodium dodecyl sulfate, and sodium dodecylbenzenesulfonate. Furthermore, the mass ratio of the dispersant to the copper powder is 0.1-0.5: 0.1-0.5.

[0084] In some examples, in step S110 , the temperature of the replacement reaction is 30° C. to 50° C., and the time is 10 min to 30 min.

[0085] In some examples, step S110 includes the following steps:

[0086] The copper powder, dispersant and water are stirred evenly to form a mixed solution A;

[0087] Stir the silver source, complexing agent and water to form a mixed solution B;

[0088] Mixture B is slowly added dropwise to the stirred mixture A to carry out a replacement reaction.

[0089] It can be understood that the copper core obtained in step S110 has gaps, and the gaps are filled with silver.

[0090] In some of these examples, before the displacement reaction in step S110, it includes:

[0091] Step S120: Activate the copper powder with an acid solution.

[0092] Optionally, in step S120, the acid solution includes sulfuric acid.

[0093] Optionally, in step S120, the mass concentration of the acid solution is 1% - 10%.

[0094] Optionally, in step S120, in the activation treatment, the mass ratio of the copper powder to the volume of the acid solution is (10 - 100) g : (100 - 1000) mL.

[0095] In some of these examples, step S120 includes the following steps:

[0096] Mix the copper powder, dispersant and acid solution and stir, filter and wash them in sequence.

[0097] Optionally, in step S120, the dispersant includes at least one of polyvinylpyrrolidone, OP - 10, Triton - 100, sodium dodecyl sulfate and sodium dodecylbenzenesulfonate. Further, the mass ratio of the dispersant to the copper powder is 0.1 - 1 : 10 - 100.

[0098] Optionally, in step S120, the stirring temperature is 20°C - 40°C and the time is 10 min - 30 min.

[0099] Step S200: Perform a second reduction reaction on the intermediate, the first silver precursor solution and the second reducing agent to form a silver layer on the surface of the intermediate layer far from the copper core.

[0100] For the method for preparing the silver - coated copper composite material provided by this application, by performing a first reduction reaction on the copper core and the main metal precursor solution and controlling the concentration of the first reducing agent in the nickel precursor solution, an appropriate doping amount of a phosphorus - containing intermediate layer can be formed on the surface of the copper core, and the bonding force between the intermediate layer, the copper core and the silver layer is relatively good; then performing a second reduction reaction on the intermediate, the first silver precursor solution and the second reducing agent to form a silver layer on the surface of the intermediate layer far from the copper core, while ensuring the conductivity and conversion efficiency, effectively improving the oxidation - resistant temperature of the silver - coated copper composite material and enhancing the thermal stability of the silver - coated copper composite material.

[0101] In some of these examples, in step S200, the second reducing agent includes at least one of sodium hypophosphite, sodium borohydride, ascorbic acid, glucose and sodium potassium tartrate. Further, the mass ratio of the dispersant to the intermediate is 0.2 - 2 : 10 - 30.

[0102] In some of these examples, in step S200, the first silver precursor solution includes a silver source and a complexing agent. Further, the silver source includes silver nitrate. Further, the complexing agent includes at least one of ethylenediaminetetraacetic acid, sodium ethylenediaminetetraacetate, potassium sodium tartrate, and sodium citrate. It can be understood that the sodium ethylenediaminetetraacetate includes but is not limited to at least one of disodium ethylenediaminetetraacetate and trisodium ethylenediaminetetraacetate. Further, the mass ratio of the silver source to the intermediate is 1-3:10-30; further, the mass ratio of the complexing agent to the silver source is 5-10:1-3.

[0103] In some of these examples, in step S200, the reaction solution of the second reduction reaction includes a dispersant. Further, the dispersant includes at least one of polyvinylpyrrolidone, OP-10, Triton-100, sodium dodecyl sulfonate, and sodium dodecylbenzenesulfonate. Further, the mass ratio of the dispersant to the intermediate is 0.1-0.5:10-30.

[0104] In some of these examples, in step S200, the temperature of the second reduction is 30°C to 50°C, and the time is 10 min to 30 min.

[0105] In some of these examples, step S200 includes the following steps:

[0106] Stir the intermediate, the second reducing agent, the dispersant, and water evenly to form a mixed solution C;

[0107] Stir the silver source, the complexing agent, and water evenly to form a mixed solution D;

[0108] Slowly drip the mixed solution D into the stirred mixed solution C for the second reduction reaction.

[0109] One embodiment of the present application provides an application of the above silver-coated copper composite material or the silver-coated copper composite material prepared by the above method for preparing a silver-coated copper composite material in the preparation of a conductive paste or a solar cell.

[0110] One embodiment of the present application provides a conductive paste, including the above silver-coated copper composite material or the silver-coated copper composite material prepared by the above method for preparing a silver-coated copper composite material.

