Modified sepiolite fiber as well as preparation method and application thereof

By using acid activation and microwave heating to synergistically modify sepiolite fibers, the problem of uneven fiber distribution was solved, and high-performance sepiolite fibers were prepared for reinforced concrete, which improved the mechanical properties and acid resistance of the material and expanded its application range.

CN120647163APending Publication Date: 2025-09-16UNIV OF SCI & TECH LIAONING

Patent Information

Application Number
CN202510914339.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-03
Publication Date
2025-09-16

AI Technical Summary

Technical Problem

In practical applications, existing sepiolite fibers have problems with uneven fiber distribution and difficulty in dispersion, which affects their reinforcement effect in composite materials. Existing modification methods are difficult to meet the needs of high-performance materials, especially when processed at high temperatures, which can easily lead to structural damage or excessive energy consumption.

Method used

The acid activation-microwave heating synergistic modification method is adopted to treat sepiolite fiber with hydrochloric acid and microwave heating to remove impurities and promote fiber dissociation, increase its specific surface area and crystallinity, and enhance its dispersibility and activity.

Benefits of technology

The prepared sepiolite fibers with better dispersion and higher activity are used to strengthen concrete materials, significantly improving their mechanical properties and acid resistance. They are suitable for catalysis, adsorption, chemical synthesis and concrete materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120647163A_ABST
    Figure CN120647163A_ABST
Patent Text Reader

Abstract

The invention aims to provide a modified sepiolite fiber as well as a preparation method and a use method thereof, aiming at the defects of the performance and modification technology of the existing sepiolite fiber. The invention relates to a modified sepiolite fiber, which is a sepiolite fiber obtained by carrying out acid activation-microwave heating synergistic modification on a sepiolite raw ore, wherein the sepiolite fibers are single fibers and small bundle fibers; and the crystallinity of the sepiolite fiber is 75-88%. The sepiolite fiber is prepared by adopting an acid activation-microwave heating synergistic modification method, and through the synergistic treatment of hydrochloric acid and microwave heating, the microstructure and the specific surface area of the sepiolite fiber are effectively improved, so that the fiber distribution is more uniform, the activity of the sepiolite fiber is improved, and the application range of the sepiolite is expanded. And the concrete reinforced by the modified sepiolite fiber is better in mechanical property and has certain acid resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of mineral material extraction and application, and particularly relates to the preparation of sepiolite fiber and a preparation method and application thereof. Background Art

[0002] As a fibrous, magnesium-rich silicate clay mineral with a layered chain structure, sepiolite's unique crystal structure endows it with a range of remarkable properties. Its numerous nanoscale pores contribute to its exceptional adsorption properties, while its abundant active sites provide it with significant ion exchange capacity. Furthermore, sepiolite exhibits excellent thermal stability, maintaining its structural stability even at high temperatures. Most importantly, its excellent fiber dispersibility enables it to be evenly dispersed in a variety of matrices, bonding more tightly to the matrix and enhancing the performance of the matrix material.

[0003] However, in practical applications, there are still many difficulties in the practical application of natural sepiolite. Due to the strong hydrogen bonds and van der Waals forces between its fibers, the natural depolymerization effect is poor and it is difficult to fully disperse. The fiber distribution is as follows: Figure 1 This uneven fiber distribution not only affects the reinforcing effect of natural sepiolite fibers in composite materials but also leads to unstable product quality. These defects significantly limit the direct application of natural sepiolite fibers, preventing them from fully realizing their excellent properties in actual production, making it difficult to meet the stringent requirements for high-performance materials in various fields. This hinders the efficient utilization of sepiolite resources in a wider range of fields, resulting in significant limitations on its practical application.

[0004] Currently, a variety of methods exist for modifying sepiolite, which can improve certain properties, but some limitations remain. For example, while some acid activation methods offer high efficiency and are suitable for large-scale processing, they only remove some impurities and have limited effects on optimizing the sepiolite's microstructure. Certain heat treatment methods can easily damage the sepiolite's fiber structure, compromising its performance, while also consuming significant energy and resulting in treatment efficiencies insufficient to meet practical production needs. Furthermore, existing modification methods struggle to achieve the desired results in terms of increasing sepiolite's crystallinity and improving fiber dispersibility, failing to meet the demand for high-performance sepiolite materials in various fields.

