A modified sulfide and its preparation method, sulfide electrolyte material, battery element, and battery.

By coating the sulfide surface with an MxByOz fast ion conductor layer, the instability of sulfides in air is solved, maintaining high ionic conductivity and making it suitable for the electrochemical performance of batteries.

CN120622505BActive Publication Date: 2026-11-10NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202510788210.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-12
Publication Date
2026-11-10
Estimated Expiration
2045-06-12

AI Technical Summary

Technical Problem

In existing technologies, sulfides are unstable in air and readily react with water vapor to form hydroxides and hydrogen sulfide, leading to reduced purity and decreased ionic conductivity, which affects battery performance.

Method used

A fast ion conductor layer, MxByOz, is coated onto the sulfide surface and a protective layer is formed by sintering to improve stability and maintain ionic conductivity. The coating thickness is ≤100nm, and the main components are oxides of Li, K, and Na or boron compounds.

Benefits of technology

It improves the stability of sulfides in air while maintaining high ionic conductivity, ensuring that the electrochemical performance of the battery is not affected, making it suitable for solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120622505B_ABST
    Figure CN120622505B_ABST
Patent Text Reader

Abstract

This invention relates to the field of electrolyte technology, specifically to a modified sulfide and its preparation method, a sulfide electrolyte, a battery element, and a battery. The modified sulfide includes a sulfide core and a coating layer covering at least a portion of the surface of the sulfide core, the coating layer comprising M... x B y O z Where M is one or more of Li, Na, and K, 1≤x≤3, 1≤y≤4, 2≤z≤7. The coating layer on the surface of this modified sulfide can form a protective layer on the material surface, improving the material's stability in air. Moreover, the coating layer is a fast ion conductor, which does not affect the rapid conduction of ions, enabling the modified sulfide to maintain excellent electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrolyte technology, specifically to a modified sulfide and its preparation method, sulfide electrolyte materials, battery elements, and batteries. Background Technology

[0002] Sulfides (such as Li₂S) are key raw materials for sulfide electrolytes and have shown great potential in cutting-edge energy fields such as solid-state batteries. However, sulfide samples are extremely unstable in air. When exposed to air, they react rapidly with water vapor to generate highly alkaline hydroxides (such as lithium hydroxide) and highly toxic hydrogen sulfide gas, resulting in reduced purity and altered chemical properties.

[0003] Studies have shown that surface coating of sulfides can improve their stability, thus mitigating this problem. As a key electrolyte raw material, sulfides' high ionic conductivity ensures rapid ion migration during battery charging and discharging, enabling high-rate charging and discharging and improving battery power performance. However, in existing technologies, coating sulfides typically significantly reduces their ionic conductivity, thus affecting battery performance. Therefore, researching and developing modified sulfides that improve stability without compromising ionic conductivity is of great significance. Summary of the Invention

[0004] Based on this, the present invention provides a modified sulfide, the coating layer on the surface of which can serve as a protective layer to improve the stability of the material in air, and the coating layer is a fast ion conductor, which does not affect its ionic conductivity.

[0005] The modified sulfide provided by this invention includes a sulfide core and a coating layer covering at least a portion of the surface of the sulfide core, wherein the coating layer includes M x B y O z , where M is one or more of Li, K, and Na, 1≤x≤3, 1≤y≤4, 2≤z≤7.

[0006] The thickness of the coating layer in the modified sulfide described above is ≤100nm.

[0007] The thickness of the coating layer in the modified sulfide described above is 1-20 nm.

[0008] From the modified sulfide described above, M in the coating layer x B y O z The proportion of the substance in terms of amount is ≥80%.

[0009] The modified sulfide described above has a lithium sulfide core.

[0010] The modified sulfide described above has a core particle size D50 of 1-40 μm, preferably 3-15 μm.

[0011] The present invention also provides a method for preparing a modified sulfide, comprising at least: using a method containing M x B y O z The process involves coating the sulfide core with raw materials, where M is one or more of Li, K, and Na, 1≤x≤3, 1≤y≤4, and 2≤z≤7. This preparation method yields modified sulfide products with high ionic conductivity and excellent stability in air.

[0012] The present invention also provides a method for preparing a modified sulfide, comprising the following steps: sintering a raw material containing a sulfide and a boron-containing compound at ≥300°C to obtain the modified sulfide; wherein the boron-containing compound includes at least one of boric acid and its derivatives or boron oxides, and the sulfide contains residual alkali impurities.

[0013] The method for preparing this modified sulfide provided by the present invention transforms alkaline impurities such as lithium salts in the sulfide into a coating layer in situ. This not only improves the stability of the material in air but also reduces the content of lithium salt impurities in lithium sulfide. At the same time, the generated fast ion conductor helps maintain the electrochemical performance of the material. The residual boric acid and its derivatives or boron oxides are also beneficial to the subsequent preparation of sulfide electrolytes.

[0014] The sintering treatment described above for the preparation of modified sulfides includes: pre-reaction at 180-230℃ for 3-5 hours under a protective atmosphere, followed by sintering at 300-500℃ for 10-12 hours.

