Substrate comprising nanowires
By integrating nanowire structures on microstructure substrates and using atomic layer deposition and dry etching technology, the problem of increasing the surface area of microstructure substrates is solved, and the efficient storage capacity and electrochemical performance of energy storage devices are improved.
Patent Information
- Application Number
- CN202380072293.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-11
- Filing Date
- 2023-10-10
- Publication Date
- 2025-08-01
AI Technical Summary
The prior art is difficult to effectively increase the available surface area of microstructure substrates at the micro or nanoscale, affecting the performance of energy storage devices.
By integrating nanowire structures on microstructure substrates, using atomic layer deposition technology and dry etching methods, elongated nanowires are formed to increase surface area, and thermal annealing is performed in combination with gas-liquid-solid synthesis technology to control the growth of nanowires.
The expanded surface area of the microstructure substrate is significantly increased, and the storage capacity and electrochemical performance of energy storage devices are improved.
Smart Images

Figure CN120418913A_ABST
Abstract
Description
[0001] The present invention relates to the field of micro - energy storage devices. More specifically (but not exclusively), the present invention relates to planar substrates and / or micro - structured substrates, on the surface of which sub - structures with dimensions measurable on the nanoscale are integrated. The present invention also relates to a method for manufacturing said sub - structures.
[0002] References in the text described below are marked in the text in the following way: []; and are listed in the reference table. Background Art
[0003] Substrates for manufacturing energy storage devices are made, for example, of carriers made of semiconductor or dielectric materials and can take the form of thin discs, also called "wafers". Initially, such a carrier has a planar surface corresponding to a two - dimensional (2D) topology. However, depending on the intended use of the substrate, it is advantageous to hollow out the surface of the substrate on the micron or nanoscale such that the surface presents a three - dimensional (3D) topology, thereby forming a micro - structured or nano - structured substrate.
[0004] Such a micro - structured substrate has a larger available surface area, i.e., the unfolded surface area, compared to a planar (or smooth) substrate. A micro - structured substrate can deposit a larger amount of material on its surface, especially on the side surfaces of the micro - structures, which can, for example, improve the performance of electrical energy storage devices, increase the number of components that can be integrated on the substrate, etc.
[0005] For example, a micro - structured silicon substrate with a surface area gain related to its rough structure is described in patent application [1]. Such micro - structures are generally achieved by surface treatment, such as chemical or physical etching, micro - structure growth, or electrodeposition of materials inside a mold at the micron or even nanoscale, followed by dissolution of the mold.
[0006] Energy storage devices cannot avoid the continuous need for miniaturization of electronic components. There has always been a need to develop solutions that can increase the available surface area visible outside the substrate while maintaining the dimensions of the original carrier used to manufacture the substrate; especially since it has been demonstrated that increasing the available surface area can improve the performance of solid - state micro - batteries, micro - capacitors, or micro - supercapacitors.
[0007] To meet this need, a first object of the present invention is to modify the surface of a micro - structured or nano - structured substrate to increase its available surface area.
[0008] In addition, methods are known for forming thin layers of material on a substrate, such as methods for producing a lithium-containing material layer. These layered substrates are particularly used in batteries, for example for forming electrodes or electrolyte barrier layers, or for any other electrical storage device. These layers can be deposited by techniques such as Atomic Layer Deposition (ALD, usually abbreviated as ALD), Chemical Vapor Layer Deposition (ALCVD, usually abbreviated as ALCVD), or Atomic Layer Epitaxy (ALE) deposition techniques using precursors. In particular, the ALD technique is a thin film deposition technique based on gas-solid reactions, aiming to expose the surface on which a layer of material is desired to be deposited to different successive chemical precursors.
[0009] Patent application [2] describes a method that implements atomic layer deposition of a precursor of a first metal, which can be an organometallic complex, for example containing a transition metal (such as nickel) or other types of metals such as aluminum; this method is capable of manufacturing a compound containing a thin layer of a lithium-containing material. The thickness of these layers is from 1 nm to 1 μm, composed of complex, electrochemically active materials, and these materials are, among other characteristics, uniform and adapted to conform to the more or less complex surface undulations of a microstructured substrate.
