Coated positive electrode active material, positive electrode, and secondary battery
By forming an oxide-containing and phosphoric acid compound layer on the surface of the positive electrode active material, the problems of transition metal dissolution and electrolyte decomposition in the secondary battery are solved, and the stability and life of the battery are improved.
Patent Information
- Application Number
- CN202380088720.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-26
- Filing Date
- 2023-12-04
- Publication Date
- 2025-08-01
AI Technical Summary
There are problems in the existing secondary batteries that reduce and dissolution of transition metals and decomposition of electrolytes, resulting in battery deterioration.
An oxide-containing layer and a phosphorus-containing layer are formed on the surface of the positive electrode active material. The proportion of phosphorus-containing compound in the phosphorus-containing layer is more than 0.1%. The oxide layer is formed by atomic layer deposition and mechanochemical methods. The phosphorus-containing compound is combined with the oxide layer to prevent the positive electrode active material from contacting the electrolyte.
It effectively inhibits the dissolution of metal and the decomposition reaction of electrolyte, and improves the stability and life of the battery.
Smart Images

Figure CN120418987A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a coated positive electrode active material, a positive electrode, and a secondary battery. Background Art
[0002] In conventional secondary batteries, side reactions such as reduction and dissolution of transition metals contained in the active material and decomposition reactions of the electrolytic solution caused thereby occur. The side reactions promote the deterioration of the secondary battery.
[0003] Non-Patent Document 1 describes adding tris(trimethylsilyl)phosphate to the electrolytic solution to improve the cycle characteristics of a lithium-rich positive electrode material [Li 0.2 Ni 0.13 Mn 0.54 Co 0.13 O2. Patent Document No. 1 discloses a positive electrode having a positive electrode active material, the positive electrode active material including composite oxide particles, a coating layer, and a surface layer, the coating layer being provided on at least a part of the composite oxide particles and formed of an oxide containing at least one coating element selected from nickel (Ni) and manganese (Mn) and lithium (Li), and the surface layer being provided on at least a part of the coating layer and containing phosphorus (P). Patent Document No. 2 discloses a positive electrode active material for a non-aqueous electrolyte secondary battery, in which protrusion-shaped aluminum-containing oxide and / or aluminum-containing hydroxide are uniformly dispersed and adhered on the surface of the positive electrode active material particles.
[0004] Prior Art Documents
[0005] Non-Patent Document 1: J.Zhang et al. “Artificial Interface Deriving from Sacrificial Tris(trimethylsilyl)phosphate Additive for Lithium Rich Cathode Materials” Electrochimica Acta 117 (2014) 99 - 104
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 2008 - 016235
[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 2009 - 245917 Summary of the Invention
[0008] Problems to be Solved by the Invention
[0009] The present disclosure provides a coated positive electrode active material in which the dissolution of a metal is suppressed.
[0010] Means for Solving the Problems
[0011] The coated positive electrode active material of the present disclosure includes a positive electrode active material, an oxide layer, and a phosphorus-containing layer.
[0012] The oxide layer coats at least a part of the surface of the particles of the positive electrode active material.
[0013] The phosphorus-containing layer coats at least a part of the surface of the oxide layer.
[0014] The oxide layer contains an oxide and is in contact with the surface of the particles.
[0015] The phosphorus-containing layer contains a phosphoric acid compound.
[0016] The mass ratio of P contained in the phosphorus-containing layer to the positive electrode active material is 0.1% or more.
[0017] Effects of the Invention
[0018] The present disclosure provides a coated positive electrode active material in which the elution of a metal is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 FIG. is a cross-sectional view schematically showing the general structure of the coated positive electrode active material 10 of Embodiment 1.
[0020] Figure 2A FIG. is a process diagram showing a method for manufacturing a positive electrode.
[0021] Figure 2B FIG. is a process diagram showing another method for manufacturing a positive electrode.
[0022] Figure 3 FIG. is a cross-sectional view schematically showing the general structure of the positive electrode 16 of Embodiment 3.
[0023] Figure 4 FIG. is a longitudinal cross-sectional view schematically showing the secondary battery 100 of Embodiment 4. DETAILED DESCRIPTION OF THE INVENTION
[0024] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. The present disclosure is not limited to the following embodiments.
[0025] (Embodiment 1)
[0026] Figure 1It is a cross-sectional view showing a schematic structure of the coated positive electrode active material 10 of Embodiment 1. The coated positive electrode active material 10 includes a positive electrode active material, an oxide layer 12 covering at least a part of the surface of the particles 11 of the positive electrode active material, and a phosphorus-containing layer 13 covering at least a part of the surface of the oxide layer 12. The oxide layer 12 contains an oxide and is in contact with the surface of the particles 11. The phosphorus-containing layer 13 contains a phosphoric acid compound. The mass ratio of P (phosphorus) contained in the phosphorus-containing layer 13 is 0.1% or more with respect to the positive electrode active material.
[0027] The mass ratio of P can be determined, for example, by inductively coupled plasma atomic emission spectrometry (ICP-AES) using an analytical device iCAP7400 Duo (manufactured by Thermo Fisher Scientific Inc.).
[0028] The ratio of the mass of P at the interface between the surface of the particles 11 of the positive electrode active material and the oxide layer 12 to the mass of P on the surface of the particles of the coated positive electrode active material 10 can be 3% or less. The ratio of the mass of the phosphoric acid compound at the interface between the surface of the particles 11 of the positive electrode active material and the oxide layer 12 to the mass of the phosphoric acid compound on the surface of the particles of the coated positive electrode active material 10 can be 3% or less. There may be no phosphoric acid compound at the interface between the surface of the particles 11 of the positive electrode active material and the oxide layer 12.
[0029] In a battery, when the positive electrode active material comes into contact with the electrolyte, side reactions such as the dissolution of metal from the positive electrode active material and the generation of gas due to the decomposition reaction of the electrolyte occur, resulting in battery degradation. On the other hand, in order to prevent the positive electrode active material from coming into contact with the electrolyte, if a film of a phosphoric acid compound such as tris(trimethylsilyl) phosphate (TMSP) is formed on the surface of the positive electrode active material, the surface of the positive electrode active material deteriorates due to contact with TMSP as an acidic substance, and the battery capacity decreases. In the coated positive electrode active material 10 of the present disclosure, the oxide layer 12 is in contact with the surface of the particles 11 of the positive electrode active material to cover the surface, and the phosphorus-containing layer 13 is covered thereon. With such a structure, it is possible to suppress the dissolution of metal while preventing the contact between the phosphoric acid compound and the positive electrode active material and suppressing the deterioration of the positive electrode active material.
[0030] As disclosed in Non-Patent Document 1, when adding, for example, TMSP to the electrolytic solution, since the content rate of TMSP that can be dissolved in the electrolytic solution is limited, it is impossible to use a sufficient amount of TMSP to improve the characteristics. When adding TMSP to the electrolytic solution, a film of TMSP itself is formed on the positive electrode, and the mass ratio of P in the film is about 0.0051% by mass with respect to the total amount of the positive electrode active material. In the coated positive electrode active material of the present disclosure, the mass ratio of P contained in the phosphorus-containing layer 13 with respect to the positive electrode active material is 0.1% or more. With such a structure, it is possible to sufficiently prevent the contact between the positive electrode active material and the electrolytic solution and suppress the metal elution of the positive electrode active material.
