Low-cost high-chromium high-carbon high-manganese wear-resistant steel smelting process

Through the combined process of dephosphorization converter, AOD furnace and LF furnace, the problem of high production cost and low efficiency in smelting of high chromium, high carbon, high manganese wear-resistant steel is solved, and an efficient and low-cost smelting process is achieved, with high purity of molten steel and high alloy yield.

CN120400672APending Publication Date: 2025-08-01GANSU JIU STEEL GRP HONGXING IRON & STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510865430.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-06-26
Publication Date
2025-08-01

AI Technical Summary

Technical Problem

The existing high-chromium, high-carbon, high-manganese wear-resistant steel smelting process has problems such as high production costs, low efficiency and low alloy yield.

Method used

The combined process of dephosphorization converter, AOD furnace and LF furnace is adopted to dephosphorize and alloy by blowing top oxygen and bottom gas, reducing the use of vacuum equipment, achieving efficient refining, high alloy yield and reducing smelting costs.

Benefits of technology

The process flow is shortened, production efficiency is improved, alloy consumption is reduced, molten steel has high purity, high alloy yield and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120400672A_ABST
    Figure CN120400672A_ABST
Patent Text Reader

Abstract

The invention provides a low-cost high-chromium high-carbon high-manganese wear-resistant steel smelting process, and relates to the technical field of ferrous metallurgy, the low-cost high-chromium high-carbon high-manganese wear-resistant steel smelting process comprises a process route of converter dephosphorization, AOD refining, LF furnace refining and slab continuous casting, a dephosphorization converter is used for removing P of molten iron to be smaller than or equal to 0.005%, AOD is used for keeping carbon and removing S, LF furnace chemical components and temperature are finely adjusted, high-carbon tapping is used for reducing inclusions in steel, and a carburant is saved; refining is not carried out through RH or VD vacuum equipment, and the method has the advantages of being short in technological process, high in smelting efficiency and high in purity of molten steel; meanwhile, after stainless steel is smelted through the AOD furnace, residual Cr and Si elements are used for increasing Cr and Si, ferrochrome and ferrosilicon are saved, alloying of the Mn element is achieved in the AOD furnace, the alloy yield is high, the smelting cost is low, and good economic benefits and social benefits are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of iron and steel metallurgy, and relates to a smelting process for high-chromium, high-carbon, high-manganese wear-resistant steel with low cost. Background Art

[0002] As a kind of iron and steel functional material, high-manganese steel is a low-magnetic iron and steel material that basically does not generate magnetic induction under the action of a magnetic field. Its room-temperature structure is required to be a stable austenite, so it is also called austenitic steel. High-carbon, high-manganese steel with a C content of 0.9% - 1.35% and a Mn content of 11.5% - 14% is a classic wear-resistant steel. After water toughening treatment, a single austenite structure can be obtained, which has excellent toughness and non-magnetic properties. Its characteristic is that under the action of a large impact force and contact stress, its surface layer will rapidly harden, thus generating a wear-resistant surface layer, while the interior remains austenite, maintaining excellent impact toughness, and is widely used in industries such as mining, coal, metallurgy, railway, and electric power.

[0003] Chromium element can increase the strength and hardness of steel. When the chromium content in steel is within a certain range, the tensile strength and hardness of the steel will increase significantly; chromium can form a dense passivation film on the surface of the steel, significantly improving the corrosion resistance of the steel; chromium can also improve the wear resistance of the steel, making the steel have better durability under friction and wear conditions. Therefore, high-chromium, high-carbon, high-manganese steel has become an important direction in the research field of wear-resistant steel due to its excellent quality.

[0004] High-chromium, high-carbon, high-manganese wear-resistant steel castings are traditional products and have been widely used in China for a long time. However, the castings have low strength, poor toughness, and short service life, and have gradually been replaced by hot-rolled steel plates in recent years. At present, the smelting process of high-chromium, high-carbon, high-manganese steel hot-rolled steel plates in China is: electric furnace → intermediate frequency furnace → LF furnace refining → VD furnace refining → ingot casting. The above process has high production costs and low efficiency.