[0010] A second object of the present invention is to modify the surface of a substrate to increase its available surface area by implementing such a layer deposition method compatible with a microstructured substrate, the surface of which is complex and difficult to obtain by any surface treatment method of the prior art.
[0011] Patent application [3] describes a composite substrate composed of the following parts: a glass layer coated with a metal layer usually of molybdenum (Mo), indium (In) microcolumns perpendicular to the surface of the substrate and convex at the top, a copper (Cu) layer covering the convex tops of these indium microcolumns, and copper(I) sulfide (Cu2S) nanowires growing only starting from the tops of the microcolumns. Summary of the Invention
[0012] The present invention relates to a microstructured substrate comprising a body and a plurality of elongated basic microstructures extending from the body, characterized in that the microstructured substrate comprises a plurality of nanowires located on at least one region of the surface of the body and on the surface of the basic microstructures extending from the body within this region. This substrate structure integrated with nanowires can further increase the developed surface area by at least 10 times, thereby correspondingly increasing the storage capacity of a storage device integrating the above substrate.
[0013] Within the scope of the present invention, the terms "microstructured" or "microstructure" apply indifferently to surfaces with undulations, the shape of which has dimensions measurable both in the micrometer and nanometer scales.
[0014] Preferably, the elongate basic microstructures are microcolumns or microtubes (a microtube being a microcolumn hollowed out at its center).
[0015] According to the present invention, the body of the microstructured substrate and the basic microstructures extending along the body are advantageously made of the same material, preferably selected from materials consisting of or comprising: silicon (Si), silicon dioxide (SiO2), gallium arsenide (GaAs), silicon nitride (Si3N4), and indium phosphide (InP).
[0016] Preferably, the basic microstructures include a cross-section selected from circular, oval, rectangular, square, and triangular cross-sections.
[0017] Preferably, the nanowires comprise a material selected from oxides, preferably selected from silicon dioxide (SiO2), zinc oxide (ZnO), and titanium dioxide (TiO2), and preferably, the nanowires consist only of SiO2.
[0018] Preferably, the nanowires have a cross-section with a diameter of 20 nm to 250 nm and a length of 100 nm to 10 μm. Advantageously, the nanowires have a cross-section with a diameter of 50 nm to 200 nm and a length of 0.5 μm to 2 μm. The structure of these nanowires is characterized by electron microscopy techniques, more specifically by scanning electron microscopy (SEM), and the evaluation of the nanowire size and structure is performed using images collected by this technique.
[0019] Preferably, the developed surface area of the region containing the nanowires is 2 to 50 times, advantageously 10 to 40 times, and even 15 to 35 times the developed surface area of the region without nanowires. The surface area gain associated with the presence of the nanowires is indirectly measured by an electrochemical method using capacitive, Faradaic, or pseudocapacitive materials (the electrochemical properties of which are intrinsically related to the developed surface area). The developed surface area is a representation of the total surface area introduced by creating pores and tortuosity by adding micro- and nano-objects relative to the initial object; this is typically represented by a value greater than 1 (i.e., surface area gain) (where 1 represents the surface area gain of the initial object).
[0020] The present invention also relates to a method for manufacturing a planar substrate or a microstructured substrate as described above in connection with the present invention, the method comprising the following steps: a - covering a planar substrate or a microstructured substrate with a thin layer of SiO2; b - depositing a layer of non-oxidized metal using an atomic layer deposition technique; c - Perform lithography on at least one region of the surface of the planar or microstructured substrate that has undergone steps a - and b -; d - Perform an etching process; and e - Perform thermal annealing, preferably by implementing at least one temperature stage.
[0021] Step a - advantageously includes depositing a SiO2 nanometer thin film by low - pressure chemical vapour deposition (also abbreviated as "LPCVD").
[0022] Step b - includes Atomic Layer Deposition (also abbreviated as "ALD"). The layer deposited by this atomic layer deposition technique is deposited using precursors, as described in reference [2], by Atomic Layer Chemical Deposition (usually abbreviated as "ALCVD") or by Atomic Layer Epitaxy (usually abbreviated as "ALE"). In particular, the ALD technique is a thin - film deposition technique based on gas - solid reactions, aiming to expose the surface on which a layer of material is desired to be deposited to different consecutive chemical precursors.
