Modified polybenzimidazole alloy and preparation method thereof

By mixing low-melting point polyaryletherketone into polybenzimidazole and adding a compatible agent, the problem of polybenzimidazole thermoplastic processing is solved, and the high-temperature stability and mechanical properties of the modified alloy are improved.

CN120574474AActive Publication Date: 2025-09-02江苏君华特种高分子材料股份有限公司 +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202510928526.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-07
Publication Date
2025-09-02
Estimated Expiration
2045-07-07

AI Technical Summary

Technical Problem

Polybenzimidazole is difficult to thermoplastic and when combined with polyaryletherketone, there are problems such as insufficient dimensional stability of high temperature and weak oxidation resistance medium.

Method used

Modified polybenzimidazole alloy is prepared by mixing low-melting point polyaryletherketone with a compatibility agent added, and melt blending is made by airflow mixing and a twin-screw extruder.

Benefits of technology

It improves the processing flowability and mechanical properties of the alloy, enhances thermal stability, and improves dimensional stability and oxidation resistance in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005485520040000021
    Figure BDA0005485520040000021
  • Figure BDA0005485520040000031
    Figure BDA0005485520040000031
  • Figure BDA0005485520040000051
    Figure BDA0005485520040000051
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer material modification, in particular to a modified polybenzimidazole alloy and a preparation method thereof.The modified polybenzimidazole alloy is prepared from, by weight, 15-40 parts of polybenzimidazole, 50-70 parts of low-melting-point polyaryletherketone, 0.1-8 parts of compatilizer, 0-1.5 parts of antioxidant and 0-0.8 part of lubricant; the polybenzimidazole, the low-melting-point polyaryletherketone and the compatilizer are subjected to melt blending, extrusion and granulation and then mixed with the remaining materials, and melt blending, extrusion and granulation are carried out again to prepare the composite material; according to the invention, polyaryletherketone with low melting point and good processing fluidity is mixed in polybenzimidazole, so that the problem that the polybenzimidazole is difficult to be subjected to thermoplastic processing molding is solved, and the obtained modified alloy has better mechanical property and thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer material modification, and in particular to a modified polybenzimidazole alloy and a preparation method thereof. Background Art

[0002] Polyaryletherketone (PAEK) is a high-performance specialty engineering plastic with excellent mechanical properties, thermal stability, chemical stability, and radiation resistance. It is widely used in aerospace, electronics, automotive, and other fields. Commercial PAEK (such as PEEK and PEKK) has become a core material for the manufacture of precision parts due to its excellent mechanical strength, fatigue resistance, and thermoplastic processability. However, its low glass transition temperature (typically <150°C) leads to insufficient high-temperature dimensional stability, prone to creep deformation under continuous thermal loads, and weak resistance to strong oxidizing media, limiting its further application in high-temperature environments.

[0003] Polybenzimidazole (PBI), a representative of heterocyclic aromatic polymers, possesses extremely high thermal stability (Tg≈400°C), excellent flame retardancy, and chemical inertness. However, due to its extremely rigid molecular chain, it has extremely poor solubility. Furthermore, its melting temperature is higher than its decomposition temperature, making it difficult to melt process and thermoform. PBI is typically processed using solution methods (typically soluble only in strong acid solvents such as methanesulfonic acid), which is inefficient and costly, severely limiting the choice of molding process.

[0004] How to achieve a good combination of the two and optimize performance is the technical problem to be solved by the present invention. Summary of the Invention

[0005] To address the above technical issues, a modified polybenzimidazole alloy and a method for preparing the same are provided. The present invention addresses the difficulty in thermoplastic molding of polybenzimidazole by blending polyaryletherketone (PEK) with a low melting point and good processing fluidity into the polybenzimidazole. The resulting modified alloy exhibits excellent mechanical properties and thermal stability.

[0006] In order to achieve the above objectives, the present invention is implemented through the following technical solutions:

[0007] A modified polybenzimidazole alloy comprises the following materials in parts by weight:

[0008] 15-40 parts of polybenzimidazole,

[0009] 50-70 parts of low melting point polyaryletherketone,

[0010] Compatibilizer 0.1-8 parts,

[0011] Antioxidant 0-1.5 parts,

[0012] Lubricant 0-0.8 parts;

[0013] The low-melting-point polyaryletherketone has a melting point of 303-307°C, a melt index of 10-20 g / 10 min under a 2.16 kg load test at 400°C, and a density of 1.25-1.3 g / cm 3 .

