A composite modifier for recycled rubber and plastic asphalt based on shear force-temperature-interface modification, its preparation method and application

By leveraging the synergistic effect of a twin-screw extruder and a silane coupling agent, the bonding between tire rubber powder and low-density polyethylene is activated, forming a secondary cross-linked network. This solves the problem of poor storage stability of rubber and polyethylene in asphalt, achieving high efficiency compatibility and performance improvement of modified asphalt.

CN120484361BActive Publication Date: 2026-11-10TONGJI UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202510781054.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-12
Publication Date
2026-11-10
Estimated Expiration
2045-06-12

AI Technical Summary

Technical Problem

In existing technologies, the multiphase system formed by rubber and polyethylene in asphalt suffers from poor storage stability and inadequate high and low temperature modification effects. Furthermore, traditional activation methods are inefficient and fail to fully realize the modification effect.

Method used

A shear-force-temperature-interface modification method was adopted. Through the three-zone gradient temperature control of a twin-screw extruder and the synergistic effect of a silane coupling agent, the interaction between tire rubber powder and low-density polyethylene was activated to form a secondary cross-linking network, thereby improving compatibility and modification effect.

Benefits of technology

It achieves high compatibility of modified asphalt, balances and improves high-temperature performance, low-temperature performance, storage stability and anti-aging performance, while reducing costs, and has significant economic and social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to a recycled rubber-plastic asphalt composite modifier based on shear force-temperature-interface modification, its preparation method, and its application. The recycled rubber-plastic asphalt composite modifier comprises 65-75 parts tire rubber powder, 17-25 parts polyethylene, 8-12 parts aromatic oil, and 0-2 parts silane coupling agent (excluding 0). The raw materials are mixed and added to a twin-screw extruder, where a three-zone gradient temperature control is used (feeding zone, plasticizing zone, and homogenizing zone). Finally, granulation is performed to obtain the recycled rubber-plastic asphalt composite modifier. Compared with existing technologies, this invention innovatively utilizes the shear force of the twin-screw extruder, high temperature, and the interfacial activation of the silane coupling agent, synergistically combining physical melting and recombination with chemical interfacial activation to efficiently improve the integration, activation efficiency, and effect of tire rubber powder and polyethylene, significantly enhancing the performance of the modified asphalt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of transportation engineering construction materials technology, and in particular to a recycled rubber-plastic asphalt composite modifier based on shear force-temperature-interface modification, its preparation method and application. Background Technology

[0002] Asphalt pavement is the most widely used type of pavement on high-grade highways, and with the increasing demands for highway reconstruction, expansion, and maintenance, the consumption of asphalt, as a crucial component, will continue to rise. Asphalt binder is key to the function and lifespan of asphalt pavement, and its quality requirements are constantly increasing. Currently, polymer-modified asphalts such as SBS, SEBS, and TPS are frequently used in large-scale high-grade highway asphalt pavements to improve material performance. However, polymers such as SBS have issues such as needing improvement in aging resistance, and they are also costly, resource-intensive, and lack environmental friendliness. Therefore, there is an urgent need to develop low-cost, sustainable modified asphalt materials to support the construction of high-quality and green highways.

[0003] Tires and plastics contain high-molecular polymers that can improve asphalt quality, making them excellent raw materials for asphalt modification. Recycled rubber and plastic modified asphalt, through the recycling of waste tires, polyethylene, and other resources, can achieve improved durability, adhesion, material sustainability, and cost control. The synergistic existence of rubber's softening properties and asphalt's hardening properties during aging can enhance the aging performance of modified asphalt, while the regular molecular chain structure and crystallization behavior of polyethylene can improve the elasticity and deformation resistance of asphalt. However, as composite materials, the rubber and polyethylene phases form a multiphase system in asphalt. Due to differences in modification preparation processes and polymer handling methods, the free distribution and cross-linking of rubber and polyethylene in the asphalt phase are random, leading to poor storage stability and difficulty in fully realizing their high and low temperature modification effects.