[0031] As the positive electrode active material, a lithium-containing transition metal oxide, a lithium-containing transition metal phosphate, a transition metal fluoride, a polyanion material, a fluorinated polyanion material, a transition metal sulfide, a transition metal oxysulfide, a transition metal oxynitride, etc. can be used. In particular, when using a lithium-containing transition metal oxide or a lithium-containing transition metal phosphate as the positive electrode active material, it is possible to reduce the manufacturing cost of the battery and increase the average discharge voltage. As the lithium-containing transition metal oxide, lithium cobaltate, lithium nickel cobalt aluminate, lithium nickel cobalt manganate, lithium nickel manganate, etc., can be mentioned. As the lithium-containing transition metal phosphate, lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium nickel phosphate, etc., can be mentioned.
[0032] The positive electrode active material may include a lithium nickel oxide having a layered rock salt-type crystal structure. Among the metal elements other than Li contained in the lithium nickel oxide, the proportion of Ni may be 50 atomic% or more. The lithium nickel oxide may also contain other transition metals. The lithium nickel oxide can be used to achieve a high working voltage. According to the configuration of the coated positive electrode active material of Embodiment 1, it is possible to suppress the elution of metal ions from the positive electrode active material. Since nickel is easily eluted from the positive electrode active material, the elution suppression effect brought by the technology of the present disclosure is particularly expected.
[0033] The lithium nickel oxide can be represented by the following compositional formula (I). Element M1 is at least one selected from V, Co, and Mn. Element M2 is at least one selected from Mg, Al, Ca, Ti, Cu, Zn, and Nb. The compositional formula (I) satisfies 0.9 ≤ α ≤ 1.10, -0.05 ≤ β ≤ 0.05, 0.5 ≤ x1 < 1, 0 ≤ x2 ≤ 0.5, and 0 < 1 - x1 - x2 ≤ 0.5.
[0034] Li α Ni x1 M1 x2 M2 (1-x1-x2) O 2+β ···(I)
[0035] The oxide-containing layer 12 is a layer containing an oxide, covering at least a part of the surface of the positive electrode active material particles 11 and in contact with the surface of the positive electrode active material particles 11. The oxide-containing layer 12 is formed by placing an oxide at a position in contact with at least a part of the surface of the positive electrode active material particles 11.
[0036] The oxide-containing layer 12 may consist essentially of an oxide. "The oxide-containing layer 12 consists essentially of an oxide" means that in the oxide-containing layer 12, the mass ratio of the oxide is 97% by mass or more. The mass ratio of the oxide in the oxide-containing layer 12 may be 98% by mass or more, or may be 99% by mass or more. The oxide-containing layer 12 may also consist only of an oxide.
[0037] The thickness of the oxide-containing layer 12 may be 1 nm or more and 2 μm or less, more preferably 3 nm or more and 10 nm or less.
[0038] The oxide may include an oxide containing at least one element selected from a metal element and a metalloid element.
[0039] The oxide may be a compound that easily binds to a phosphate compound described later. The oxide may be a basic oxide or an amphoteric oxide, preferably an oxide that is basic with respect to the positive electrode active material and insoluble in the electrolytic solution. Although the mechanism is uncertain, it is speculated that such an oxide remains stably on the positive electrode surface even after the battery is charged and discharged, and as a result, the effect of the phosphate compound remaining on the positive electrode surface is high.
[0040] The oxide may contain at least one of Si, Zr, Al, and Ti. The oxide may contain at least one of Si, Zr, and Al.
[0041] The oxide may contain at least one of SiO2, ZrO2, Al2O3, and TiO2. The oxide may contain at least one of SiO2, ZrO2, and Al2O3.
[0042] The oxide may contain at least one of Si and Zr. The oxide may contain at least one of SiO2 and ZrO2. SiO2 and ZrO2 are generally basic with respect to the positive electrode active material and insoluble in the electrolytic solution.
[0043] The oxide-containing layer 12 may also contain Li. The oxide may be a composite oxide of the above elements and Li.
[0044] The phosphorus-containing layer 13 is a layer containing a phosphoric acid compound and coats at least a part of the surface of the oxide-containing layer 12. The phosphorus-containing layer 13 is formed by the phosphoric acid compound being located on at least a part of the surface of the oxide-containing layer 12 that coats at least a part of the surface of the particles 11 of the positive electrode active material. The phosphorus-containing layer 13 may be in contact with the surface of the oxide-containing layer 12. The phosphorus-containing layer 13 may not be in contact with the surface of the particles 11 of the positive electrode active material.
[0045] The phosphorus-containing layer 13 may be substantially composed of a phosphoric acid compound. "The phosphorus-containing layer 13 is substantially composed of a phosphoric acid compound" means that in the phosphorus-containing layer 13, the mass ratio of the phosphoric acid compound is 97% by mass or more. The mass ratio of the phosphoric acid compound in the phosphorus-containing layer 13 may be 98% by mass or more, or may be 99% by mass or more. The phosphorus-containing layer 13 may be composed only of a phosphoric acid compound.
[0046] In this specification, "phosphoric acid compound" refers to an oxyacid of phosphorus. Phosphoric acid compounds are, for example, phosphoric acid, phosphonic acid, hypophosphorous acid, pyrophosphoric acid, phosphate esters, phosphonate esters, hypophosphite esters, their derivatives, and their condensates. The phosphoric acid compound may be an organophosphorus compound. In this specification, an organophosphorus compound refers to a compound containing carbon and phosphorus. The phosphoric acid compound may be a compound having a carbon-phosphorus bond.
[0047] The thickness of the phosphorus-containing layer 13 may be 0.05 μm or more and 2 μm or less, more preferably 0.05 μm or more and 1 μm or less.
[0048] The phosphoric acid compound may bind to the oxide of the oxide-containing layer 12.
[0049] The phosphoric acid compound may contain a P-O-P bond. The phosphoric acid compound may be polyphosphoric acid, polyphosphate esters, and their derivatives.
[0050] The phosphoric acid compound may contain a structure represented by Chemical Formula (1).
[0051]
[0052] In Chemical Formula (1), n1 and n2 are independently integers of 0 or more. R 1 、R 2 、R 4 and R 5 independently represent -OR or -(CH2) m1 X1. R 3 and R independently represent a direct bonding bond with the oxide in the oxide-containing layer 12, a hydrogen atom, -(CH2) m2X2, trimethylsilyl or triethylsilyl. m1 is an integer from 0 to 15. m2 is a natural number from 1 to 3. X1 and X2 independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxyl group, a cyano group or a fluorine atom. When there are multiple R 2 s, the multiple R 2 s are independent of each other. When there are multiple R 4 s, the multiple R 4 s are independent of each other.
[0053] The phosphoric acid compound has such a structure that it is relatively stable even in a high-voltage environment. Therefore, even when the upper limit voltage of the secondary battery is high, for example, when it exceeds 4.3 V, side reactions such as oxidation decomposition of the electrolyte can be sufficiently suppressed, and metal dissolution of the positive electrode active material can be suppressed.
[0054] In Chemical Formula (1), n1 and n2 can independently be 1 or more. At least one of n1 and n2 can be 1 or more. n1 and n2 can independently be 500 or less. X1 can be a hydrogen atom. X2 can also be a hydrogen atom.
