Near-isothermal hot spinning forming method and heat compensation method for metal workpiece

By setting up a heating system and a spinning wheel system on the spinning equipment, near-isothermal hot spinning of difficult-to-deform alloy materials can be achieved, which solves the problem of inaccurate temperature control, improves the forming quality and efficiency, and meets the manufacturing needs of high-precision workpieces.

CN120772330AActive Publication Date: 2025-10-14GUIZHOU AVIATION TECHN DEV CO LTD

Patent Information

Application Number
CN202411229815.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2025-10-14
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The existing hot spinning forming method for difficult-to-deform alloy materials cannot accurately adjust and control the temperature of the material deformation zone, resulting in poor temperature uniformity and unable to meet the workpiece manufacturing requirements.

Method used

A near-isothermal hot spinning method is adopted. By setting a heating system on the spinning equipment, the spinning temperature of the blank is monitored and adjusted in real time to ensure that the temperature fluctuation during the spinning process is within ±20°C. Combined with the synchronous operation of the heating system and the spinning wheel system, precise temperature control is achieved.

Benefits of technology

It improves the deformation capacity of difficult-to-deform metal materials, reduces deformation resistance, improves forming quality and efficiency, and meets the manufacturing requirements of high-precision workpieces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120772330A_ABST
    Figure CN120772330A_ABST
Patent Text Reader

Abstract

The invention discloses a near-isothermal hot spinning forming method and a heat compensation method for a metal workpiece. The forming method comprises the steps that a blank heated to the spinning preheating temperature is transferred and clamped on a workbench, and the blank is located in an effective heat compensation area arranged in a heat compensation system; the blank is subjected to temperature measurement to judge whether the blank temperature meets the temperature before blank spinning so as to determine whether the blank is subjected to temperature compensation waiting in a heat compensation system or not; and then near-isothermal hot spinning forming is completed in a heat compensation system according to a preset spinning program, the heat compensation system continuously compensates the temperature of the blank during spinning and monitors the spinning temperature in real time, and it is guaranteed that the fluctuation range of the spinning temperature does not exceed + / -20 DEG C in the process from spinning deformation to spinning deformation ending. According to the near-isothermal spinning forming technology, spinning equipment of a measurable and controllable semi-closed active heat compensation system is utilized, and the deformation temperature of high-temperature alloy, titanium alloy and other difficult-to-deform metal materials is controlled within a small fluctuation range in the spinning process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hot spinning, in particular to a near-isothermal hot spinning method and a heat supplement method for a metal workpiece. Background Art

[0002] High-temperature alloys, such as titanium alloys, are difficult to deform due to their high strength, excellent corrosion resistance, high temperature resistance, high toughness, and good weldability. Casings and other parts manufactured from these materials are widely used in aerospace engines. Currently, these parts are primarily manufactured using a ring-forming process involving ring blanks and machining. This process often involves large machining allowances, resulting in high raw material costs. Furthermore, the large amount of machining removed leads to high processing costs and part deformation caused by high residual stresses. Therefore, the development and application of near-net-shape forming technology in the manufacture of difficult-to-deform metal ring forgings is urgent.

[0003] The spinning process utilizes the plastic deformation of metal to form various rotationally symmetrical hollow workpieces from metal blanks through rotation and localized pressure. This process features high machining accuracy and efficiency, resulting in thinner wall thicknesses close to the actual wall thickness of the part, and small machining allowances. It is a near-net-shape forming process widely used in aerospace, military equipment, automotive parts, and other fields. Currently, aircraft engine casing parts are typically ring-shaped, making them well-suited for spin forming. However, difficult-to-deform alloys also suffer from poor room temperature plasticity, high forming temperatures, and a narrow deformation temperature window. This places higher demands on precise control of the deformation temperature during hot spinning of difficult-to-deform metal parts.