[0005] Chinese patent application CN112237899A discloses a lanthanum-magnesium-modified sepiolite for phosphorus removal from black and odorous water. The modified sepiolite is prepared by modifying natural sepiolite with a mixed solution of lanthanum and magnesium salts. The modified sepiolite fiber exhibits a saturated adsorption capacity of up to 119 mg / g. -1 Compared with the natural sepiolite before modification, the lanthanum-magnesium modified sepiolite has a wide pH value (6-9) application range and is highly selective for orthophosphate in water bodies, especially for phosphorus in urban black and odorous water bodies (0.5-2.0 mg·L-1 ) excellent adsorption treatment. This method requires the prepared sepiolite to be dried for a long time at high temperature, which has strict requirements on the raw material ratio and is easily disturbed, affecting the performance of the prepared sepiolite fiber.

[0006] Chinese patent application publication number CN118440476A discloses a core-shell structured sepiolite fiber. Specifically, a hydrothermal method is used to electrostatically load nano-attapulgite onto the surface of sepiolite fibers with a large specific surface area. The -OH groups on the nano-attapulgite surface polymerize with the Si-OH groups on the sepiolite surface, forming a composite inorganic filler with a "core-shell" structure. This unique "core-shell" structure allows the nano-attapulgite fiber to form a mechanical linkage with the PBAT matrix during blending with PBAT, enhancing the interfacial bonding between the two phases and improving stress transfer between the nano-attapulgite and the PBAT phase, thereby enhancing the reinforcing effect. This invention addresses the problem of inorganic filler agglomeration in the PBAT matrix and improves the reinforcing effect. However, this method requires prolonged heating, consumes a lot of energy, and has a long preparation cycle. Summary of the Invention

[0007] The present invention addresses the shortcomings of existing sepiolite fiber performance and modification technologies by providing a modified sepiolite fiber and methods for its preparation and use. The present invention utilizes a synergistic modification method involving acid activation and microwave heating to prepare the sepiolite fiber. The synergistic treatment with hydrochloric acid and microwave heating effectively improves the microstructure and specific surface area of ​​the sepiolite fiber, resulting in a more uniform fiber distribution and enhanced activity, thus expanding the application range of sepiolite. Furthermore, concrete reinforced with the modified sepiolite fiber exhibits improved mechanical properties and a certain degree of acid resistance.

[0008] In order to achieve the purpose of the present invention, the following technical solutions are adopted:

[0009] A modified sepiolite fiber is a sepiolite fiber obtained by synergistic modification of sepiolite ore by acid activation and microwave heating;

[0010] Among them, sepiolite fibers are single fibers and small bundles of fibers;

[0011] The crystallinity of sepiolite fiber is 75~88%, and the better one is 77~88.39%.

[0012] Furthermore, the modified sepiolite fiber has a sepiolite content of 60-81%, preferably, a sepiolite content of 69-81%.

[0013] Furthermore, the modified sepiolite fiber has a specific surface area of ​​60~132 m 2 ·g-1 Preferably, the specific surface area is 116.99~131.14 m 2 ·g -1 .

[0014] The present invention also provides a method for preparing the modified sepiolite fiber, comprising the following steps:

[0015] (1) Soaking the raw sepiolite powder in deionized water for 10 to 20 hours, then stirring for 1 to 2 hours, filtering the upper suspension, and drying the resulting filter residue to obtain pretreated sepiolite powder;

[0016] (2) mixing the acid solution with the pretreated sepiolite powder, stirring the mixture thoroughly to react, and then allowing the mixture to stand for a suitable time; then washing the precipitated product with water several times, filtering it, and drying it to obtain the acid-treated sepiolite powder;

[0017] (3) Acid-treated sepiolite powder is subjected to microwave heat treatment to obtain modified sepiolite fibers.

[0018] Preferably, in the preparation method of the modified sepiolite fiber, the acid solution in step (2) is hydrochloric acid with a concentration of 0.6-1.2 mol·L -1 , more preferably 0.8 mol·L -1 .

[0019] Preferably, in the method for preparing the modified sepiolite fiber, the power of the microwave in step (3) is 1-2 KW, more preferably 2 KW.

[0020] Preferably, in the method for preparing the modified sepiolite fiber, the time of the microwave heat treatment in step (3) is 8 to 15 minutes, more preferably 8 minutes.

[0021] The present invention also provides the use of the modified sepiolite fiber as a reinforcing material for strengthening concrete; the amount of the modified sepiolite fiber added is 0.4-0.5% of the total mass of the dry matter of the concrete.