[0023] The lithography in step c - aims to limit the growth of SiO2 nanowires only to the substrate regions where nanowires are desired to exist. Such a step allows the formation of a resin mask that protects these target regions (which are a few square millimeters) where nanowires are desired to exist and leaves the areas of the substrate not covered by the mask "bare" to the material (catalyst) from the precursor.
[0024] The dry - etching catalyst in step d - is for retaining it only on the target regions, and this step is advantageously carried out by reactive ion etching (also known as "RIE"). Preferably, the RIE etching is carried out using a RIE - ICP device sold by a company as a reactor, such as a device known by the model Sentech Si500 (ICP - RIE). This dry - etching is based on generating a reactive plasma in a reactor at a pressure of 5 mTorr, preferably at 10 °C, based on a gas mixture of Cl2 / Ar (10 sccm, 30 sccm).
[0025] Step e - Advantageously, an annealing is carried out implementing the vapour - liquid - solid synthesis technique (also abbreviated as "VLS"); the advantage of this technique is that it does not require the use of a gaseous silane precursor as is commonly known in the literature. The growth is directly related on the one hand to the transformation of the SiO2 thin layer generated in step a - into the gaseous phase and on the other hand to the presence of the catalyst generated in step b -. Advantageously, step e - comprises at least two stages: a first stage allowing the formation of metal clusters to control the diameter of the future nanowires; a second stage capable of triggering the nanowire growth phenomenon.
[0026] Preferably, the non - oxidizing metal deposited in step b - is selected from platinum, silver, gold, gallium, indium, titanium, tin, zinc, antimony, copper, nickel, beryllium, iron, cobalt, chromium, aluminum, ruthenium, rhodium and palladium, preferably consisting of platinum. It should be noted that the precursor of the first metal can be in liquid or powder form. For example, the precursor of the first metal can be selected from the following precursors: MeCpPtMe3, FeCl2, FeCp2, Fe(thd)3, La(thd)3, CoCp2, MnCp2, Mn(thd)3, NiCp2, TiCl4, NbOEt5, Cr(OCl)2, preferably consisting of MeCpPtMe3.
[0027] Preferably, step e - comprises two temperature stages: a first stage of 200 °C to 1200 °C applied for less than 5 minutes; and a second stage of 300 °C to 1400 °C applied for less than 15 minutes.
[0028] The present invention also relates to a use of a micro - structure substrate as described above in connection with the present invention for manufacturing a micro - energy storage device, which device is preferably selected from: batteries, supercapacitors and dielectric and electrolytic capacitors of micron - or even nano - scale dimensions, energy recovery components, or a type of sensor device requiring the use of a large specific surface area.
[0029] The present invention is also described in the following detailed description by means of an experimental part which details some embodiments by way of examples, which examples are given only by way of illustration and should not be considered restrictive, and the present invention is also described by means of the drawings which will be briefly described in the following part. Description of the Drawings
[0030] Figure 1 – Figure 1 Shows X - ray reflectometry (XRR) measurements carried out on a thin layer of nickel oxide (NiO) deposited by ALD on a silicon substrate;
[0031] Figure 2 – Figure 2 Shows a scanning electron microscope (SEM) view after synthesizing nanowires by the VLS (vapor-liquid-solid mechanism) technique;
[0032] Figure 3 – Figure 3 Shows the curve of rapid thermal annealing (RTA) for growing SiO2 nanowires;
[0033] Figure 4 – Figure 4 Shows the XRR measurement results of platinum (Pt) thin films with thicknesses of 5 nm, 10 nm, 15 nm, and 20 nm;
[0034] Figure 5A Figure 5B Figure 5C Figure 5D – Figures 5A to 5D Shows the image obtained by SEM for a SiO2 layer thickness of 15 nm and a Pt layer thickness of 10 nm;
[0035] Figure 6 – Figure 6 Shows the SEM magnification of the substrate surface after being annealed at 900 °C for 1 minute;
[0036] Figure 7 – Figure 7 Shows the SEM magnification of the substrate surface after being annealed at 950 °C for 1 minute;
[0037] Figure 8 – Figure 8 Shows the SEM magnification of the substrate surface after being annealed at 900 °C for 1 minute and then at 1050 °C for 3 minutes;
[0038] Figure 9 – Figure 9 Shows the SEM magnification of the substrate surface after being annealed at 950 °C for 1 minute and then at 1100 °C for 3 minutes; and
[0039] Figure 10 – Figure 10 Shows the variation of the normalized areal capacitance of ruthenium dioxide (RuO2) thin films deposited on different types of substrates with the scan rate, which enables the estimation of the effective electrochemical gain. Experimental section
[0040] Materials and Methods The reagents used were purchased from Chemical Company and used without further purification.