[0004] Currently, the primary heating method for hot spinning is flame heating, which uses a flame to heat the billet, the spinning wheel, and other parts separately. This method has the advantages of simple heating, high heating efficiency, and a wide temperature range. However, this heating method is open-type, and the flame only covers a portion of the billet. Although it can cover all parts of the spun billet through reciprocating sweeping, the flame size, heated area, and distance between the flame and the billet are all manually adjusted, resulting in large fluctuations and arbitrariness. Furthermore, ambient temperature has a significant impact on the heating temperature. The required heating time and flame size for normal processing of the spun billet vary in different seasons, resulting in different heating temperature rise rates and temperature distributions in different areas of the billet. Because the forming temperature range of parts made of difficult-to-deform metal materials such as titanium alloys and high-temperature alloys is narrow, strict requirements on the deformation temperature range and temperature uniformity are imposed to ensure forming quality. However, flame heating methods have disadvantages such as large temperature fluctuations, low heating precision, and low heating efficiency. This method cannot achieve temperature stability, resulting in unstable wrinkling, cracking, poor wall thickness uniformity, die sticking, and even substandard mechanical properties in difficult-to-deform alloys during hot spinning.

[0005] To improve temperature accuracy and stability, numerous studies have been conducted. Some studies have used temperature equipment to measure the temperature of the blank and provide feedback to a heating device to control heating. For example, patent documents CN103706716B, CN106964682A, and CN111842603B disclose a method for precise temperature control during hot spinning of titanium alloy thin-walled components. During the hot spinning process, this method utilizes infrared thermal imaging equipment to monitor the deformation zone of the titanium alloy blank in real time. Based on the actual temperature of the deformation zone of the titanium alloy blank as fed back by the infrared thermal imaging equipment, the temperature of the deformation zone of the titanium alloy blank is adjusted in real time using a local heating device to control the temperature within a certain range. This achieves precise temperature control during hot spinning of titanium alloy thin-walled components, resulting in a titanium alloy thin-walled component. Under open heating conditions, the measurement error of the workpiece using a multi-point infrared thermometer is too large, making it impossible to accurately obtain the actual temperature of the material deformation zone during spinning and to adjust and control it, resulting in a failure to meet temperature measurement accuracy requirements.

[0006] Some studies have also used composite heating methods. For example, patent CN109108139 B discloses a composite heating-based spinning method for titanium-based alloy materials. First, a flame gun is used to preheat the blank, mandrel, and spinning wheel. Then, a follow-up induction heating coil is used to heat the blank to the spinning temperature. During the spinning process, an infrared thermal imager is used to monitor the temperature, and a flame gun is used to heat the blank in the spinning area behind the spinning wheel. However, difficult-to-deform alloy materials have high forming temperatures, a narrow thermal working window, and are sensitive to temperature and strain rate. The composite heating method is complex and still suffers from poor temperature uniformity in different zones, making it unable to meet the manufacturing requirements of high-precision workpieces.

[0007] Therefore, in order to improve the deformation ability of the material, reduce the deformation resistance, and improve the forming quality and forming efficiency, it is necessary to develop a new near-isothermal hot spinning forming method for the manufacture of difficult-to-deform alloy material workpieces. Summary of the Invention

[0008] The purpose of the present invention is to solve the problem that the existing hot spinning forming method of difficult-to-deform alloy materials cannot accurately adjust and control the temperature of the material deformation zone and has poor temperature uniformity, resulting in the inability to meet the workpiece manufacturing requirements, and to provide a near-isothermal hot spinning forming method and a heat supplement method for metal workpieces.

[0009] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0010] A near-isothermal hot spinning method for a metal workpiece comprises the following steps:

[0011] Heat the blank to the spinning preheating temperature;

[0012] The heated blank is transferred and clamped on a workbench that rotates with the main shaft of the spinning equipment, wherein a supplementary heating system is installed on the periphery of the workbench, and the blank is located in an effective supplementary heating zone set by the supplementary heating system;

[0013] Measure the temperature of the blank after clamping and determine the blank temperature T 坯 Whether the temperature of the blank before spinning meets the process requirements like Then start the spinning equipment to start spinning; if The heating system is used to heat the blank to meet the temperature requirement. Then start the spinning equipment to carry out spinning;

[0014] A near-isothermal hot spinning process is used in the spinning equipment to spin the blank. During the near-isothermal hot spinning, the heating system is used to actively heat the blank, and the spinning temperature of the blank's spinning deformation zone is monitored in real time to ensure that the spinning temperature fluctuates within a range of no more than ±20°C from the start to the end of the spinning deformation process.