[0015] In the above-described method for preparing modified sulfides, the mass of the boron-containing compound is 0.05-0.5% of the mass of the sulfide.

[0016] The modified sulfide is prepared by the above-described method, wherein the sulfide is obtained by carbothermic reduction and alcohol purification.

[0017] The present invention also provides a sulfide electrolyte material, which is prepared from raw materials including sulfides, wherein the sulfides include the modified sulfides described above.

[0018] The sulfide electrolyte material provided by this invention has few impurities, high purity, and excellent performance.

[0019] The present invention also provides a battery element comprising the above-described sulfide electrolyte material, wherein the battery element is stable in air.

[0020] The present invention also provides a battery comprising the above-described sulfide electrolyte material or the above-described battery element, wherein the battery has better energy density and cycle stability.

[0021] This invention improves the stability of sulfides in air by creating a coating layer on the surface of the sulfide, thereby forming a protective layer on the material surface. The coating material is M. x B y O z As a fast ion conductor, it does not affect the rapid conduction of ions, thus enabling sulfides to maintain their excellent electrochemical properties. Attached Figure Description

[0022] Figure 1 XPS test results of element B in the modified lithium sulfide samples prepared in Examples 1, 4, and 3;

[0023] Figure 2 The images show the XRD patterns of the solid electrolytes prepared in Example 1 and Comparative Example 1. Detailed Implementation

[0024] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0025] This invention provides a modified sulfide comprising a sulfide core and a coating layer covering at least a portion of the surface of the sulfide core. The coating layer includes M... x B y O z , where M is one or more of Li, K, and Na, 1≤x≤3, 1≤y≤4, 2≤z≤7.

[0026] This invention involves creating a sulfide surface containing M x B y O z The coating layer forms a protective layer on the material surface, thereby improving the stability of sulfides in air. Moreover, the coating layer material is a fast ion conductor, which does not affect the rapid conduction of ions and enables it to maintain excellent electrochemical performance.

[0027] It is understood that the coating layer described above, which covers at least a portion of the surface of the sulfide core, means that the coating layer can be formed on at least a portion of the surface of the sulfide particles. Preferably, the coating portion is formed on more areas of the surface of the sulfide particles, and more preferably, the coating layer is formed on the entire surface of the sulfide particles, that is, the morphology of the modified sulfide presents a uniform core-shell structure.

[0028] An appropriate coating thickness can maintain excellent electrochemical performance while ensuring the modified sulfide's ionic conductivity and improving its stability. Therefore, the coating thickness is ≤300 nm. For example, the coating thickness can be 1 nm, 10 nm, 20 nm, 30 nm, 50 nm, 80 nm, 100 nm, 120 nm, 150 nm, 180 nm, 200 nm, 250 nm, 300 nm, or any value within the range of any two of the above. Preferably, the coating thickness is 1-100 nm, which achieves a good balance of ionic conductivity, stability, and electrochemical performance.

[0029] Understandably, the coating layer may only contain M. x B y O z It may also contain other coating materials suitable for sulfide coating, such as hydrophobic materials (e.g., polymethyl(trifluoropropyl)siloxane), lithium fluoride, conductive polymers (e.g., polypyrrole, polyaniline, or polythiophene), etc.

[0030] In some specific embodiments, the coating thickness is 1-20 nm. Under this condition, stability is taken into account without increasing grain boundaries, and the ionic conductivity is better. Moreover, the coating of this thickness can be formed by in-situ transformation of impurities contained in the sulfide itself.

[0031] The thickness of the coating layer can be determined by transmission electron microscopy (TEM).

[0032] In some specific embodiments, M in the coating layer x B y O z The amount of substance is ≥80%. M in the coating layer x B y O z The percentage of the substance is calculated by fitting the XPS test results of boron to M. x B y O z The ratio of the areas of the graphs is obtained by conversion based on quanta. (M) x B y O zIf the number of atoms of element B is y, then the percentage of the amount of substance is 1 / y of the area ratio, and then normalization can be performed.

[0033] The sulfide core mentioned above is not specifically limited; it can be lithium sulfide, sodium sulfide, potassium sulfide, etc. Lithium sulfide is the most common, and this sulfide can be used in the preparation of lithium-ion batteries.

[0034] In this invention, the particle size of the sulfide is not specifically limited. In practical applications, particles with a particle size D50 of 1-40 μm are usually selected as raw materials for electrolyte preparation. Therefore, based on this requirement, the particle size D50 of the sulfide in this invention is usually 1-40 μm, preferably 3-15 μm.

[0035] Taking lithium sulfide as an example, the purity of the modified sulfide is maintained at ≥99% after being exposed to dry air with a dew point of -40℃ for 30 minutes.

[0036] This invention provides a method for preparing modified sulfides, comprising at least: using a mixture containing M x B y O z The process involves coating the sulfide core with raw materials, where M is one or more of Li, K, and Na, 1≤x≤3, 1≤y≤4, and 2≤z≤7. In other words, M is formed by directly coating the sulfide surface to create a core containing M. x B y O z The coating layer.

