Porous magnesium alloy material and preparation method and application thereof

Through seepage casting method and surface coating treatment, a pore-controllable porous magnesium alloy material was prepared, which solved the problem of uncontrollable pore structure and fast degradation rate in bone defect repair in existing magnesium alloy materials, improved the corrosion resistance and mechanical properties of the material, and promoted bone healing.

CN120519752APending Publication Date: 2025-08-22HENAN UNIV OF URBAN CONSTR
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510657849.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-21
Publication Date
2025-08-22

AI Technical Summary

Technical Problem

The existing magnesium and magnesium alloy materials have problems such as uncontrollable pore structure, fast degradation rate and insufficient mechanical properties in bone defect repair, which is difficult to meet the needs of bone repair.

Method used

The seepage casting method was used to prepare a porous magnesium alloy matrix using NaCl as a pore-forming agent, and a hydroxyapatite coating was formed on the substrate surface by microarc oxidation and electrochemical deposition, and the strontium-doped hydroxyapatite coating was further grown in situ on the coating to optimize the chemical composition and surface structure of the magnesium alloy.

Benefits of technology

The pore controllability and connectivity of porous magnesium alloy materials are achieved, corrosion resistance and mechanical properties are improved, degradation rate is delayed, cell adhesion and bone generation during bone repair, and continuous bone repair support is provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005412954490000081
    Figure BDA0005412954490000081
Patent Text Reader

Abstract

The invention belongs to the technical field of magnesium alloy materials, and discloses a porous magnesium alloy material and a preparation method and application thereof. NaCl is used as a pore forming agent, magnesium alloy is subjected to a seepage casting method, alkali solution dipping and annealing, a porous magnesium alloy matrix is obtained, then micro-arc oxidation deposition of a hydroxyapatite coating is carried out, and then electrochemical deposition of the strontium-doped hydroxyapatite coating is carried out. The chemical composition of the magnesium alloy is optimized, the mechanical property of the porous magnesium alloy material is improved, and the added elements have biocompatibility. The porous matrix is prepared by adopting a seepage casting method, and the porous matrix with controllable pores and communicating pores can be obtained by controlling the particle size of the pore forming agent. And through the design of the surface coating, the corrosion resistance, the wear resistance and the mechanical strength of the magnesium alloy implant are further improved, the degradation rate is delayed, and bone healing can be promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnesium alloy materials, and in particular to a porous magnesium alloy material and a preparation method and application thereof. Background Art

[0002] Bone defect repair is a major challenge in orthopedic clinical practice. Magnesium and magnesium alloy materials have become a research hotspot in the field of degradable bone implant materials due to their elastic modulus, degradability and biocompatibility that are close to that of human bones.

[0003] However, existing magnesium and magnesium alloy materials also have certain problems. For example, pure magnesium has poor corrosion resistance and a rapid degradation rate, which can easily lead to hydrogen encapsulation and insufficient strength during the implant repair process. The degradation rate of magnesium alloys in a physiological environment is also higher than the rate of bone tissue regeneration, causing the material to structurally collapse within 3 to 6 months of implantation, making it unable to provide sustained support for new bone and losing its therapeutic and repair functions. Moreover, traditional preparation processes for porous magnesium alloys, such as powder metallurgy and foaming, make it difficult to achieve coordinated control of porosity and pore connectivity, resulting in mechanical properties that cannot meet the requirements of load-bearing bone repair. Although 3D printing technology can precisely control the pore gradient structure as needed, the higher the precision, the higher the cost, making it difficult for the general public to use.

[0004] Therefore, there is an urgent need to develop a porous magnesium alloy material with controllable pore structure, suitable degradation rate, efficient osteogenic activity and simple preparation process, which is of great significance to the development of bone defect repair technology. Summary of the Invention

[0005] The purpose of the present invention is to provide a porous magnesium alloy material and its preparation method and application, so as to solve the problems of uncontrollable pore structure, fast degradation rate and mechanical properties of existing magnesium and magnesium alloy materials that cannot meet the requirements of bone repair.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a porous magnesium alloy material, comprising the following steps:

[0008] (1) Using NaCl as a pore-forming agent, a magnesium alloy is subjected to an infiltration casting method to obtain a magnesium alloy blank; the magnesium alloy blank is immersed in a NaOH solution to obtain a porous magnesium alloy blank; the porous magnesium alloy blank is annealed to obtain a porous magnesium alloy matrix;

