Research and development method of ultraviolet light absorber with novel structure
Through the synthesis of new structural ultraviolet absorbers, the problem of the degradation of traditional ultraviolet absorbers under environmental factors such as light, heat, and water has been solved, and efficient and stable ultraviolet protection effect has been achieved.
Patent Information
- Application Number
- CN202510595267.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2025-08-01
AI Technical Summary
Under the influence of environmental factors such as light, heat, and water, traditional ultraviolet absorbers have reduced absorption performance and reduced internal protection capabilities.
A new structural UV absorber consisting of pyrene-triazine hybrid, MOF-supported benzotriazole, silica-coated nano-zinc oxide, carbon quantum dot-modified titanium dioxide, PLGA microcapsules, chitosan-hyaluronic acid composite membrane, Eu3+@MOF fluorescent materials and gibberellin-nanoselenium composite, is synthesized and crosslinked through a specific process to form a stable structure.
It improves the stability and absorption performance of ultraviolet absorbers in complex environments, enhances the protection ability of the material, and has efficient ultraviolet absorption ability, photocatalytic properties, excellent mechanical properties and anti-oxidation properties.
Smart Images

Figure CN120399635A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ultraviolet absorbers, and specifically to a research and development method for novel structure ultraviolet absorbers. Background Art
[0002] With the deepening of people's understanding of the harm of ultraviolet rays and the continuous improvement of the requirements for the anti-ultraviolet performance of materials in various industries, ultraviolet absorbers have been widely used in many fields. Whether it is sunscreen products in daily life or materials such as plastics, coatings, and rubbers in industrial production, ultraviolet absorbers play a crucial role. They can effectively reduce the damage of ultraviolet rays to materials, extend the service life of materials, and improve the quality and performance of products.
[0003] Traditional ultraviolet absorbers, such as benzophenones, benzotriazoles, etc., have been widely used in the past few decades. These traditional absorbers can absorb ultraviolet rays to a certain extent and provide protection for materials. However, with the increasing complexity and diversity of application scenarios, traditional ultraviolet absorbers are prone to degradation, migration, etc. under the action of environmental factors such as light, heat, and water, thus reducing their protection effect. Taking benzophenone absorbers as an example, in high-temperature and high-humidity environments, their molecular structure is prone to change, resulting in a decrease in absorption performance; at the same time, during long-term use, the absorber may migrate from the inside of the material to the surface, which not only affects the appearance of the material but also reduces the internal protection ability of the material. Summary of the Invention
[0004] Aiming at the deficiencies of the prior art, the present invention provides a research and development method for novel structure ultraviolet absorbers, which solves the problems that the absorption performance of traditional ultraviolet absorbers decreases and the internal protection ability decreases under the action of environmental factors such as light, heat, and water.
[0005] To achieve the above objectives, the present invention is realized through the following technical solutions: A novel structure ultraviolet absorber, comprising the following raw materials in parts by weight: 25 - 30 parts of pyrene-triazine hybrid, 10 - 20 parts of MOF-loaded benzotriazole, 15 - 20 parts of silica-coated zinc oxide nanoparticles, 10 - 15 parts of carbon quantum dot-modified titanium dioxide, 8 - 12 parts of PLGA microcapsules, 7 - 13 parts of chitosan-hyaluronic acid composite film, Eu 3+ @MOF fluorescent material 12 - 18 parts, gibberellin-nano selenium complex 8 - 12 parts, ionic liquid PF6 5 - 8 parts, cashew phenol epoxy crosslinking agent 5 - 7 parts.
[0006] A preparation method of the novel structure ultraviolet absorber, comprising the following steps: S1. React pyrene with a triazine-containing reactant in an anhydrous tetrahydrofuran solvent, and obtain a pyrene-triazine hybrid through column chromatography purification. Disperse the MOF material in N,N-dimethylformamide, react with a benzotriazole solution, and obtain MOF-loaded benzotriazole through separation, washing, and drying. S2. Disperse nano-zinc oxide in absolute ethanol, adjust the pH, and then dropwise add a tetraethyl orthosilicate solution. React, wash, and dry to obtain silica-coated nano-zinc oxide. Prepare a carbon quantum dot solution through reaction, mix it with a titanium dioxide nanoparticle dispersion, react, and process to obtain carbon quantum dot-modified titanium dioxide. S3. Dissolve PLGA in dichloromethane, add the pyrene-triazine hybrid, MOF-loaded benzotriazole, silica-coated nano-zinc oxide, and carbon quantum dot-modified titanium dioxide. After ultrasonic emulsification, drop it into an aqueous solution containing polyvinyl alcohol, and obtain PLGA microcapsules with absorbents through treatment. Mix a chitosan acetate solution with a hyaluronic acid aqueous solution, add a cross-linking agent to react, spread, dry, and wash to obtain a chitosan-hyaluronic acid composite membrane. S4. Disperse the MOF material in DMF, react with an Eu 3+ solution, and process to obtain an Eu 3+ @MOF fluorescent material. Prepare nano-selenium through a chemical reduction method, and mix it with a gibberellin ethanol solution to react to obtain a gibberellin-nano-selenium complex.
[0007] S5. Add the PLGA microcapsules with absorbents, chitosan-hyaluronic acid composite membrane, Eu 3+ @MOF fluorescent material, and gibberellin-nano-selenium complex by weight parts to a reaction kettle. Use the ionic liquid PF6 as the solvent and dispersion medium, stir and mix, then add a cardanol epoxy cross-linking agent, raise the temperature to react, and cool and discharge to complete the preparation.
[0008] Preferably, the S1 specifically includes the following steps: S101. In a reaction vessel under nitrogen protection, dissolve pyrene in anhydrous tetrahydrofuran, cool to 0 - 5 °C, dropwise add a tetrahydrofuran solution containing a triazine-containing reactant, control the reaction temperature at 0 - 5 °C during the dropping, raise the temperature to 40 - 50 °C after dropping, react for 8 - 10 hours, distill off the solvent under reduced pressure, and then separate and purify by column chromatography to obtain a pyrene-triazine hybrid. S102. Disperse the MOF material in an appropriate amount of N,N-dimethylformamide, ultrasonically treat for 30 minutes for dispersion, then add a DMF solution of benzotriazole, stir and react at 60 - 70 °C for 12 - 15 hours, then centrifuge and separate, wash the precipitate with DMF, and then wash with ethanol, and vacuum dry at 60 °C for 10 - 12 hours to obtain MOF-loaded benzotriazole.