[0004] In recent years, studies have explored activation treatments for rubber powder and polyethylene using various pretreatment methods, such as melt blending or high-temperature desulfurization. For example, patent CN103709770A discloses a polyethylene / rubber powder blend modified asphalt and its preparation method. Rubber powder, polyethylene, and a crosslinking agent are melt-extruded using a twin-screw extruder at 160℃–190℃ to obtain a polyethylene / rubber powder blend, which is then mixed and sheared with base asphalt to obtain modified asphalt. However, this activation method suffers from insufficient targeting and low activation efficiency. Therefore, there is an urgent need to develop new activation methods that can increase the content and effect of tire rubber and polyethylene plastics while ensuring their full compatibility and maximizing the modification effect. Summary of the Invention

[0005] The purpose of this invention is to overcome the problems of poor storage stability and poor high and low temperature modification in the existing technology of combining rubber and polyethylene, and to provide a recycled rubber-plastic asphalt composite modifier based on shear force-temperature-interface modification, its preparation method and application.

[0006] The objective of this invention can be achieved through the following technical solutions:

[0007] One of the technical solutions of the present invention is to provide a recycled rubber-plastic asphalt composite modifier based on shear force-temperature-interface modification, comprising 65-75 parts of tire rubber powder, 17-25 parts of polyethylene, 8-12 parts of aromatic oil, and 0-2 parts of silane coupling agent (excluding 0).

[0008] In some specific embodiments, the tire rubber powder is selected from tire rubber powder with a particle size of 40-60 mesh, Mooney viscosity ≤95, and relative density of 1-1.15;

[0009] The polyethylene is selected from polyethylene with a relative density of 0.94 to 1.15, a particle size of ≤3 mm, and a melt flow index (MFI) of ≥1 g / 10 min;

[0010] The aromatic oil is selected from those with a kinematic viscosity of 10–40 mm. 2 / s of aromatic oil;

[0011] The silane coupling agent is 3-aminopropyltriethoxysilane.

[0012] More preferably, the tire rubber powder is selected from tire rubber powder with a particle size of 40-60 mesh, Mooney viscosity ≤95, and relative density of 1-1.1;

[0013] The polyethylene is selected from polyethylene with a relative density of 0.95 to 1.05, a particle size of ≤2 mm, and a melt flow index (MFI) of (1 to 4) g / 10 min.

[0014] The second technical solution of the present invention is to provide a method for preparing a recycled rubber-plastic asphalt composite modifier as described in one of the above technical solutions, comprising the following steps:

[0015] S1. Mix tire rubber powder, polyethylene, aromatic oil, and silane coupling agent according to the mass parts to obtain mixture A;

[0016] S2. Add the mixture A from step S1 into a twin-screw extruder and use a three-zone gradient temperature control in the feeding zone, plasticizing zone, and homogenizing zone to obtain mixture B;

[0017] S3. Granulate the mixture B from step S2 into granules to form a recycled rubber-plastic asphalt composite modifier.

[0018] In some specific embodiments, in step S2, the twin-screw extruder rotates at a speed of 15 r / min.

[0019] In some specific embodiments, in step S2, the temperatures of the feeding zone, plasticizing zone, and homogenizing zone are 200–240°C, 240–300°C, and 260–300°C, respectively.

[0020] As a more preferred option, the temperature ratio of the feeding zone, plasticizing zone, and homogenizing zone is 240℃, 260℃, and 260℃, respectively.

[0021] In some specific embodiments, in step S3, the particle size is 1 to 3 mm.

[0022] The third technical solution of the present invention is to provide an application of the recycled rubber-plastic asphalt composite modifier as described in one of the above technical solutions in the preparation of modified asphalt.

[0023] In some specific embodiments, the method for preparing modified asphalt using the recycled rubber-plastic asphalt composite modifier includes the following steps:

[0024] Recycled rubber-plastic asphalt composite modifier is added to flowing base asphalt, and the mixture is stirred, sheared, and mixed at high temperature. After heat preservation and development, modified asphalt is obtained.

[0025] The mass ratio of the base asphalt to the recycled rubber and plastic asphalt composite modifier is 100:(15-35).

[0026] In some specific implementations, the high temperature is 175–185°C;

[0027] The stirring speed is 300-500 r / min each time, and the stirring time is 20-30 min each time;

[0028] The shearing speed is 4000–5000 r / min, and the shearing time is 50–70 min;

[0029] The temperature for heat preservation and development is 175-180℃, and the heat preservation and development time is 20-40 minutes.

[0030] As a preferred option, the high temperature is 185°C, and the temperature for heat preservation and development is 175°C.