[0037] When directly coating as described above, M x B y O z The dosage is generally controlled at 0.1-3%, and there are no specific restrictions on the coating method; it can be wet coating or dry coating.

[0038] The present invention also provides another method for preparing modified sulfides, comprising at least the following steps: sintering a raw material containing sulfides and boron-containing compounds at ≥300°C to obtain modified sulfides, wherein the boron-containing compounds include at least one of boric acid and its derivatives or boron oxides, and the sulfides contain residual alkali impurities.

[0039] This method involves adding boric acid and its derivatives or boron oxides, causing them to react with residual alkali on the sulfide surface to form a compound containing M. x B y O zThe coating layer (such as LiBO2, Li3BO3) effectively prevents lithium sulfide from undergoing side reactions with water in air, increasing the material's stability in air and helping to maintain its original properties. Furthermore, in-situ conversion of impurities helps reduce the content of undesirable impurities in the sulfide. Additionally, the residual boric acid and its derivatives or boron oxides in the modified sulfide have melting points lower than the phase-forming temperature of the sulfide electrolyte. During further sintering to prepare the sulfide electrolyte, they melt into a liquid state, promoting mass transfer between components and facilitating electrolyte crystal growth. This allows for the production of electrolytes with superior ionic conductivity at lower sintering temperatures.

[0040] Furthermore, to ensure a more complete reaction, the sintering process involves: pre-reacting at 180-230℃ for 3-5 hours under a protective atmosphere, followed by sintering at 300-500℃ for 10-12 hours. The pre-reaction process allows boric acid to initially become molten and come into contact with the reactants, after which the temperature is increased to allow for a complete reaction.

[0041] Specifically, the pre-reaction temperature can be 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, or any two of the above values, and the pre-reaction time can be 3h, 4h, 5h, or any two of the above values. The sintering temperature can be 300℃, 350℃, 400℃, 450℃, 500℃, or any two of the above values, and the sintering time can be 10h, 11h, 12h, or any two of the above values.

[0042] There are no specific restrictions on the heating rate during sintering; a conventional heating procedure can be followed. For example, a heating rate of 1-3℃ / min can be used. After sintering, the particles are ground to the target particle size and ready for use.

[0043] In the above, the mass of the boron-containing compound is 0.05-0.5% of the sulfide mass, for example, it can be 0.05%, 0.1%, 0.15%, 0.2%, 0.3%, 0.4%, 0.5%, or any range between two of the above values. Under this condition, the coating effect is better and there is no waste of raw materials.

[0044] In the above method, sulfides are mixed with boron-containing compounds to form a preliminary coating, and the form of the preliminary coating is not specifically limited. For example, a dry process or a wet process can be used for the preliminary coating.

[0045] For example, when using a dry process, sulfides and boric acid and its derivatives or boron oxides can be mixed by ball milling, mortar and pestle / grinding machine or juicer. There are no restrictions on the specific parameters, as long as the mixture is uniform.

[0046] When using a wet process, lithium sulfide can first be dissolved or dispersed in an organic solvent and stirred uniformly for 1-2 hours. Then, boric acid and its derivatives or boron oxides are added to the mixture and stirred for another 1-2 hours. After mixing, the solvent in the system is removed by raising the temperature or by filtration, thus obtaining a mixture suitable for sintering. The organic solvent can be aprotic organic solvent or an alcohol solvent, such as anhydrous ethanol, anhydrous methanol, anhydrous n-propanol, or anhydrous isopropanol.

[0047] The modified sulfide of this invention can be obtained by sintering after initial coating. The use of boric acid and its derivatives or boron oxides in this invention is not specifically limited. For example, boric acid or boron trioxide can be used.

[0048] The method of obtaining the aforementioned sulfides is not limited. Preferably, sulfides (such as lithium sulfide) are prepared by carbothermal reduction. This is because the carbothermal reduction method for preparing lithium sulfide is convenient and inexpensive, and is currently the main method for industrial-scale preparation of lithium sulfide. Furthermore, when using this method to prepare sulfides, excess carbon is usually used to ensure complete reaction. The excess carbon needs to be further removed by alcohol purification. During alcohol purification, residual alkalis (Li₂CO₃, LiOH, Li₂O) that are difficult to completely remove are generated, affecting the material's performance. The method of this application can simultaneously remove this impurity phase.

[0049] Understandably, when removing excess carbon from sulfides prepared by carbothermal reduction using alcohol purification, the sulfides can be washed in an alcohol solvent. Furthermore, the alcohol purification step and wet coating process can be performed simultaneously: the sulfides are dispersed in an organic solvent, then boric acid and its derivatives or boron oxides are added, and the solvent is removed by filtration, thus simultaneously achieving the effects of excess carbon removal and coating. There are no specific limitations on the organic solvent; commonly used organic solvents in the art can be used, such as anhydrous ethanol, anhydrous methanol, anhydrous n-propanol, and anhydrous isopropanol.