[0009] Preferably, in S101, the column chromatography method is silica gel column, and the mixed solution of petroleum ether and ethyl acetate with a volume ratio of 3:1 is used as the eluent. In S102, the MOF material includes UiO-66-NH2, and the molar ratio of benzotriazole to MOF in the DMF solution is 3:1.
[0010] Preferably, S2 specifically includes the following steps: S201. Disperse nano-zinc oxide in absolute ethanol, ultrasonically disperse for 30 minutes to form a uniform suspension, add ammonia water to adjust the pH, slowly dropwise add an absolute ethanol solution of tetraethyl orthosilicate under stirring, stir and react at room temperature for 4 - 6 hours, then centrifuge and separate, wash the precipitate with absolute ethanol, and vacuum dry at 60°C for 8 - 10 hours to obtain silica-coated nano-zinc oxide; S202. Put citric acid and ethylenediamine in a reaction vessel, react at 180 - 200°C for 2 - 3 hours to prepare a carbon quantum dot solution. Then disperse titanium dioxide nanoparticles in water, ultrasonically disperse evenly and add the carbon quantum dot solution, stir and react at room temperature for 6 - 8 hours, then centrifuge and separate, wash the precipitate with deionized water, and vacuum dry at 80°C for 6 - 8 hours to obtain carbon quantum dot-modified titanium dioxide.
[0011] Preferably, in S201, the pH is 9 - 10, and the mass ratio of tetraethyl orthosilicate to nano-zinc oxide is 1:5. In S202, the mass ratio of carbon quantum dots to titanium dioxide is 1:10 - 1:15.
[0012] Preferably, S3 specifically includes the following steps: S301. Weigh PLGA and dissolve it in dichloromethane, then add pyrene-triazine hybrid, MOF-loaded benzotriazole, silica-coated nano-zinc oxide, and carbon quantum dot-modified titanium dioxide by weight parts, ultrasonically emulsify to make it evenly dispersed, then drop it into an aqueous solution containing 2% - 3% polyvinyl alcohol by mass fraction, and then carry out emulsification at a stirring rate of 500 - 1000 revolutions per minute to form a water-in-oil emulsion. During the stirring process, gradually heat up to 40 - 50°C, distill off dichloromethane under reduced pressure, centrifuge and separate, wash the precipitate with deionized water, and freeze-dry to obtain PLGA microcapsules with absorbents; S302. Prepare a 2% chitosan acetate solution and a 1% hyaluronic acid aqueous solution respectively, mix the chitosan acetate solution and the hyaluronic acid aqueous solution in a volume ratio of 1:1, stir evenly, add a cross-linking agent, continue to stir and react for 2 - 3 hours, evenly spread the mixed solution on a glass plate, naturally dry into a film at room temperature, then soak and wash with deionized water to remove unreacted substances, and vacuum dry at 50°C for 4 - 6 hours to obtain a chitosan-hyaluronic acid composite film.
[0013] Preferably, S4 specifically includes the following steps: S401. Disperse the MOF material in DMF. After ultrasonic dispersion until uniform, add the DMF solution of Eu 3+ . Stir and react at 80 - 90 °C for 15 - 18 hours, then perform centrifugal separation. Wash the precipitate with DMF, then wash with ethanol, and dry in vacuum at 70 °C for 12 - 15 hours to obtain the Eu 3+ @MOF fluorescent material; S402. Prepare nano-selenium by chemical reduction method. React the sodium selenite solution with the ascorbic acid solution to generate nano-selenium particles. Dissolve gibberellin in ethanol, add the nano-selenium particles, ultrasonic disperse until uniform, then stir and react at room temperature for 4 - 6 hours, and remove ethanol by reduced pressure distillation to obtain the gibberellin-nano-selenium complex.
[0014] Preferably, in S401, the MOF material includes ZIF-8, and the molar ratio of Eu 3+ in the DMF solution of Eu 3+ to MOF is 1:10 - 1:15. The reaction conditions for generating nano-selenium particles in S402 are a temperature of 50 - 60 °C and a pH value of 5 - 6.
[0015] Preferably, S5 specifically includes the following steps: S501. Trim the chitosan-hyaluronic acid composite film into blocks with a side length of 5 - 10 mm. Add the PLGA microcapsules with absorbent, chitosan-hyaluronic acid composite film, Eu 3+ @MOF fluorescent material, and gibberellin-nano-selenium complex to the reaction kettle by weight; S502. Then add ionic liquid PF6 to the reaction kettle by weight. Stir and mix at 50 - 60 °C for 2 - 3 hours, add cardanol epoxy crosslinking agent, raise the temperature to 70 - 80 °C, continue to stir and react for 4 - 6 hours, and then cool to room temperature to complete the preparation.
[0016] The present invention provides a research and development method for a novel structure ultraviolet absorber, having the following beneficial effects: 1. In the present invention, the pyrene-triazine hybrid broadens the absorption wavelength range by virtue of its unique structure. The MOF-loaded benzotriazole improves the stability and dispersibility by using the MOF pores. The silica-coated nano-zinc oxide improves the aggregation and poor stability of nano-zinc oxide. The carbon quantum dot-modified titanium dioxide expands the light response range of titanium dioxide, making the absorber have stable and efficient absorption performance in environments such as light, heat, and water, and solving the problem that the absorption performance of traditional ultraviolet absorbers decreases and the internal protection ability reduces under the action of environmental factors such as light, heat, and water.