[0005] After retrieval, the Chinese invention patent application with the application number 202310548812.9 discloses a method for smelting high-manganese steel in a converter. This method adds carbon balls and high-carbon ferromanganese in stages according to the oxygen blowing amount during the converter smelting process to improve the metal recovery rate of manganese, shorten the production cycle, and reduce the production cost of high-manganese steel. The technical defects of the above patent application are that the alloy recovery rate is low, and under low-carbon conditions, carbon addition smelting is required, and RH furnace vacuum treatment must be used. The process flow is long, the alloy consumption is high, and the production efficiency is low. Summary of the Invention

[0006] The purpose of the present invention is to provide a smelting process for high-chromium, high-carbon, high-manganese wear-resistant steel with low cost in view of the problems existing in the prior art, and solve the problems of shortening the process flow, reducing alloy consumption, and improving production efficiency in the current smelting of high-chromium, high-carbon, high-manganese wear-resistant steel.

[0007] To this end, the present invention adopts the following technical solutions: A smelting process for high-chromium, high-carbon, high-manganese wear-resistant steel with low cost, comprising the following steps: Step 1, converter dephosphorization: Pour blast furnace hot metal into a dephosphorization converter, and add scrap steel with a scrap ratio of 7% - 10%. Blow oxygen from the top and nitrogen or carbon dioxide gas from the bottom. The top blowing gas flow rate is 27000 - 32000 m 3 / h, and the bottom blowing gas flow rate is 2500 - 3000 m 3 / h; Add 10 - 15 Kg / t of active lime for high-speed desiliconization and dephosphorization. The blowing time is 7 - 10 min. After obtaining semi-steel, tap the steel. The semi-steel, by mass percentage of chemical composition, contains C: 2.5 - 3.2%, Mn: 0.05 - 0.30%, P ≤ 0.005%, S ≤ 0.050%, and the rest is Fe and inevitable impurities. The semi-steel tapping temperature is 1320℃ - 1380℃.

[0008] Step 2, AOD refining: Return the obtained semi-steel to the charging bay and pour it into an AOD furnace. Add scrap steel. Blow oxygen from the top and side for decarburization in the AOD furnace. Add high-carbon ferromanganese, lime, electrolytic manganese, aluminum pellets and fluorite from the high-level bin in stages for decarburization, reduction and primary alloying of Mn. At the same time, reduce the residual Si element and Cr element in the AOD furnace lining to achieve primary alloying of Si and Cr; The AOD tapping temperature is 1615 - 1650℃. After being treated in the AOD furnace, the initial high-chromium, high-carbon, high-manganese molten steel is obtained. Its chemical composition, by mass percentage, contains C: 0.85 - 0.95%, Si: 0.10 - 0.20%, Mn: 11.0 - 12.5%, Cr: 1.0 - 2.0%, and the rest is Fe and inevitable impurities; In step 2, the AOD deoxidation adopts the full-aluminum reduction method. The slag basicity, calculated as (CaO) / (SiO2 + Al2O3), is controlled at 2.9 - 3.2 during the oxidation stage and 2.5 - 2.8 during the reduction stage.

[0009] Step 3, LF furnace refining: Lift the initial high-chromium, high-carbon, high-manganese molten steel obtained after being treated in the AOD furnace in step 2 to the LF furnace. Add 1 - 2 Kg / t of fluorite to raise the temperature and melt the slag, and then add alloy materials to fine-tune the chemical composition to achieve secondary alloying; Adjust the bottom blowing flow rate to 20 L / min, blow open the slag surface by 200 mm, and the weak blowing time is 25 min. The LF furnace tapping temperature is 1465 - 1485℃; After being treated in the LF furnace, the high-chromium, high-carbon, high-manganese molten steel is obtained. Its chemical composition, by mass percentage, contains C: 0.90 - 1.30%, Si: 0.30 - 0.80%, Mn: 11.5 - 14.0%, Cr: 1.0 - 2.5%, P ≤ 0.025%, S ≤ 0.015%, and the rest is Fe and inevitable impurities.

[0010] Step 4, slab continuous casting: The high-chromium, high-carbon, high-manganese molten steel obtained after being treated in the LF furnace in S3 is hoisted to a slab continuous caster, the casting speed is 0.6 - 0.8 m / min, and the superheat of the molten steel is 25 °C to obtain qualified slabs.