[0015] In the technical solution of the present invention, the blank is first heated to the spinning preheating temperature in a heating device, and then transferred and clamped on the workbench of the spinning device. The workbench rotates with the main shaft of the spinning device, and can drive the blank to be selected for subsequent spinning; the spinning device is provided with a spinning system and a heat supplement system, and the spinning system is used to realize local spinning deformation of the blank, and is used to form the shape of the workpiece and ensure dimensional accuracy; the heat supplement system is installed on the periphery of the workbench, and the heat supplement system forms an effective heat supplement zone, and the blank is located in the effective heat supplement zone, that is, through the above-mentioned setting, the effective heat supplement zone can envelop the entire blank, and subsequently supplement the heat lost by the blank during the transfer, fixation and spinning process and the environmental heat conduction. At the same time, the heat supplement system on the spinning device will not interfere with the radial and axial movement of the spinning system in the blank, thereby ensuring the synchronous realization of spinning and heating during the workpiece forming process. Before spinning, the temperature of the blank after clamping and fixing is measured and it is judged whether the blank temperature meets the blank pre-spinning temperature required by the spinning process. If the blank temperature meets the blank pre-spinning temperature required by the spinning process at this time, the spinning equipment should be started for spinning; if the blank temperature is lower than the blank pre-spinning temperature required by the spinning process at this time, the blank should be actively heated by the heating system to the blank pre-spinning temperature before spinning is started, that is, in this step, the temperature is quickly increased by starting the heating system, and the heating system effectively heats the blank in the heating zone to prevent the blank temperature from continuing to lose, so that the blank temperature reaches the spinning condition required by the process, that is, reaches the pre-spinning temperature, and starts spinning under the temperature condition that the blank temperature reaches the pre-spinning temperature of the blank; during the spinning process, the heating system is continued to be used to heat the blank, and at the same time, the deformation temperature in the spinning deformation zone of the blank, that is, the spinning temperature, is monitored and recorded in real time, so that the spinning temperature does not fluctuate by more than ±20°C from the start to the end of spinning, and the spinning temperature T 旋 The maximum and minimum values ​​of are both within the temperature fluctuation range required by the process, that is, a measurable and controllable heat supplement system is used to maintain the deformation temperature of the metal material in a smaller fluctuation range during the forming process, thereby achieving near-isothermal spinning deformation. Such a setting can reduce the deformation resistance of difficult-to-deform metal materials, maintain a higher deformation capacity of the metal material during the spinning process, improve the forming quality and forming efficiency, and meet the workpiece manufacturing requirements. At the same time, the deformation parameters of the hot-spun products of this technical solution are consistent and traceable.

[0016] Through the above technical solution, the spinning temperature is higher than the recrystallization temperature of the metal material. The spinning forming process of the present invention is hot processing, and the metal material will undergo dynamic recrystallization, which helps to eliminate work hardening, thereby improving the plasticity and toughness of the metal material. The consistency of the formed workpiece product is very good and can meet the manufacturing requirements of high-precision workpieces. The technical solution of the present invention is suitable for difficult-to-deform metals with a narrow forming temperature range, and is also applicable to non-difficult-to-deform metals.

[0017] In the present invention, the effective temperature compensation zone refers to the area formed in the heating system that can heat the workpiece to reach the required temperature and has a uniform temperature distribution. The heating area that can achieve the heating and temperature compensation effect in the heating system may be larger than the effective heating area. Because some heating areas have low temperatures or uneven temperature distribution due to the layout of heating elements, they are not suitable for heating and temperature control of the blanks. Through the reasonable layout of heating elements, the effective temperature compensation zone of the heating system is guaranteed, and the quality of the workpiece is guaranteed.

[0018] Blank temperature before spinning This is the starting temperature for spinning. When the billet temperature reaches the pre-spinning temperature, the difficult-to-deform metal material has a higher deformation capacity. It also provides a temperature basis for the spinning temperature fluctuation range to not exceed ±20°C during near-isothermal hot spinning. The pre-spinning temperature of the billet is within the spinning temperature range. The pre-spinning temperature of the billet can be determined based on metal processing experience. For new metal materials, the pre-spinning temperature of the billet can be obtained using numerical simulation software or calculation formulas.

