A method for reducing large-end cracking of cold-forged differential half-shaft gears

By optimizing the mold structure and process flow, and combining normalizing, spheroidizing annealing, shot blasting and lubrication treatments, the problem of large-end cracking in cold-forged differential half-shaft gears was solved, achieving efficient cold forging and automated production.

CN120644935BActive Publication Date: 2026-11-10TAICANG JIUXIN PRECISION MOLD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510932951.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-08
Publication Date
2026-11-10
Estimated Expiration
2045-07-08

AI Technical Summary

Technical Problem

The large end of the cold-forged differential half-shaft gear is prone to cracking during the forging process, which is difficult to solve effectively with existing technology. In addition, traditional processes have problems such as large equipment investment, material oxidation and decarburization.

Method used

Optimize the mold structure design and combine processes such as normalizing, spheroidizing annealing, shot blasting, phosphating and molybdenum disulfide powder coating to improve the fluidity and lubricity of metal materials, reduce material flow resistance, ensure uniform structure and adhesion of lubricating layer, and adopt cold extrusion forming.

Benefits of technology

It significantly reduces the cracking defect at the large end of the tooth profile, improves the forming quality and material yield, reduces production costs, and is suitable for mass automated production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120644935B_ABST
    Figure CN120644935B_ABST
Patent Text Reader

Abstract

This invention discloses a method for reducing large-end cracking in cold-forged differential half-shaft gears. The specific steps of this process include: sawing, normalizing, spheroidizing annealing, turning, shot blasting, phosphating, molybdenum disulfide powder coating, and cold extrusion of the gear teeth. This process improves the spheroidization grade of the material, reduces the hardness of the cold-extruded billet, avoids the occurrence of granular bainite in the spheroidized structure, solves the problems of not being able to reduce the material hardness and not being able to improve the material's plastic deformation capacity, improves the quality of cold forging, and reduces defects such as incomplete filling of the gear teeth and large-end cracking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of automotive parts manufacturing technology, specifically a method for reducing cracking at the large end of cold-forged differential half-shaft gears. Background Technology

[0002] In recent years, the development of new energy vehicles in China has been rapid, with an increasingly high penetration rate. Electric vehicles (EVs), in particular, have electric motors that operate at high speeds, exceeding 20,000 rpm, resulting in excellent acceleration performance; their 0-100 km / h acceleration time has been reduced to below 4 seconds. These performance characteristics place higher demands on automotive gears, requiring high fatigue strength at the gear tooth root to withstand the impacts, vibrations, and noise generated during high-speed operation and acceleration. Therefore, the requirements for gear steel are becoming increasingly stringent, necessitating increased strength for gears and gear shafts. Various gears may utilize higher-strength materials, making forging more difficult, especially cold forging. Cold forging is a manufacturing process that shapes metal at room temperature using molds and pressure machinery, offering advantages such as high strength, high precision, and high material utilization. However, cold forging involves high forming forces and high mold costs; therefore, cost reduction and efficiency improvement have always been the industry's focus, with spheroidizing of the billet being a crucial aspect.

[0003] Currently, the materials used for straight bevel gears in passenger car differentials are generally low-carbon alloy steels such as 20CrMo, 20MnCr5, and 20CrMnTiH. The forging of straight bevel gears in differentials typically employs a combined warm-cold forming process, which involves warm forging followed by cold finishing. This process has disadvantages such as billet heating and decarburization, high equipment investment, the need for automated mass production, and large tonnage for cold finishing of the tooth surface. Many manufacturers also use a one-step cold forging process for forging straight bevel gears in differentials. These gear steels require spheroidizing annealing softening treatment to improve the plasticity and fluidity of the metal.

[0004] While existing technologies can improve the plasticity and fluidity of metal materials through spheroidizing annealing, poor spheroidization can lead to increased deformation ratios due to the larger diameter of the tooth end, making it prone to quality problems such as large-end cracking. Some manufacturers increase subsequent machining allowances to remove cracks, but microcracks can extend into the forging, and the product still faces the risk of early cracking failure. Summary of the Invention

[0005] Purpose of the invention: In order to overcome the shortcomings of the prior art, the present invention provides a method to reduce the cracking of the large end of the cold forged differential half-shaft gear. The method optimizes the mold structure design, reduces the material flow resistance, and increases the fluidity of the metal material, fundamentally solving quality problems such as incomplete tooth filling and easy cracking at the large end of the tooth. Moreover, the structure is uniform, so that the product does not have abnormal structure.