[0014] Furthermore, the density of the polybenzimidazole is 1.1-1.4 g / cm 3 , the glass transition temperature is 425-436℃.

[0015] Furthermore, the compatibilizer is selected from one of polyaryletherketone with bisimide side groups and maleic anhydride grafted PEEK;

[0016] Furthermore, the specific chemical structure of the polyaryletherketone having bisimide side groups is as follows:

[0017]

[0018] The product is obtained by polycondensation of bisphenol AF containing an imide and 4,4'-difluorobenzophenone, with a number average molecular weight of 10,000-30,000 g / mol, a weight average molecular weight of 30,000-60,000 g / mol, and a PDI in the range of 1-3. For a specific method, see the applicant's patent CN 119390967 A: bisphenol AF containing an imide having the above chemical structure and 4,4'-difluorobenzophenone are reacted with sodium carbonate and / or potassium carbonate in the presence of a reaction solvent and a water-carrying agent, followed by azeotropic dehydration at 120-140°C for 1-2 hours, and then polycondensation at 160-180°C for 4-12 hours to obtain the product (see Example 1 of the patent for a specific embodiment).

[0019] Furthermore, the antioxidant is selected from inorganic phosphates; and the lubricant is selected from calcium stearate.

[0020] The preparation method of the modified polybenzimidazole alloy comprises the following steps:

[0021] S1. Weigh polybenzimidazole and a compatibilizer according to the formula amount, use an air flow mixer for intermittent premixing, apply a pressure of 1.3-1.5 MPa during premixing, set the premixing temperature to 110-130° C., and premix for 30-90 min. Then, melt-blending and extruding are carried out in a twin-screw extruder at 400-430° C., and granulation is performed to obtain modified polybenzimidazole;

[0022] S2. Weigh the low-melting-point polyaryletherketone and the compatibilizer according to the formula, and perform intermittent premixing using an airflow mixer. During the premixing, the pressure is 1.3-1.5 MPa, the premixing temperature is 110-130° C., and the premixing time is 30-90 min. Then, the mixture is melt-blended, extruded, and granulated in a twin-screw extruder at 330-360° C. to obtain the modified polyaryletherketone.

[0023] S3. After the modified polybenzimidazole and modified polyaryletherketone are dried under a protective atmosphere (130-160°C oven, heat preservation for 60-130 min), the formulated amount of antioxidant and lubricant are added, and the mixture is mixed at a speed of 150-250 rpm for 10-30 min. Then, the mixture is melt-blended, extruded and granulated in a twin-screw extruder at 405-425°C to obtain a modified polybenzimidazole alloy.

[0024] Beneficial technical effects:

[0025] The present invention melt-dopes polyaryletherketone (PBI) with a low melting point to prepare a modified alloy, and the resulting alloy has good processing performance and excellent comprehensive performance. The use of a large amount of low-melting-point polyaryletherketone mixed in PBI can reduce the processing temperature window of PBI and improve processing fluidity, making the alloy easier to form and process. By adding a compatibilizer, the compatibility between polyaryletherketone and PBI is improved, making the performance of the alloy more stable. The modified alloy has good mechanical properties, thermal stability, molding shrinkage, toughness, etc. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, rather than all embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0027] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate circumstances, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments can have different values. It should be noted that, for example, the value described as "within the range of ab", "between the range of ab" does not include endpoint values ​​a and b; the value described as "for ab", "is ab", "ab" includes endpoint values ​​a and b.

[0028] In the following examples, the experimental methods without specific conditions are generally measured according to national standards; if there is no corresponding national standard, the general standard requirements or general methods are used.

[0029] The specific chemical structure of the polyaryletherketone with bisimide side groups used below is as follows:

[0030]

[0031] Specifically, the product of Example 1 of the applicant's patent CN 119390967 A is used.

[0032] Example 1

[0033] A modified polybenzimidazole alloy, comprising the following materials in parts by weight: 30 parts of polybenzimidazole (fully aromatic) (commercially available, Shandong Zhengentropy Energy Technology Co., Ltd.), 50 parts of low-melting-point polyaryletherketone (commercially available, Vickers), 3 parts of a compatibilizer, 0.5 parts of an antioxidant, and 0.3 parts of a lubricant;

[0034] The melting point of low-melting-point polyaryletherketone is 307°C and the density is 1.27g / cm 3 The melt index is 15 g / 10 min (400° C., 2.16 kg); the compatibilizer is polyaryletherketone having a bisimide side group; the antioxidants are sodium dihydrogen phosphate and disodium hydrogen phosphate, with a mass ratio of 1:2; and the lubricant is calcium stearate.