[0017] 2. By virtue of the large conjugated system of pyrene and the ultraviolet absorption characteristics of triazine compounds, the pyrene-triazine hybrid in the present invention has strong absorption ability. The large specific surface area and unique pore structure of the MOF material improve the dispersibility and stability of benzotriazole, enhancing its absorption ability. The silica-coated nano-zinc oxide improves the problems of easy agglomeration and limited stability of nano-zinc oxide, and better exerts its absorption performance. The carbon quantum dot-modified titanium dioxide enhances the absorption of titanium dioxide to visible light and the separation efficiency of photogenerated electrons and holes, enabling the absorbent to provide more reliable protection for the material to be protected.
[0018] 3. Through the protection of the MOF material for the loaded substance, the encapsulation of the absorbent by the PLGA microcapsule, and the carrier effect of the chitosan-hyaluronic acid composite film, the present invention reduces the performance change of the absorbent under the action of light. Materials such as PLGA and MOF itself have good thermal stability and form a stable structure through crosslinking, enabling the novel absorbent to withstand higher temperatures. The silica shell of the silica-coated nano-zinc oxide, the crosslinking treatment of the chitosan-hyaluronic acid composite film, etc. all improve the overall water resistance, and the performance can still remain stable after long-term immersion, reducing the decline in the protection effect caused by water leaching. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic flow chart of the preparation method of the novel structure ultraviolet absorbent proposed by the present invention. DETAILED DESCRIPTION OF THE EMBODIMENTS
[0020] Next, the technical solutions of the present invention will be clearly and completely described in conjunction with the drawings of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative work fall within the scope of protection of the present invention.
[0021] The embodiment of the present invention provides a novel structure ultraviolet absorbent, which includes the following raw materials in parts by weight: 25-30 parts of pyrene-triazine hybrid, 10-20 parts of MOF-loaded benzotriazole, 15-20 parts of silica-coated nano-zinc oxide, 10-15 parts of carbon quantum dot-modified titanium dioxide, 8-12 parts of PLGA microcapsule, 7-13 parts of chitosan-hyaluronic acid composite film, Eu 3+ @MOF fluorescent material 12-18 parts, gibberellin-nano selenium complex 8-12 parts, ionic liquid PF6 5-8 parts, cashew phenol epoxy crosslinking agent 5-7 parts.
[0022] Specifically, by adding the pyrene-triazine hybrid, which has a unique molecular structure and can efficiently absorb ultraviolet light, convert it into other forms of energy, and reduce the direct irradiation of ultraviolet light on the protected material, thereby improving the ultraviolet resistance of the material. At the same time, it may have a certain improvement effect on the optical properties of the material.
[0023] By adding silica-coated zinc oxide nanoparticles, zinc oxide nanoparticles themselves have good ultraviolet absorption ability, and silica coating can improve their dispersibility and stability in the system, prevent zinc oxide nanoparticles from agglomerating, so as to play the ultraviolet absorption role more evenly, and also enhance the weather resistance and chemical stability of the material.
[0024] By adding carbon quantum dot-modified titanium dioxide, carbon quantum dots can improve the light absorption efficiency of titanium dioxide, expand its light response range, and the modified titanium dioxide can more effectively use ultraviolet light for photocatalytic reactions, thereby decomposing organic pollutants in the environment, and at the same time enhancing the self-cleaning and antibacterial properties of the material.
[0025] By adding PLGA microcapsules, they can be used as carriers to encapsulate some functional substances inside and release them slowly, thereby prolonging the effective action time of the material, improving the durability of the material, and also improving the processing performance and flexibility of the material.
[0026] By adding a chitosan-hyaluronic acid composite film, which has good film-forming properties and biocompatibility, can form a uniform protective film on the surface of the material, thereby improving the surface smoothness and waterproofness of the material, and at the same time having a certain blocking effect on ultraviolet light, enhancing the anti-ultraviolet aging ability of the material.
[0027] By Eu 3+ @MOF fluorescent material can emit fluorescence after absorbing ultraviolet light, which can be used to indicate the ultraviolet absorption of the material, thus playing the role of an ultraviolet absorption indicator. At the same time, its fluorescence properties may also bring some special optical effects to the material.
[0028] By adding gibberellin-nano selenium complex, the comprehensive efficiency of the ultraviolet absorber system in agricultural application scenarios is enhanced. The synergistic effect of nano selenium and gibberellin helps to regulate the interaction between the ultraviolet absorber and the crop surface, enabling the absorber to better adhere and evenly distribute on the crop surface, improving the ultraviolet absorption efficiency, reducing the damage of ultraviolet light to the crop. At the same time, it has a positive impact on the stability of the absorber system, inhibiting the change of the internal molecular structure in the system caused by ultraviolet irradiation, ensuring that the ultraviolet absorber continuously and stably plays its role in a complex agricultural environment, and then creating a good microenvironment for crop growth and enhancing the overall adaptability of the crop under ultraviolet stress.
[0029] By adding ionic liquid PF6 to replace traditional organic solvents (such as toluene), zero VOC emissions can be achieved, which can improve the compatibility and dispersibility of each component in the system, so that each raw material can be better mixed evenly, improve the overall performance of the material, and also have a certain regulating effect on the electrical properties of the material.
[0030] By adding cardanol epoxy crosslinker, through crosslinking reaction, the water resistance of the coating can be enhanced, and each component can be connected together to form a three-dimensional network structure, thereby improving the mechanical properties, heat resistance and stability of the material, and endowing the material with better physical properties and service life.
[0031] Through the mutual cooperation among the raw materials, a multi-functional system is formed. Pyrene-triazine hybrids, silica-coated zinc oxide nanoparticles, carbon quantum dot-modified titanium dioxide, etc. are mainly responsible for ultraviolet absorption and photocatalysis; PLGA microcapsules and chitosan-hyaluronic acid composite membranes improve the physical properties and protective properties of the material; Eu³⁺@MOF fluorescent material is used as an indicator; gibberellin-nano selenium complex enhances the antioxidant capacity; ionic liquid regulates the compatibility; cardanol epoxy crosslinker improves the mechanical properties and stability, thus having multiple functions such as efficient ultraviolet absorption capacity, good photocatalytic performance, excellent mechanical properties, antioxidant performance, and weather resistance.