[0041] Surface Area Measurement The surface area gain (area enlargement factor, AEF) was indirectly measured by cyclic voltammetry in a three - electrode system. The electrolyte used was sulfuric acid (H2SO4) diluted to 0.5 M, the reference electrode was an Ag / AgCl electrode, the counter electrode was made of platinum, and the working electrode corresponded to the fabricated sample, which was covered with a thin platinum layer (30 nm) deposited by ALD (microstructured substrate, i.e., hierarchical skeleton). The scan rate was 50 mV / s.
[0042] Measurement of Deposited Film Thickness The thickness of the layer was measured by X - ray reflectometry (XRR), which is an interferometric technique capable of obtaining quantitative information about interface roughness, density, and the thickness of amorphous or crystalline thin layers. The measurement was carried out after the alignment stage of the sample height and surface. This measurement involved directing an X - ray beam onto the sample surface at a low incident angle θ and collecting the reflected intensity. A measurement result was obtained that could depict the variation of the reflected intensity with the incident angle (2θ), as Figure 1 shown. The curve typically exhibits a plateau at 2θ < θ c (where θ c corresponds to the critical angle), followed by a decline containing one or more oscillations, and the period of the oscillations is related to the thickness of the layer by the following relationship: where m is the order of the oscillation, θ m is the corresponding angle in radians (as Figure 1 shown), and d is the thickness of the layer.
[0043] The slope of the oscillations can be used to deduce the surface roughness. The change in slope after the oscillations can be used to deduce the density of the layer. X - ray reflectometry is a technique capable of accurately measuring the thickness of thin layers (about 5 nm to 100 nm) using Equation 1, provided that the layer has low roughness, which makes it the preferred technique for ALD depositions carried out within the scope of this work. The X - ray reflectometry measurements were carried out on a company's rotating copper anode system.
[0044] The surface morphology of the sample was observed by top - down, cross - sectional, and grazing - incidence scanning electron microscopy (SEM) using a FEI Magellan 400 TM .
[0045] The nanowire size distribution was carried out by SEM, and the nanowire size measurement was performed using ImageJ TM software.
[0046] Within the scope of the present invention, the mass percentage expressed as % w / w defines the mass percentage of a certain component used in the preparation, which is relative to the total mass of the object under consideration (mixture, material (such as composite material, etc.), film, etc.). Examples
[0047] Part 1: Synthesis of silicon dioxide (SiO2) by dry oxidation (LPCVD, low-pressure chemical vapor deposition) - Wafer cleaning: Piranha cleaning solution (mixture of sulfuric acid H2SO4 and hydrogen peroxide H2O2) 1:1 (20 minutes), rinsing with deionized water, drying with N2, HF 1% (2 minutes), EDI rinsing, drying with N2; - Introduce the silicon wafer into the furnace under a N2 atmosphere at 500 °C and 2 slm (standard liters per minute, at T = 0 °C and P = 1 bar); - Heat up to 675 °C within 30 minutes (10 °C / minute); - Heat up to 900 °C within 1 hour (10 °C / minute); - Pre-oxidize at 900 °C for 30 minutes, introducing 2 slm of N2 and 0.2 slm of O2; - Oxidize at 900 °C for 42 minutes (15 nm of SiO2 – deposition rate 0.357 nm / minute), introducing 2 slm of O2; - Cool down to 500 °C within 1 hour, introducing 2 slm of N2.