[0019] Spinning temperature T 旋 It refers to the temperature of the spinning deformation zone of the blank after the spinning wheel contacts the blank and the spinning force is applied during spinning. The spinning temperature is the instantaneous spinning temperature. The spinning temperature should be determined according to the deformation temperature range based on the specific material type, spinning conditions, etc., that is, the spinning temperature is not a fixed value, but a temperature range with a certain fluctuation amplitude. In the near-isothermal hot spinning process of the present invention, the fluctuation range of the spinning temperature is between the maximum and minimum values ​​required by the process, so as to achieve strict control of the spinning temperature, which can ensure that the metal material has sufficient plasticity while avoiding the occurrence of cracks, metal accumulation and other spinning defects caused by too high or too low temperature. The spinning temperature T of the blank 旋 The fluctuation range within a spinning pass (i.e., from the beginning to the end of a single spinning pass) is no more than ±20°C, that is, within a spinning pass, the maximum value of the spinning temperature T 旋max and the minimum value T 旋min The difference is no more than 40 ° C. The spinning temperature can be obtained according to the thermal processing diagram corresponding to the workpiece material. The spinning temperature for a specific metal material is a range value, which can be obtained through the material manual or thermal simulation test.

[0020] As a preferred embodiment of the present invention, the spinning preheating temperature is 300-1200° C. For different metal materials, the spinning preheating temperature of the blank is determined according to the spinning process.

[0021] As a preferred embodiment of the present invention, the time taken to transfer the heated blank and clamp it on the workbench of the spinning equipment is taken as the transfer time, and the transfer time is required to be no more than 90s. In the above technical solution, the blank heated to the preheating temperature for spinning loses heat during the transfer process and the process of clamping and fixing it to the workbench, resulting in a drop in the temperature of the blank. Before spinning, the blank temperature may not reach the start spinning temperature condition allowed by the process, and the hot spinning of the difficult-to-deform metal cannot be carried out immediately. The spinning process needs to be started after the heating system heats the blank to meet the spinning conditions. This makes the process flow complicated. Therefore, the transfer time is required to be as short as possible, which can reduce the heat loss of the blank during the transfer and fixing process, reduce the temperature drop, and help reduce the waiting time for the blank to be heated, while reducing energy loss. However, the shorter the transfer time, the higher the flexibility requirements of the transfer device and the fixing device. Taking all factors into consideration, the transfer time ranges from 40 to 90s. For different metal materials, the transfer time of different metal materials is determined according to the spinning processing requirements, equipment status and other factors. The shorter the transfer time, the better.

[0022] As a preferred embodiment of the present invention, the spinning equipment includes a machine body, a heat supplement system and a rotary wheel system, the heat supplement system and the rotary wheel system are arranged on the machine body, a workbench is installed on the main shaft of the machine body, the rotary wheel system includes a rotary wheel assembly, the heat supplement system includes a furnace body and a temperature control system, the temperature control system includes a furnace body temperature measurement module, a control module and a heating module, the heating module includes a plurality of heating elements; a furnace cavity is formed in the furnace body, and the heating elements are arranged on the inner wall of the furnace cavity, which are used to form an effective temperature supplement zone in the furnace cavity; a rotary wheel movement groove is provided on the furnace body, and the rotary wheel assembly passes through the rotary wheel movement groove to ensure that the rotary wheel assembly can move freely along the radial and axial directions of the blank; the furnace body temperature measurement module is used to detect the temperature of the effective temperature supplement zone, and the furnace body temperature measurement module and the heating module are both electrically connected to the control module.