[0032] Please refer to the appendix Figure 1 , a preparation method of a novel structure ultraviolet absorber, comprising the following steps: S1. React pyrene with a triazine-containing reactant in an anhydrous tetrahydrofuran solvent, and obtain pyrene-triazine hybrid through column chromatography purification. Disperse the MOF material in N,N-dimethylformamide and react with benzotriazole solution, and obtain MOF-loaded benzotriazole through separation, washing and drying. S1 specifically includes the following steps: S101. In a reaction vessel protected by nitrogen, dissolve pyrene in anhydrous tetrahydrofuran, cool to 0-5°C, and dropwise add a tetrahydrofuran solution of a triazine-containing reactant. Control the reaction temperature at 0-5°C during the dropping process, and raise the temperature to 40-50°C after dropping. React for 8-10 hours, remove the solvent by vacuum distillation, and separate and purify by column chromatography to obtain pyrene-triazine hybrid. S102. Disperse the MOF material in an appropriate amount of N,N-dimethylformamide, ultrasonically treat for 30 minutes for dispersion, then add a DMF solution of benzotriazole, stir and react at 60-70°C for 12-15 hours, then centrifuge, wash the precipitate with DMF, then wash with ethanol, and vacuum dry at 60°C for 10-12 hours to obtain MOF-loaded benzotriazole.
[0033] In S101, the column chromatography method uses a silica gel column, and a mixed solution of petroleum ether and ethyl acetate with a volume ratio of 3:1 is used as the eluent. In S102, the MOF material includes UiO-66-NH2, and the molar ratio of benzotriazole in the DMF solution to MOF is 3:1.
[0034] Specifically, by reacting pyrene with a triazine-containing reactant in an anhydrous tetrahydrofuran solvent and purifying it by column chromatography, a pyrene-triazine hybrid is obtained. The MOF material is dispersed in N,N-dimethylformamide and reacted with a benzotriazole solution, and after separation, washing, and drying, MOF-loaded benzotriazole is obtained, thus successfully synthesizing a main absorbent with specific structures and properties. The unique molecular structure of the pyrene-triazine hybrid endows it with efficient and broad-spectrum ultraviolet absorption ability, which can effectively broaden the absorption wavelength range; MOF-loaded benzotriazole utilizes the special pore structure of MOF to improve the stability and dispersibility of benzotriazole, realizing an innovative construction of the core components of the ultraviolet absorbent and laying a foundation for the subsequent preparation of high-performance ultraviolet absorbents.
[0035] S2. Disperse nano-zinc oxide in absolute ethanol, adjust the pH, and then dropwise add tetraethyl orthosilicate solution. After reaction, washing, and drying, silica-coated nano-zinc oxide is obtained. A carbon quantum dot solution is prepared through a reaction, and it is mixed and reacted with a titanium dioxide nanoparticle dispersion liquid and processed to obtain carbon quantum dot-modified titanium dioxide. S2 specifically includes the following steps: S201. Disperse nano-zinc oxide in absolute ethanol, ultrasonically disperse for 30 minutes to form a uniform suspension, add ammonia water to adjust the pH, and slowly dropwise add an absolute ethanol solution of tetraethyl orthosilicate under stirring. Stir and react at room temperature for 4 - 6 hours, then centrifuge and separate, wash the precipitate with absolute ethanol, and vacuum dry at 60 °C for 8 - 10 hours to obtain silica-coated nano-zinc oxide; S202. Put citric acid and ethylenediamine in a reaction vessel and react at 180 - 200 °C for 2 - 3 hours to prepare a carbon quantum dot solution. Then disperse titanium dioxide nanoparticles in water, ultrasonically disperse evenly, add the carbon quantum dot solution, stir and react at room temperature for 6 - 8 hours, then centrifuge and separate, wash the precipitate with deionized water, and vacuum dry at 80 °C for 6 - 8 hours to obtain carbon quantum dot-modified titanium dioxide.
[0036] In S201, the pH is 9 - 10, and the mass ratio of tetraethyl orthosilicate to nano-zinc oxide is 1:5. In S202, the mass ratio of carbon quantum dots to titanium dioxide is 1:10 - 1:15.
[0037] Specifically, by dispersing zinc oxide nanoparticles in absolute ethanol, adjusting the pH and then dropping in tetraethyl orthosilicate solution, reacting, washing, and drying, zinc oxide nanoparticles coated with silica are obtained. By reacting, a carbon quantum dot solution is prepared, which is mixed and reacted with a titanium dioxide nanoparticle dispersion and then processed to obtain carbon quantum dot-modified titanium dioxide, thereby constructing a component with enhanced stability. The zinc oxide nanoparticles coated with silica improve the stability of the zinc oxide nanoparticles, prevent their aggregation in the system and reduce photocatalytic side reactions, while enhancing the ultraviolet shielding effect; the carbon quantum dot-modified titanium dioxide expands the light response range of titanium dioxide, improves the photocatalytic efficiency, inhibits the recombination of photo-generated carriers, realizes the optimization of the stability and photocatalytic performance of the ultraviolet absorber, and ensures that the absorber plays a stable role in complex environments.
[0038] S3. Dissolve PLGA in dichloromethane, add pyrene-triazine hybrid, MOF-loaded benzotriazole, zinc oxide nanoparticles coated with silica, and carbon quantum dot-modified titanium dioxide. After ultrasonic emulsification, drop it into an aqueous solution containing polyvinyl alcohol, and obtain PLGA microcapsules with absorbers after treatment. Mix the chitosan acetate solution and the hyaluronic acid aqueous solution, add a cross-linking agent and react, then spread, dry, and wash to obtain a chitosan-hyaluronic acid composite film; S3 specifically includes the following steps: S301. Weigh PLGA and dissolve it in dichloromethane, then add pyrene-triazine hybrid, MOF-loaded benzotriazole, zinc oxide nanoparticles coated with silica, and carbon quantum dot-modified titanium dioxide according to parts by weight. After ultrasonic emulsification to make them evenly dispersed, drop it into an aqueous solution containing 2%-3% polyvinyl alcohol by mass fraction, and then carry out emulsification to form a water-in-oil emulsion under stirring at a stirring rate of 500-1000 revolutions per minute. During the stirring process, gradually heat up to 40-50 °C, distill off dichloromethane under reduced pressure, carry out centrifugal separation, wash the precipitate with deionized water, and freeze-dry to obtain PLGA microcapsules with absorbers. S302. Prepare a chitosan acetate solution with a mass fraction of 2% and a hyaluronic acid aqueous solution with a mass fraction of 1% respectively. Mix the chitosan acetate solution and the hyaluronic acid aqueous solution according to a volume ratio of 1:1, stir evenly, add a cross-linking agent, and continue stirring and reacting for 2-3 hours. Spread the mixed solution evenly on a glass plate, naturally dry it into a film at room temperature, then soak and wash it with deionized water to remove unreacted substances, and vacuum-dry it at 50 °C for 4-6 hours to obtain a chitosan-hyaluronic acid composite film.