[0009] (2) Micro-arc oxidation was performed in electrolyte A using a porous magnesium alloy substrate as an anode and a stainless steel plate as a cathode to obtain a material having a hydroxyapatite coating;

[0010] (3) Using the material with the hydroxyapatite coating as the cathode and the platinum sheet as the anode, electrochemical deposition is performed in electrolyte B to obtain a material with a strontium-doped hydroxyapatite coating, which is the porous magnesium alloy material;

[0011] The chemical composition of the magnesium alloy in step (1) comprises, by mass percentage, 3-7% Zn, 2-5% Ca, 0.5-2% Ti, 0.1-1% Zr, 0.01-0.5% La, 0.1-0.7% Y, and the balance being Mg.

[0012] Preferably, in the above-mentioned method for preparing a porous magnesium alloy material, the particle size of the NaCl in step (1) is 50 to 300 μm; and the immersion time is 30 to 150 min.

[0013] Preferably, in the above-mentioned method for preparing a porous magnesium alloy material, the temperature of the annealing treatment in step (1) is 180-200° C.; and the time of the annealing treatment is 1-3 hours.

[0014] Preferably, in the above-mentioned method for preparing a porous magnesium alloy material, the porosity of the porous magnesium alloy substrate in step (1) is 40-80%.

[0015] Preferably, in the above-mentioned method for preparing a porous magnesium alloy material, the composition of the electrolyte A in step (2) includes: 0.01-0.2 mol / L of sodium dihydrogen phosphate and 0.01-0.4 mol / L of calcium acetate.

[0016] Preferably, in the above-mentioned method for preparing a porous magnesium alloy material, the parameters of the micro-arc oxidation in step (2) are: a current density of 0.05 to 2 A / cm 2 ; Frequency is 500~800Hz; Duty cycle is 10~40%; Time is 10~30min.

[0017] Preferably, in the above-mentioned method for preparing a porous magnesium alloy material, the composition of the electrolyte B in step (3) includes: 0.01-0.2 mol / L of sodium dihydrogen phosphate, 0.01-0.4 mol / L of calcium acetate, and 0.1-0.2 mol / L of strontium nitrate.

[0018] Preferably, in the above-mentioned method for preparing a porous magnesium alloy material, the parameters of the electrochemical deposition in step (3) are: a current density of 0.02 to 0.5 A / cm 2 ; Temperature is 60~80℃; Time is 10~40min.

[0019] The present invention also provides a porous magnesium alloy material prepared by the method for preparing the porous magnesium alloy material.

[0020] The present invention also provides an application of a porous magnesium alloy material in preparing a bone defect implant material.

[0021] It can be seen from the above technical solutions that compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention optimizes the chemical composition of the magnesium alloy, which on the one hand improves the mechanical properties of the porous magnesium alloy material, and on the other hand improves the corrosion resistance of pure magnesium or traditional magnesium alloys and slows down the degradation rate. At the same time, the added elements are biocompatible, can promote tissue growth, and also provide certain anti-inflammatory and bactericidal properties.

[0023] (2) The present invention adopts the infiltration casting method to prepare the porous matrix. By controlling the particle size of the pore-forming agent, a porous matrix with controllable pores and interconnected pores can be obtained.

[0024] (3) The present invention also prepares a coating on the surface of the porous substrate. The hydroxyapatite coating prepared by micro-arc oxidation is generated in situ from the substrate, has strong bonding with the substrate, and is a micron-porous coating that can interact with new bone tissue, improve cell adhesion, and provide the corrosion resistance and mechanical properties required in the bone repair process. Furthermore, a strontium-doped hydroxyapatite coating is in situ grown on the hydroxyapatite coating. The hydroxyapatite coating serves as a transition layer to improve the problem of easy cracking and weak bonding with the substrate after the doping element. Strontium in the strontium-doped hydroxyapatite coating can promote osteogenesis, promote interaction between the implant and bone tissue, and continuously play a bone repair role. Through the design of the above-mentioned surface coating, the present invention further improves the corrosion resistance, wear resistance, and mechanical strength of the magnesium alloy implant, slows down the degradation rate, and can also promote bone healing. DETAILED DESCRIPTION