[0031] In some specific embodiments, the base asphalt is petroleum asphalt.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) This invention innovatively utilizes the shear force of a twin-screw extruder, high temperature, and the interfacial activation of a silane coupling agent to synergistically enhance the integration, activation efficiency, and effect of tire rubber powder and polyethylene. Firstly, this invention utilizes the shear force of a twin-screw extruder and the activation effect of a three-zone gradient heating to dissociate the stable internal structure of the tire rubber powder and polyethylene, allowing them to combine and form a secondary cross-linked network, integrating their properties. During the entire shear and high-temperature process, the silane coupling agent releases active amino groups to enhance the surface activity of the rubber-plastic elastomer, thereby more efficiently improving the compatibility of the modifier with asphalt and balancing the modification effect (balancing the improvement of high-temperature performance, low-temperature performance, storage stability, and anti-aging performance, while ensuring viscosity remains within a reasonable range).

[0034] (2) Compared with SBS, the low-density polyethylene selected in this invention has more significant resistance to deformation and cost advantages. Moreover, low-density polyethylene can be derived from common plastic waste, and the source is controllable and widely available.

[0035] (3) The tire rubber powder and low-density polyethylene selected in this invention can both be derived from solid waste. While ensuring performance, it can also significantly reduce costs and solve the urgent problem of industrial solid waste treatment, thus having significant economic and social benefits.

[0036] (4) The preparation process of this invention is simple, efficient, easy to operate, and low in cost, and it is easy to promote and apply in practical engineering. Detailed Implementation

[0037] The present invention will now be described in detail with reference to specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0038] Unless otherwise specified, the raw materials or processing techniques used in the following embodiments and comparative examples are all conventional commercially available raw materials or conventional processing techniques in the art.

[0039] Example 1

[0040] This embodiment provides a recycled rubber-plastic asphalt composite modifier and modified asphalt based on shear force-temperature-interface modification.

[0041] In this embodiment, the composition and mass ratio of each raw material of the modifier are as follows: 68 parts of 60-mesh waste tire rubber powder, 20 parts of recycled low-density polyethylene, 10 parts of aromatic oil, and 2 parts of silane coupling agent. Among them, the waste tire rubber powder was purchased from Chengdu Sitong Rubber & Plastics Co., Ltd., and is 60-mesh rubber powder processed from truck tires by ambient temperature crushing method; the recycled low-density polyethylene was purchased from Yuyao Hechang Plastics Co., Ltd., and is black 2MFI / RLDPE; the aromatic oil was purchased from Hengshui Junwei New Material Technology Co., Ltd., and is a special aromatic oil for road asphalt; the silane coupling agent is 3-aminopropyltriethoxysilane, purchased from Dongguan Kangjin New Material Technology Co., Ltd.

[0042] The basic properties of waste tire rubber powder, recycled low-density polyethylene and aromatic oil are shown in Tables 1, 2 and 3.

[0043] Table 1 Basic Properties of Waste Tire Rubber Powder

[0044] index value unit relative density 1.05~1.15 / Mooney viscosity ML(1+4) 100℃ 91 Pa·s Ash 6 % Acetone extract 1.5 % Rubber hydrocarbon content 48 % Carbon black content 32 %

[0045] Table 2 Basic Properties of Recycled Low-Density Polyethylene

[0046] index value unit color black —— Particle size 2~3 mm density 0.98 <![CDATA[g / cm 3 ]]> Melt Flow Index (MFI) 2 g / 10min Elongation at break 300 %

[0047] Table 3. Product Indicators of Aromatic Oils for Road Asphalt

[0048] Testing items value unit Kinematic viscosity (the ratio of dynamic viscosity to density) 25 <![CDATA[100℃,mm 2 / s]]> Open flash point 220 ℃ Moisture 0.01 % density 0.96 <![CDATA[g / m 3 ]]> Appearance brown -

[0049] The preparation method of the recycled rubber-plastic asphalt composite modifier based on shear force-temperature-interface modification includes the following steps:

[0050] (1) Add waste tire rubber powder, recycled low-density polyethylene, aromatic oil and silane coupling agent to a container in a mass ratio of 68:20:10:2, stir and mix evenly to obtain mixture A;

[0051] (2) Add mixture A into a twin-screw extruder with a speed of 15 r / min. Use three-zone gradient temperature control with temperatures of 240℃, 260℃ and 260℃ in the feeding zone, plasticizing zone and homogenizing zone respectively. Do not use the circulating shear extrusion mode to prepare mixture B.

[0052] (3) Mixture B is passed through an air cooler and granulated by a pelletizer to form 1-3 mm particles to obtain recycled rubber-plastic asphalt composite modifier.