[0011] The beneficial effects of the present invention are as follows: 1. The present invention uses a dephosphorization converter to dephosphorize hot metal to P ≤ 0.005%, uses an AOD to protect carbon and desulfurize, and the LF furnace finely adjusts the chemical composition and temperature. High-carbon tapping reduces inclusions in steel and saves carburizer. Without refining by RH or VD vacuum equipment, the process flow is short, the smelting efficiency is high, and the purity of the molten steel is high; 2. The present invention uses the residual Cr and Si elements after smelting stainless steel in the AOD furnace to increase Cr and Si, saves ferrochrome alloy and ferrosilicon alloy, realizes the alloying of Mn element in the AOD furnace, has a high alloy yield rate and low smelting cost. Description of the Drawings

[0012] Figure 1 It is a process flow schematic diagram of the present invention. Detailed Embodiments

[0013] The technical solutions of the present invention will be described in detail below in conjunction with the drawings and embodiments.

[0014] Example 1 This example is applied to a 100t AOD furnace. As Figure 1 shown, the process route is dephosphorization converter → AOD → LF → slab continuous casting. The specific steps include: Step 1, converter dephosphorization: Use a metallurgical crane to pour 95t of blast furnace hot metal into the dephosphorization converter, add scrap steel 7.1t, the scrap ratio is 7.5%, blow oxygen from the top and nitrogen from the bottom, the top blowing gas flow rate is 28000m 3 / h, and the bottom blowing gas flow rate is 2550 3 / h; Add 10.5 Kg / t of active lime for high-speed desiliconization and dephosphorization, and the blowing time is 7.6 min. After obtaining semi-steel, tap the steel; The semi-steel, by chemical composition in mass percentage, is C: 3.15%, Mn: 0.19%, P: 0.003%, S: 0.049%, and the rest are Fe and inevitable impurities. The tapping temperature of the semi-steel is 1331 °C.

[0015] Through Step 1, the hot metal can be dephosphorized to P ≤ 0.005% to obtain semi-steel with a high C content and a low P content, creating conditions for efficient refining in the AOD.

[0016] Step 2, AOD refining: Return the semi-steel obtained in Step 1 to the charging bay, and pour it into a 100t AOD furnace. Add 3.5t of scrap steel. Blow oxygen from the side of the top of the AOD furnace for decarburization while blowing from the bottom. Add ferromanganese, lime, electrolytic manganese, aluminum pellets and fluorite from the high-level bin in stages for decarburization, reduction and primary alloying of Mn. At the same time, reduce the residual Si and Cr elements in the AOD furnace lining to achieve primary alloying of Si and Cr. The tapping temperature of the AOD is 1620°C; After being treated by the AOD furnace, the initial high-chromium, high-carbon and high-manganese molten steel is obtained. Its chemical composition is by mass percentage: C: 1.20%, Si: 0.11%, Mn: 11.3%, Cr: 1.1%, and the rest is Fe and inevitable impurities.

[0017] In Step 2, the AOD deoxidation adopts the full-aluminum reduction method. The basicity of the slag is calculated as (CaO) / (SiO2 + Al2O3): controlled at 3.2 in the oxidation stage and 2.8 in the reduction stage.

[0018] Through Step 2, the primary alloying of the molten steel is realized. There is no need to blow low C in a conventional converter to achieve the goal of dephosphorization. High-carbon tapping reduces inclusions in the steel and saves carburizer. After smelting stainless steel in the AOD furnace, the residual Cr and Si elements are used to increase Cr and Si, saving ferrochrome alloy and ferrosilicon alloy. The Mn element is alloyed in the AOD furnace, with high alloy yield and low smelting cost.

[0019] Step 3, LF furnace refining: Lift the initial high-chromium, high-carbon and high-manganese molten steel obtained after being treated by the AOD furnace in Step 2 to the LF furnace. Add 1.1 Kg / t of fluorite to the molten steel to raise the temperature and melt the slag. Then add alloy materials to fine-tune the chemical composition to achieve secondary alloying. The bottom blowing flow rate is adjusted to 20 L / min, the slag surface is blown open by 200 mm, and the weak blowing time is 25 min. The tapping temperature of the LF furnace is 1467°C; After being treated by the LF furnace, the high-chromium, high-carbon and high-manganese molten steel is obtained. Its chemical composition is by mass percentage: C: 1.25%, Si: 0.72%, Mn: 11.8%, Cr: 1.1%, P: 0.009%, S ≤ 0.003%, and the rest is Fe and inevitable impurities.