[0025] The present invention provides a method for preparing a porous magnesium alloy material, comprising the following steps:

[0026] (1) Using NaCl as a pore-forming agent, a magnesium alloy is subjected to an infiltration casting method to obtain a magnesium alloy blank; the magnesium alloy blank is immersed in a NaOH solution to obtain a porous magnesium alloy blank; the porous magnesium alloy blank is annealed to obtain a porous magnesium alloy matrix;

[0027] (2) Micro-arc oxidation was performed in electrolyte A using a porous magnesium alloy substrate as an anode and a stainless steel plate as a cathode to obtain a material having a hydroxyapatite coating;

[0028] (3) The material with the hydroxyapatite coating is used as the cathode and the platinum sheet is used as the anode, and electrochemical deposition is performed in electrolyte B to obtain a material with a strontium-doped hydroxyapatite coating, which is the porous magnesium alloy material.

[0029] In the present invention, the chemical composition of the magnesium alloy in step (1) comprises, by mass percentage, 3-7% Zn, 2-5% Ca, 0.5-2% Ti, 0.1-1% Zr, 0.01-0.5% La, 0.1-0.7% Y, and the balance being Mg. Preferably, the mass percentage of Zn is preferably 4-6%, more preferably 4.2-5.5%, more preferably 4.6%; the mass percentage of Ca is preferably 2.5-5%, more preferably 3-4%, more preferably 3.5%; the mass percentage of Ti is preferably 0.8-1.8%, more preferably 1-1.5%, more preferably 1.1%; the mass percentage of Zr is preferably 0.2-0.7%, more preferably 0.3-0.5%, more preferably 0.4%; the mass percentage of La is preferably 0.05-0.4%, more preferably 0.1-0.35%, more preferably 0.2%; the mass percentage of Y is preferably 0.1-0.6%, more preferably 0.2-0.55%, more preferably 0.5%.

[0030] In the present invention, the preparation method of the magnesium alloy in step (1) is: the raw materials are proportioned according to the chemical composition of the magnesium alloy, and then the raw materials are heated to 750°C and kept warm for 60 minutes to melt, and then a refining agent (CaO, CaF2 and CaCO3 in a mass ratio of 5:3:2) of 2% of the total mass of the magnesium alloy is added and refined at 800°C for 30 minutes, and then poured and cooled to obtain the magnesium alloy.

[0031] In the present invention, the heating temperature of the magnesium alloy in the infiltration casting method in step (1) is 680°C.

[0032] In the present invention, the particle size of the NaCl in step (1) is preferably 50 to 300 μm, more preferably 50 to 250 μm, and even more preferably 100 to 250 μm.

[0033] In the present invention, the immersion temperature in step (1) is preferably 25-40°C, more preferably 25-30°C, and more preferably 25°C; the immersion time is preferably 30-150 min, more preferably 60-120 min, and more preferably 90 min; and ultrasound is also included in the immersion process.

[0034] In the present invention, the concentration of the NaOH solution in step (1) is preferably 0.1 to 3 mol / L, more preferably 1 to 3 mol / L, and even more preferably 2 mol / L.

[0035] In the present invention, the temperature of the annealing treatment in step (1) is preferably 180-200°C, more preferably 180-190°C, and more preferably 180°C; the time of the annealing treatment is preferably 1-3h, more preferably 2-3h, and more preferably 2h.

[0036] In the present invention, the porosity of the porous magnesium alloy substrate in step (1) is preferably 40 to 80%, more preferably 52 to 70%, and even more preferably 68%.

[0037] In the present invention, the composition of the electrolyte A in step (2) includes: sodium dihydrogen phosphate is preferably 0.01 to 0.2 mol / L, more preferably 0.02 to 0.1 mol / L, more preferably 0.045 mol / L; calcium acetate is preferably 0.01 to 0.4 mol / L, more preferably 0.1 to 0.3 mol / L, more preferably 0.23 mol / L.

[0038] In the present invention, the parameters of the micro-arc oxidation in step (2) are: the current density is preferably 0.05 to 2 A / cm 2 , more preferably 0.2 to 1 A / cm 2 , more preferably 0.8A / cm 2 ; The frequency is preferably 500-800Hz, more preferably 600-800Hz, and more preferably 700Hz; the duty cycle is preferably 10-40%, more preferably 15-30%, and more preferably 20%; the time is preferably 10-30min, more preferably 12-20min, and more preferably 15min.