[0111] The conductive paste provided by the present application, including the above silver-coated copper composite material or the silver-coated copper composite material prepared by the above method for preparing a silver-coated copper composite material, has good thermal stability.

[0112] One embodiment of the present application provides a solar cell, including the above silver-coated copper composite material, the silver-coated copper composite material prepared by the above method for preparing a silver-coated copper composite material, or an electrode formed by using the above conductive paste.

[0113] In some of these examples, the solar cell includes, but is not limited to, perovskite cells and crystalline silicon cells, and the crystalline silicon cells include, but are not limited to, at least one of PERC cells (passivated emitter and rear cell), HJT cells (heterojunction cell), and TOPCon cells (tunnel oxide passivated contact cell).

[0114] Among them, low-temperature conductive paste is required for the front and back sides of the HJT solar panel. The silver-coated copper composite material provided by this application and the silver-coated copper composite material prepared by the above-mentioned preparation method of the silver-coated copper composite material are particularly suitable for use in low-temperature conductive paste.

[0115] One embodiment of this application provides a photovoltaic module, including the above-mentioned solar cell.

[0116] One embodiment of this application provides an electrical device, including the above-mentioned solar cell or the above-mentioned photovoltaic module.

[0117] The following further describes this application in detail in conjunction with specific embodiments, but the embodiments of this application are not limited thereto.

[0118] Example 1

[0119] (1) Weigh 50 g of copper powder and 0.1 g of dispersant (polyvinylpyrrolidone), pour them into a beaker containing 500 ml of sulfuric acid solution with a mass fraction of 1%, stir for 10 min at a temperature of 30 °C, and obtain activated copper powder through filtration and washing.

[0120] (2) Weigh 30 g of the activated copper powder obtained in step (1), 0.1 g of dispersant (polyvinylpyrrolidone), and 500 ml of deionized water in sequence, pour them into a three-necked beaker with a stirrer, stir and mix evenly to form a solid-liquid mixture A. Weigh 0.1 g of silver nitrate, 5 g of complexing agent (sodium potassium tartrate), and 50 ml of deionized water, pour them into a beaker, stir and mix to form solution B. Slowly drip solution B into the stirring solid-liquid mixture A for reaction for 20 min, and obtain a copper core with a silver mass content of 0.2% through filtration and washing.

[0121] (3) Weigh 30 g of the silver core prepared in step (2), pour it into an electroless nickel plating bath with a stirrer for electroless nickel plating (the first reduction reaction), and obtain 30.3 g of nickel-copper-phosphorus intermediate through filtration and washing to form a nickel-phosphorus intermediate layer on the surface of the copper core; among them, the formula for electroless nickel plating is: nickel sulfate hexahydrate 400 g / L, sodium hypophosphite 300 g / L, sodium dodecylbenzenesulfonate 5 g / L; the temperature of the first reduction reaction is 70 °C and the time is 2 min; the mass ratio of the nickel-phosphorus intermediate layer in the nickel-copper-phosphorus intermediate is 1%, and the mass ratio of phosphorus in the nickel-phosphorus intermediate layer is 2.21%.

[0122] Among them, the mass percentage of the nickel-phosphorus intermediate layer in the nickel-copper-phosphorus intermediate = (the mass of the nickel-copper-phosphorus intermediate - the mass of the silver core) / the mass of the nickel-copper-phosphorus intermediate × 100%; The scanning electron microscope image of the nickel-copper-phosphorus intermediate is as shown in Figure 1 shown, and the surface scanning elemental analysis diagram of the nickel-copper-phosphorus intermediate is as shown in Figure 2 shown. The result diagram of the mass percentage of phosphorus in the nickel-phosphorus intermediate layer measured by X-ray fluorescence method (XRF) is as shown in Figure 3 shown.

[0123] (4) Weigh 0.1 g of dispersant (polyvinylpyrrolidone), 1 g of reducing agent (glucose), 20 g of the nickel-copper-phosphorus intermediate prepared in step (3), and 500 ml of deionized water in sequence, pour them into a three-necked beaker with a stirrer, and stir and mix evenly to form a solid-liquid mixture C. Weigh 1 g of silver nitrate, 5 g of complexing agent (sodium potassium tartrate), and 50 ml of deionized water, pour them into the beaker, and stir and mix to form solution D. Solution D is slowly added dropwise to the solid-liquid mixture C under stirring for reaction. The reaction time is 10 min. After filtration and washing, a silver-coated copper composite material with an average particle size of 3.5 μm is obtained, and the mass percentage of silver in the silver-coated copper composite material is 3%.

[0124] Example 2

[0125] It is basically the same as Example 1, except that in step (3), the chemical nickel plating formula is: nickel sulfate hexahydrate 400 g / L, sodium hypophosphite 500 g / L, sodium dodecylbenzenesulfonate 5 g / L; The mass percentage of phosphorus in the nickel-copper-phosphorus intermediate prepared in step (3) is 4.57%.