[0022] Furthermore, the modified sepiolite fiber is used in a method for preparing reinforced concrete, comprising: mixing crushed iron ore waste rock of different particle sizes and cement as dry materials, along with the modified sepiolite fiber, adding water and stirring evenly to obtain a concrete material slurry; then pouring the slurry into a mold, vibrating it, and curing it for 28 days; wherein the iron ore waste rock, river sand, and cement are configured according to conventional proportions, the modified sepiolite fiber is added in an amount of 0.4-0.5% of the mass of the dry material, and the water-cement ratio is 0.49-0.51.

[0023] Furthermore, with the application of the modified sepiolite fiber, the particle size range and mass proportion of the iron ore waste rock crushing product are 4.75 mm~+2.80 mm, accounting for 1.8%, -2.80 mm~+1.70 mm, accounting for 28.2%, -1.70 mm~+0.27 mm, accounting for 49.0%, -0.27 mm~+0.074 mm, accounting for 19.0% and -0.074 mm, accounting for 2.0%.

[0024] The basic principle of the modification of sepiolite fiber of the present invention is: using acid to activate the sepiolite material to promote the porosity of the sepiolite, and heat-treating the fully activated sepiolite material to dissociate the aggregated bundles of sepiolite, thereby optimizing the structure of the sepiolite and improving the specific surface area, adsorption performance and crystallinity of the sepiolite fiber.

[0025] The present invention utilizes the characteristics of modified sepiolite fiber with high specific surface area and adsorption performance, and its active fiber dispersion is more uniform and loose. When added to concrete material, it has strong binding ability with various material particles in the concrete material and good dispersion effect. In addition, the sepiolite fiber has higher crystallinity, thereby having a better effect on improving the mechanical strength of the concrete material.

[0026] Compared with the prior art, the present invention has the following advantages:

[0027] 1. Based on the strong bonding strength between layers and fiber bundles of raw sepiolite, this invention activates sepiolite fibers with an appropriate concentration of inorganic acid. This effectively removes impurities, imparts an appropriate pore size and high specific surface area to the sepiolite, and significantly enhances its activity. Furthermore, microwave dispersion technology is used to promote the dissociation of sepiolite fibers, significantly enhancing their dispersibility and specific surface area.

[0028] 2. The preparation method of the present invention uses commonly used reagents, does not require long-term hydrothermal reaction, and does not use toxic and harmful substances. It can prepare sepiolite fibers with low cost and excellent dispersion effect, and has the potential for large-scale industrial production.

[0029] 3. The sepiolite fiber of the present invention is a green and environmentally friendly material and can be widely used in the fields of catalysis, adsorption, chemical synthesis and concrete materials.

[0030] 4. After 28 days of curing, the flexural strength of the concrete reinforced with the sepiolite fiber of the present invention is not less than 12 MPa and the compressive strength is not less than 52 MPa. Compared with the iron ore waste rock concrete material under the same conditions, the flexural strength is increased by 20%±5% and the compressive strength is increased by 13%±5%.

[0031] 5. The reinforced concrete material of the present invention exhibits excellent acid resistance. Compared to concrete materials without modified sepiolite fiber, the samples with modified sepiolite fiber exhibited a lower mass loss rate and more stable mechanical property retention in sulfuric acid solution. Iron ore waste rock concrete with a 0.5% modified sepiolite fiber dosage experienced a mass loss rate of less than 1.10% after 14 days of immersion in sulfuric acid solution at a pH of 3. Its flexural strength was no less than 11 MPa, and its compressive strength was no less than 46 MPa, both exceeding those of concrete without acid attack. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 , SEM morphology of natural sepiolite fiber;

[0033] Figure 2 , XRD patterns and SEM morphology of crude purified sepiolite fibers;

[0034] Figure 3 , XRD patterns and SEM morphology of sepiolite reinforced fibers modified by acid activation and microwave heating;

[0035] Figure 4 , SEM morphology of the concrete material of Comparative Example 1;

[0036] Figure 5 , SEM morphology of the reinforced concrete material of Example 3;

[0037] Figure 6 , SEM morphology of the reinforced concrete material of the experimental example after acid immersion for 14 days. DETAILED DESCRIPTION

[0038] To facilitate understanding of the present invention, the present invention will be described more comprehensively below with reference to specific embodiments.