[0055] In Chemical Formula (1), m1 can be an integer from 0 to 11 or an integer from 0 to 6. When m1 is an integer from 0 to 6, side reactions can be further suppressed.
[0056] In Chemical Formula (1), m2 can be 1 or 2.
[0057] The phosphoric acid compound is, for example, a silyl phosphite, a phosphonic acid, a phosphoric acid, a pyrophosphoric acid, and their condensates. The phosphoric acid compound can be a silyl phosphite, can be tris(trimethylsilyl) phosphate (TMSP), or can be a compound derived from TMSP such as a condensate of TMSP. In Chemical Formula (1), R 1 , R 2 , R 4 and R 5 can independently represent -OR, and R 3 and R can independently represent a direct bonding bond with the oxide in the oxide layer 12, a hydrogen atom or a trimethylsilyl group.
[0058] In Chemical Formula (1), R 3 can represent a direct bonding bond with the oxide.
[0059] The direct bonding bond with the oxide can be bonded to the metal element or semi-metal element of the oxide.
[0060] The phosphorus-containing layer 13 can contain one or two or more phosphoric acid compounds.
[0061] The phosphorus-containing layer 13 covers at least a part of the surface of the oxide-containing layer 12. With such a structure, direct contact between the phosphoric acid compound and the positive electrode active material can be prevented. Therefore, deterioration of the positive electrode active material can be suppressed, and side reactions such as elution of metals in the positive electrode can be suppressed.
[0062] The phosphorus-containing layer 13 may cover the entire surface of the oxide-containing layer 12.
[0063] The phosphorus-containing layer 13 may be in contact with the oxide-containing layer 12.
[0064] The phosphoric acid compound may or may not form a chemical bond with the oxide in the oxide-containing layer 12. The phosphoric acid compound may be physically attached to the oxide-containing layer 12.
[0065] In the coated positive electrode active material 10, the mass ratio of P to the positive electrode active material may be 3% by mass or less, or may be 2% by mass or less. The mass ratio of P to the positive electrode active material may be 0.1% by mass or more and 2% by mass or less.
[0066] The coated positive electrode active material 10 has, for example, the shape of particles. There is no particular limitation on the shape of the particles of the coated positive electrode active material 10. The shape of the particles of the coated positive electrode active material 10 is needle-like, flaky, spherical, or ellipsoidal.
[0067] (Manufacturing method of coated positive electrode active material)
[0068] The coated positive electrode active material 10 can be manufactured, for example, by the following method.
[0069] Prepare a powder of the positive electrode active material. The powder of the positive electrode active material is coated with an oxide by atomic layer deposition (ALD), whereby an oxide-containing layer 12 is formed on the surface of the particles 11 of the positive electrode active material. The oxide-containing layer 12 can also be formed by low-temperature ALD. Low-temperature ALD refers to an atomic layer deposition method in which the film formation temperature is, for example, 200°C or lower. The atomic layer deposition method may also be plasma ALD using a plasma-excited gas.
[0070] The method for forming the oxide-containing layer 12 is not limited to the above. The oxide-containing layer 12 can be formed by mechanochemical method. The positive electrode active material and the oxide are mixed in an appropriate ratio to obtain a mixture, and the mixture is ground to impart mechanical energy to the mixture. The grinding process can use a mixing device such as a ball mill.
[0071] Next, prepare a solution containing a phosphoric acid compound and a solvent.
[0072] As described above, the phosphoric acid compound contains, for example, a structure represented by Chemical Formula (1). The phosphoric acid compound in the raw material stage is in a state before it can condense with each other and / or combine with an oxide, and can be distinguished from the phosphoric acid compound contained in the phosphorus-containing layer 13.
[0073] The phosphoric acid compound in the raw material stage contains, for example, a structure represented by Chemical Formula (2).
[0074]
[0075] In Chemical Formula (2), R 7 represents a hydrogen atom, -(CH2) k1 Y1, a trimethylsilyl group, or a triethylsilyl group. R 6 and R 8 independently of each other represent -OR or -(CH2) k2 Y2. R represents a hydrogen atom, -(CH2) k3 Y3, a trimethylsilyl group, or a triethylsilyl group. k1 and k3 are independently natural numbers from 1 to 3. k2 is an integer from 0 to 15. Y1, Y2, and Y3 independently of each other represent a hydrogen atom, a hydroxyl group, an amino group, a carboxyl group, a cyano group, or a fluorine atom.
[0076] The phosphoric acid compound in the raw material stage may contain at least one selected from silyl phosphite esters and phosphoric acid. The silyl phosphite ester may be TMSP.
[0077] As the solvent, cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, etc. can be used. Examples of the cyclic carbonate include propylene carbonate (PC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), etc. Examples of the chain carbonate include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), etc. Examples of the cyclic carboxylic acid ester include γ-butyrolactone (GBL), γ-valerolactone (GVL), etc. The solvent can be used alone or in combination of two or more. From the viewpoint of the manufacturing process, a solvent with a high boiling point is preferred. The boiling point of the solvent is, for example, 200 °C or higher.
[0078] The concentration of the phosphoric acid compound in the solution can be 0.1 wt% to 20 wt%.
[0079] Next, the prepared solution is brought into contact with the particles 11 of the positive electrode active material having an oxide layer 12 formed on the surface. This contact can be carried out by immersing the above particles in the solution. Alternatively, the solution can also be sprayed onto the above particles, etc., and carried out by coating. For example, the positive electrode active material containing the above particles can be formed into a layer, and the solution can be coated on this layer, or this layer can be immersed in the solution, thereby bringing the solution into contact with the particles of the positive electrode active material. The contact time with the solution is, for example, 15 minutes or more and 120 minutes or less, and the temperature is, for example, 20°C or more and 60°C or less.
[0080] The particles of the positive electrode active material in contact with the solution are vacuum dried. The vacuum drying time can be, for example, 5 minutes or more and 48 hours or less. In this way, the coated positive electrode active material 10 of Embodiment 1 is obtained. Vacuum drying means drying under a pressure lower than atmospheric pressure.
[0081] The particles of the positive electrode active material can be washed after contact with the solution and before vacuum drying. For example, the particles of the positive electrode active material are washed using a solvent. The solvent for washing can be the solvent used in the solution containing the above phosphoric acid compound and solvent, and can be, for example, DMC. According to the above, by-products such as decomposition products of the phosphoric acid compound can be removed. Thereby, in the positive electrode, the generation of gas caused by the reaction of the by-product with the electrolyte can be suppressed.
[0082] (Embodiment 2)
[0083] The method for manufacturing the positive electrode of Embodiment 2 satisfies at least one of the following (A) and (B).
[0084] (A) Includes: forming an oxide-containing layer on at least a part of the surface of the particles of the positive electrode active material; forming a positive electrode active material layer containing the particles having the oxide-containing layer formed thereon on the positive electrode current collector; bringing a solution containing a phosphoric acid compound and a solvent into contact with the positive electrode active material layer; and drying the positive electrode active material layer after this contact.
[0085] (B) Includes: forming an oxide-containing layer on at least a part of the surface of the particles of the positive electrode active material; bringing a solution containing a phosphoric acid compound and a solvent into contact with the particles having the oxide-containing layer formed thereon; vacuum drying the particles after this contact; and forming a positive electrode active material layer containing the obtained dried particles on the positive electrode current collector.