[0050] The method for preparing sulfides via carbothermic reduction is not specifically limited. For example, lithium sulfide can be prepared using the following method:

[0051] The lithium source and carbon source are mixed in a certain proportion. The lithium salt is one or a combination of lithium sulfate and anhydrous lithium sulfate. The carbon source can be a soluble carbon source or an insoluble carbon source. The soluble carbon source can be one or more of glucose, fructose, sucrose, maltose, lactose, starch, etc., while the insoluble carbon source can be one or more of multi-walled / single-walled carbon nanotubes, graphene, activated carbon, biochar, carbon black, Super-P, VGCF, etc.

[0052] Obtaining the precursor raw material: When using an insoluble carbon source, first grind it in a mortar for 0.5-1 hour, then crush it in a crusher, juicer, or mixer at 1000-2000 rpm for 15-60 seconds to achieve thorough mixing. To achieve thorough mixing, a soluble carbon source, such as glucose, is preferred. The molar ratio of lithium salt to carbon source is 2-4, preferably 3-4. Dissolve it in deionized water and stir magnetically or mechanically for 6-24 hours. Then, spray dry it or evaporate the solvent to obtain the precursor. Finally, grind it in a mortar, crusher, juicer, or mixer to obtain fine precursor raw material.

[0053] The precursor material treated as described above is placed in an inert atmosphere reactor for a preliminary reaction of lithium and carbon sources. A muffle furnace or tube furnace can be used as the reaction vessel. For example, the heating temperature can be controlled at 600-900℃, preferably 750-860℃, for 3-10 hours, with a temperature gradient of 150-250℃ for 1-3 hours, 300-500℃ for 1-3 hours, and a final temperature hold for 3-8 hours. Lithium sulfide is obtained under these conditions, with a heating rate of 0.5℃ / min-2℃ / min. Alternatively, lithium sulfide can be obtained directly by sintering at 700-800℃ for 6-10 hours. After sintering, the resulting product is thoroughly ground and pulverized for use in sintering coating treatment.

[0054] The present invention also provides a sulfide electrolyte material, comprising the modified sulfide described above or the modified sulfide prepared by the above preparation method. This sulfide electrolyte has few impurities, high purity, and excellent performance.

[0055] Furthermore, the sulfide electrolyte is an all-solid-state electrolyte. For example, the sulfide electrolyte can be obtained by ball milling LiCl, P2S5, and the aforementioned lithium sulfide, followed by calcination at 400-600°C.

[0056] The present invention also provides a battery element comprising the aforementioned sulfide electrolyte material. It is understood that the battery element can be a positive electrode, a negative electrode, or a battery cell. The sulfide electrolyte can be contained in the positive active layer of the positive electrode, in the negative active layer of the negative electrode, or simply located between the positive and negative electrodes.

[0057] The present invention also provides a battery comprising the aforementioned sulfide electrolyte material or battery element. This battery can be a liquid battery, a solid-state battery, or a semi-solid-state battery, but is typically a solid-state battery.

[0058] The modified sulfide of the present invention will be described in detail below with reference to specific embodiments.

[0059] Example 1

[0060] Step 1: Weigh a certain amount of anhydrous lithium sulfate and glucose according to the molar ratio of lithium source to carbon source of 1:3, dissolve them in deionized water and stir for 12 hours, and then spray dry to obtain powder precursor.

[0061] Step 2: Place the powder precursor in a tube furnace under an argon atmosphere and hold at 750°C for 8 hours to obtain lithium sulfide sinter. Grind the lithium sulfide sinter thoroughly with a mortar and pestle for later use.

[0062] Step 3: The ground sintered material is added to anhydrous isopropanol at a solid-liquid mass ratio of 1:30 and stirred for 2 hours. Boric acid is added at 0.05% of the lithium sulfide sample mass, and the mixture is stirred for 2 hours. After mixing, the material is filtered and dried to remove excess carbon and complete the coating process, resulting in a uniformly mixed material. The mixture is then pre-reacted at 200°C for 3 hours under an argon atmosphere, followed by sintering at 300°C for 10 hours at a heating rate of 3°C / min. After the reaction, the material is ground and pulverized to obtain modified lithium sulfide.

[0063] Example 2

[0064] The difference between this embodiment and Embodiment 1 is that the carbon source is coconut shell carbon, which is mixed by ball milling, the coating material is boron trioxide, and the subsequent sintering temperature is 350℃, as detailed below:

[0065] Step 1: Weigh a certain amount of anhydrous lithium sulfate and coconut shell carbon according to the molar ratio of lithium source to carbon source of 1:3, grind them in a mortar for 1 hour, and then crush them in a crusher at 1500 rpm for 30 seconds to make them fully mixed and uniform, so as to obtain the powder precursor.

[0066] Step 2: Place the powder precursor in a tube furnace under an argon atmosphere and hold at 750°C for 8 hours to obtain lithium sulfide sinter. Grind the lithium sulfide sinter thoroughly with a mortar and pestle for later use.