[0020] Through the LF refining in Step 3, without refining by RH or VD vacuum equipment, it has the advantages of short process flow, high smelting efficiency and high purity of the molten steel.

[0021] Step 4, continuous casting: Lift the high-chromium, high-carbon and high-manganese molten steel obtained after being treated by the LF furnace in Step 3 to the slab continuous caster. The typical casting speed is 0.7 m / min, and the superheat of the molten steel is 25°C to obtain qualified slabs.

[0022] Example 2 This embodiment is applied to a 100t AOD furnace, and the process route is: phosphorus removal converter → AOD → LF → slab continuous casting. The specific steps are as follows: Step 1, converter dephosphorization: Use a metallurgical crane to pour 93t of hot metal from the blast furnace into the phosphorus removal converter, and add 8t of scrap steel. The scrap steel ratio is 8.6%. Blow oxygen from the top and nitrogen from the bottom. The top blowing gas flow rate is 30000m 3 / h, and the bottom blowing gas flow rate is 2800 3 / h; Add 12.5 Kg / t of active lime for high-speed desiliconization and dephosphorization. The blowing time is 8.5 min. After obtaining semi-steel, tap the steel. By mass percentage, the chemical composition of the semi-steel is: C: 2.98%, Mn: 0.15%, P: 0.003%, S: 0.031%, and the rest is Fe and unavoidable impurities. The tapping temperature of the semi-steel is 1350 °C.

[0023] Through Step 1, the dephosphorization of hot metal can be ≤0.005%, obtaining semi-steel with a high C content and a low P content, creating conditions for efficient refining in the AOD furnace.

[0024] Step 2, AOD refining: Return the semi-steel obtained in Step 1 to the charging bay and pour it into a 100t AOD furnace. Add 2.8t of scrap steel. Blow oxygen for decarburization by combined blowing from the top side of the AOD furnace. Add high-carbon ferromanganese, lime, electrolytic manganese, aluminum pellets, and fluorite in stages from the high-level bin for decarburization, reduction, and primary alloying of Mn. At the same time, reduce the residual Si and Cr elements in the AOD furnace lining to achieve primary alloying of Si and Cr. The tapping temperature of the AOD is 1636 °C; After being treated in the AOD furnace, the initial high-chromium, high-carbon, high-manganese molten steel is obtained. By mass percentage, its chemical composition is: C: 1.0%, Si: 0.15%, Mn: 12.5%, Cr: 1.3%, and the rest is Fe and unavoidable impurities.

[0025] In Step 2, the AOD deoxidation adopts the full-aluminum reduction method. The basicity of the slag is calculated as (CaO) / (SiO2 + Al2O3): controlled at 3.0 in the oxidation stage and 2.6 in the reduction stage.

[0026] Through Step 2, the primary alloying of molten steel is achieved. There is no need to blow low C as in a conventional converter to achieve the goal of dephosphorization. High-carbon tapping reduces inclusions in the steel and saves carburizer. After smelting stainless steel in the AOD furnace, the residual Cr and Si elements are used to increase Cr and Si, saving ferrochromium alloy and ferrosilicon alloy. The Mn element is alloyed in the AOD furnace, with a high alloy recovery rate and low smelting cost.

[0027] Step 3, LF furnace refining: Lift the initial high-chromium, high-carbon, high-manganese molten steel obtained after AOD furnace treatment in Step 2 to the LF furnace, add 1.5 Kg / t of steel of fluorite to raise the temperature and melt the slag, then add alloy materials to finely adjust the chemical composition to achieve secondary alloying. Adjust the bottom blowing flow rate to 20 L / min, blow open the slag surface by 200 mm, and the weak blowing time is 25 min. The tapping temperature of the LF furnace is 1472 °C. After being treated by the LF furnace, high-chromium, high-carbon, high-manganese molten steel is obtained. Its chemical composition is by mass percentage: C: 1.05%, Si: 0.50%, Mn: 13%, Cr: 1.35%, P: 0.015%, S: 0.004%, and the rest is Fe and unavoidable impurities.

[0028] Through the LF refining in Step 3, without refining by RH or VD vacuum equipment, it has the advantages of short process flow, high smelting efficiency, and high purity of molten steel.