[0039] Example 1

[0040] A modified sepiolite fiber is a sepiolite fiber obtained by synergistic modification of sepiolite ore by acid activation and microwave heating;

[0041] Among them, sepiolite fibers are single fibers and small bundles of fibers, with a crystallinity of 77% and a specific surface area of ​​116.99m 2 ·g -1 ; The sepiolite content in the sepiolite fiber is 69%.

[0042] The preparation method of the modified sepiolite fiber comprises the following steps:

[0043] 1) Add 1000 mL of deionized water to 20 g of natural sepiolite, soak for 12 h, stir for 2 h, filter and dry the upper suspension to obtain crude sepiolite. XRD, surface area, and SEM analysis were performed on the crude sepiolite sample obtained. The XRD pattern and SEM morphology are shown in the attached figure. Figure 2 According to XRD pattern calculation, the original ore contains about 27% sepiolite. After crude purification, the sepiolite content is about 35%, and the sepiolite content has increased by nearly 8%, indicating that crude purification is beneficial to improving the purity of sepiolite. The specific surface area of ​​sepiolite has increased from 88.6 m 2 ·g -1 Increased to 114.1 m 2 ·g -1 ; SEM analysis showed that natural sepiolite was in an aggregated state, and the sepiolite fibers after crude purification were slightly deagglomerated.

[0044] 2) Take 5 g of crude purified sepiolite and mix with 0.8 mol·L -1 The mixture was mixed with hydrochloric acid solution, stirred with a magnetic stirrer for 2 h, allowed to stand for 2 h, and washed with deionized water three times after sufficient reaction, filtered and dried to obtain acid-activated sepiolite.

[0045] 3) 1 g of acid-activated sepiolite was irradiated at 1 kW microwave power for 12 minutes to obtain modified sepiolite fibers. XRD, surface area, and SEM analysis were performed on the resulting modified sepiolite fiber sample. XRD patterns revealed the disappearance of the characteristic calcite peaks, indicating complete decomposition of calcite. The relative content of sepiolite increased to approximately 69%, and the crystallinity reached 77%. The surface area of ​​the sepiolite increased to 116.99 m². 2 ·g -1 SEM analysis shows that the impurities in natural sepiolite are completely removed, the depolymerization effect of sepiolite fibers is enhanced, and the fibers are in a more dispersed state.

[0046] Example 2

[0047] A modified sepiolite fiber is a sepiolite fiber obtained by synergistic modification of sepiolite ore by acid activation and microwave heating;

[0048] Among them, sepiolite fibers are single fibers and small bundles of fibers, with a crystallinity of 88% and a specific surface area of ​​131.14 m 2 ·g -1 ; The sepiolite content in the sepiolite fiber is 81%.

[0049] The modified sepiolite fiber was prepared by taking 5 g of crude purified sepiolite prepared in Example 1 and mixing it with a concentration of 0.8 mol·L -1The mixture was mixed with a hydrochloric acid solution, stirred for 2 hours using a magnetic stirrer, allowed to stand for 2 hours, and after sufficient reaction, washed three times with deionized water, filtered, and dried to obtain acid-activated sepiolite. Subsequently, 1 g of acid-activated sepiolite was irradiated at 2 kW microwave power for 8 minutes to obtain modified sepiolite fiber. The sample obtained in this example was analyzed by XRD, specific surface area, and SEM. The modified sepiolite fiber was in the best condition when irradiated at 2 kW microwave power for 8 minutes. The XRD pattern and SEM morphology are shown in the attached figure. Figure 3 The XRD spectrum shows that the characteristic peak of calcite disappears, indicating that calcite is completely decomposed. The relative content of sepiolite increases to 81%, and the crystallinity reaches 87.39%. The specific surface area of ​​sepiolite increases to 131.14 m 2 ·g -1 .

[0050] Comparative Example 1

[0051] A method for preparing sepiolite fiber is as follows: 5 g of crude purified sepiolite prepared in Example 1 is mixed with a 0.8 mol·L -1 The mixture was mixed with a hydrochloric acid solution and stirred with a magnetic stirrer for 2 hours. The mixture was allowed to stand for 2 hours. After sufficient reaction, the mixture was washed three times with deionized water, filtered, and dried to obtain sepiolite fibers. XRD patterns showed that the relative content of sepiolite increased to 51%, and the crystallinity reached 43.37%.