[0067] Step 3: The ground sintered material is dissolved and stirred in anhydrous isopropanol at a solid-liquid mass ratio of 1:30 for 2 hours. Boron trioxide is added at 0.5% of the lithium sulfide sample mass, and the mixture is stirred for 2 hours. After mixing, the material is filtered and dried to remove excess carbon and complete the coating process, resulting in a uniformly mixed material. The mixture is then pre-reacted at 200°C for 3 hours under an argon atmosphere, followed by sintering at 350°C for 10 hours at a heating rate of 3°C / min. After the reaction, the material is ground and pulverized to obtain modified lithium sulfide.

[0068] Example 3

[0069] The difference between this embodiment and Embodiment 1 is that the carbon source is corn stalks, and ball milling is used for mixing.

[0070] Step 1: Weigh a certain amount of anhydrous lithium sulfate and corn stalks according to the molar ratio of lithium source to carbon source of 1:3, grind them in a mortar for 1 hour, and then crush them in a crusher at 1500 rpm for 30 seconds to make them fully mixed and uniform, so as to obtain the powder precursor.

[0071] Step 2: Place the powder precursor in a tube furnace under an argon atmosphere and hold at 750°C for 8 hours to obtain lithium sulfide sinter. Grind the lithium sulfide sinter thoroughly with a mortar and pestle for later use.

[0072] Step 3: The ground sintered material is dissolved and stirred in anhydrous isopropanol at a solid-liquid mass ratio of 1:30 for 2 hours. Boric acid is then added at 0.3% of the lithium sulfide sample mass, and the mixture is stirred for another 2 hours. After mixing, the material is filtered and dried to remove excess carbon and complete the coating process, resulting in a uniformly mixed material. The mixture is then pre-reacted at 200°C for 3 hours under an argon atmosphere, followed by sintering at 300°C for 10 hours at a heating rate of 3°C / min. After the reaction, the material is ground and pulverized to obtain modified lithium sulfide.

[0073] Example 4

[0074] The difference between this embodiment and Embodiment 1 is that boric acid is not added in step 3, and after filtering and drying to remove excess carbon, lithium tetraborate is directly used for dry coating.

[0075] Step 1: Weigh a certain amount of anhydrous lithium sulfate and glucose according to the molar ratio of lithium source to carbon source of 1:3, dissolve them in deionized water and stir for 12 hours, and then spray dry to obtain powder precursor.

[0076] Step 2: Place the powder precursor in a tube furnace under an argon atmosphere and hold at 750°C for 8 hours to obtain lithium sulfide sinter. Grind the lithium sulfide sinter thoroughly with a mortar and pestle for later use.

[0077] Step 3: Add the ground sintered material to anhydrous isopropanol at a solid-liquid mass ratio of 1:30 and stir for 2 hours. After the process, filter and dry to remove excess carbon to obtain the corresponding material; mix it with 0.15% lithium tetraborate in a high-speed blender for 5 minutes to obtain modified lithium sulfide.

[0078] Example 5

[0079] The difference between this embodiment and Embodiment 1 is that boric acid is not added in step 3, and after filtering and drying to remove excess carbon, lithium metaborate is directly used for wet coating.

[0080] Step 1: Weigh a certain amount of anhydrous lithium sulfate and glucose according to the molar ratio of lithium source to carbon source of 1:3, dissolve them in deionized water and stir for 12 hours, and then spray dry to obtain powder precursor.

[0081] Step 2: Place the powder precursor in a tube furnace under an argon atmosphere and hold at 750°C for 8 hours to obtain lithium sulfide sinter. Grind the lithium sulfide sinter thoroughly with a mortar and pestle for later use.

[0082] Step 3: The ground sintered material is added to anhydrous isopropanol at a solid-liquid mass ratio of 1:30 and stirred for 2 hours. After the stirring is complete, the material is filtered and dried to remove excess carbon, and the corresponding material is obtained. This material is then ball-milled with 0.3% lithium metaborate in anhydrous toluene solution for 1 hour, and the solvent is evaporated to remove the solvent, thus obtaining modified lithium sulfide.

[0083] Example 6

[0084] The difference between this embodiment and Embodiment 1 is that boric acid is not added in step 3, and after filtering and drying to remove excess carbon, lithium tetraborate is directly used for dry coating.

[0085] Step 1: Weigh a certain amount of anhydrous lithium sulfate and glucose according to the molar ratio of lithium source to carbon source of 1:3, dissolve them in deionized water and stir for 12 hours, and then spray dry to obtain powder precursor.

[0086] Step 2: Place the powder precursor in a tube furnace under an argon atmosphere and hold at 750°C for 8 hours to obtain lithium sulfide sinter. Grind the lithium sulfide sinter thoroughly with a mortar and pestle for later use.

[0087] Step 3: Add the ground sintered material to anhydrous isopropanol at a solid-liquid mass ratio of 1:30 and stir for 2 hours. After the process, filter and dry to remove excess carbon to obtain the corresponding material; mix it with 0.1% lithium tetraborate in a high-speed blender for 5 minutes to obtain modified lithium sulfide.

[0088] Example 7

[0089] The difference between this embodiment and Embodiment 1 is that boric acid is not added in step 3, and after filtering and drying to remove excess carbon, lithium tetraborate is directly used for dry coating.