[0086] Figure 2A It is a process diagram showing the method for manufacturing the positive electrode.
[0087] In step S1, an oxide-containing layer is formed on at least a part of the surface of the particles of the positive electrode active material.
[0088] The oxide-containing layer is a layer containing an oxide. The oxide is, for example, the oxide described in Embodiment 1.
[0089] In step S1, the oxide-containing layer can be formed by atomic layer deposition (ALD) or mechanochemical method. The oxide-containing layer can be formed by ALD.
[0090] In step S2, a positive electrode active material layer containing particles formed with the oxide-containing layer is formed on the positive electrode current collector. In step S2, the positive electrode active material layer is formed, for example, as follows.
[0091] Prepare a positive electrode paste containing the positive electrode active material obtained in step S1. For example, the positive electrode active material, a binder, and a conductive assistant are dispersed in a dispersion medium to prepare the positive electrode paste.
[0092] The positive electrode paste is coated on the positive electrode current collector to form a positive electrode active material layer. Specifically, the positive electrode paste is coated on the positive electrode current collector to form a coating film. The dispersion medium is removed from the coating film to obtain the positive electrode active material layer. As a method for removing the dispersion medium, a method of heating the coating film can be cited. As the dispersion medium, for example, N-methyl-2-pyrrolidone (NMP) or the like is used. In this way, a positive electrode active material layer is formed on the positive electrode current collector.
[0093] In step S3, a solution containing a phosphoric acid compound and a solvent is brought into contact with the positive electrode active material layer. In step S3, the contact between the solution and the positive electrode active material layer can be carried out by immersing the positive electrode active material layer formed on the positive electrode current collector in the solution, or by coating the solution on the positive electrode active material layer. The contact time is, for example, 15 minutes or more and 120 minutes or less.
[0094] The solution containing the phosphoric acid compound and the solvent is, for example, the solution described in Embodiment 1. That is, the phosphoric acid compound can contain the structure represented by the above chemical formula (2). The phosphoric acid compound can contain TMSP. The solvent can be the solvent described in Embodiment 1.
[0095] In step S4, the positive electrode active material layer is dried. In step S4, the drying time can be, for example, 5 minutes or more and 48 hours or less.
[0096] The positive electrode active material layer can be washed after step S3 and before step S4. For example, the positive electrode active material layer is washed with a solvent. The solvent for washing can be the solvent used in the solution containing the phosphoric acid compound and the solvent, and can be, for example, DMC. According to the above, by-products such as decomposition products of the phosphoric acid compound can be removed. Thus, in the positive electrode, the generation of gas caused by the reaction between the by-products and the electrolyte can be suppressed.
[0097] Figure 2BIt is a process diagram showing another manufacturing method of the positive electrode.
[0098] In step ST1, similar to step S1, an oxide-containing layer is formed on at least a part of the surface of the positive electrode active material particles.
[0099] In step ST2, a solution containing a phosphoric acid compound and a solvent is brought into contact with the positive electrode active material particles obtained in step ST1. The contact between the solution and the positive electrode active material particles can be carried out by immersing the positive electrode active material particles in the solution, or by spraying the solution onto the positive electrode active material particles or by coating.
[0100] In step ST3, the positive electrode active material particles obtained in step ST2 are vacuum-dried. Vacuum drying means drying under a pressure lower than atmospheric pressure. In step ST3, the vacuum drying time can be, for example, 5 minutes or more and 48 hours or less.
[0101] In step ST4, a positive electrode active material layer is formed on the positive electrode current collector. In step ST4, using the positive electrode active material particles obtained in step ST3, a positive electrode active material layer is formed on the positive electrode current collector in the same manner as in step S2.
[0102] The positive electrode active material particles can be washed after step ST2 and before step ST3.
[0103] The manufacturing method of the positive electrode of the present disclosure can satisfy (A).
[0104] The manufacturing method of the positive electrode of the present disclosure can satisfy both (A) and (B) simultaneously. The manufacturing method of the positive electrode of the present disclosure can include: forming an oxide-containing layer on at least a part of the surface of the positive electrode active material particles; bringing a solution containing a phosphoric acid compound and a solvent into contact with the particles having the oxide-containing layer formed thereon; vacuum-drying the particles after the contact; forming a positive electrode active material layer containing the obtained dried particles on the positive electrode current collector; bringing a solution containing a phosphoric acid compound and a solvent into further contact with the positive electrode active material layer; and vacuum-drying the positive electrode active material layer after the contact. That is, the manufacturing method of the positive electrode of the present disclosure can perform step S3 and step S4 after steps ST1 to ST4.
[0105] (Embodiment 3)
[0106] Figure 3 It is a cross-sectional view showing the general structure of the positive electrode 16 of Embodiment 3. The positive electrode 16 includes a positive electrode current collector 14 and a positive electrode active material layer 15 supported on the positive electrode current collector 14. The positive electrode active material layer 15 contains the coated positive electrode active material of Embodiment 1.
[0107] The positive electrode active material layer 15 may contain only the coated positive electrode active material of Embodiment 1 as the positive electrode active material, or may contain a positive electrode active material different from the coated positive electrode active material of Embodiment 1. The positive electrode active material layer 15 may contain the coated positive electrode active material on its surface.
[0108] The positive electrode active material layer 15 may further contain other materials such as a binder, an ion conductor, and a conductive additive.
[0109] As the positive electrode current collector 14, for example, a metal foil can be used. As the metal constituting the positive electrode current collector 14, for example, aluminum, titanium, an alloy containing these metal elements, and stainless steel can be cited.
[0110] The positive electrode 16 is manufactured, for example, by the manufacturing method of Embodiment 2.
[0111] (Embodiment 4)
[0112] The secondary battery of Embodiment 4 includes the positive electrode, negative electrode, and electrolyte of Embodiment 3. By using the positive electrode of Embodiment 3, the characteristics of the secondary battery such as charge-discharge efficiency can be improved.
[0113] Figure 4 FIG. is a schematic longitudinal sectional view showing the secondary battery 100 of Embodiment 4. The secondary battery 100 is a cylindrical battery including a cylindrical battery case, a wound electrode group 24, and an electrolytic solution (not shown). The electrode group 24 is housed in the battery case and is in contact with the electrolytic solution.
[0114] The battery case is composed of a case body 25 which is a bottomed cylindrical metal container and a sealing body 26 which seals the opening of the case body 25. A gasket 37 is disposed between the case body 25 and the sealing body 26. The airtightness of the battery case is ensured by the gasket 37. Inside the case body 25, insulating plates 27 and 28 are respectively disposed at both ends of the electrode group 24 in the winding axis direction of the electrode group 24.
[0115] The case body 25 has, for example, a stepped portion 31. The stepped portion 31 can be formed by locally stamping the side wall of the case body 25 from the outside. The stepped portion 31 can be formed in a ring shape along the circumferential direction of a virtual circle defined by the case body 25 on the side wall of the case body 25. At this time, the sealing body 26 is supported, for example, by the surface on the opening side of the stepped portion 31.
[0116] The sealing body 26 includes a filter 32, a lower valve body 33, an insulating member 34, an upper valve body 35, and a lid 36. In the sealing body 26, these components are laminated in this order. The sealing body 26 is attached to the opening of the case body 25 in such a manner that the lid 36 is located outside the case body 25 and the filter 32 is located inside the case body 25.