[0006] Technical Solution: To achieve the above objectives, the present invention provides a method for reducing large-end cracking of cold-forged differential half-shaft gears. The specific steps of this process are as follows: Step 1: Sawing the material Select cylindrical bar stock with a specified diameter according to the drawing requirements, and then cut it into blanks using a cutting machine; Step 2: Normalizing treatment After the billet is cut, it is placed in a box-type resistance furnace for heating at 870~950℃ and held for 3.5h~4h. It is then air-cooled to 570~650℃ for isothermal treatment for 5h~6h. Finally, it is taken out of the furnace and air-cooled to room temperature to eliminate granular bainite and homogenize the structure. Step 3: Spheroidizing Annealing After normalizing, the billet is subjected to spheroidizing annealing treatment. The billet in the box-type resistance furnace is heated again to a temperature of 720℃~760℃ and held for 3h~4h. Then, the cooling system in the box-type resistance furnace is turned on to rapidly cool the billet to 650℃~660℃. After holding for 5h~6h, it is cooled to 400℃~450℃ without blowing air in the furnace and then taken out of the furnace. This process increases the spheroidization rate and reduces the hardness. Step 4: Turning The softened blank is machined into ends and outer diameters of specified dimensions using a lathe. Step 5: Shot blasting The blanks after turning are shot blasted using a drum shot blasting machine. The diameter of the shot particles in the shot blasting machine is 1.2~1.5mm, and the shot blasting time is 25~30min. This is to remove the adhering substances on the surface of the bar stock, improve the surface roughness of the workpiece, and improve the adhesion of the phosphating saponification lubricating film. Step Six: Phosphate Saponification Treatment The preform after shot blasting is subjected to phosphating and saponification treatment. The phosphating temperature is 70℃~85℃ and the time is 15min~20min to form a phosphating layer with a thickness of 10μm~15μm. The saponification temperature is 70℃~85℃ and the time is 5min~8min to form a saponification layer with a thickness of 5μm~8μm. When phosphating and saponifying the billet after shot blasting, zinc phosphate is used for phosphating. Due to its high density and good adhesion, a stable zinc phosphate layer can withstand pressures exceeding 2000 MPa. The aqueous solvent used for phosphating contains raw zinc phosphate (Zn(H,PO)) and phosphate (HPO), causing a series of chemical reactions in the billet during phosphating. The phosphating layer serves as a support layer for the saponified lubricant, which is then coated on top. This lubricant support layer firmly bonds the lubricant to the outer surface of the billet. The lubricant coating acts as a sliding layer, reducing friction between the extruded part and the die. This lubricant layer must not peel off; otherwise, scratches and grooves caused by cold welding will immediately appear on the workpiece, leading to scratches and damage to the die.

[0007] Step 7: Molybdenum disulfide powder coating The phosphated billet is then coated with an ultrafine molybdenum disulfide solution for surface lubrication. The coated area is the upper half of the billet. Step 8: Cold extrusion of tooth profile After the upper and lower dies are opened, the lubricated blank is placed between the upper and lower dies. The lower punch is installed at the axial position of the lower die. The upper die is sleeved on the outside of the inner punch of the upper die. The upper die and the inner punch of the upper die, which are located above the blank, move downward with the slide of the press. After the upper and lower dies are closed, the press continues to move downward, so that the blank is deformed into a forging under the extrusion of the lower punch. After extrusion is complete, the press moves upward with the upper toothed die back and separates from the lower die. The press ejector rod pushes out the formed forging after the extrusion is complete. The lower die is provided with an inlet, and the inlet is provided with an inclined surface.

[0008] As a further preferred embodiment of the present invention, in step one, the diameter of the blank is 5mm to 8mm smaller than the inner diameter of the lower die.