[0090] Step 1: Weigh a certain amount of anhydrous lithium sulfate and glucose according to the molar ratio of lithium source to carbon source of 1:3, dissolve them in deionized water and stir for 12 hours, and then spray dry to obtain powder precursor.

[0091] Step 2: Place the powder precursor in a tube furnace under an argon atmosphere and hold at 750°C for 8 hours to obtain lithium sulfide sinter. Grind the lithium sulfide sinter thoroughly with a mortar and pestle for later use.

[0092] Step 3: Add the ground sintered material to anhydrous isopropanol at a solid-liquid mass ratio of 1:30 and stir for 2 hours. After the process, filter and dry to remove excess carbon to obtain the corresponding material; mix it with 0.1% lithium metaborate using a high-speed blender for 5 minutes to obtain modified lithium sulfide.

[0093] Comparative Example 1

[0094] The difference between this comparative example and Example 1 is that the sintering coating process is missing, as detailed below:

[0095] Step 1: Weigh a certain amount of anhydrous lithium sulfate and glucose according to the molar ratio of lithium source to carbon source of 1:3, dissolve them in deionized water and stir for 12 hours, and then spray dry to obtain powder precursor.

[0096] Step 2: Place the powder precursor in a tube furnace under an argon atmosphere and hold at 750°C for 8 hours to obtain lithium sulfide sinter. Grind the lithium sulfide sinter thoroughly with a mortar and pestle for later use.

[0097] Step 3: The ground sintered material is added to anhydrous isopropanol at a solid-liquid mass ratio of 1:30 and stirred for 2 hours. After that, it is filtered and dried to remove excess carbon, and purified lithium sulfide is obtained. The above lithium sulfide is pre-reacted at 200°C for 3 hours under an argon atmosphere, and then sintered at 300°C for 10 hours with a heating rate of 3°C / min. After the reaction is completed, the material is ground and pulverized to obtain lithium sulfide sample.

[0098] Comparative Example 2

[0099] The difference between this comparative example and Example 2 is that the sintering coating process is missing, as detailed below:

[0100] Step 1: Weigh a certain amount of anhydrous lithium sulfate and coconut shell carbon according to the molar ratio of lithium source to carbon source of 1:3, grind them in a mortar for 1 hour, and then crush them in a crusher at 1500 rpm for 30 seconds to make them fully mixed and uniform, so as to obtain the powder precursor.

[0101] Step 2: Place the powder precursor in a tube furnace under an argon atmosphere and hold at 750°C for 8 hours to obtain lithium sulfide sinter. Grind the lithium sulfide sinter thoroughly with a mortar and pestle for later use.

[0102] Step 3: The ground sintered material is added to anhydrous isopropanol at a solid-liquid mass ratio of 1:30 and stirred for 2 hours. After that, it is filtered and dried to remove excess carbon, and purified lithium sulfide is obtained. The above lithium sulfide is pre-reacted at 200°C for 3 hours under an argon atmosphere, and then sintered at 300°C for 10 hours with a heating rate of 3°C / min. After the reaction is completed, the material is ground and pulverized to obtain lithium sulfide sample.

[0103] Comparative Example 3

[0104] The difference between this comparative example and Example 3 is that the sintering coating process is missing, as detailed below:

[0105] Step 1: Weigh a certain amount of anhydrous lithium sulfate and corn stalk carbon according to the molar ratio of lithium source to carbon source of 1:3, grind them in a mortar for 1 hour, and then crush them in a crusher at 1500 rpm for 30 seconds to make them fully mixed and uniform, so as to obtain the powder precursor.

[0106] Step 2: Place the powder precursor in a tube furnace under an argon atmosphere and hold at 750°C for 8 hours to obtain lithium sulfide sinter. Grind the lithium sulfide sinter thoroughly with a mortar and pestle for later use.

[0107] Step 3: The ground sintered material is added to anhydrous isopropanol at a solid-liquid mass ratio of 1:30 and stirred for 2 hours. After that, it is filtered and dried to remove excess carbon, and purified lithium sulfide is obtained. The above lithium sulfide is pre-reacted at 200°C for 3 hours under an argon atmosphere, and then sintered at 300°C for 10 hours with a heating rate of 3°C / min. After the reaction is completed, the material is ground and pulverized to obtain lithium sulfide sample.

[0108] Performance testing:

[0109] (1) Confirmation of the coating layer

[0110] XPS (X-ray photoelectron spectroscopy) was performed on the lithium sulfides prepared in the above examples and comparative examples. The XPS results of the lithium elemental analysis show that the surface portion of the lithium in the sulfide samples prepared in the examples is in the form of Li. x B y O z The presence of this form indicates that the lithium sulfide surface contains Li... x B y O z The coating layer. The test results are shown in Table 1 below.

[0111] Table 1

[0112]

[0113] (2) Coating thickness, Li in the coating layer x B y O z The percentage of the substance in terms of the amount of matter and the detection of lithium sulfide particle size.