[0029] Step 4, continuous casting: Lift the high-chromium, high-carbon, high-manganese molten steel obtained after LF furnace treatment in Step 3 to the slab continuous caster, and the typical casting speed is 0.7 m / min, and the superheat of the molten steel is 25 °C to obtain qualified slabs.

[0030] Example 3 This example is applied to a 100t AOD furnace, and the process route is dephosphorization converter → AOD → LF → slab continuous casting. The specific steps include: Step 1, converter de-P: Use a metallurgical crane to pour 90t of blast furnace hot metal into the dephosphorization converter, add 9t of scrap steel, and the scrap ratio is 10%. Blow oxygen from the top and nitrogen from the bottom. The top blowing gas flow rate is 32000 m 3 / h, and the bottom blowing gas flow rate is 3000 3 / h; Add 15 Kg / t of steel of active lime for high-speed desiliconization and dephosphorization, and the blowing time is 9.8 min. After obtaining semi-steel, tap the steel. The semi-steel, by chemical composition by mass percentage, is C: 3.17%, Mn: 0.19%, P: 0.005%, S: 0.020%, and the rest is Fe and unavoidable impurities. The tapping temperature of the semi-steel is 1372 °C.

[0031] Through Step 1, the de-P of hot metal can be ≤0.005%, and semi-steel with a high C content and a low P content can be obtained, creating conditions for efficient AOD refining.

[0032] Step 2, AOD refining: Return the semi-steel obtained in Step 1 to the charging bay and pour it into a 100t AOD furnace. Add 3.5t of scrap steel. Blow oxygen from the top and side for decarburization in the AOD furnace. Add high-carbon ferromanganese, lime, electrolytic manganese, aluminum pellets and fluorite from the high-position bin in stages for decarburization, reduction and primary alloying of Mn. At the same time, reduce the residual Si and Cr elements in the AOD furnace lining to achieve primary alloying of Si and Cr. The tapping temperature of the AOD furnace is 1636 °C; After being treated by the AOD furnace, the initial high-chromium, high-carbon, high-manganese molten steel is obtained. Its chemical composition is calculated by mass percentage: C: 0.9%, Si: 0.20%, Mn: 13.5%, Cr: 1.8%, and the rest is Fe and inevitable impurities.

[0033] In step 2, the AOD deoxidation adopts the full-aluminum reduction method. The basicity of the slag is calculated as (CaO) / (SiO2 + Al2O3): it is controlled at 3.2 in the oxidation stage and 2.8 in the reduction stage.

[0034] Through step 2, the primary alloying of the molten steel is achieved. There is no need to blow low C in a conventional converter to achieve the goal of dephosphorization. High-carbon tapping reduces inclusions in the steel and saves carburizer. The residual Cr and Si elements after smelting stainless steel in the AOD furnace are used to increase Cr and Si, saving ferrochromium alloy and ferrosilicon alloy. The Mn element is alloyed in the AOD furnace, with high alloy recovery rate and low smelting cost.

[0035] Step 3, LF furnace refining: The initial high-chromium, high-carbon, high-manganese molten steel obtained after being treated by the AOD furnace in step 2 is lifted to the LF furnace. 1.8 Kg / t of steel of fluorite is added to heat up and melt the slag, and then alloy materials are added to slightly adjust the chemical composition to achieve secondary alloying. The bottom blowing flow rate is adjusted to 20 L / min, the slag surface is blown open by 200 mm, and the weak blowing time is 25 min. The tapping temperature of the LF furnace is 1478 °C; After being treated by the LF furnace, the high-chromium, high-carbon, high-manganese molten steel is obtained. Its chemical composition is calculated by mass percentage: C: 0.95%, Si: 0.32%, Mn: 14%, Cr: 1.85%, P: 0.022%, S: 0.005%, and the rest is Fe and inevitable impurities.

[0036] Through the LF refining in step 3, without refining by RH or VD vacuum equipment, it has the advantages of short process flow, high smelting efficiency, and high purity of the molten steel.

[0037] Step 4, continuous casting: The high-chromium, high-carbon, high-manganese molten steel obtained after being treated by the LF furnace in step 3 is lifted to the slab continuous caster. The typical casting speed is 0.7 m / min, and the superheat of the molten steel is 25 °C to obtain qualified slabs.