[0009] As a further preferred embodiment of the present invention, in step three, the billet is placed in a box-type resistance furnace for reheating.

[0010] As a further preferred embodiment of the present invention, in step three, the cooling system switch is a nitrogen circulation switch, and the cooling rate is 30℃ / h~80℃ / h.

[0011] As a further preferred embodiment of the present invention, in step four, the shot blasting machine is a drum-type shot blasting machine.

[0012] As a further preferred embodiment of the present invention, in step five, the diameter of the shot particles in the shot blasting machine is 1.2mm~1.5mm. As a further preferred embodiment of the present invention, in step seven, the concentration of the ultrafine molybdenum disulfide solution is greater than 15%.

[0013] As a further preferred embodiment of the present invention, in step seven, the surface friction coefficient μ of the blank after surface lubrication treatment is 0.05~0.06.

[0014] As a further preferred embodiment of the present invention, in step eight, the angle of the inclined surface provided on the mold inlet is 30°~60°.

[0015] As a further preferred embodiment of the present invention, the angle of the inclined surface increases as the difficulty of extruding and forming the billet increases.

[0016] Beneficial effects: The method for reducing large-end cracking of cold-forged differential half-shaft gears described in this invention has the following advantages compared with the prior art: (1) By optimizing the mold structure design, the material flow resistance was reduced and the fluidity of the metal material was increased, which fundamentally solved the cause of cracks. (2) The microstructure obtained by this process is a uniformly distributed ferrite matrix and spheroidized pearlite, avoiding the formation of granular bainite, so that the product does not have abnormal microstructure; (3) This process solves the problem that the material is prone to over-softening after traditional normalizing and annealing due to the low carbon content. It effectively reduces the material defect rate and ensures that the material has better mechanical properties in subsequent processing, thereby improving the material yield. (4) The bevel gear forgings obtained by cold forging the billet through this process have good forming quality, full tooth filling, and basically no cracking at the large end, which reduces costs and is suitable for mass automated production. (5) Through the provided lubrication treatment process, the lubrication layer has strong adhesion and uniform thickness, reducing the risk of blockage of the mold vent hole; (6) By utilizing this process, the quality of cold forging can be significantly improved, and the problems of incomplete tooth filling and large-end cracking can be reduced. Attached Figure Description

[0017] Figure 1 This is a schematic diagram of the process flow of the present invention; Figure 2 This is a full sectional view of a cold extrusion toothed die; Detailed Implementation

[0018] The present invention will be further illustrated below with reference to specific embodiments.

[0019] The present invention discloses a method for reducing large-end cracking of cold-forged differential half-shaft gears. The specific steps of the process include: sawing, normalizing treatment, spheroidizing annealing treatment, turning, shot blasting treatment, phosphating and saponification treatment, molybdenum disulfide powder coating, and cold extrusion of the gear teeth.

[0020] Before sawing, the raw materials need to be inspected upon arrival at the factory. Gear steel raw materials are generally low-carbon alloy steels such as 20CrMo, 20MnCr5, 20CrMnTiH, and 20CrNiMo. They are required to have a normalized structure, with a normalized structure of grade 1 to 3, a grain size of ≥ 5, a hardness of HB140 to 190, and no granular bainite, mixed grains, Widmanstätten structure, or other undesirable structures. If they do not meet the requirements, they must be subjected to isothermal normalizing treatment after cutting. Example