[0117] Each of the components constituting the sealing body 26 is, for example, in the shape of a circular plate or a ring. Except for the insulating component 34, each of the above components is electrically connected to each other.
[0118] The electrode group 24 has a positive electrode 21, a negative electrode 22, and a separator 23. The positive electrode 21, the negative electrode 22, and the separator 23 are all in strip shape. The width direction of the strip-shaped positive electrode 21 and negative electrode 22 is, for example, parallel to the winding axis of the electrode group 24. The separator 23 is disposed between the positive electrode 21 and the negative electrode 22. The positive electrode 21 and the negative electrode 22 are wound in a spiral shape with the separator 23 sandwiched between these electrodes.
[0119] When observing a cross-section of the secondary battery 100 in a direction perpendicular to the winding axis of the electrode group 24, the positive electrode 21 and the negative electrode 22 are alternately laminated in the radial direction of a virtual circle defined by the housing main body 25 with the separator 23 sandwiched between these electrodes.
[0120] The positive electrode 21 is electrically connected to the lid 36 that also serves as a positive terminal via a positive electrode lead 29. One end of the positive electrode lead 29 is connected, for example, near the center of the positive electrode 21 in the length direction of the positive electrode 21. The positive electrode lead 29 passes through a through-hole formed in the insulating plate 27 and extends from the positive electrode 21 to the filter 32. The other end of the positive electrode lead 29 is, for example, welded to the surface of the filter 32 on the side of the electrode group 24.
[0121] The negative electrode 22 is electrically connected to the housing main body 25 that also serves as a negative terminal via a negative electrode lead 30. One end of the negative electrode lead 30 is connected, for example, to the end of the negative electrode 22 in the length direction of the negative electrode 22. The other end of the negative electrode lead 30 is, for example, welded to the inner bottom surface of the housing main body 25.
[0122] Hereinafter, each structure of the secondary battery 100 will be specifically described.
[0123] The positive electrode 21 is the positive electrode of Embodiment 3.
[0124] The negative electrode 22 contains a material having the property of occluding and releasing metal ions (such as lithium ions). The negative electrode 22 contains, for example, a negative electrode active material. The negative electrode may include a negative electrode current collector and a negative electrode active material layer supported on the surface of the negative electrode current collector.
[0125] The negative electrode current collector is, for example, a foil made of a metal material such as stainless steel, nickel, nickel alloy, copper, or copper alloy.
[0126] The negative electrode active material layer contains a negative electrode active material. The negative electrode active material may be a material having the ability to occlude and release lithium ions. Examples of the negative electrode active material include lithium titanate, graphite, silicon, silicon compound, NiBi alloy, etc.
[0127] The negative electrode active material layer may contain other materials such as a conductive assistant, an ion conductor, and a binder.
[0128] The electrolyte may contain a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. The concentration of the lithium salt in the electrolyte may be, for example, 0.5 mol / L or more and 2 mol / L or less. By controlling the lithium salt concentration within the above range, an electrolyte with excellent ion conductivity and moderate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.
[0129] As the non-aqueous solvent, cyclic carbonates, chain carbonates, cyclic ethers, chain ethers, nitriles, amides, etc. can be used. One of these solvents can be used, or two or more can be used in combination.
[0130] As the lithium salt, lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(perfluoroethylsulfonyl)imide (LiN(SO2C2F5)2), LiAsF6, LiCF3SO3, lithium difluoro(oxalato)borate, etc. can be used. One of these electrolyte salts can be used, or two or more can be used in combination.
[0131] The electrolyte may further contain a phosphoric acid compound, and may contain, for example, TMSP. The electrolyte may not contain phosphorus.
[0132] Generally, it is preferable to interpose a separator between the positive electrode and the negative electrode. The separator 23 has a high ion permeability and has appropriate mechanical strength and insulation. As the separator 23, a microporous film, a spunbond, a non-woven fabric, etc. can be used. As the material of the separator 23, a polymer can be used, for example. The polymer can be, for example, a polyolefin such as polypropylene and polyethylene.
[0133] In the secondary battery of the present disclosure, the electrolyte can be impregnated, for example, in a polymer provided as a separator. That is, the secondary battery of the present disclosure can have a structure in which the electrolyte and the polymer are used in combination.
[0134] The secondary battery of the present disclosure may further include a solid electrolyte as an electrolyte. That is, the secondary battery of the present disclosure may have a hybrid structure in which an electrolytic solution and a solid electrolyte are used in combination. Examples of the solid electrolyte material include a halide solid electrolyte, a sulfide solid electrolyte, an oxide solid electrolyte, or an organic polymer solid electrolyte. In the present disclosure, a "halide solid electrolyte" refers to a solid electrolyte containing a halogen element as a main component in anions. A "sulfide solid electrolyte" refers to a solid electrolyte containing sulfur as a main component in anions. An "oxide solid electrolyte" refers to a solid electrolyte containing oxygen as a main component in anions. The main component in anions refers to the anion with the largest amount of substance among all anions constituting the solid electrolyte. The coating material in the secondary battery of the present disclosure may include a halide solid electrolyte.
[0135] In the present disclosure, as an example of the structure of the secondary battery of Embodiment 3, a Figure 4 secondary battery having a structure example shown in which a laminated electrode group and an electrolytic solution are housed in an outer package, and the laminated electrode group is formed by laminating a positive electrode and a negative electrode with a separator therebetween, has been described. However, the secondary battery of the present disclosure is not limited to this structure example. The secondary battery of the present disclosure may be in any form such as cylindrical, square, coin-shaped, button-shaped, laminated type, etc. Further, as the electrode group in the secondary battery of the present disclosure, an electrode group in another form such as an electrode group formed by winding a positive electrode and a negative electrode with a separator therebetween may be applied instead of the laminated electrode group.
[0136] The application target of the coating for the positive electrode active material and the positive electrode of the present disclosure is not limited to the secondary battery 100. In addition to lithium secondary batteries, the coating for the positive electrode active material and the positive electrode of the present disclosure can be applied to various secondary batteries such as sodium secondary batteries and magnesium secondary batteries.
[0137] (Other Embodiments)
[0138] (Supplementary Note)
[0139] Based on the descriptions of the above embodiments, the following technical solutions are disclosed.
[0140] (Technical Solution 1)
[0141] A coated positive electrode active material, comprising a positive electrode active material, an oxide-containing layer, and a phosphorus-containing layer,
[0142] wherein the oxide-containing layer coats at least a part of the surface of the particles of the positive electrode active material,
[0143] the phosphorus-containing layer coats at least a part of the surface of the oxide-containing layer,
[0144] the oxide-containing layer contains an oxide and is in contact with the surface of the particles,
[0145] The phosphorus-containing layer contains a phosphoric acid compound,
[0146] The mass ratio of P contained in the phosphorus-containing layer to the positive electrode active material is 0.1% or more.
[0147] With this technical configuration, the dissolution of metal from the positive electrode can be suppressed.
[0148] (Technical solution 2)
[0149] For the positive electrode active material coated according to Technical solution 1, the oxide layer is substantially composed of the oxide. With such a technical configuration, the deterioration of the positive electrode active material can be suppressed and the dissolution of metal from the positive electrode can be suppressed.