[0048] Part 2: Deposition of Pt catalyst by atomic layer deposition (ALD)
[0049] Deposit a platinum layer by ALD, with the reactants being "Pt" and molecular oxygen.
[0050] Place the sample obtained in Part 1 into the ALD chamber (Beneq model TFS200), reduce the pressure to 2 mBar, and adjust the temperature to 300 °C.
[0051] To form an atomic monolayer, different steps (corresponding to one cycle) are required: Inject nitrogen into the source containing the first reactant (1) (i.e., MeCpPtMe3, (trimethyl)methylcyclopentadienylplatinum(IV), provided by Chemical Company, marked with a purity of 99%, whose temperature is maintained at 54 °C) for 500 ms, wait for 100 ms to increase the pressure in the precursor chamber, and then the source is opened for 500 ms (pulse time). Then perform a 2 - second purge to expel excess substances and reaction products. Then inject the second reactant (2) in the form of gaseous O2 for 500 ms, and then perform a 1 - second purge. The deposition rate is (angstroms / cycle), and the deposition thickness can be precisely controlled between 5 nm and 60 nm.
[0052] Part 3: Lithography to select the target area
[0053] 1 - Wafer cleaning and deoxidation:
[0054] Place the wafer obtained in Part 2 into an acetone beaker for 5 minutes, and then into isopropyl alcohol for 5 minutes to degrease the wafer. Then dry the wafer at 110 °C for 10 minutes.
[0055] 2 - Glue coating and exposure:
[0056] Coat with hexamethyldisilazane (HMDS) adhesion promoter (speed = 2000 revolutions per minute (rpm); acceleration = 1000 revolutions per minute per second (rpm / s); time = 20 s).
[0057] Coat with AZ1505 resin (speed = 3000 revolutions per minute; acceleration = 1000 revolutions per minute per second; time = 20 s).
[0058] Anneal at 110 °C for 1 minute without relaxation time.
[0059] Expose for 3 s in hard contact mode without relaxation time.
[0060] Develop in MIF 726 for 50 s, and then rinse with deionized water for 30 s.
[0061] This lithography can form a resin mask that protects a target area of several square millimeters and leaves the area on the substrate where platinum is not covered by the mask "exposed".
[0062] Part 4: Dry etching of the catalyst to retain it only in the target area
[0063] Platinum etching is carried out by RIE - ICP This physical - chemical dry etching is achieved by physically bombarding with Cl2 / Ar (10 sccm, 30 sccm) plasma in a reactor at a pressure of 5 mTorr and a temperature of 10 °C. The ICP source generates a high - density plasma through inductive coupling between the RF antenna and the plasma. The RF antenna generates an alternating RF magnetic field and induces an RF electric field, which accelerates the electrons participating in the ionization of gas molecules. For platinum etching, the power of the power supply is set to 600 W, while the power of the RF generator is set to 200 W. The etching rate is (angstroms per second, i.e., 10 - 10 meters per second: this is the speed at which platinum is etched to form the structure).
[0064] Part 5: Rapid Thermal Annealing (RTA)
[0065] Annealing is carried out in a rapid thermal annealing furnace sold by the company in two stages under a nitrogen atmosphere.
[0066] The synthesis technique implemented is called vapor - liquid - solid (VLS). The first stage at 1000 °C (10 °C / second) is maintained for 1 minute to de - wet the Pt catalyst. In this step, small Pt clusters (i.e., droplets) with diameters of several tens of nanometers form on the SiO2 surface, and gaseous SiO is formed. SiO diffuses into the droplets and precipitates at the metal / substrate interface during the second supersaturation / precipitation stage. This leads to the growth of SiO2 nanowires. The growth is directly related to the transformation of the previously synthesized SiO2 layer on the substrate in Part 1 into the gaseous phase and the presence of the catalyst (here platinum).