[0039] Specifically, by sequentially implementing the above operation steps, a special component applicable to the biomedical field is prepared. The PLGA microcapsules with absorbents achieve effective encapsulation and sustained-release control of various ultraviolet absorbers, reducing the toxicity to biological cells; the chitosan-hyaluronic acid composite film has good biocompatibility, moisturizing property and film-forming property, and can provide protection and repair for tissues such as skin in biomedical application scenarios, realizing the functional expansion and optimization of ultraviolet absorbers in the biomedical field and meeting the strict requirements for safety and functionality in the biomedical field.
[0040] S4. Disperse the MOF material in DMF and react with Eu 3+ solution, and treat to obtain Eu 3+ @MOF fluorescent material. Prepare nano-selenium by chemical reduction method, and mix and react with gibberellin ethanol solution to obtain gibberellin-nano-selenium composite; S4 specifically includes the following steps: S401. Take the MOF material and disperse it in DMF. After ultrasonic dispersion is uniform, add the DMF solution of Eu 3+ . Stir and react at 80 - 90 °C for 15 - 18 hours, then centrifuge and separate. Wash the precipitate with DMF, then wash with ethanol, and vacuum dry at 70 °C for 12 - 15 hours to obtain Eu 3+ @MOF fluorescent material; S402. Prepare nano-selenium by chemical reduction method. React sodium selenite solution with ascorbic acid solution to generate nano-selenium particles. Dissolve gibberellin in ethanol, add nano-selenium particles, ultrasonic disperse uniformly, and stir and react at room temperature for 4 - 6 hours. Distill off ethanol under reduced pressure to obtain gibberellin-nano-selenium composite.
[0041] The MOF material in S401 includes ZIF-8, and the molar ratio of Eu 3+ in the DMF solution of Eu 3+ to MOF is 1:10 - 1:15. The reaction conditions for generating nano-selenium particles in S402 are temperature 50 - 60 °C and pH value 5 - 6.
[0042] Specifically, by dispersing the MOF material in DMF and reacting with Eu 3+ solution, and treating to obtain Eu 3+ @MOF fluorescent material, preparing nano-selenium by chemical reduction method, and mixing and reacting with gibberellin ethanol solution to obtain gibberellin-nano-selenium composite, thereby obtaining the key component applicable to the agricultural field. Eu 3+@MOF fluorescent materials can convert part of the ultraviolet light into visible light required for plant photosynthesis, promoting plant growth; the gibberellin-nano selenium complex can enhance the stress resistance of crops under ultraviolet stress, ensure the normal growth and development of crops, realizing the targeted functional development of ultraviolet absorbers in the agricultural field, and providing a new means of light regulation and stress resistance enhancement for agricultural production.
[0043] S5. By weight, PLGA microcapsules with absorbents, chitosan-hyaluronic acid composite film, Eu 3+ @MOF fluorescent materials and gibberellin-nano selenium complex are added to the reaction kettle. Using ionic liquid PF6 as the solvent and dispersion medium, after stirring and mixing, cardanol epoxy crosslinking agent is added, the temperature is raised for reaction, and after cooling, the product is discharged to complete the preparation; S5 specifically includes the following steps: S501. Trim the chitosan-hyaluronic acid composite film into blocks with a side length of 5-10 mm. By weight, PLGA microcapsules with absorbents, chitosan-hyaluronic acid composite film, Eu 3+ @MOF fluorescent materials and gibberellin-nano selenium complex are added to the reaction kettle. S502. Then, by weight, ionic liquid PF6 is added to the reaction kettle. After stirring and mixing at 50-60 °C for 2-3 hours, cardanol epoxy crosslinking agent is added, the temperature is raised to 70-80 °C, and stirring and reaction continue for 4-6 hours, and then cooled to room temperature to complete the preparation.
[0044] Specifically, by adding each component to the reaction kettle by weight, using ionic liquid PF6 as the solvent and dispersion medium, adding cardanol epoxy crosslinking agent after stirring and mixing, raising the temperature for reaction, and cooling and discharging to complete the preparation, so as to effectively integrate each functional component and construct a complete new structure ultraviolet absorber system. Ionic liquid PF6 ensures the uniform dispersion of each component, and cardanol epoxy crosslinking agent promotes the crosslinking and curing of each component, forming a stable three-dimensional network structure, improving the physical properties and chemical stability of the absorber, and realizing the preparation of a new type of ultraviolet absorber with multi-field function integration.
[0045] The following is a further introduction in combination with specific examples: Example 1: The new structure ultraviolet absorber includes the following raw materials by weight: 30 parts of pyrene-triazine hybrid, 20 parts of MOF-loaded benzotriazole, 20 parts of silica-coated nano zinc oxide, 15 parts of carbon quantum dot-modified titanium dioxide, 12 parts of PLGA microcapsules, 13 parts of chitosan-hyaluronic acid composite film, Eu 3+ 18 parts of @MOF fluorescent materials, 12 parts of gibberellin-nano selenium complex, 8 parts of ionic liquid PF6, and 7 parts of cardanol epoxy crosslinking agent.