[0150] (Technical solution 3)
[0151] For the positive electrode active material coated according to Technical solution 1 or 2, the oxide contains at least one selected from Si, Zr, Al, and Ti. With such a technical configuration, the dissolution of metal from the positive electrode can be suppressed.
[0152] (Technical solution 4)
[0153] For the positive electrode active material coated according to any one of Technical solutions 1 to 3, the oxide contains at least one selected from Si and Zr. With such a technical configuration, the dissolution of metal from the positive electrode can be further suppressed.
[0154] (Technical solution 5)
[0155] For the positive electrode active material coated according to any one of Technical solutions 1 to 4, the oxide contains at least one selected from SiO2 and ZrO2. With such a technical configuration, the dissolution of metal from the positive electrode can be further suppressed.
[0156] (Technical solution 6)
[0157] For the positive electrode active material coated according to any one of Technical solutions 1 to 5, the phosphoric acid compound is bonded to the oxide. With such a technical configuration, the dissolution of metal from the positive electrode can be suppressed.
[0158] (Technical solution 7)
[0159] For the positive electrode active material coated according to any one of Technical solutions 1 to 6, the phosphoric acid compound contains a P—O—P bond. With such a technical configuration, the dissolution of metal from the positive electrode can be suppressed.
[0160] (Technical solution 8)
[0161] The coated positive electrode active material according to any one of Technical Solutions 1 to 7, wherein the phosphoric acid compound contains a structure represented by Chemical Formula (1).
[0162]
[0163] n1 and n2 are independently integers of 0 or more,
[0164] R 1 、R 2 、R 4 and R 5 independently represent -OR or -(CH2) m1 X1,
[0165] R 3 and R independently represent a direct bonding bond with the oxide, a hydrogen atom, -(CH2) m2 X2, a trimethylsilyl group or a triethylsilyl group,
[0166] m1 is an integer from 0 to 15,
[0167] m2 is a natural number from 1 to 3,
[0168] X1 and X2 independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxyl group, a cyano group or a fluorine atom,
[0169] In the case where there are multiple Rs 2 s, the multiple Rs 2 s are independent of each other,
[0170] In the case where there are multiple Rs 4 s, the multiple Rs 4 s are independent of each other.
[0171] Due to the phosphoric acid compound having such a structure, it is relatively stable even in a high-voltage environment. Therefore, even when the upper limit voltage of the battery is high, side reactions such as oxidation decomposition of the electrolyte can be sufficiently suppressed, and metal dissolution of the positive electrode active material can be inhibited. In addition, the effect of suppressing side reactions can last for a longer time.
[0172] (Technical Solution 9)
[0173] The coated positive electrode active material according to Technical Solution 8, wherein in the Chemical Formula (1), R 1 、R 2 、R 4 and R 5 independently represent -OR, and R 3 and R independently represent a direct bonding bond with the oxide, a hydrogen atom or a trimethylsilyl group. By such a technical configuration, metal dissolution of the positive electrode active material can be further suppressed.
[0174] (Technical Solution 10)
[0175] For the coated positive electrode active material according to Technical Solution 8 or 9, in the chemical formula (1), R 3 represents a direct bonding bond with the oxide. With such a technical configuration, the metal dissolution of the positive electrode active material can be further suppressed.
[0176] (Technical Solution 11)
[0177] For the coated positive electrode active material according to any one of Technical Solutions 1 to 10, the positive electrode active material contains lithium nickel oxide, and the proportion of Ni among the metal elements other than Li contained in the lithium nickel oxide is 50 atomic% or more. With such a technical configuration, a high operating voltage of the battery can be achieved.
[0178] (Technical Solution 12)
[0179] A positive electrode includes a positive electrode current collector and a positive electrode active material layer carried on the positive electrode current collector,
[0180] and the positive electrode active material layer contains the coated positive electrode active material according to Technical Solutions 1 to 11.
[0181] With this technical configuration, side reactions in the positive electrode can be suppressed. Thereby, battery characteristics can be improved.
[0182] (Technical Solution 13)
[0183] A secondary battery includes the positive electrode, a negative electrode, and an electrolyte according to Technical Solution 12.
[0184] With this technical configuration, the characteristics of the secondary battery can be improved.
[0185] (Technical Solution 14)
[0186] A method for manufacturing a positive electrode, the positive electrode includes a positive electrode current collector and a positive electrode active material layer carried on the positive electrode current collector,
[0187] The manufacturing method satisfies at least one of (A) and (B) selected from the following.
[0188] (A) includes:
[0189] forming an oxide-containing layer on at least a part of the surface of the particles of the positive electrode active material,
[0190] forming the positive electrode active material layer containing the particles on the positive electrode current collector,
[0191] bringing a solution containing a phosphoric acid compound and a solvent into contact with the positive electrode active material layer, and
[0192] After the contact, the positive electrode active material layer is dried.
[0193] (B) includes:
[0194] An oxide-containing layer is formed on at least a part of the surface of the particles of the positive electrode active material,
[0195] A solution containing a phosphoric acid compound and a solvent is brought into contact with the particles on which the oxide-containing layer has been formed,
[0196] After the contact, the particles are dried under vacuum, and
[0197] The positive electrode active material layer containing the dried particles is formed on the positive electrode current collector.
[0198] By Technical Solution 14, the positive electrode of the present disclosure can be efficiently manufactured.
[0199] (Technical Solution 15)
[0200] According to the method for manufacturing a positive electrode described in Technical Solution 14, when (A) is satisfied, it further includes cleaning the positive electrode active material layer after the contact of the solution and before the drying, and when (B) is satisfied, it further includes cleaning the particles after the contact of the solution and before the drying. With this technical configuration, a positive electrode that further suppresses side reactions such as oxidative decomposition of the electrolyte can be manufactured.
[0201] (Technical Solution 16)
[0202] According to the method for manufacturing a positive electrode described in Technical Solution 14 or 15, the oxide-containing layer is formed by atomic layer deposition or mechanochemical method. With this technical configuration, the positive electrode of the present disclosure can be efficiently manufactured.
[0203] (Technical Solution 17)
[0204] According to the method for manufacturing a positive electrode described in any one of Technical Solutions 14 to 16,
[0205] The phosphoric acid compound contains a structure represented by Chemical Formula (2).
[0206]
[0207] R 7 represents a hydrogen atom, -(CH2) k1 Y1, trimethylsilyl or triethylsilyl,
[0208] R 6 and R 8 independently of each other represent -OR or -(CH2) k2 Y2,
[0209] R represents a hydrogen atom, -(CH2) k3 Y3, trimethylsilyl or triethylsilyl,
[0210] k1 and k3 are independently natural numbers from 1 to 3,
[0211] k2 is an integer from 0 to 15,
[0212] Y1, Y2 and Y3 independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxyl group, a cyano group or a fluorine atom.
[0213] Due to the phosphoric acid compound having such a structure, even in the case of a high upper limit voltage, side reactions such as oxidation decomposition of the electrolyte can be sufficiently suppressed, metal dissolution of the positive electrode active material can be suppressed, and the positive electrode can be efficiently manufactured.
[0214] (Technical Solution 18)
[0215] According to the method for manufacturing a positive electrode according to any one of Technical Solutions 14 to 17, the phosphoric acid compound contains tris(trimethylsilyl) phosphate. With such a technical configuration, metal dissolution of the positive electrode active material can be suppressed, and the positive electrode can be manufactured more efficiently.