[0039] In the present invention, the composition of the electrolyte B in step (3) includes: sodium dihydrogen phosphate is preferably 0.01 to 0.2 mol / L, more preferably 0.02 to 0.1 mol / L, more preferably 0.03 mol / L; calcium acetate is preferably 0.01 to 0.4 mol / L, more preferably 0.05 to 0.3 mol / L, more preferably 0.1 mol / L; strontium nitrate is preferably 0.1 to 0.2 mol / L, more preferably 0.1 to 0.15 mol / L, more preferably 0.12 mol / L.

[0040] In the present invention, the parameters of the electrochemical deposition in step (3) are: the current density is preferably 0.02 to 0.5 A / cm 2 , more preferably 0.1 to 0.4 A / cm 2 , more preferably 0.2A / cm 2 The temperature is preferably 60 to 80°C, more preferably 60 to 70°C, and more preferably 65°C; the time is preferably 10 to 40 minutes, more preferably 12 to 30 minutes, and more preferably 13 minutes.

[0041] The present invention also provides a porous magnesium alloy material prepared by a method for preparing the porous magnesium alloy material.

[0042] The present invention also provides an application of a porous magnesium alloy material in preparing a bone defect implant material.

[0043] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts are within the scope of protection of the present invention.

[0044] Example 1

[0045] This embodiment provides a method for preparing a porous magnesium alloy material, comprising the following steps:

[0046] (1) Using NaCl with a particle size of 100 to 250 μm as a pore-forming agent, a magnesium alloy was cast by infiltration casting to obtain a magnesium alloy blank; the magnesium alloy blank was ultrasonically immersed in a 2 mol / L NaOH solution at 25°C for 90 min to remove the NaCl, thereby obtaining a porous magnesium alloy blank; the porous magnesium alloy blank was annealed at 180°C for 2 h to obtain a porous magnesium alloy matrix with a porosity of 68%;

[0047] (2) The porous magnesium alloy substrate was used as the anode and the stainless steel plate was used as the cathode. Micro-arc oxidation was performed in electrolyte A (0.045 mol / L sodium dihydrogen phosphate and 0.23 mol / L calcium acetate). The parameters were: current density 0.8 A / cm 2 , frequency is 700 Hz, duty cycle is 20%, and time is 15 min to obtain a material with hydroxyapatite coating;

[0048] (3) The material with hydroxyapatite coating was used as cathode and platinum sheet was used as anode, and electrochemical deposition was carried out in electrolyte B (sodium dihydrogen phosphate 0.03 mol / L, calcium acetate 0.1 mol / L, strontium nitrate 0.12 mol / L). The parameters were: current density 0.2 A / cm 2 , temperature is 65° C., time is 13 min, and a material with a strontium-doped hydroxyapatite coating is obtained, that is, a porous magnesium alloy material.

[0049] The chemical composition of the magnesium alloy in step (1) comprises, by mass percentage, 4.6% Zn, 3.5% Ca, 1.1% Ti, 0.4% Zr, 0.2% La, 0.5% Y, and the balance being Mg.

[0050] Example 2

[0051] This embodiment provides a method for preparing a porous magnesium alloy material, comprising the following steps:

[0052] (1) Using NaCl with a particle size of 50 to 150 μm as a pore-forming agent, a magnesium alloy was cast by infiltration casting to obtain a magnesium alloy blank; the magnesium alloy blank was ultrasonically immersed in a 1 mol / L NaOH solution at 30°C for 60 min to remove the NaCl, thereby obtaining a porous magnesium alloy blank; the porous magnesium alloy blank was annealed at 185°C for 1 h to obtain a porous magnesium alloy matrix with a porosity of 52%;

[0053] (2) The porous magnesium alloy substrate was used as the anode and the stainless steel plate was used as the cathode. Micro-arc oxidation was performed in electrolyte A (0.027 mol / L sodium dihydrogen phosphate and 0.08 mol / L calcium acetate). The parameters were: current density 0.07 A / cm 2 , frequency is 700 Hz, duty cycle is 30%, and time is 10 min to obtain a material with hydroxyapatite coating;

[0054] (3) The material with hydroxyapatite coating was used as cathode and platinum sheet was used as anode, and electrochemical deposition was carried out in electrolyte B (sodium dihydrogen phosphate 0.027 mol / L, calcium acetate 0.1 mol / L, strontium nitrate 0.1 mol / L) with the following parameters: current density 0.06 A / cm 2 , temperature is 60° C., time is 10 min, and a material with a strontium-doped hydroxyapatite coating is obtained, that is, a porous magnesium alloy material.