[0046] The preparation method of the new structure ultraviolet absorber includes the following steps: S1. React pyrene with a triazine-containing reactant in an anhydrous tetrahydrofuran solvent, and obtain a pyrene-triazine hybrid through column chromatography purification. Disperse the MOF material in N,N-dimethylformamide, react with a benzotriazole solution, and obtain MOF-supported benzotriazole through separation, washing, and drying. S2. Disperse nano-zinc oxide in absolute ethanol, adjust the pH, and then dropwise add a tetraethyl orthosilicate solution. React, wash, and dry to obtain silica-coated nano-zinc oxide. Prepare a carbon quantum dot solution through a reaction, mix it with a titanium dioxide nanoparticle dispersion, react, and process to obtain carbon quantum dot-modified titanium dioxide. S3. Dissolve PLGA in dichloromethane, add the pyrene-triazine hybrid, MOF-supported benzotriazole, silica-coated nano-zinc oxide, and carbon quantum dot-modified titanium dioxide. After ultrasonic emulsification, drop it into an aqueous solution containing polyvinyl alcohol, and obtain PLGA microcapsules with absorbents through treatment. Mix a chitosan acetate solution with a hyaluronic acid aqueous solution, add a cross-linking agent to react, spread, dry, and wash to obtain a chitosan-hyaluronic acid composite film. S4. Disperse the MOF material in DMF, react with an Eu 3+ solution, and process to obtain Eu 3+ @MOF fluorescent material. Prepare nano-selenium through a chemical reduction method, mix it with a gibberellic acid ethanol solution to react to obtain a gibberellic acid-nano-selenium complex. S5. Add the PLGA microcapsules with absorbents, chitosan-hyaluronic acid composite film, Eu 3+ @MOF fluorescent material, and gibberellic acid-nano-selenium complex by weight parts to a reaction kettle. Use the ionic liquid PF6 as a solvent and dispersion medium, stir and mix, then add a cardanol epoxy cross-linking agent, raise the temperature to react, cool and discharge to complete the preparation.
[0047] S1 specifically includes the following steps: S101. In a reaction vessel under nitrogen protection, dissolve pyrene in anhydrous tetrahydrofuran, cool to 0 °C, dropwise add a tetrahydrofuran solution containing a triazine-containing reactant, control the reaction temperature at 0 °C during the dropping, raise the temperature to 45 °C after dropping, react for 9 hours, distill off the solvent under reduced pressure, and then separate and purify by column chromatography to obtain a pyrene-triazine hybrid. S102. Disperse the MOF material in an appropriate amount of N,N-dimethylformamide, ultrasonically treat for 30 minutes to disperse, then add a DMF solution of benzotriazole, stir and react at 65 °C for 14 hours, then centrifuge and separate, wash the precipitate with DMF, then wash with ethanol, and vacuum dry at 60 °C for 11 hours to obtain MOF-supported benzotriazole.
[0048] In S101, the silica gel column is used for column chromatography, and the mixed solution of petroleum ether and ethyl acetate with a volume ratio of 3:1 is used as the eluent. In S102, the MOF material includes UiO-66-NH2, and the molar ratio of benzotriazole in the DMF solution to MOF is 3:1.
[0049] S2 specifically includes the following steps: S201: Disperse zinc oxide nanoparticles in absolute ethanol, ultrasonically disperse for 30 minutes to form a uniform suspension, add ammonia water to adjust the pH, slowly dropwise add the absolute ethanol solution of tetraethyl orthosilicate under stirring, stir and react at room temperature for 5 hours, then centrifuge and separate, wash the precipitate with absolute ethanol, and vacuum dry at 60 °C for 9 hours to obtain silica-coated zinc oxide nanoparticles; S202: Put citric acid and ethylenediamine in a reaction vessel, react at 190 °C for 2.5 hours to prepare a carbon quantum dot solution, then disperse titanium dioxide nanoparticles in water, ultrasonically disperse evenly and add the carbon quantum dot solution, stir and react at room temperature for 7 hours, then centrifuge and separate, wash the precipitate with deionized water, and vacuum dry at 80 °C for 7 hours to obtain carbon quantum dot-modified titanium dioxide.
[0050] In S201, the pH is 8, and the mass ratio of tetraethyl orthosilicate to zinc oxide nanoparticles is 1:5. In S202, the mass ratio of carbon quantum dots to titanium dioxide is 1:12.
[0051] S3 specifically includes the following steps: S301: Weigh PLGA and dissolve it in dichloromethane, then add pyrene-triazine hybrid, MOF-loaded benzotriazole, silica-coated zinc oxide nanoparticles, and carbon quantum dot-modified titanium dioxide by weight, ultrasonically emulsify to make them evenly dispersed, then drop it into an aqueous solution containing 2.5% by mass of polyvinyl alcohol, and then emulsify to form a water-in-oil emulsion under stirring at a stirring rate of 700 revolutions per minute. During the stirring process, gradually heat up to 45 °C, distill off dichloromethane under reduced pressure, centrifuge and separate, wash the precipitate with deionized water, and freeze-dry to obtain PLGA microcapsules with absorbents; S302: Prepare a 2% by mass chitosan acetate solution and a 1% by mass hyaluronic acid aqueous solution respectively, mix the chitosan acetate solution and the hyaluronic acid aqueous solution in a volume ratio of 1:1, stir evenly, add a crosslinking agent, continue to stir and react for 2.5 hours, evenly spread the mixed solution on a glass plate, naturally dry it into a film at room temperature, then soak and wash it with deionized water to remove unreacted substances, and vacuum dry at 50 °C for 5 hours to obtain a chitosan-hyaluronic acid composite film.
[0052] S4 specifically includes the following steps: S401: Take the MOF material and disperse it in DMF, ultrasonically disperse evenly, and then add Eu 3+The DMF solution was stirred and reacted at 85 °C for 17 hours, then centrifuged and separated. After washing the precipitate with DMF, it was further washed with ethanol and dried in vacuo at 70 °C for 13 hours to obtain Eu 3+ @MOF fluorescent material; S402. Prepare nano-selenium by chemical reduction method. React sodium selenite solution with ascorbic acid solution to generate nano-selenium particles. Dissolve gibberellin in ethanol, add nano-selenium particles, and after ultrasonic dispersion, stir and react at room temperature for 5 hours, and remove ethanol by vacuum distillation to obtain gibberellin-nano-selenium composite.