[0021] Step 1: Sawing the material Select a cylindrical bar with a specified diameter according to the drawing requirements, and then cut it into blank 1 using a cutting machine; Step 2: Normalizing treatment After the billet 1 is cut, it is placed in a box-type resistance furnace and heated to 870°C for 3.5 hours. It is then air-cooled to 570°C for 5 hours and isothermal treatment. Finally, it is taken out of the furnace and air-cooled to room temperature to eliminate granular bainite and homogenize the structure. Step 3: Spheroidizing Annealing The billet 1 in the box-type resistance furnace is heated again to 720℃ and held for 3 hours. Then, the nitrogen circulation cooling system in the box-type resistance furnace is turned on and the cooling rate is 30℃ / h to quickly cool the billet to 650℃. After holding for 5 hours, it is cooled to 400℃ without blowing air in the furnace and then taken out of the furnace, so as to improve the spheroidization rate and reduce the hardness. Step 4: Turning The softened blank 1 is machined to a specified size for the end and outer diameter using a lathe; Step 5: Shot blasting The blank 1 after turning was shot blasted using a drum shot blasting machine. The diameter of the shot particles in the shot blasting machine was 1.2 mm, and the shot blasting time was 25 min, in order to remove the adhering substances on the surface of the bar stock, improve the surface roughness of the workpiece, and improve the adhesion of the phosphating saponification lubricating film. Step Six: Phosphate Saponification Treatment The shot-blasted blank 1 was subjected to phosphating and saponification treatment at a temperature of 70°C for 15 minutes to form a phosphating layer with a thickness of 10 μm. The saponification temperature was 70°C for 5 minutes to form a saponification layer with a thickness of 5 μm. Step 7: Molybdenum disulfide powder coating The phosphated billet is surface lubricated and coated with an ultrafine molybdenum disulfide solution with a concentration greater than 15%. The coating area is the upper half of the billet. The surface friction coefficient μ of the billet after surface lubrication treatment is 0.05. Step 8: Cold extrusion of tooth profile After the upper toothed die 2 and the lower die 4 are opened, the lubricated blank is placed in the middle of the upper toothed die 2 and the lower die 4. The lower punch 5 is installed at the axial position of the lower die 4. The upper toothed die 2 is sleeved on the outside of the upper toothed die inner punch 1. The upper toothed die 2 and the upper toothed die inner punch 1, which are located above the blank 1, move downward with the slide of the press. After the upper toothed die 2 and the lower die 4 are closed, the press continues to move downward, so that the blank is deformed into a forging 3 under the extrusion of the lower punch 5. After extrusion is completed, the press moves upward with the upper toothed die 2 and disengages from the lower die 4. The press ejector rod pushes out the formed forging 3 after the extrusion is completed. The lower die 4 is provided with an inlet 6, and the inlet 6 is provided with a 30° inclined surface. The angle of the inclined surface increases as the difficulty of extruding and forming the blank increases. Example

[0022] Step 1: Sawing the material Select cylindrical bar stock with a specified diameter according to the drawing requirements, and then cut it into blanks using a cutting machine; Step 2: Normalizing treatment The blanks after cutting are placed in a box-type resistance furnace for heating at 928℃ and held for 3.8 hours; then air-cooled to 615℃ for isothermal treatment for 5.6 hours, and then air-cooled to room temperature to eliminate granular bainite and homogenize the microstructure. Step 3: Spheroidizing Annealing The billet in the box-type resistance furnace is reheated to 735℃ and held for 3.5 hours. Then, the nitrogen circulation cooling system in the box-type resistance furnace is turned on and the billet is rapidly cooled to 655℃ at a cooling rate of 60℃ / h. After holding for 5.5 hours, it is cooled to 425℃ without blowing air in the furnace and then taken out of the furnace, which improves the spheroidization rate and reduces the hardness. Step 4: Turning The softened blank 1 is machined to a specified size for the end and outer diameter using a lathe; Step 5: Shot blasting The blank 1 after turning was shot blasted using a drum shot blasting machine. The diameter of the shot particles in the shot blasting machine was 1.4 mm, and the shot blasting time was 28 min, in order to remove the adhering substances on the surface of the bar stock, improve the surface roughness of the workpiece, and improve the adhesion of the phosphating saponification lubricating film. Step Six: Phosphate Saponification Treatment The shot-blasted blank 1 was subjected to phosphating and saponification treatment at a temperature of 75°C for 18 minutes to form a phosphating layer with a thickness of 12 μm. The saponification temperature was 75°C for 6 minutes to form a saponification layer with a thickness of 6 μm. Step 7: Molybdenum disulfide powder coating The phosphated billet is surface lubricated and coated with an ultrafine molybdenum disulfide solution with a concentration greater than 15%. The coating area is the upper half of the billet. The surface friction coefficient μ of the billet after surface lubrication treatment is 0.05. Step 8: Cold extrusion of tooth profile After the upper toothed die 2 and the lower die 4 are opened, the lubricated blank is placed in the middle of the upper toothed die 2 and the lower die 4. The lower punch 5 is installed at the axial position of the lower die 4. The upper toothed die 2 is sleeved on the outside of the upper toothed die inner punch 1. The upper toothed die 2 and the upper toothed die inner punch 1, which are located above the blank 1, move downward with the slide of the press. After the upper toothed die 2 and the lower die 4 are closed, the press continues to move downward, so that the blank is deformed into a forging 3 under the extrusion of the lower punch 5. After extrusion is completed, the press moves upward with the upper toothed die 2 and disengages from the lower die 4. The press ejector rod pushes out the formed forging 3 after the extrusion is completed. The lower die 4 is provided with an inlet 6, and the inlet 6 is provided with a 50° inclined surface. The angle of the inclined surface increases as the difficulty of extruding and forming the blank increases. Example