[0052] Comparative Example 2

[0053] A method for preparing sepiolite fiber comprises irradiating 1 g of the crudely purified sepiolite prepared in Example 1 with a microwave power of 2 kW for 8 minutes to obtain sepiolite fiber. XRD patterns indicate that the relative content of sepiolite increases to 47%, and the crystallinity reaches 50.26%.

[0054] Comparative Example 3

[0055] A concrete preparation method comprises preparing 1350 g of iron ore waste rock, 450 g of cement, and 225 mL of water. The particle size range and mass proportion of the crushed iron ore waste rock are 4.75 mm to +2.80 mm (1.8%), -2.80 mm to +1.70 mm (28.2%), -1.70 mm to +0.27 mm (49.0%), -0.27 mm to +0.074 mm (19.0%), and -0.074 mm (2.0%). The above materials are mixed uniformly in a cement mortar mixer, and the mixed mortar is poured into a mold. The mold is then removed after curing for 24 hours to obtain the iron ore waste rock concrete material. The flexural and compressive strengths of the material are tested after curing for 28 days. The test results show a flexural strength of 10 MPa and a compressive strength of 46.38 MPa. Subsequently, the modified sepiolite-iron ore waste rock concrete material was subjected to scanning electron microscopy examination and analysis, e.g. Figure 2 The results show that more calcium silicate hydrate appeared in the cured samples, which is the product of cement hydration. The irregular and rough iron ore waste rock has a high specific surface area and is in full contact with the calcium silicate hydrate. This process effectively fills the pore structure between the iron ore waste rock particles, which is beneficial to maintaining the mechanical strength of the iron ore waste rock concrete material.

[0056] Example 3

[0057] A method for preparing reinforced concrete comprises taking 1350 g of iron ore waste rock, 450 g of cement, 9 g of modified sepiolite fiber prepared in Example 2, and 225 mL of water, wherein the particle size range and mass proportion of the iron ore waste rock crushing product are 4.75 mm to +2.80 mm, accounting for 1.8%, -2.80 mm to +1.70 mm, accounting for 28.2%, -1.70 mm to +0.27 mm, accounting for 49.0%, -0.27 mm to +0.074 mm, accounting for 19.0%, and -0.074 mm, accounting for 2.0%; placing the above materials in a cement mortar mixer and stirring evenly, then pouring the mixed mortar into a mold to form, curing for 24 hours, and then demolding to obtain a modified sepiolite fiber-iron ore waste rock concrete material, and testing the flexural strength and compressive strength of the material after curing for 28 days. The test results show that the flexural strength is 12.10 MPa, which is 21% higher than that of comparative example 1; the compressive strength is 52.62 MPa, which is 13.5% higher than that of comparative example 1. Subsequently, the modified sepiolite fiber-iron ore waste rock concrete material was subjected to scanning electron microscope detection and analysis, as shown in FIG. Figure 3The results show that the modified sepiolite fiber bundles connect the mineral particles to each other, and the modified sepiolite fibers play a good bridging role in the cracks that appear after loading. At the same time, the modified sepiolite fibers further fill the pore structure and reduce the pores, which provides support for the modified sepiolite fibers to improve the mechanical properties of iron ore waste rock concrete materials.

[0058] Comparative Example 4

[0059] A method for preparing reinforced concrete is the same as that of Example 3, except that the sepiolite fiber is the product prepared in Comparative Example 1.

[0060] The resulting sepiolite fiber-iron ore waste concrete material was cured for 28 days and tested for its flexural and compressive strengths. The test results showed a flexural strength of 10.8 MPa and a compressive strength of 49.86 MPa.

[0061] Comparative Example 5

[0062] A method for preparing reinforced concrete is the same as that of Example 3, except that the sepiolite fiber is the product prepared in Comparative Example 2.

[0063] The resulting sepiolite fiber-iron ore waste concrete material was cured for 28 days and tested for its flexural and compressive strengths. The test results showed a flexural strength of 10.4 MPa and a compressive strength of 48.23 MPa.

[0064] Experimental example

[0065] The reinforced concrete obtained in Example 3, after curing for 28 days, was immersed in a sulfuric acid solution with a pH of 3 for 14 days. After acid immersion, its mass loss rate, flexural strength, and compressive strength were tested. The test results showed that after 14 days of acid immersion, the mass loss rate was 1.10%, the flexural strength was 11.88 MPa, and the compressive strength was 46.50 MPa.