[0126] Example 3

[0127] It is basically the same as Example 1, except that in step (3), the chemical nickel plating formula is: nickel sulfate hexahydrate 400 g / L, sodium hypophosphite 400 g / L, sodium dodecylbenzenesulfonate 5 g / L; The mass percentage of phosphorus in the nickel-copper-phosphorus intermediate prepared in step (3) is 3.13%.

[0128] Example 4

[0129] It is basically the same as Example 1, except that in step (4), solution D includes 3 g of silver nitrate, 15 g of complexing agent, and 100 ml of deionized water, and the mass percentage of silver in the prepared silver-coated copper composite material is 10%.

[0130] Comparative Example 1

[0131] Prepare the solid-liquid mixture A according to the steps of Example 1 (2); Weigh 10 g of silver nitrate, 20 g of complexing agent (sodium potassium tartrate), and 50 ml of deionized water, pour them into a beaker, stir and mix to form solution B. Slowly add solution B dropwise to the solid-liquid mixture A under stirring for reaction. The reaction time is 20 min. After filtration and washing, silver-coated copper powder with a silver mass content of 20% is obtained.

[0132] Comparative Example 2

[0133] Weigh 0.1 g of dispersant (polyvinylpyrrolidone), 1 g of reducing agent (glucose), 50 g of copper powder activated in step (1), and 500 ml of deionized water in sequence, pour them into a three-necked beaker with a stirrer, stir and mix evenly to form a solid-liquid mixture C. Weigh 15 g of silver nitrate, 20 g of complexing agent (sodium potassium tartrate), and 50 ml of deionized water, pour them into a beaker, stir and mix to form solution D. Slowly add solution D dropwise to the solid-liquid mixture C under stirring for reaction. The reaction time is 10 min. After filtration and washing, silver-coated copper powder with a silver mass content of 25% is obtained.

[0134] Comparative Example 3

[0135] It is basically the same as Example 1, except that the chemical nickel plating formula is: nickel sulfate hexahydrate 400 g / L, hydrazine hydrate 500 g / L, sodium dodecylbenzenesulfonate 5 g / L; the mass ratio of phosphorus in the nickel-copper-phosphorus intermediate prepared in step (3) is 0%.

[0136] Comparative Example 4

[0137] It is basically the same as Example 1, except that in step (3), the chemical nickel plating formula is: nickel sulfate hexahydrate 400 g / L, sodium hypophosphite 800 g / L, sodium dodecylbenzenesulfonate 5 g / L; the mass ratio of phosphorus in the nickel-phosphorus intermediate layer prepared in step (3) is 8.58%.

[0138] Resistivity test: The composite materials prepared in each example and comparative example are formulated into slurries with a solid content of 90% using the same resin system. After being processed by a homogenizer and a three-roll mill, they are screen-printed into circuits, baked at 200 °C and cooled to room temperature, and the resistance is tested using the four-probe method. The line width, line length, and line width are measured respectively, and the resistivity is calculated using the bulk resistivity formula ρ = R * L / S;

[0139] Antioxidant temperature test: The TGA method is used to measure the oxidation weight gain of the samples. The sample weights are 5 mg respectively, and the temperature at which the weight gain starts is recorded, which is the antioxidant temperature.

[0140] The results are shown in Table 1.

[0141] Table 1

[0142]

[0143] As can be seen from Table 1, compared with Comparative Examples 1-2 of the traditional technology, the oxidation resistance temperature of the silver-coated copper composites prepared in each embodiment is significantly increased, the thermal stability performance is significantly improved, the resistivity is reduced, and the conductivity is improved; there is no intermediate layer in Comparative Example 1 and Comparative Example 2, and the oxidation resistance is insufficient, resulting in silver-copper migration and an increase in resistivity; the intermediate layer in Comparative Example 2 does not contain phosphorus, the oxidation resistance is insufficient, and the bonding force between the nickel layer and the copper layer will decrease, generating gaps and resulting in an increase in resistivity. The difference between Comparative Example 3 and Example 1 is only that a nickel-phosphorus-free reducing agent is used for nickel plating, so that the prepared nickel-copper-phosphorus intermediate does not contain phosphorus elements, its oxidation resistance is insufficient, and the bonding force between the intermediate layer and the copper core will decrease, generating gaps and resulting in an increase in resistivity; the concentration of the phosphorus-containing reducing agent in the electroless nickel plating formula of Comparative Example 4 is too high, and the mass proportion of phosphorus in the nickel-phosphorus intermediate layer is relatively high, resulting in too high resistivity and significantly reduced conductivity.