[0035] The preparation method of the modified polybenzimidazole alloy comprises the following steps:

[0036] Raw material pretreatment: low melting point polyaryletherketone and PBI were dried at 120 °C for 4 hours respectively;

[0037] S1. According to the formula, 30 parts by weight of polybenzimidazole and 25 wt% to 40 wt% of the compatibilizer were weighed and premixed in an air flow mixer. During the premixing, the pressure was applied to 1.4 MPa and the mixing was intermittent. The mixing temperature was 120° C. and the mixing time was 1 h. The mixture was then melt-blended and extruded in a twin-screw extruder at a screw speed of 150 rpm and a temperature of 400-430° C., and granulated. The mixture was then subjected to an air-cooled conveyor belt and a gantry pelletizer to obtain modified polybenzimidazole particles.

[0038] S2. According to the formula amount, 50 parts by weight of low-melting-point polyaryletherketone and the remaining formula amount of compatibilizer were weighed, and premixed by an airflow mixer. During premixing, the pressure was 1.4 MPa, and the mixing was intermittent. The mixing temperature was 120° C. and the time was 1 h. Then, the mixture was melt-blended, extruded, and granulated in a twin-screw extruder at a screw speed of 150 rpm and 330-360° C., and an air-cooled conveyor belt was used. After the gantry pelletizer, modified polyaryletherketone particles were obtained;

[0039] S3. The modified polybenzimidazole particles and modified polyaryletherketone particles obtained above were placed in an oven at 150°C for 2 hours under nitrogen protection. After drying, 0.5 parts by weight of an antioxidant and 0.3 parts by weight of a lubricant were added, and the mixture was mixed in a high-speed mixer at a speed of 200 rpm for 15 minutes. Then, the mixture was melt-blended, extruded and granulated in a twin-screw extruder at 405-425°C to obtain a modified polybenzimidazole alloy.

[0040] The sheet was extruded using a single-screw extruder with a main engine speed of 8 rad / min, a haul-off speed of 6 rad / min, a sizing sleeve temperature of 200°C, and a mold temperature of 410°C. After the sheet was extruded normally, the specimen was machined and the mechanical properties tested. The results are shown in Table 1.

[0041] Example 2

[0042] A modified polybenzimidazole alloy comprises the following materials in parts by weight: 20 parts of polybenzimidazole (fully aromatic) (commercially available, Shandong Zhengentropy Energy Technology Co., Ltd.), 60 parts of low-melting-point polyaryletherketone (commercially available, Vickers), 5 parts of a compatibilizer, 0.5 parts of an antioxidant, and 0.3 parts of a lubricant;

[0043] The melting point of low-melting-point polyaryletherketone is 307°C and the density is 1.27g / cm 3 The melt index is 15 g / 10 min (400° C., 2.16 kg); the compatibilizer is polyaryletherketone having a bisimide side group; the antioxidants are sodium dihydrogen phosphate and disodium hydrogen phosphate, with a mass ratio of 1:2; and the lubricant is calcium stearate.

[0044] The preparation method of the modified alloy in this case is the same as that in Example 1.

[0045] Example 3

[0046] A modified polybenzimidazole alloy, comprising the following materials in parts by weight: 40 parts of polybenzimidazole (fully aromatic) (commercially available, Shandong Zhengentropy Energy Technology Co., Ltd.), 70 parts of low-melting-point polyaryletherketone (commercially available, Vickers), 8 parts of a compatibilizer, 0.8 parts of an antioxidant, and 0.8 parts of a lubricant;

[0047] The melting point of low-melting-point polyaryletherketone is 307°C and the density is 1.27g / cm 3 The melt index is 15 g / 10 min (400° C., 2.16 kg); the compatibilizer is polyaryletherketone having a bisimide side group; the antioxidants are sodium dihydrogen phosphate and disodium hydrogen phosphate, with a mass ratio of 1:2; and the lubricant is calcium stearate.

[0048] The preparation method of the modified alloy in this case is the same as that in Example 1.