[0066] The data show that the reinforced concrete reinforced with modified sepiolite has strong acid resistance and can be used under certain acidic conditions. Subsequently, the acid-soaked samples were tested and analyzed by scanning electron microscopy. Figure 4 The results show that after 14 days of acid leaching, the sepiolite fiber morphology inside the sample disappeared and was covered with many small agglomerated particles. This is because the modified sepiolite fiber has a high specific surface area and many active sites, and has good adsorption capacity. During the acid leaching process, it absorbs a large amount of H ionized by the sulfuric acid solution. + and SO4 2- The fiber structure of the modified sepiolite in a strong acid environment is destroyed, forming agglomerated particles attached to the surface of the iron ore waste rock particles, preventing further erosion by sulfuric acid, which is beneficial to protecting the mechanical properties of the modified sepiolite-iron ore waste rock concrete material.

[0067] The above is only a preferred embodiment of the present invention. It should be pointed out that due to the differences in mineral composition and equipment, there are slight differences in the physical properties of the prepared materials. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A modified sepiolite fiber, characterized in that: The sepiolite fiber is modified by acid activation and microwave heating of sepiolite ore; Among them, sepiolite fibers are single fibers and small bundles of fibers; the crystallinity of sepiolite fibers is 75~88%.

2. The modified sepiolite fiber according to claim 1, characterized in that The sepiolite content in sepiolite fiber is 60~81%.

3. The modified sepiolite fiber according to claim 1, characterized in that The specific surface area of ​​sepiolite fiber is 60~132 m 2 ·g -1 .

4. The method for preparing the modified sepiolite fiber according to claim 1, characterized in that: The following steps are involved: (1) Soaking the raw sepiolite powder in deionized water for 10-20 hours, then stirring for 1-2 hours, filtering the upper suspension, and drying to obtain pretreated sepiolite powder; (2) mixing the acid solution with the pretreated sepiolite powder, stirring the mixture thoroughly to react, and then allowing the mixture to stand for a suitable time; then washing the precipitated product with water several times, filtering it, and drying it to obtain the acid-treated sepiolite powder; (3) Acid-treated sepiolite powder was selected and subjected to microwave heat treatment to obtain modified sepiolite fiber.

5. The method for preparing the modified sepiolite fiber according to claim 4, characterized in that: The acid solution in step (2) is hydrochloric acid with a concentration of 0.6~1.2 mol·L -1 .

6. The method for preparing the modified sepiolite fiber according to claim 4, characterized in that: The power of the microwave in step (3) is 1~2 KW.

7. The method for preparing modified sepiolite fiber according to claim 4, characterized in that: The time of microwave heat treatment in step (3) is 8 to 16 minutes.

8. The use of the modified sepiolite fiber according to claim 1, characterized in that: As a reinforcing material for reinforced concrete, the addition amount of modified sepiolite fiber is 0.4~0.5% of the total mass of concrete dry matter.

9. The use of the modified sepiolite fiber according to claim 8, characterized in that: The reinforced concrete preparation method comprises: mixing crushed iron ore waste rock of different particle sizes and cement as dry materials, and modified sepiolite fiber, adding water and stirring evenly to obtain a concrete material slurry; then pouring the slurry into a mold, vibrating it, and curing it for 28 days; wherein the iron ore waste rock, river sand, and cement are configured according to conventional proportions, the modified sepiolite fiber is added in an amount of 0.4-0.5% of the mass of the dry material, and the water-cement ratio is 0.49-0.

51.

10. The use of the modified sepiolite fiber according to claim 9, characterized in that: The particle size range and mass proportion of the iron ore waste rock crushing products are as follows: 4.75 mm~+2.80 mm, accounting for 1.6~2.0%, -2.80 mm~+1.70 mm, accounting for 27.2~29.2%, -1.70 mm~+0.27 mm, accounting for 48.0~50.0%, -0.27 mm~+0.074 mm, accounting for 18.0~20.0%, and -0.074 mm, accounting for 1.8~2.2%.

Citation Information

Patent Citations

  • Lanthanum-magnesium modified sepiolite for removing phosphorus from black and odorous water body

    CN112237899A

  • Sepiolite fiber and attapulgite modified PBAT composite material with core-shell structure

    CN118440476A

Cited By

  • A nano-zeolite modified emulsified asphalt fog seal material and a preparation method thereof