[0067] The second stage at 1100 °C is maintained for 5 minutes to promote the growth of SiO2 nanowires. The diameter, length, and density (number of nanowires per mm 2 of nanowires) are controlled by the properties of the initial SiO2 and Pt thin films and the annealing parameters (holding temperature and time in the high - temperature stage, the first stage allows the formation of Pt clusters to control the future diameter of the nanowires; the second stage triggers the growth phenomenon by controlling the nanowire length). The images obtained by SEM magnification are shown in Figure 2 with a scale for observing the nanowire dimensions. Figure 3 The curve of temperature change with time for each stage is shown. Analysis and Results
[0068] After thermal annealing by examining different thickness parameters of the SiO2 thin layer and Pt layer (5 nm, 10 nm, 15 nm, 20 nm), different silicon samples were processed. The Pt thin layer was measured by XRR, and the spectra are shown in Figure 4 .
[0069] The samples were observed by SEM microscope.
[0070] By changing the thickness of SiO2 from 10 nm to 15 nm, the inventors observed the presence of very robust match - stick - shaped nanowires that are strictly perpendicular to the surface, with an average length greater than 1 μm and a diameter possibly greater than 80 nm.
[0071] The statistical study of the SEM images can determine the average nanowire diameter and length parameters. The general method involves processing and analyzing the images to define the boundaries of the constituent objects. Then, the analysis of the images can calculate the space occupied by each object (length, diameter, intersection with other objects, surface area, etc.) pixel - by - pixel.
[0072] For a Pt layer thickness of 15 nm, the results are shown in Table 2: [Table 2] <![CDATA[Thickness of SiO2 layer (nm)]]> Average diameter (nm) Average length (μm) 5 30-47 12-20 10 33-53 15-20 15 32-70 2-3 20 47-75 1-3
[0073] For a SiO2 layer thickness of 15 nm and a Pt layer thickness of 10 nm, other results are shown in Table 3 and the obtained images are shown in Figures 5A - 5D as follows: [Table 3] Sample number Average diameter (nm) Average length (μm) 1 70-100 0.9-1 2 79-90 1.4-1.6 3 104-120 1.2-1.4 4 114-145 1.09
[0074] Study of temperature stage-related phenomena:
[0075] The role of the two annealing stages was determined with the aid of SEM images. The first stage promotes platinum dewetting by forming Pt droplets on the surface, and during the second temperature stage, the evaporated SiO2 condenses under these droplets: - Figure 6 corresponding to substrates annealed at 900 °C for 1 minute; - Figure 7 corresponding to substrates annealed at 950 °C for 1 minute; - Figure 8 corresponding to substrates annealed at 900 °C for 1 minute and then at 1050 °C for 3 minutes; - Figure 9 corresponding to substrates annealed at 950 °C for 1 minute and then at 1100 °C for 3 minutes.
[0076] Figures 6 to 8 The importance of the first stage for promoting catalyst (Pt) dewetting to enable nanowire growth is shown. Figure 8 Specifically, the first stage at 900 °C is not sufficient to promote growth in the second stage. Figure 9 It is shown that an initial growth can be obtained after a first stage at 950 °C followed by a second stage at 1100 °C. Figure 9 The importance of the second stage duration for the nanowire length is also shown, with a duration of 3 minutes applied here (whereas in other results described in this experimental section, a duration of 5 minutes was applied for the second stage).
[0077] Measurement of the surface area gain brought by nanowires :
[0078] The inventors have verified that the high surface area capacitance of components incorporating a substrate according to the present invention is closely related to its structure, even if the structure contains infinitely complex structural elements in terms of the material structure and even if they are substantially wound around each other. The high surface area capacitance results from a large surface area relative to the projected area, which is provided by microcolumns (microstructured substrate) covered with nanowires. The method used to determine the surface area gain involves using a parameter called the "Area Enlargement Factor" ("AEF") and comparing the AEFs of different structures and their respective contributions, where the AEF is measured independently, first in a 2D plane, then in 3D, and also in 2D and 3D with nanowires.
[0079] Different measurements were carried out under the same conditions to calculate the surface area gain (AEF) measured by cyclic voltammetry with a three - electrode system. The electrolyte used was sulfuric acid (H2SO4) diluted to 0.5 M, the reference electrode was an Ag / AgCl electrode, the counter - electrode was made of platinum, and the working electrode was platinum (30 nm) deposited by ALD on the sample to be tested (microstructured "skeleton"). The scan rate was 50 mV / s. The projected area observed during the measurement was 0.407 cm 2 . The results are shown in Table 4 below: [Table 4]
[0080] Thus, Table 4 shows that the measurement method can back - calculate the 3D gain (entries in the 3rd and 4th rows of the table) calculated from the 3D structure model according to the microtube type. This method demonstrates that in the examples cited in the rest of Table 2 (entries in rows 5 to 8 respectively), the nanowires provide a surface area gain of 2 to 19.