[0216] Examples
[0217] Hereinafter, the present disclosure will be described in more detail using examples. The following examples are merely illustrative and not limiting.
[0218] (Example 1)
[0219] For a positive electrode active material having a composition of LiNi 0.8 Mn 0.2 O2, a film of SiO2 is formed on the surface of the positive electrode active material by low-temperature ALD at 200 °C or lower. The thickness of the film measured by spectroscopic ellipsometry is 9.8 nm.
[0220] The positive electrode active material coated with the oxide, acetylene black (AB), and polyvinylidene fluoride (PVDF) are added to N-methyl-2-pyrrolidone (NMP) and stirred to prepare a positive electrode slurry. The mass ratio of these materials in the positive electrode active material layer is positive electrode active material: AB: PVDF = 96: 2: 2.
[0221] The positive electrode slurry is coated on the surface of an aluminum foil (1.45 cm × 1.45 cm), and after the coating film is dried, it is rolled to form a positive electrode active material layer. In this way, a plate in which the positive electrode active material layer is supported on the positive electrode current collector is obtained.
[0222] Tris(trimethylsilyl) phosphate (TMSP) was added to dimethyl carbonate (DMC) to obtain a TMSP solution. The concentration of TMSP in the TMSP solution was 2% by mass.
[0223] The electrode plate was immersed in 1 mL of the TMSP solution. After standing at room temperature for 5 minutes, the electrode plate was taken out and washed with DMC. The washed electrode plate was dried in vacuo for 30 minutes. Thus, a phosphorus-containing layer was formed. The amount of phosphorus (P) contained in the phosphorus-containing layer was measured by inductively coupled plasma (ICP) emission analysis. As a result, the mass ratio of P to the positive electrode active material used was 0.18% by mass. In addition, when calculating this ratio, the mass of the positive electrode active material can be the charged amount.
[0224] The positive electrode of Example 1 was obtained as described above. The positive electrode obtained as described above contains, at least near its surface, a coated positive electrode active material, and the coated positive electrode active material has an oxide layer covering the surface of the particles of the positive electrode active material and a phosphorus-containing layer covering at least a part of the surface of the oxide layer. It is speculated that the mass ratio of P in the coated positive electrode active material to the positive electrode active material is greater than the above measurement result of 0.18% by mass.
[0225] Using the positive electrode of Example 1, a Li metal foil as a counter electrode, a separator, and an electrolyte, an evaluation cell of Example 1 was fabricated. As the separator, a PP / PE / PP three-layer separator was used. The concentration of LiPF6 in the electrolyte was 13 mol / L. The solvent of the electrolyte contained ethylene carbonate (EC) and DMC at a volume ratio of EC:DMC = 25:75.
[0226] (Example 2)
[0227] A film of Al2O3 was formed during the formation of the oxide layer by low-temperature ALD. The thickness of the film measured by spectroscopic ellipsometry was 11.8 nm. Except for this, the positive electrode of Example 2 was fabricated in the same manner as in Example 1. Using the positive electrode of Example 2, an evaluation cell of Example 2 was fabricated in the same manner as in Example 1.
[0228] (Example 3)
[0229] A film of ZrO2 was formed during the formation of the oxide layer by low-temperature ALD. The thickness of the film measured by spectroscopic ellipsometry was 6.1 nm. Except for this, the positive electrode of Example 3 was fabricated in the same manner as in Example 1. Using the positive electrode of Example 3, an evaluation cell of Example 3 was fabricated in the same manner as in Example 1.
[0230] (Comparative Example 1)
[0231] Having LiNi 0.8 Mn 0.2The positive electrode active material composed of O2, acetylene black (AB), and polyvinylidene fluoride (PVDF) were added to N-methyl-2-pyrrolidone (NMP) and stirred to prepare the positive electrode paste. The mass ratio of these materials in the positive electrode active material layer was positive electrode active material:AB:PVDF = 96:2:2.
[0232] The positive electrode paste was coated on the surface of an aluminum foil (1.45 cm × 1.45 cm). After the coating film was dried, it was calendered to form a positive electrode active material layer. Thus, the positive electrode of Comparative Example 1 was fabricated. That is, the positive electrode of Comparative Example 1 did not contain the coated positive electrode active material having an oxide layer and a phosphorus-containing layer.
[0233] Using the positive electrode of Comparative Example 1, an evaluation cell of Comparative Example 1 was fabricated in the same manner as in Example 1.
[0234] (Comparative Example 2)
[0235] A SiO2 film was formed on the surface of the positive electrode active material having a composition of LiNi 0.8 Mn 0.2 O2 in the same manner as in Example 1. Using this positive electrode active material, a positive electrode active material layer was formed on the positive electrode current collector in the same manner as in Comparative Example 1. Thus, the positive electrode of Comparative Example 2 was fabricated.
[0236] Using the positive electrode of Comparative Example 2, an evaluation cell of Comparative Example 2 was fabricated in the same manner as in Example 1.
[0237] (Comparative Example 3)
[0238] An Al2O3 film was formed in the same manner as in Example 2 during the formation of the oxide layer by low-temperature ALD. Except for this, the positive electrode of Comparative Example 3 was fabricated in the same manner as in Comparative Example 2. Using the positive electrode of Comparative Example 3, an evaluation cell of Comparative Example 3 was fabricated in the same manner as in Example 1.
[0239] (Comparative Example 4)
[0240] A ZrO2 film was formed in the same manner as in Example 3 during the formation of the oxide layer by low-temperature ALD. Except for this, the positive electrode of Comparative Example 4 was fabricated in the same manner as in Comparative Example 2. Using the positive electrode of Comparative Example 4, an evaluation cell of Comparative Example 4 was fabricated in the same manner as in Example 1.
[0241] (Comparative Example 5)
[0242] A TiO2 film was formed during the formation of the oxide layer by low-temperature ALD. The thickness of the film measured by spectroscopic ellipsometry was 3.2 nm. Except for this, the positive electrode of Comparative Example 5 was fabricated in the same manner as in Comparative Example 2. Using the positive electrode of Comparative Example 5, an evaluation cell of Comparative Example 5 was fabricated in the same manner as in Example 1.
[0243] (Comparative Example 6)
[0244] The positive electrode active material having a composition of LiNi 0.8 Mn 0.2 O2, acetylene black (AB), and polyvinylidene fluoride (PVDF) were added to N-methyl-2-pyrrolidone (NMP) and stirred to prepare a positive electrode paste. The mass ratio of these materials in the positive electrode active material layer was positive electrode active material:AB:PVDF = 96:2:2.
[0245] The positive electrode paste was coated on the surface of an aluminum foil (1.45 cm × 1.45 cm). After the coating film was dried, it was calendered to form a positive electrode active material layer. Thus, a plate in which the positive electrode active material layer was supported on the positive electrode current collector was obtained.
[0246] The plate was immersed in the TMSP solution in the same manner as in Example 1, washed with DMC, and then vacuum dried. The positive electrode of Comparative Example 6 was obtained through the above steps.
[0247] Using the positive electrode of Comparative Example 6, an evaluation cell of Comparative Example 6 was fabricated in the same manner as in Example 1.