[0053] The composition and weight distribution of each raw material in the modified asphalt are as follows: 100 parts asphalt and 30 parts recycled rubber-plastic asphalt composite modifier. The asphalt was purchased from Sinopec Zhenhai Refining & Chemical Branch and is No. 70 road petroleum asphalt.

[0054] The preparation method of this modified asphalt includes the following steps:

[0055] (1) Heat 100 parts of base asphalt at about 172°C until it is fully fluid.

[0056] (2) Slowly add 30 parts of recycled rubber and plastic asphalt composite modifier to the base asphalt. During this process, use a mixer to continuously stir at a speed of about 400 r / min for 30 min until there are no obvious particles, and obtain mixture B.

[0057] (3) The mixture B was sheared using a high-speed shearing machine at a speed of 4500 r / min for 60 min to obtain mixture C.

[0058] (4) Mixture C was continuously stirred using a mixer at a speed of 500 r / min for 30 min to obtain mixture D.

[0059] All operations in steps (2) to (4) were performed at 185°C.

[0060] (5) Keep mixture D warm for 30 minutes at a temperature of 175°C. After the development is complete, recycled rubber-plastic composite modified asphalt is obtained.

[0061] Example 2

[0062] This embodiment provides a recycled rubber-plastic asphalt composite modifier and modified asphalt based on shear force-temperature-interface modification.

[0063] In this embodiment, the composition and mass ratio of each raw material of the modifier are as follows: 64 parts of 60-mesh waste tire rubber powder, 19 parts of recycled low-density polyethylene, 16 parts of aromatic oil, and 1 part of silane coupling agent. Among them, the waste tire rubber powder was purchased from Chengdu Sitong Rubber & Plastics Co., Ltd., and is 60-mesh rubber powder processed from truck tires by ambient temperature crushing method; the recycled low-density polyethylene was purchased from Yuyao Hechang Plastics Co., Ltd., and is black 2MFI / RLDPE; the aromatic oil was purchased from Hengshui Junwei New Material Technology Co., Ltd., and is a special aromatic oil for road asphalt; the silane coupling agent is 3-aminopropyltriethoxysilane, purchased from Dongguan Kangjin New Material Technology Co., Ltd.

[0064] The basic properties of waste tire rubber powder, recycled low-density polyethylene, and aromatic oil are the same as in Example 1.

[0065] The preparation method of the recycled rubber-plastic asphalt composite modifier based on shear force-temperature-interface modification includes the following steps:

[0066] (1) Add waste tire rubber powder, recycled low-density polyethylene, aromatic oil and silane coupling agent to a container in a mass ratio of 64:19:16:1 and stir evenly to obtain mixture A;

[0067] (2) Add mixture A into a twin-screw extruder with a speed of 15 r / min. Use three-zone gradient temperature control with temperatures of 240℃, 260℃ and 260℃ in the feeding zone, plasticizing zone and homogenizing zone respectively. Do not use the circulating shear extrusion mode to prepare mixture B.

[0068] (3) Mixture B is passed through an air cooler and granulated by a pelletizer to form 1-3 mm particles to obtain recycled rubber-plastic asphalt composite modifier.

[0069] The composition and mass ratio of each raw material in the modified asphalt of this embodiment, as well as the preparation method, are the same as those in Example 1.

[0070] Example 3

[0071] This embodiment provides a recycled rubber-plastic asphalt composite modifier and modified asphalt based on shear force-temperature-interface modification.

[0072] In this embodiment, the composition and mass ratio of each raw material of the modifier and the preparation method are the same as in Example 1.

[0073] The composition and weight distribution of each raw material in the modified asphalt are as follows: 100 parts asphalt and 20 parts recycled rubber-plastic asphalt composite modifier. The asphalt was purchased from Sinopec Zhenhai Refining & Chemical Branch and is No. 70 road petroleum asphalt.

[0074] The preparation method of this modified asphalt includes the following steps:

[0075] (1) Heat 100 parts of base asphalt at about 172°C until it is fully fluid.

[0076] (2) Slowly add 20 parts of recycled rubber and plastic asphalt composite modifier to the base asphalt. During this process, use a mixer to continuously stir at a speed of about 400 r / min for 30 min until there are no obvious particles, and obtain mixture B.

[0077] (3) The mixture B was sheared using a high-speed shearing machine at a speed of 4500 r / min for 60 min to obtain mixture C.