[0053] In S401, the MOF material includes ZIF-8, Eu 3+ in the DMF solution of Eu 3+ The molar ratio of Eu to MOF is 1:12. The reaction conditions for generating nano-selenium particles in S402 are temperature 55 °C and pH value 5.5.
[0054] S5 specifically includes the following steps: S501. Trim the chitosan-hyaluronic acid composite film into blocks with a side length of 6 mm. By weight, add PLGA microcapsules with absorbent, chitosan-hyaluronic acid composite film, Eu 3+ @MOF fluorescent material, and gibberellin-nano-selenium composite into the reaction kettle; S502. Then add ionic liquid PF6 to the reaction kettle by weight, stir and mix at 55 °C for 2.5 hours, add cardanol epoxy crosslinking agent, raise the temperature to 75 °C, continue to stir and react for 5 hours, and then cool to room temperature to complete the preparation.
[0055] Example 2: The difference between this example and Example 1 above is that: The novel structure ultraviolet absorber includes the following raw materials by weight: 25 parts of pyrene-triazine hybrid, 10 parts of MOF-loaded benzotriazole, 15 parts of silica-coated nano-zinc oxide, 10 parts of carbon quantum dot-modified titanium dioxide, 8 parts of PLGA microcapsules, 7 parts of chitosan-hyaluronic acid composite film, Eu 3+ 12 parts of @MOF fluorescent material, 8 parts of gibberellin-nano-selenium composite, 5 parts of ionic liquid PF6, and 5 parts of cardanol epoxy crosslinking agent.
[0056] Example 3: The difference between this example and Example 1 above is that: The novel structure ultraviolet absorber includes the following raw materials by weight: 27.5 parts of pyrene-triazine hybrid, 15 parts of MOF-loaded benzotriazole, 17.5 parts of silica-coated nano-zinc oxide, 12.5 parts of carbon quantum dot-modified titanium dioxide, 10 parts of PLGA microcapsules, 10 parts of chitosan-hyaluronic acid composite film, Eu3+ 15 parts of @MOF fluorescent material, 10 parts of gibberellin-nano selenium complex, 6.5 parts of ionic liquid PF6, and 6 parts of cardanol epoxy crosslinker.
[0057] Table 1: The comparison in the above table is with traditional ultraviolet absorbers. From Table 1, it can be seen that different amounts of pyrene-triazine hybrids, MOF-loaded benzotriazole, silica-coated zinc oxide nanoparticles, carbon quantum dot-modified titanium dioxide, PLGA microcapsules, chitosan-hyaluronic acid composite films, Eu 3+ @MOF fluorescent material, gibberellin-nano selenium complex, ionic liquid PF6, and cardanol epoxy crosslinker can affect the absorbance, transmittance, change rate, and water resistance of the ultraviolet absorber, thereby realizing the optimization and synergy of the absorber's performance in multiple aspects such as ultraviolet absorption ability, light stability, and water resistance, and solving the problem of insufficient stability of traditional ultraviolet absorbers.
[0058] Although the embodiments of the present invention have been shown and described, it will be understood by those of ordinary skill in the art that various changes, modifications, substitutions, and variations can be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A novel-structured ultraviolet absorber, characterized in that, It includes the following raw materials in parts by weight: 25-30 parts of pyrene-triazine hybrid, 10-20 parts of MOF-supported benzotriazole, 15-20 parts of silica-coated nanozinc oxide, 10-15 parts of carbon quantum dot-modified titanium dioxide, 8-12 parts of PLGA microcapsules, 7-13 parts of chitosan-hyaluronic acid composite film, 3+ 12-18 parts of Eu@MOF fluorescent material, 8-12 parts of gibberellin-nano selenium complex, 2. Preparation method of novel structure ultraviolet absorber, characterized in that: Applied to the novel-structured ultraviolet absorber described in claim 1, the method includes the following steps: S1. React pyrene with a triazine-containing reactant in an anhydrous tetrahydrofuran solvent, and obtain a pyrene-triazine hybrid through column chromatography purification. Disperse the MOF material in N,N-dimethylformamide, react with a benzotriazole solution, and obtain MOF-loaded benzotriazole through separation, washing, and drying. S2. Disperse nano zinc oxide in absolute ethanol, adjust the pH, and then dropwise add a tetraethyl orthosilicate solution. React, wash, and dry to obtain silica-coated nano zinc oxide. Prepare a carbon quantum dot solution through reaction, mix it with a titanium dioxide nanoparticle dispersion, react and process to obtain carbon quantum dot-modified titanium dioxide. S3. Dissolve PLGA in dichloromethane, add the pyrene-triazine hybrid, MOF-loaded benzotriazole, silica-coated nano zinc oxide, and carbon quantum dot-modified titanium dioxide. After ultrasonic emulsification, drop it into an aqueous solution containing polyvinyl alcohol, and obtain PLGA microcapsules with the absorber through processing. Mix a chitosan acetate solution with a hyaluronic acid aqueous solution, add a crosslinking agent to react, then spread, dry, and wash to obtain a chitosan-hyaluronic acid composite film. S4. Disperse the MOF material in DMF and react with Eu 3+ solution, and treat to obtain Eu 3+ @MOF fluorescent material. Prepare nano-selenium by chemical reduction method, mix and react with gibberellin ethanol solution to obtain gibberellin-nano-selenium complex; S5. PLGA microcapsules with absorbent, chitosan-hyaluronic acid composite film, Eu 3+ @MOF fluorescent material, gibberellin-nano selenium complex are added to a reaction kettle. Using ionic liquid PF6 as the solvent and dispersion medium, after stirring and mixing, cardanol epoxy crosslinking agent is added, the temperature is raised for reaction, and after cooling, the product is discharged to complete the preparation.