[0114] The thickness of the coating layer was measured using transmission electron microscopy (TEM), and the results are shown in Table 2 below.

[0115] Li in the coating layer x B y Oz The percentage of the amount of substance refers to the M calculated by fitting the XPS (X-ray photoelectron spectroscopy) results of boron. x B y O z The proportion of the substance of [a substance] to the total boron content is specifically 1 / y of the area ratio in the spectrum (where y=1). See the results below. Figure 1 and Table 2 below.

[0116] in, Figure 1 The XPS detection results of lithium boron sulfide in Examples 1, 4, and 3 are provided by... Figure 1 It can be seen that in Examples 1 and 3, boron is used in the form of H. a B b O c B b O c (0≤a≤3, 1≤b≤4, c=(a+3b) / 2, specifically H3BO3) and Li x B y O z (Specifically, it exists in the form of LiBO2 and / or Li3BO3) and Li x B y O z The presence of this as the primary form indicates that the added boron compound reacts with the residual alkali on the surface to generate compounds including Li. x B y O z The coating layer, in which Li x B y O z The proportion of each substance is over 80%.

[0117] The particle size of lithium sulfide in the above embodiments and comparative examples was measured using a laser particle size analyzer, and the results are shown in Table 2 below.

[0118] Table 2

[0119]

[0120] (3) The lithium sulfide in Example 1 and Comparative Example 1 were used to prepare solid electrolytes according to the following methods. Then, the prepared solid electrolyte powders were analyzed by XRD. The results are as follows: Figure 2 As shown. The preparation method of solid electrolyte powder is as follows: LiCl, P2S5 and lithium sulfide are mixed in a molar ratio of 3:1:4. They are mixed evenly with a mortar and pestle for 0.5 hours, then transferred to a ball mill jar for high-energy ball milling for 4 hours with a ball-to-powder ratio of 10:1. Finally, the mixed electrolyte powder is calcined at 500℃, crushed and granulated to obtain solid electrolyte powder.

[0121] Depend on Figure 2It can be seen that the solid electrolyte prepared from the sulfide sample in Example 1 has a purer phase. The reason for this is that the sulfide sample in the example allows for a more complete reaction of the sulfide electrolyte, resulting in a purer phase. In contrast, the sulfide sample in Comparative Example 1 may have had an incomplete reaction under the same conditions, resulting in the presence of certain impurities.

[0122] (4) The initial purity of the modified lithium sulfide and the lithium sulfide sample in the above examples and the purity after exposure to air at a dew point of -40°C for 30 minutes were detected. The purity retention rate (%) was calculated. The sample was divided into two parts. One part was used directly to prepare solid electrolyte, and the other part was exposed to the above conditions for 30 minutes before being used to prepare solid electrolyte. The ionic conductivity of the solid electrolyte prepared using unexposed and exposed lithium sulfide was detected respectively. The preparation method of solid electrolyte refers to the method in performance test (3). The detection method is as follows, and the detection results are shown in Table 3 below.

[0123] The purity measurement method refers to the patent with publication number CN117782766A. The mass percentage of S element is obtained by measurement, and then the mass percentage of lithium sulfide is calculated, which is the purity of lithium sulfide (Li2S+Li2S2).

[0124] Purity retention rate (%) = Purity after 30 minutes of exposure / Initial purity;

[0125] Ionic conductivity of sulfide electrolyte: In a glove box, 220 mg of electrolyte was placed in a mold battery with a diameter of 10 mm. The battery was pressed for 10 minutes under a pressure of 4 tons. The thickness of the electrolyte sheet was measured with a micrometer screw gauge. The impedance was measured at 25°C using an electrochemical workstation. The ionic conductivity was calculated based on the thickness / (impedance * area).

[0126] Table 3

[0127]

[0128] The results above show that the modified sulfides (i.e., coated lithium sulfides) prepared in Examples 1-7, due to the presence of the coating layer, do not show significant changes in purity retention or ionic conductivity of the prepared solid electrolyte even after exposure to air. In contrast, the sulfides (i.e., uncoated lithium sulfides) prepared in Comparative Examples 1-3 show a significant decrease in purity after exposure to air, and the ionic conductivity of the prepared solid electrolyte also decreases significantly. This indicates that the coating layer of the present invention has a protective effect, reduces the occurrence of side reactions, and is beneficial to improving the stability of the material in air, while having little impact on the ionic conductivity of the electrolyte.

[0129] Further comparison of the ionic conductivity of the solid electrolytes prepared in Examples 1-7 without exposed lithium sulfide shows that the ionic conductivity of the solid electrolytes prepared in Examples 1, 2, 3, 6, and 7 is better than that in Examples 4 and 5. This indicates that when the coating thickness is 1-20 nm, stability and ionic conductivity can be better balanced.