[0078] (4) Mixture C was continuously stirred using a mixer at a speed of 500 r / min for 30 min to obtain mixture D.

[0079] All operations in steps (2) to (4) were performed at 185°C.

[0080] (5) Keep mixture D warm for 30 minutes at a temperature of 175°C. After the development is complete, recycled rubber-plastic composite modified asphalt is obtained.

[0081] Comparative Example 1

[0082] This comparative example provides a recycled rubber-plastic asphalt composite modifier and the preparation of modified asphalt.

[0083] Compared with Example 1, most of them are the same, the only difference being that the raw material composition of the modifier does not contain silane coupling agent.

[0084] The mass proportions of the comparative modifier are as follows: 68 parts of 60-mesh waste tire rubber powder, 20 parts of recycled low-density polyethylene, and 10 parts of aromatic oil.

[0085] Comparative Example 2

[0086] This comparative example provides a recycled rubber-plastic asphalt composite modifier and modified asphalt.

[0087] Compared with Example 1, they are mostly the same, with the only difference being:

[0088] In preparing the modifier, the raw materials were not prepared using a twin-screw extruder, but were prepared in a dispersed form according to the same mass ratio as in Example 1.

[0089] The dispersion process involves simply stirring and mixing the raw materials in a container.

[0090] Comparative Example 3

[0091] This comparative example provides a recycled rubber-plastic asphalt composite modifier and modified asphalt.

[0092] Compared to Example 1, most aspects are the same, with the only difference being the composition and mass ratio of the modifier raw materials. Specifically, the mass ratio is as follows: 77 parts of 60-mesh waste tire rubber powder and 23 parts of recycled low-density polyethylene. Furthermore, this modifier is not prepared using a twin-screw extruder but is prepared in a dispersed form according to the mass ratio of each raw material.

[0093] Comparative Example 4

[0094] This comparative example provides an SBS-modified asphalt and its preparation. The composition and mass proportions of each raw material are as follows: 100 parts base asphalt and 4 parts SBS. The SBS is type 791, purchased from the Beijing Yanshan Branch of China Petroleum & Chemical Corporation.

[0095] All other steps are the same as in Example 1.

[0096] Comparative Example 5

[0097] This comparative example provides a desulfurized tire rubber powder modified asphalt and its preparation. The composition and mass proportions of each raw material are as follows: 100 parts of base asphalt and 20 parts of desulfurized tire rubber powder. The desulfurized tire rubber powder is 60-mesh truck tire desulfurized rubber powder, purchased from Chengdu Sitong Rubber & Plastics Co., Ltd., and is formed by high-temperature desulfurization of 60-mesh truck tire rubber powder produced by room-temperature pulverization. The basic properties of the desulfurized tire rubber powder are shown in Table 4. The preparation method of this desulfurized tire rubber powder modified asphalt is the same as in Example 1.

[0098] Table 4 Basic Properties of Desulfurized Tire Rubber Powder

[0099] index value unit relative density 1.15 / Ash 4.5 % Acetone extract 6 % Rubber hydrocarbon content 48 % Carbon black content 32 %

[0100] Comparative Example 6

[0101] This comparative example provides a recycled rubber-plastic asphalt composite modifier and modified asphalt.

[0102] Compared with Example 1, most of them are the same, the only difference is that in step (2), the temperatures of the feeding zone, plasticizing zone and homogenizing zone are set to 180℃, 200℃ and 200℃ respectively.

[0103] The modified asphalts prepared in Examples 1-3 and Comparative Examples 1-6 were tested, and the results are shown in Table 5:

[0104] Table 5 Comparison of Asphalt Performance between Examples and Comparative Examples

[0105]

[0106]

[0107] As can be seen from the table above, the embodiments of the present invention can achieve a good balance between high-temperature performance (reflected in the increase of softening point), low-temperature performance (reflected in the increase of ductility), and storage stability (reflected in the decrease of softening point difference) compared with all comparative examples, and all indicators meet and exceed the requirements of "Road Waste Tire Rubber Powder Rubber Asphalt (JT / T798-2019)".

[0108] Compared with Comparative Example 1, Example 1 improved the high-temperature performance, low-temperature performance, and storage stability of the modified asphalt. It can be seen that in this invention, the surface activity of the rubber-plastic elastomer can be enhanced by releasing active amino groups through the silane coupling agent during the entire shear and high-temperature process, thereby more efficiently improving the compatibility of the modifier and the asphalt and improving the modification effect in a balanced way.