[0055] The chemical composition of the magnesium alloy in step (1) comprises, by mass percentage, 3% Zn, 4.5% Ca, 1.6% Ti, 0.4% Zr, 0.1% La, 0.1% Y, and the balance being Mg.

[0056] Example 3

[0057] This embodiment provides a method for preparing a porous magnesium alloy material, comprising the following steps:

[0058] (1) Using NaCl with a particle size of 100 to 300 μm as a pore-forming agent, a magnesium alloy was cast by infiltration casting to obtain a magnesium alloy blank; the magnesium alloy blank was ultrasonically immersed in a 0.5 mol / L NaOH solution at 30°C for 80 min to remove the NaCl, thereby obtaining a porous magnesium alloy blank; the porous magnesium alloy blank was annealed at 190°C for 2 h to obtain a porous magnesium alloy matrix with a porosity of 59%;

[0059] (2) The porous magnesium alloy substrate was used as the anode and the stainless steel plate was used as the cathode. Micro-arc oxidation was performed in electrolyte A (0.11 mol / L sodium dihydrogen phosphate and 0.3 mol / L calcium acetate). The parameters were: current density 0.5 A / cm 2 , frequency is 800 Hz, duty cycle is 25%, and time is 10 min to obtain a material with hydroxyapatite coating;

[0060] (3) The material with hydroxyapatite coating was used as cathode and platinum sheet was used as anode, and electrochemical deposition was carried out in electrolyte B (0.1 mol / L sodium dihydrogen phosphate, 0.35 mol / L calcium acetate, 0.14 mol / L strontium nitrate). The parameters were: current density 0.3 A / cm 2 , temperature is 80° C., time is 10 min, and a material with a strontium-doped hydroxyapatite coating is obtained, that is, a porous magnesium alloy material.

[0061] The chemical composition of the magnesium alloy in step (1) comprises, by mass percentage, 5.5% Zn, 3% Ca, 1.5% Ti, 0.6% Zr, 0.4% La, 0.2% Y, and the balance being Mg.

[0062] Example 4

[0063] This embodiment provides a method for preparing a porous magnesium alloy material, comprising the following steps:

[0064] (1) Using NaCl with a particle size of 250 to 300 μm as a pore-forming agent, a magnesium alloy was cast by infiltration casting to obtain a magnesium alloy blank; the magnesium alloy blank was ultrasonically immersed in a 2 mol / L NaOH solution at 25°C for 120 min to remove the NaCl, thereby obtaining a porous magnesium alloy blank; the porous magnesium alloy blank was annealed at 200°C for 1 h to obtain a porous magnesium alloy matrix with a porosity of 73%;

[0065] (2) The porous magnesium alloy substrate was used as the anode and the stainless steel plate was used as the cathode. Micro-arc oxidation was performed in electrolyte A (0.15 mol / L sodium dihydrogen phosphate and 0.4 mol / L calcium acetate). The parameters were: current density 1 A / cm 2 , frequency is 800 Hz, duty cycle is 30%, and time is 15 min to obtain a material with hydroxyapatite coating;

[0066] (3) The material with hydroxyapatite coating was used as cathode and platinum sheet was used as anode, and electrochemical deposition was carried out in electrolyte B (0.015 mol / L sodium dihydrogen phosphate, 0.3 mol / L calcium acetate, 0.2 mol / L strontium nitrate). The parameters were: current density 0.4 A / cm 2, temperature is 80° C., time is 20 min, and a material with a strontium-doped hydroxyapatite coating is obtained, that is, a porous magnesium alloy material.

[0067] The chemical composition of the magnesium alloy in step (1) comprises, by mass percentage, Zn 7%, Ca 2%, Ti2%, Zr 1%, La 0.2%, Y 0.6%, and the balance Mg.