Claims

1. A smelting process for high-chromium, high-carbon and high-manganese wear-resistant steel with low cost, characterized in that, It includes the following steps: Step 1, converter dephosphorization: Pour blast furnace hot metal into a dephosphorization converter, add scrap steel with a scrap ratio of 7% - 10%, blow oxygen from the top and nitrogen or carbon dioxide gas from the bottom; add 10 - 15 Kg / t of steel of active lime for high-speed desiliconization and dephosphorization, and the blowing time is 7 - 10 min. After obtaining semi-steel, tap the steel. Step 2, AOD refining: Return the semi-steel to the charging bay and pour it into the AOD furnace, add scrap steel, blow oxygen for decarburization by combined blowing from the top side of the AOD furnace, and add high-carbon ferromanganese, lime, electrolytic manganese, aluminum pellets and fluorite in stages from the high-level bin for decarburization, reduction and primary alloying of Mn. At the same time, reduce the residual Si element and Cr element in the AOD furnace lining to achieve primary alloying of Si and Cr; the tapping temperature of the AOD furnace is 1615 - 1650 °C, and the initial high-chromium, high-carbon and high-manganese molten steel is obtained after being treated by the AOD furnace. Step 3, LF furnace refining: Lift the initial high-chromium, high-carbon and high-manganese molten steel to the LF furnace, add 1 - 2 Kg / t of steel of fluorite to heat up and melt the slag, then add alloy materials to slightly adjust the chemical composition to achieve secondary alloying. Adjust the bottom blowing flow rate to 20 L / min, blow open the slag surface by 200 mm, and the weak blowing time is 25 min. The tapping temperature of the LF furnace is 1465 - 1485 °C, and the high-chromium, high-carbon and high-manganese molten steel is obtained after being treated by the LF furnace. Step 4, continuous casting: Lift the high-chromium, high-carbon and high-manganese molten steel to the slab continuous caster, the casting speed is 0.6 - 0.8 m / min, and the superheat of the molten steel is 25 °C to obtain qualified slabs.

2. The smelting process of a high-chromium, high-carbon, high-manganese wear-resistant steel with low cost according to claim 1, characterized in that, In step 2, the AOD deoxidation adopts the full-aluminum reduction method, and the basicity of the slag is calculated as (CaO) / (SiO2 + Al2O3): controlled at 2.9 - 3.2 in the oxidation stage and 2.5 - 2.8 in the reduction stage.

3. A smelting process for a high-chromium, high-carbon and high-manganese wear-resistant steel with low cost, characterized in that, In step 1, the top blowing gas flow rate is 27,000 - 32,000 m 3 / h, and the bottom blowing gas flow rate is 2,500 - 3,000 m 3 / h.

4. A smelting process for high-chromium, high-carbon and high-manganese wear-resistant steel with low cost according to claim 1, characterized in that, In step 1, the semi-steel, by chemical composition in mass percentage, is: C: 2.5 - 3.2%, Mn: 0.05 - 0.30%, P ≤ 0.005%, S ≤ 0.050%, and the rest is Fe and inevitable impurities; the tapping temperature of the semi-steel is 1320 °C - 1380 °C.

5. A smelting process for high-chromium, high-carbon and high-manganese wear-resistant steel with low cost according to claim 1, characterized in that, In step 2, the chemical composition of the initial high-chromium, high-carbon and high-manganese molten steel in mass percentage is: C: 0.85 - 0.95%, Si: 0.10 - 0.20%, Mn: 11.0 - 12.5%, Cr: 1.0 - 2.0%, P ≤ 0.015%, S ≤ 0.005%, and the rest is Fe and inevitable impurities.

6. A smelting process for high-chromium, high-carbon and high-manganese wear-resistant steel with low cost according to claim 1, characterized in that, In step 3, the chemical composition of the high-chromium, high-carbon and high-manganese molten steel in mass percentage is: C: 0.90 - 1.30%, Si: 0.30 - 0.80%, Mn: 11.5 - 14.0%, Cr: 1.0 - 2.5%, P ≤ 0.025%, S ≤ 0.005%, and the rest is Fe and inevitable impurities.

Citation Information

Patent Citations

  • Method for smelting high manganese steel in converter

    CN116590488A