[0109] Compared to Comparative Examples 2 and 6, Example 1 improved the low-temperature performance, storage stability, and anti-aging properties of the modified asphalt while ensuring that the viscosity remained within a reasonable range. It can be seen that in this invention, the shear force of the twin screw and the activation effect of the three-zone gradient heating can be used to dissociate the tire rubber powder from the stable internal structure of polyethylene, and the two can combine to form a secondary cross-linked network, integrating the properties of both.

[0110] Compared to Comparative Example 3, Example 1 shows that although Comparative Example 3 has better high-temperature performance, its waste tire rubber powder and recycled low-density polyethylene have not been activated, resulting in poor compatibility and large internal particles. This leads to poor low-temperature ductility and storage stability, as well as excessively high viscosity, which affects the compaction during construction.

[0111] Compared with Comparative Examples 4 and 5, Example 1 also improved the high-temperature performance, storage stability, and anti-aging performance of modified asphalt in a balanced way, which is significantly better than traditional asphalt modifiers. It can be seen that the modifier prepared by the present invention has a more comprehensive effect on improving the high and low temperature performance, aging performance, and storage stability of asphalt compared with SBS and desulfurized rubber powder.

[0112] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A composite modifier for recycled rubber-plastic asphalt based on shear force-temperature-interface modification, characterized in that, It includes 65-75 parts tire rubber powder, 17-25 parts polyethylene, 8-12 parts aromatic oil, and 0-2 parts silane coupling agent, wherein the silane coupling agent is not 0 parts. The tire rubber powder is selected from tire rubber powder with a particle size of 40-60 mesh, Mooney viscosity ≤95, and relative density of 1-1.15; The polyethylene is selected from polyethylene with a relative density of 0.94~1.15, a particle size ≤3 mm, and a melt flow index (MFI) ≥1 g / 10 min; The aromatic oil is selected from those with a kinematic viscosity of 10~40 mm. 2 / s of aromatic oil; The silane coupling agent is 3-aminopropyltriethoxysilane; The recycled rubber-plastic asphalt composite modifier is prepared by a method including the following steps: S1. Mix tire rubber powder, polyethylene, aromatic oil, and silane coupling agent according to the mass parts to obtain mixture A; S2. Add the mixture A from step S1 into a twin-screw extruder. The twin-screw extruder rotates at 15 r / min and uses a three-zone temperature control system consisting of a feeding zone, a plasticizing zone, and a homogenizing zone. The temperatures of the feeding zone, plasticizing zone, and homogenizing zone are 200~240℃, 240~300℃, and 260~300℃, respectively, to obtain mixture B. S3. Granulate the mixture B from step S2 into granules to form a recycled rubber-plastic asphalt composite modifier.

2. The recycled rubber-plastic asphalt composite modifier according to claim 1, characterized in that, In step S3, the particle size is 1~3 mm.

3. The application of a recycled rubber-plastic asphalt composite modifier as described in any one of claims 1 or 2 in the preparation of modified asphalt.

4. The application according to claim 3, characterized in that, The method for modifying asphalt using the aforementioned recycled rubber-plastic asphalt composite modifier includes the following steps: Recycled rubber-plastic asphalt composite modifier is added to flowing base asphalt, and the mixture is stirred, sheared, and mixed at high temperature. After heat preservation and development, modified asphalt is obtained. The mass ratio of the base asphalt to the recycled rubber and plastic asphalt composite modifier is 100:(15~35).

5. The application according to claim 4, characterized in that, The high temperature is 175~185℃; The stirring speed is 300~500 r / min each time, and the stirring time is 20~30 min each time; The shearing speed is 4000~5000 r / min, and the shearing time is 50~70 min; The temperature for heat preservation and development is 175~180℃, and the heat preservation and development time is 20~40 minutes.

6. The application according to claim 4, characterized in that, The base asphalt is petroleum asphalt.

Citation Information

Patent Citations

  • Polyethylene / rubber powder blend modified asphalt and preparation method thereof

    CN103709770A

  • Asphalt modifier, preparation method and asphalt mixture containing asphalt modifier

    CN107501967A

  • SBS (styrene-butadiene-styrene) polyphosphoric acid composite high-viscosity and high-elasticity modified asphalt and preparation method thereof

    CN116925558A