[0248] [Evaluation of Metal Dissolution Amount]
[0249] For the evaluation cells of the examples and comparative examples, at an ambient temperature of 25°C, charge and discharge were repeatedly performed 2 times with a constant current value of 0.1C until the voltage reached 4.5V, and then with a constant current value of 0.1C until the voltage reached 2.5V. Then, constant current charging was performed with a current value of 0.2C until the voltage reached 4.5V, and then the voltage of 4.5V was maintained at an ambient temperature of 55°C for 3 days.
[0250] Then, the amount of Mn dissolved in the counter electrode was measured by ICP emission analysis. The evaluation results are shown in Table 1.
[0251] Table 1
[0252] oxide phosphoric acid compound Mn elution amount (μmol) Example 1 <![CDATA[SiO2]]> TMSP 0.0360 Example 2 <![CDATA[Al2O3]]> TMSP 0.0510 Example 3 <![CDATA[ZrO2]]> TMSP 0.0096 Comparative Example 1 - - 0.1200 Comparative Example 2 <![CDATA[SiO2]]> - 0.0870 Comparative Example 3 <![CDATA[Al2O3]]> - 0.0810 Comparative Example 4 <![CDATA[ZrO2]]> - 0.0830 Comparative Example 5 <![CDATA[TiO2]]> - 0.1000 Comparative Example 6 - TMSP 0.0590
[0253] (Investigation)
[0254] In Examples 1 to 3, the amount of Mn eluted was less than that in Comparative Example 1 in which the positive electrode active material did not have a film. Further, in Examples 1 to 3, the amount of Mn eluted was less than that in Comparative Examples 2 to 5 in which the positive electrode active material was only covered with an oxide. Based on the above, in Examples 1 to 3, the elution of metal from the positive electrode active material was suppressed. If the oxide contains SiO2 or ZrO2, the elution of Mn is further suppressed. It is presumed that SiO2 or ZrO2 also remains stably on the surface of the positive electrode after the battery is charged and discharged, and as a result, the effect of the phosphate compound remaining on the surface of the positive electrode is high, and the effect of suppressing the elution of metal from the positive electrode active material is high.
[0255] Industrial applicability
[0256] The technology of the present disclosure can be applied to secondary batteries used as power sources for mobile communication devices, portable electronic devices, electric vehicles, and the like.
Claims
1. A coated positive electrode active material comprising a positive electrode active material, an oxide-containing layer, and a phosphorus-containing layer, wherein the oxide-containing layer coats at least a part of the surface of the particles of the positive electrode active material, the phosphorus-containing layer coats at least a part of the surface of the oxide-containing layer, the oxide-containing layer contains an oxide and is in contact with the surface of the particles, the phosphorus-containing layer contains a phosphoric acid compound, the mass ratio of P contained in the phosphorus-containing layer to the positive electrode active material is 0.1% or more.
2. The coated positive electrode active material according to claim 1, wherein the oxide-containing layer consists essentially of the oxide.
3. The coated positive electrode active material according to claim 1, wherein the oxide contains at least one selected from Si, Zr, Al, and Ti.
4. The coated positive electrode active material according to claim 3, wherein the oxide contains at least one selected from Si and Zr.
5. The coated positive electrode active material according to claim 4, wherein the oxide contains at least one selected from SiO2 and ZrO2.
6. The coated positive electrode active material according to claim 1, wherein the phosphoric acid compound is bonded to the oxide.
7. The coated positive electrode active material according to claim 1, wherein the phosphoric acid compound contains a P-O-P bond.
8. The coated positive electrode active material according to claim 7, wherein the phosphoric acid compound contains a structure represented by Chemical Formula (1), n1 and n2 are independently integers of 0 or more, R 1 、R 2 、R 4 and R 5 Independently represents -OR or -(CH2) m1 X1, R 3 R and, independently of one another, represent a direct bonding to the oxide, a hydrogen atom, -(CH2) m2 X2, a trimethylsilyl group or a triethylsilyl group, m1 is an integer of 0 to 15, m2 is a natural number of 1 to 3, X1 and X2 independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxyl group, a cyano group, or a fluorine atom, In the case of having multiple Rs 2 in the case, the multiple Rs 2 are independent of each other In the case where there are multiple Rs 4 in the case, the multiple Rs 4 are independent of each other.
9. The coated positive electrode active material according to claim 8, In the chemical formula (1), R 1 , R 2 , R 4 and R 5 each independently represents -OR, R 3 R and, independently of one another, represent a direct binding bond with the oxide, a hydrogen atom or a trimethylsilyl group.
10. The coated positive electrode active material according to claim 8, In the chemical formula (1), R 3 represents a direct bonding bond with the oxide.
11. The coated positive electrode active material according to claim 1, wherein the positive electrode active material contains a lithium nickel oxide, and the proportion of Ni among the metal elements other than Li contained in the lithium nickel oxide is 50 atomic% or more.
12. A positive electrode comprising a positive electrode current collector and a positive electrode active material layer supported on the positive electrode current collector, wherein the positive electrode active material layer contains the coated positive electrode active material according to claims 1 to 11.
13. A secondary battery comprising the positive electrode according to claim 12, a negative electrode, and an electrolyte.
14. A method for manufacturing a positive electrode, the positive electrode comprising a positive electrode current collector and a positive electrode active material layer supported on the positive electrode current collector, wherein the manufacturing method satisfies at least one of (A) and (B) selected from the following, (A) The manufacturing method includes: forming an oxide-containing layer on at least a part of the surface of the particles of the positive electrode active material, forming the positive electrode active material layer containing the particles on the positive electrode current collector, bringing a solution containing a phosphoric acid compound and a solvent into contact with the positive electrode active material layer, and after the contact, drying the positive electrode active material layer, (B) The manufacturing method includes: forming an oxide-containing layer on at least a part of the surface of the particles of the positive electrode active material, bringing a solution containing a phosphoric acid compound and a solvent into contact with the particles having the oxide-containing layer formed thereon, After the contact, the particles are dried in vacuo, and the positive electrode active material layer containing the dried particles is formed on the positive electrode current collector.
15. The method for manufacturing a positive electrode according to claim 14, when (A) is satisfied, further comprising cleaning the positive electrode active material layer after the contact of the solution and before the drying, when (B) is satisfied, further comprising cleaning the particles after the contact of the solution and before the drying.
16. The method for manufacturing a positive electrode according to claim 14, the oxide-containing layer is formed by atomic layer deposition or mechanochemical method.
17. The method for manufacturing a positive electrode according to claim 14, the phosphoric acid compound contains a structure represented by Chemical Formula (2), R 7 represents a hydrogen atom, -(CH2) k1 Y1, a trimethylsilyl group or a triethylsilyl group, R 6 and R 8 each independently represents -OR or -(CH2) k2 Y2, R represents a hydrogen atom, -(CH2) k3 Y3, trimethylsilyl or triethylsilyl, k1 and k3 are independently natural numbers from 1 to 3, k2 is an integer from 0 to 15, Y1, Y2, and Y3 independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxyl group, a cyano group, or a fluorine atom.
18. The method for manufacturing a positive electrode according to claim 14, the phosphoric acid compound contains tris(trimethylsilyl) phosphate.
Citation Information
Patent Citations
Cathode active material and manufacturing method therefor, and nonaqueous electrolyte secondary battery
JP2008016235A
Positive electrode active material for nonaqueous electrolyte secondary battery, method for manufacturing same, and positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
JP2009245917A