[0068] Comparative Example 1

[0069] This comparative example provides a method for preparing a porous magnesium alloy material, which is specifically described in Example 1. The difference is that no hydroxyapatite coating or strontium-doped hydroxyapatite coating is prepared, that is, steps (2) and (3) are not performed, and the porous magnesium alloy substrate obtained in step (1) is the porous magnesium alloy material.

[0070] Comparative Example 2

[0071] This comparative example provides a method for preparing a porous magnesium alloy material. For details, refer to Example 1, except that the magnesium alloy is a commercially available medical magnesium alloy with the brand name AZ31.

[0072] The porous magnesium alloy materials prepared in Examples 1 to 4 and Comparative Examples 1 to 2 were immersed in simulated body fluid for 28 days. The yield strength and tensile strength before and after immersion, and the corrosion rate after immersion were tested. The results are shown in Table 1.

[0073] Table 1 Performance test results of porous magnesium alloy materials

[0074]

[0075] As can be seen from Table 1, the porous magnesium alloy material of the present invention has good mechanical properties. After immersion in simulated body fluid for 28 days, the degree of mechanical property degradation is relatively low, and the corrosion rate can be as low as 0.34 mm / year. It has good corrosion resistance and can meet the mechanical support in the bone repair process and maintain the bone repair effect.

[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing a porous magnesium alloy material, characterized in that: The following steps are involved: (1) Using NaCl as a pore-forming agent, a magnesium alloy is subjected to an infiltration casting method to obtain a magnesium alloy blank; the magnesium alloy blank is immersed in a NaOH solution to obtain a porous magnesium alloy blank; the porous magnesium alloy blank is annealed to obtain a porous magnesium alloy matrix; (2) Micro-arc oxidation was performed in electrolyte A using a porous magnesium alloy substrate as an anode and a stainless steel plate as a cathode to obtain a material having a hydroxyapatite coating; (3) Using the material with the hydroxyapatite coating as the cathode and the platinum sheet as the anode, electrochemical deposition is performed in electrolyte B to obtain a material with a strontium-doped hydroxyapatite coating, which is the porous magnesium alloy material; The chemical composition of the magnesium alloy in step (1) comprises, by mass percentage, 3-7% Zn, 2-5% Ca, 0.5-2% Ti, 0.1-1% Zr, 0.01-0.5% La, 0.1-0.7% Y, and the balance being Mg.

2. The method for preparing a porous magnesium alloy material according to claim 1, wherein: The particle size of the NaCl in step (1) is 50 to 300 μm; and the immersion time is 30 to 150 minutes.

3. The method for preparing a porous magnesium alloy material according to claim 1 or 2, characterized in that: The temperature of the annealing treatment in step (1) is 180-200° C.; the time of the annealing treatment is 1-3 hours.

4. The method for preparing a porous magnesium alloy material according to claim 1, wherein: The porosity of the porous magnesium alloy substrate in step (1) is 40 to 80%.

5. The method for preparing a porous magnesium alloy material according to claim 1 or 4, characterized in that: The composition of the electrolyte A in step (2) includes: 0.01-0.2 mol / L of sodium dihydrogen phosphate and 0.01-0.4 mol / L of calcium acetate.

6. The method for preparing a porous magnesium alloy material according to claim 5, characterized in that: The parameters of the micro-arc oxidation in step (2) are: current density of 0.05-2A / cm 2 ; Frequency is 500~800Hz; Duty cycle is 10~40%; Time is 10~30min.

7. The method for preparing a porous magnesium alloy material according to claim 6, characterized in that: The composition of the electrolyte B in step (3) includes: 0.01-0.2 mol / L of sodium dihydrogen phosphate, 0.01-0.4 mol / L of calcium acetate, and 0.1-0.2 mol / L of strontium nitrate.

8. The method for preparing a porous magnesium alloy material according to claim 1 or 7, characterized in that: The parameters of the electrochemical deposition in step (3) are: current density of 0.02 to 0.5 A / cm 2 ; Temperature is 60~80℃; Time is 10~40min.

9. A porous magnesium alloy material obtained by the method for preparing a porous magnesium alloy material according to any one of claims 1 to 8.

10. Use of the porous magnesium alloy material according to claim 9 in preparing bone defect implant materials.