[0023] Step 1: Sawing the material Select cylindrical bar stock with a specified diameter according to the drawing requirements, and then cut it into blanks using a cutting machine; Step 2: Normalizing treatment After the billet is cut, it is placed in a box-type resistance furnace and heated to 950℃ for 4 hours. It is then air-cooled to 650℃ for 6 hours and isothermal treatment. Finally, it is taken out of the furnace and air-cooled to room temperature to eliminate granular bainite and homogenize the structure. Step 3: Spheroidizing Annealing The billet in the box-type resistance furnace is reheated to 760℃ and held for 4 hours. Then, the nitrogen circulation cooling system in the box-type resistance furnace is turned on and the cooling rate is 80℃ / h to quickly cool the billet to 660℃. After holding for 6 hours, it is cooled to 450℃ without blowing air in the furnace and then taken out of the furnace, which increases the spheroidization rate and reduces the hardness. Step 4: Turning The softened blank 1 is machined to a specified size for the end and outer diameter using a lathe; Step 5: Shot blasting The blank 1 after turning was shot blasted using a drum shot blasting machine. The diameter of the shot particles in the shot blasting machine was 1.5 mm, and the shot blasting time was 30 min, in order to remove the adhering substances on the surface of the bar stock, improve the surface roughness of the workpiece, and improve the adhesion of the phosphating saponification lubricating film. Step Six: Phosphate Saponification Treatment The shot-blasted blank 1 was subjected to phosphating and saponification treatment at a temperature of 85°C for 20 minutes to form a phosphating layer with a thickness of 15 μm. The saponification temperature was 85°C for 8 minutes to form a saponification layer with a thickness of 8 μm. Step 7: Molybdenum disulfide powder coating The phosphated billet was surface lubricated and coated with an ultrafine molybdenum disulfide solution with a concentration greater than 15%. The coating area was the upper half of the billet. The surface friction coefficient μ of the billet after surface lubrication treatment was 0.06. Step 8: Cold extrusion of tooth profile After the upper toothed die 2 and the lower die 4 are opened, the lubricated blank is placed in the middle of the upper toothed die 2 and the lower die 4. The lower punch 5 is installed at the axial position of the lower die 4. The upper toothed die 2 is sleeved on the outside of the upper toothed die inner punch 1. The upper toothed die 2 and the upper toothed die inner punch 1, which are located above the blank 1, move downward with the slide of the press. After the upper toothed die 2 and the lower die 4 are closed, the press continues to move downward, so that the blank is deformed into a forging 3 under the extrusion of the lower punch 5. After extrusion is completed, the press moves upward with the upper toothed die 2 and disengages from the lower die 4. The press ejector rod pushes out the formed forging 3 after the extrusion is completed. The lower die 4 is provided with an inlet 6, and the inlet 6 is provided with a 60° inclined surface. The angle of the inclined surface increases as the difficulty of extruding and forming the blank increases.

[0024] The above embodiments are only for illustrating the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.