[0130] Further comparison of the purity of the modified sulfides (i.e., coated lithium sulfide) in Examples 1-3 and the unmodified lithium sulfide (i.e., uncoated lithium sulfide) in Comparative Examples 1-3 shows that the in-situ coating method in Examples 1-3 does not significantly reduce the lithium sulfide content (i.e., purity), indicating that the in-situ coating method in Examples 1-3 does not impair the performance of lithium sulfide itself. Comparison of the ionic conductivity of electrolytes prepared from unexposed lithium sulfide samples shows that the ionic conductivity of the electrolytes prepared with coated lithium sulfide in the examples is not significantly different from that of the electrolytes prepared without coated lithium sulfide in the comparative examples, indicating that the introduction of the coating layer has little impact on the ionic conductivity performance of the solid electrolyte.

[0131] (5) The lithium sulfide in Examples 1, 4 and Comparative Example 1 were prepared as solid electrolyte powders at different calcination temperatures. The ionic conductivity (mS / cm) of the prepared solid electrolyte powders was then compared. The results are shown in Table 4 below.

[0132] The preparation method of solid electrolyte powder is as follows: LiCl, P2S5 and lithium sulfide are mixed in a molar ratio of 3:1:4. The mixture is uniformly mixed for 0.5 hours using a mortar and pestle. Then, it is transferred to a ball mill jar for high-energy ball milling for 4 hours with a ball-to-material ratio of 10:1. Finally, the mixed electrolyte powder is calcined at different preset temperatures and crushed and granulated to obtain solid electrolyte powder.

[0133] Table 4. Results of ionic conductivity of solid electrolyte powders prepared at different calcination temperatures (unit: mS / cm)

[0134]

[0135] The results above show that the solid electrolyte powders prepared by sintering lithium sulfide-coated samples in Examples 1 and 4 at 490℃ exhibit the best ionic conductivity. This indicates that the optimal sintering temperature for the lithium sulfide-coated electrolytes in Examples 1 and 4 is 490℃. In contrast, the electrolyte prepared without lithium sulfide coating in Comparative Example 1 only achieves optimal performance when sintered at 500℃. Therefore, lithium sulfide coating in Examples 1 and 4 helps to lower the sintering temperature of the solid electrolyte. The reason for this is that boron has a fluxing effect on the surface at high temperatures, which allows for better melting and reaction of the raw materials, thus helping to reduce the sintering temperature and save energy during the preparation of the solid electrolyte.

[0136] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A modified sulfide, characterized in that, It includes a sulfide core and a coating layer covering at least a portion of the surface of the sulfide core, wherein the sulfide core is lithium sulfide, and the coating layer includes M. x B y O z , where M is Li, 1≤x≤3, 1≤y≤4, 2≤z≤7.

2. The modified sulfide according to claim 1, characterized in that, The thickness of the coating layer is ≤100nm.

3. The modified sulfide according to claim 1 or 2, characterized in that, The thickness of the coating layer is 1-20 nm; and / or M in the coating layer x B y O z The proportion of the substance in terms of amount is ≥80%.

4. The modified sulfide according to claim 1, characterized in that, The particle size D50 of the modified sulfide is 1-40 μm.

5. The modified sulfide according to claim 2, characterized in that, The particle size D50 of the modified sulfide is 1-40 μm.

6. The modified sulfide according to claim 3, characterized in that, The particle size D50 of the modified sulfide is 1-40 μm.

7. The modified sulfide according to any one of claims 4-6, characterized in that, The particle size D50 of the modified sulfide is 3-15 μm.

8. A method for preparing the modified sulfide according to any one of claims 1-7, characterized in that, At least includes: using M x B y O z The step of coating the sulfide core with the raw material, wherein the sulfide core is lithium sulfide, M is Li, 1≤x≤3, 1≤y≤4, 2≤z≤7.

9. A method for preparing the modified sulfide according to any one of claims 1-7, characterized in that, Includes the following steps: The modified sulfide is obtained by sintering raw materials containing sulfides and boron compounds at ≥300°C; the boron compounds include at least one of boric acid and its derivatives or boron oxides, and the sulfide contains residual alkali impurities.

10. The method for preparing the modified sulfide according to claim 9, characterized in that, The sintering process includes: pre-reaction at 180-230℃ for 3-5 hours under a protective atmosphere, followed by sintering at 300-500℃ for 10-12 hours; and / or The mass of the boron-containing compound is 0.05-0.5% of the mass of the sulfide.

11. The method for preparing the modified sulfide according to claim 9 or 10, characterized in that, The sulfide was obtained by carbothermal reduction and alcohol purification.

12. A sulfide electrolyte material, said sulfide electrolyte material being prepared from raw materials comprising sulfides, said sulfides including the modified sulfides according to any one of claims 1-7 or the modified sulfides prepared by the preparation method according to any one of claims 8-11.

13. A battery element, characterized in that, Including the sulfide electrolyte material as described in claim 12.

14. A battery, characterized in that, Includes the sulfide electrolyte material of claim 12 or the battery element of claim 13.

Citation Information

Patent Citations

  • Digestion method of sulfide solid electrolyte and method for determining element content of sulfide solid electrolyte

    CN117782766A

  • Method for preparing sulfide solid electrolyte with low cost and high efficiency

    CN114361579A

  • Positive pole piece and preparation method thereof, battery and electric equipment

    CN119965266A