[0049] Comparative Example 1

[0050] The composition and preparation process of the alloy in this case are the same as those in Example 1, except that no compatibilizer is added.

[0051] Comparative Example 2

[0052] The composition and preparation process of the alloy in this case are the same as those in Example 1, except that the low-melting-point polyaryletherketone is replaced with conventional PEEK (model PEEK5600G, density 1.3 g / cm 3 , melting point 343°C, melt index 15g / 10min).

[0053] Test Case

[0054] The modified alloys of the above examples and comparative examples were subjected to performance tests, and the results are shown in Table 1.

[0055]

[0056] As shown in Table 1, the present invention improves the interfacial compatibility between PBI and polyaryletherketone by mixing polybenzimidazole with polyaryletherketone (PAEK) having a low melting point and good processing fluidity and combining it with a specific chemical structure compatibilizer. The resulting modified alloy has good mechanical properties and thermal stability.

[0057] The above description is only a preferred specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any technician familiar with the technical field, within the technical scope disclosed by the present invention, who makes equivalent replacements or changes based on the technical solution and inventive concept of the present invention, should be covered by the scope of protection of the present invention.

Claims

1. A modified polybenzimidazole alloy, characterized in that: The following materials are included in parts by weight: 15-40 parts of polybenzimidazole, 50-70 parts of low melting point polyaryletherketone, Compatibilizer 0.1-8 parts, Antioxidant 0-1.5 parts, Lubricant 0-0.8 parts; The low-melting-point polyaryletherketone has a melting point of 303-307°C, a melt index of 10-20 g / 10 min under a 2.16 kg load test at 400°C, and a density of 1.25-1.3 g / cm 3 .

2. The modified polybenzimidazole alloy according to claim 1, characterized in that: The density of the polybenzimidazole is 1.1-1.4 g / cm 3 , the glass transition temperature is 425-436℃.

3. The modified polybenzimidazole alloy according to claim 1, characterized in that: The compatibilizer is selected from one of polyaryletherketone with bisimide side groups and maleic anhydride grafted PEEK.

4. The modified polybenzimidazole alloy according to claim 3, characterized in that: The specific chemical structure of the polyaryletherketone having bisimide side groups is as follows: The number average molecular weight is 10,000 to 30,000 g / mol, the weight average molecular weight is 30,000 to 60,000 g / mol, and the PDI is in the range of 1-3.

5. A modified polybenzimidazole alloy according to any one of claims 1 to 4, characterized in that: The antioxidant is selected from inorganic phosphates; and the lubricant is selected from calcium stearate.

6. A method for preparing a modified polybenzimidazole alloy, characterized in that: The modified polybenzimidazole alloy according to any one of claims 1 to 5 comprises the following steps: S1. Weigh polybenzimidazole and a compatibilizer according to the formula amount, use an air flow mixer for intermittent premixing, apply a pressure of 1.3-1.5 MPa during premixing, set the premixing temperature to 110-130° C., and premix for 30-90 min. Then, melt-blending and extruding are carried out in a twin-screw extruder at 400-430° C., and granulation is performed to obtain modified polybenzimidazole; S2. Weigh the low-melting-point polyaryletherketone and the compatibilizer according to the formula, and perform intermittent premixing using an airflow mixer. During the premixing, the pressure is 1.3-1.5 MPa, the premixing temperature is 110-130° C., and the premixing time is 30-90 min. Then, the mixture is melt-blended, extruded, and granulated in a twin-screw extruder at 330-360° C. to obtain the modified polyaryletherketone. S3. After the modified polybenzimidazole and modified polyaryletherketone are dried under a protective atmosphere (130-160°C oven, heat preservation for 60-130 min), the formulated amount of antioxidant and lubricant are added, and the mixture is mixed at a speed of 150-250 rpm for 10-30 min. Then, the mixture is melt-blended, extruded and granulated in a twin-screw extruder at 405-425°C to obtain a modified polybenzimidazole alloy.

Citation Information

Patent Citations

  • High temperature polymer blends of poly(aryl ether ketone phthalazinone)

    CN105001615A

  • Isostatic pressing method for refractory polybenzimidazole

    CN109605637A

  • Preparation method of melting-point-controllable polyaryletherketone

    CN114213650A

  • High-performance polyether-ether-ketone composite material as well as preparation method and application thereof

    CN115353712A

  • Fiber sizing liquid, polyether-ether-ketone composite material and preparation method of polyether-ether-ketone composite material