[0081] An identical measurement was carried out using a supercapacitor electrode material (RuO2), and the results showed a 10 - fold gain on a microstructured surface with a 50 - fold gain (i.e., a total surface area gain of 50x10 = 500). Thus, it is demonstrated that the surface area gain of the microstructures is between 50 and 70, and the surface area gain of the nanowires is between 4 and 10. Figure 10 Shows the variation of the capacitance of a RuO2 thin layer with the scan rate on different types of substrates. Thus, the inventors were able to unexpectedly demonstrate that the cumulative gain is multiplicative rather than additive, enabling a gain between 200 and 700. In Figure 10 , we found that compared with the capacitance of a RuO2 thin layer on a planar surface (triangle), for a microtube - type structure (square), the capacitance can back - calculate a surface area gain of 50, and for a hierarchical substrate (circle), it can back - calculate a surface area gain of 500. References
[0082] The following table lists the references mentioned in the above text: [Table 1] 1 WO2015 / 052412 2 WO2022 / 069842 3 WO2020114379
Claims
1. A microstructured substrate comprising a body and a plurality of elongated basic microstructures extending from the body, characterized in that, The microstructured substrate includes a plurality of nanowires, which are located on at least one region of the surface of the body and on the surface of the basic microstructure extending from the body within the region.
2. The microstructured substrate according to claim 1, wherein the body and the basic microstructure extending along the body are made of the same material, preferably, the material is selected from the materials consisting of or only consisting of: silicon, silicon dioxide, gallium arsenide, silicon nitride, and indium phosphide.
3. The microstructured substrate according to any one of claims 1 or 2, wherein the basic microstructure includes a cross-section selected from a circular, elliptical, rectangular, square, and triangular cross-section.
4. The microstructured substrate according to any one of claims 1 to 3, wherein the nanowires include a material selected from oxides, preferably selected from silicon dioxide, zinc oxide, and titanium dioxide, and preferably, the nanowires consist only of silicon dioxide.
5. The microstructured substrate according to any one of claims 1 to 4, wherein the nanowires have a cross-section with a diameter of 20 nm to 250 nm and a length of 100 nm to 10 μm.
6. The microstructured substrate according to any one of claims 1 to 5, wherein the developed surface area of the region containing the nanowires is 2 to 50 times that of the region without nanowires.
7. A method for manufacturing the microstructured substrate according to any one of claims 1 to 6, comprising the following steps: a - covering a planar substrate or a microstructured substrate with a thin layer of silicon dioxide; b - depositing a layer of non-oxidized metal using an atomic layer deposition technique; c - performing lithography on at least one region of the surface of the planar or microstructured carrier that has undergone steps a - and b -; d - performing an etching process; and e - performing thermal annealing, preferably by implementing at least one temperature stage.
8. The method for manufacturing a microstructured substrate according to claim 7, wherein the non-oxidized metal deposited in step b - is selected from platinum, silver, gold, gallium, indium, titanium, tin, zinc, antimony, copper, nickel, beryllium, iron, cobalt, chromium, aluminum, ruthenium, rhodium, and palladium, preferably, the non-oxidized metal consists of platinum.
9. The method for manufacturing a microstructured substrate according to claim 8, wherein step e - includes two temperature stages: a first stage of applying a temperature of 200 °C to 1200 °C for less than 5 minutes; and a second stage of applying a temperature of 300 °C to 1400 °C for less than 15 minutes.
10. A use of the microstructured substrate according to any one of claims 1 to 6 for manufacturing a micro energy storage device, the micro energy storage device being preferably selected from: batteries, supercapacitors, and dielectric and electrolytic capacitors with a micron-scale or even nanoscale size, energy recovery components, or a type of sensor device that requires the use of a large specific surface area.