3. The preparation method of the novel-structured ultraviolet absorber according to claim 2, characterized in that: The specific steps of S1 are as follows: S101. In a reaction vessel under nitrogen protection, dissolve pyrene in anhydrous tetrahydrofuran, cool it to 0 - 5 °C, dropwise add a tetrahydrofuran solution of the triazine-containing reactant, control the reaction temperature at 0 - 5 °C during the dropping process, raise the temperature to 40 - 50 °C after dropping, react for 8 - 10 hours, remove the solvent by vacuum distillation, and then separate and purify by column chromatography to obtain a pyrene-triazine hybrid. S102. Disperse the MOF material in an appropriate amount of N,N-dimethylformamide, ultrasonically treat for 30 minutes for dispersion, then add a DMF solution of benzotriazole, stir and react at 60 - 70 °C for 12 - 15 hours, then centrifuge and separate, wash the precipitate with DMF, then wash with ethanol, and vacuum dry at 60 °C for 10 - 12 hours to obtain MOF-loaded benzotriazole.
4. The preparation method of the novel-structured ultraviolet absorber according to claim 3, characterized in that: In S101, the column chromatography method is a silica column, and a mixed solution of petroleum ether and ethyl acetate with a volume ratio of 3:1 is used as the eluent. In S102, the MOF material includes UiO-66-NH2, and the molar ratio of benzotriazole to MOF in the DMF solution is 3:
1.
5. The preparation method of the novel-structured ultraviolet absorber according to claim 2, characterized in that: The specific steps of S2 are as follows: S201. Disperse nano zinc oxide in absolute ethanol, ultrasonically disperse for 30 minutes to form a uniform suspension, add ammonia water to adjust the pH, slowly dropwise add an absolute ethanol solution of tetraethyl orthosilicate under stirring, stir and react at room temperature for 4 - 6 hours, then centrifuge and separate, wash the precipitate well with absolute ethanol, and vacuum dry at 60 °C for 8 - 10 hours to obtain silica-coated nano zinc oxide. S202. React citric acid and ethylenediamine in a reaction vessel at 180 - 200 °C for 2 - 3 hours to prepare a carbon quantum dot solution. Then disperse titanium dioxide nanoparticles in water, ultrasonically disperse uniformly, add the carbon quantum dot solution, stir and react at room temperature for 6 - 8 hours, then centrifuge and separate, wash the precipitate with deionized water, and vacuum dry at 80 °C for 6 - 8 hours to obtain carbon quantum dot-modified titanium dioxide.
6. The preparation method of the novel-structured ultraviolet absorber according to claim 5, characterized in that: In S201, the pH is 9 - 10, and the mass ratio of tetraethyl orthosilicate to nano - zinc oxide is 1:
5. In S202, the mass ratio of carbon quantum dots to titanium dioxide is 1:10 - 1:
15.
7. The preparation method of the novel-structured ultraviolet absorber according to claim 2, wherein: S3 specifically includes the following steps: S301. Weigh PLGA and dissolve it in dichloromethane. Then, add pyrene - triazine hybrid, MOF - loaded benzotriazole, silica - coated nano - zinc oxide, and carbon - quantum - dot - modified titanium dioxide by weight. After ultrasonic emulsification to make them evenly dispersed, drop the mixture into an aqueous solution containing 2% - 3% polyvinyl alcohol by mass fraction. Then, under stirring at a stirring rate of 500 - 1000 revolutions per minute, emulsify to form a water - in - oil emulsion. During the stirring process, gradually heat up to 40 - 50 °C, remove dichloromethane by reduced - pressure distillation, after centrifugal separation, wash the precipitate with deionized water, and freeze - dry to obtain PLGA microcapsules with absorbents. S302. Prepare a 2% chitosan acetate solution and a 1% hyaluronic acid aqueous solution respectively. Mix the chitosan acetate solution and the hyaluronic acid aqueous solution in a volume ratio of 1:1, stir evenly, add a cross - linker, and continue stirring and reacting for 2 - 3 hours. Spread the mixed solution evenly on a glass plate, naturally dry it into a film at room temperature, then soak and wash it with deionized water to remove unreacted substances, and vacuum - dry it at 50 °C for 4 - 6 hours to obtain a chitosan - hyaluronic acid composite film.
8. The preparation method of the novel-structured ultraviolet absorber according to claim 2, characterized in that: S4 specifically includes the following steps: S401. Disperse the MOF material in DMF. After ultrasonic dispersion until uniform, add the DMF solution of Eu 3+ . Stir and react at 80 - 90 °C for 15 - 18 hours, then perform centrifugal separation. After washing the precipitate with DMF, wash it with ethanol, and dry it under vacuum at 70 °C for 12 - 15 hours to obtain the Eu 3+ @MOF fluorescent material; S402. Prepare nano - selenium by chemical reduction method. React sodium selenite solution with ascorbic acid solution to generate nano - selenium particles. Dissolve gibberellin in ethanol, add nano - selenium particles, ultrasonic disperse evenly, and then stir and react at room temperature for 4 - 6 hours. Remove ethanol by reduced - pressure distillation to obtain a gibberellin - nano - selenium complex.
9. The preparation method of the novel-structured ultraviolet absorber according to claim 8, wherein: In S401, the MOF material includes ZIF-8, and the Eu 3+ in the DMF solution of Eu 3+ has a molar ratio to MOF of 1:10 - 1:
15. The reaction conditions for generating nano-selenium particles in S402 are a temperature of 50 - 60 °C and a pH value of 5 - 6.
10. The preparation method of the novel-structured ultraviolet absorber according to claim 2, characterized in that: S5 specifically includes the following steps: S501. Trim the chitosan-hyaluronic acid composite film into blocks with a side length of 5-10 mm. Add PLGA microcapsules with absorbent, chitosan-hyaluronic acid composite film, Eu 3+ MOF fluorescent material, and gibberellin-nano selenium complex into the reaction kettle according to parts by weight; S502. Then, add ionic liquid PF6 to the reaction kettle by weight. Stir and mix at 50 - 60 °C for 2 - 3 hours, add cardanol epoxy cross - linker, heat up to 70 - 80 °C, continue stirring and reacting for 4 - 6 hours, and then cool to room temperature to complete the preparation.
Citation Information
Cited By
Composite saltpetering-resistant agent, saltpetering-resistant and yellowing-resistant colored facing mortar and preparation method of composite saltpetering-resistant and yellowing-resistant colored facing mortar
CN120965165A