[0144] The technical features of the above-described embodiments can be combined arbitrarily. For the sake of brevity of description, not all possible combinations of the technical features in the above embodiments are described. However, as long as these combinations of technical features do not conflict, they should be considered to be within the scope described in this specification.

[0145] The above-described embodiments only represent several implementation manners of the present application, which are convenient for understanding the technical solutions of the present application specifically and in detail, but should not be construed as a limitation on the protection scope of the invention patent. It should be noted that for those of ordinary skill in the art, without departing from the concept of the present application, several deformations and improvements can be made, and these all belong to the protection scope of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments based on the technical solutions provided in the present application are all within the protection scope of the appended claims of the present application. Therefore, the protection scope of the patent of the present application should be subject to the content of the appended claims, and the specification can be used to explain the content of the claims.

Claims

1. A silver-coated copper composite material, characterized in that, The invention comprises a copper core, an intermediate layer and a silver layer, wherein the intermediate layer is arranged on the surface of the copper core, and the silver layer is arranged on the surface of the intermediate layer away from the copper core. The intermediate layer comprises a main metal element and a phosphorus element, wherein the main metal element comprises at least one of nickel and cobalt, and the mass of the phosphorus element accounts for 1% to 5% of the total mass of the intermediate layer.

2. The silver-coated copper composite material according to claim 1, characterized in that, The mass of the intermediate layer accounts for 0.5% to 2% of the total mass of the intermediate layer and the copper core.

3. The silver-coated copper composite material according to claim 1, wherein The copper core has voids, and the voids are filled with simple silver.

4. The silver-coated copper composite material according to claim 3, wherein The silver-clad copper composite material meets at least one of the following characteristics: (1) The mass of the silver element accounts for 0.1% to 1% of the total mass of the copper core; (2) The total mass proportion of silver element in the silver-clad copper composite material is 3% to 15%.

5. The silver-coated copper composite material according to any one of claims 1 to 4, characterized in that, The average particle size of the silver-coated copper composite material is 3.5 μm to 6.5 μm.

6. A preparation method of a silver-coated copper composite material, characterized in that, The following steps are involved: performing a first reduction reaction on a copper core and a bulk metal precursor solution to form an intermediate layer on a surface of the copper core to prepare an intermediate; the bulk metal precursor solution comprises a bulk metal source and a first reducing agent, the bulk metal source comprises at least one of a nickel source and a cobalt source, the first reducing agent comprises phosphorus, and the concentration of the first reducing agent in the bulk metal precursor solution is 100 g / L to 500 g / L; The intermediate, the first silver precursor solution and the second reducing agent are subjected to a second reduction reaction to form a silver layer on a surface of the intermediate layer away from the copper core.

7. The preparation method of the copper-coated silver composite material according to claim 6, characterized in that, The preparation method satisfies at least one of the following characteristics: (1) The first reducing agent includes sodium hypophosphite; (2) The nickel source includes nickel sulfate hexahydrate; (3) The cobalt source includes at least one of cobalt nitrate hexahydrate, cobalt chloride hexahydrate, and cobalt sulfate heptahydrate; (4) The concentration of the main metal source is 300 g / L to 500 g / L; (5) The main metal precursor solution includes a wetting agent, the wetting agent includes dodecylbenzenesulfonic acid, and the concentration of the wetting agent is 5 g / L to 10 g / L; (6) The temperature of the first reduction reaction is 60°C to 80°C; (7) The first silver precursor solution includes a silver source and a complexing agent, wherein the silver source includes silver nitrate, and the complexing agent includes at least one of ethylenediaminetetraacetic acid, ethylenediaminetetraacetic acid sodium salt, potassium sodium tartrate, and sodium citrate; (8) the second reducing agent comprises at least one of sodium hypophosphite, sodium borohydride, ascorbic acid, glucose and potassium sodium tartrate; (9) The reaction solution of the second reduction reaction includes a dispersant, and the dispersant includes at least one of polyvinyl pyrrolidone, OP-10, Triton-100, sodium dodecylsulfonate, and sodium dodecylbenzenesulfonate.

8. The preparation method of the copper-coated silver composite material according to any one of claims 6 to 7, characterized in that, The preparation of the copper core comprises the following steps: The copper powder and the second silver precursor solution are subjected to a replacement reaction to replace part of the copper atoms in the copper powder with silver elements to prepare copper cores.

9. A conductive paste, characterized in that, The invention comprises the silver-clad copper composite material according to any one of claims 1 to 5 or the silver-clad copper composite material prepared by the preparation method of the silver-clad copper composite material according to any one of claims 6 to 8.

10. A solar cell, characterized in that, Comprising a silver-coated copper composite material as described in any one of claims 1 to 5, a silver-coated copper composite material prepared by the preparation method of the silver-coated copper composite material as described in any one of claims 6 to 8, or an electrode formed by using the conductive paste as described in claim 9.

Citation Information