Claims

1. A method for reducing cracking at the large end of a cold-forged differential half-shaft gear, characterized in that, The specific steps of this process are as follows: Step 1: Sawing the material Select cylindrical bar stock with a specified diameter according to the drawing requirements, and then cut it into blanks using a cutting machine; Step 2: Normalizing treatment After the billet is cut, it is placed in a box-type resistance furnace for heating at a temperature of 870~950℃ and held for 3.5h~4h. It is then air-cooled to 570~650℃ for isothermal treatment for 5h~6h, and then removed from the furnace and air-cooled to room temperature. Step 3: Spheroidizing Annealing The billet after normalizing is subjected to spheroidizing annealing treatment at a heating temperature of 720℃~760℃ and a holding time of 3h~4h. Then, the cooling system switch in the box-type resistance furnace is turned on to rapidly cool the billet to 650℃~660℃, hold it for 5h~6h, and then cool it to 400℃~450℃ without blowing air in the furnace before being taken out of the furnace. The cooling system switch is a nitrogen circulation switch with a cooling rate of 30℃ / h~80℃ / h. Step 4: Turning The softened blank is machined into ends and outer diameters of specified dimensions using a lathe. Step 5: Shot blasting The turned blank is shot blasted using a shot blasting machine for 25-30 minutes; the diameter of the shot particles in the shot blasting machine is 1.2-1.5 mm. Step Six: Phosphate Saponification Treatment The preform after shot blasting is subjected to phosphating and saponification treatment. The phosphating temperature is 70℃~85℃ and the time is 15min~20min to form a phosphating layer with a thickness of 10μm~15μm. The saponification temperature is 70℃~85℃ and the time is 5min~8min to form a saponification layer with a thickness of 5μm~8μm. Step 7: Molybdenum disulfide powder coating The phosphated billet is then coated with an ultrafine molybdenum disulfide solution for surface lubrication. The coated area is the upper half of the billet. Step 8: Cold extrusion of tooth profile After the upper toothed die (2) and the lower die (4) are opened, the lubricated blank is placed between the upper toothed die (2) and the lower die (4). The lower punch (5) is installed at the axial position of the lower die (4). The upper toothed die (2) is sleeved on the outside of the upper toothed die inner punch (1). The upper toothed die (2) and the upper toothed die inner punch (1) located above the blank move downward with the slide of the press. After the upper toothed die (2) and the lower die (4) are closed, the press continues to move downward, so that the blank is deformed into a forging (3) under the extrusion of the lower punch (5). After extrusion is completed, the press moves upward with the upper toothed die (2) and separates from the lower die (4). The press ejector pushes out the formed forging (3) after the extrusion is completed. The lower die (4) is provided with an inlet (6), and the inlet (6) is provided with an inclined surface. The angle of the inclined surface provided on the inlet (6) is 30°~60°.

2. The method for reducing large-end cracking of cold-forged differential half-shaft gears according to claim 1, characterized in that: In step one, the diameter of the blank is 5mm to 8mm smaller than the inner diameter of the lower die.

3. The method for reducing large-end cracking of cold-forged differential half-shaft gears according to claim 1, characterized in that: In step three, the billet is placed in a box-type resistance furnace for reheating.

4. The method for reducing large-end cracking of cold-forged differential half-shaft gears according to claim 1, characterized in that: In step five, the shot blasting machine is a drum-type shot blasting machine.

5. The method for reducing large-end cracking of cold-forged differential half-shaft gears according to claim 1, characterized in that: In step seven, the concentration of the ultrafine molybdenum disulfide solution is greater than 15%.

6. The method for reducing large-end cracking of cold-forged differential half-shaft gears according to claim 1, characterized in that: In step seven, the surface friction coefficient μ of the blank after surface lubrication treatment is 0.05~0.

06.

7. The method for reducing large-end cracking of cold-forged differential half-shaft gears according to claim 1, characterized in that: The angle of the inclined surface increases as the difficulty of extruding the billet increases.

Citation Information

Patent Citations

  • Integral cold forging technique for angular wheel shaft

    CN101342566A

  • Molding process for straight bevel gear

    CN104589005A