[0023] In the above technical solution, the spinning equipment integrates a heat supplement system and a rotary wheel system, and the heat supplement system and the rotary wheel system are arranged on the machine body. The rotary wheel assembly of the rotary wheel system locally pressurizes the blank, which can form the shape and size of the workpiece; a furnace cavity is formed in the furnace body of the heat supplement system, and heating elements are arranged in the furnace cavity wall. The uniform arrangement of the heating elements forms an effective temperature supplement zone in the furnace body, and the blank is located in the effective temperature supplement zone, which can heat and supplement the temperature of the blank; at the same time, a rotary wheel movement groove is provided on the furnace body of the heat supplement system, and the rotary wheel assembly passes through the rotary wheel movement groove and is located in the rotary wheel movement groove. Such an arrangement ensures that the rotary wheel assembly can move freely along the radial and axial directions of the blank. Through the above arrangement, the furnace body of the heat supplement system is a semi-closed structure, and a semi-closed furnace cavity is formed in the furnace body. The heat supplement system on the spinning equipment will not interfere with the radial and axial movement of the spinning system, thereby ensuring the synchronous realization of spinning and heating and supplementing temperature during the workpiece forming process. The temperature control system's furnace temperature measurement module detects the temperature of the effective compensation zone and feeds the temperature signal back to the control module. The control module receives the temperature signal from the furnace temperature measurement module, compares and processes it with the compensation target temperature set by the temperature control system, and outputs a corresponding control signal to the heating module. The heating module is managed by the control module, adjusting the heating power of the heating element based on the temperature signal from the furnace temperature measurement module, continuously adjusting the temperature to maintain a stable temperature near the compensation target temperature. The connection between the furnace temperature measurement module, the heating module, and the control module in the temperature control system forms a closed-loop temperature control system for accurately monitoring and regulating the temperature of the effective compensation zone. Through precise temperature measurement by the furnace temperature measurement module, temperature control by the control module, and precise regulation by the heating module, a temperature uniformity of ±15°C and a temperature control accuracy of ±1°C in the effective compensation zone are achieved. The control module connects to the furnace temperature measurement module or the heating module via fieldbus, industrial Ethernet, or other methods, as understood by those skilled in the art, to enable data transmission and control signal reception.

[0024] As a more preferred embodiment of the present invention, the workbench of the machine body is equipped with a quick clamping structure for the blank, the bottom of the furnace body is connected to the workbench, the workbench is used to support the blank, and the clamping structure is used to fix the blank on the workbench.

[0025] As a preferred embodiment of the present invention, the control module of the supplemental heating system is configured with a target temperature within a range of 300°C to 1200°C. The control module includes a user interface, such as a display and control panel, allowing the user to set the target temperature and monitor real-time temperature and other parameters. The temperature control accuracy and temperature measurement methods of the supplemental heating system meet standard requirements.

[0026] As a preferred embodiment of the present invention, the furnace temperature measurement module includes multiple temperature sensors. The installation positions and insertion depths of the multiple temperature sensors on the furnace body are designed to reflect the actual temperature of the effective heating zone. The temperature sensors are thermocouples, which measure temperature based on the thermoelectric effect.

[0027] As a preferred embodiment of the present invention, the roller assembly includes an inner roller and an outer roller. When the roller assembly is working, the entire structure of the inner roller and a partial structure of the outer roller are in the effective temperature compensation zone of the heat compensation system. The inner roller is located on the inner side of the blank and can abut the inner wall of the workpiece blank. The outer roller is located on the outer side of the blank and can abut the outer wall of the workpiece blank. The inner roller and the outer roller pass through the roller motion groove and are located in the roller motion groove, ensuring that the inner roller and the outer roller can move independently and freely in the radial and axial directions of the blank.

[0028] In the above technical solution, the entire inner wheel and part of the outer wheel are in the effective temperature compensation zone, which can keep the inner wheel and the outer wheel warm and preheat them, reduce the temperature difference between the inner wheel, the outer wheel and the blank, further reduce the temperature drop of the workpiece during spinning, and is more conducive to controlling the spinning temperature of the blank during near-isothermal hot spinning; the inner wheel is located on the inner side of the blank, and the outer wheel is located on the outer side of the blank, and the inner wheel and the outer wheel pass through the wheel motion groove and are located in the wheel motion groove, The inner and outer wheels are guaranteed to move independently in the radial and axial directions of the worktable, spinning the wheel space according to the spinning trajectory required by the process. At the same time, the diameter and width of the wheel movement groove should be larger than the diameters of the inner and outer wheels to prevent interference during the spinning process. During the spinning process, the inner and outer wheels respectively abut the inner and outer walls of the blank, locally pressurizing the blank. Under the action of the rotation of the blank, the inner and outer wheels move in the radial and axial directions of the blank to spin the blank. The movement between the inner and outer wheels does not affect the operation of the heat supplement system. The spinning process and the heat supplement process do not interfere with each other, ensuring the realization of spinning and heating supplement during the workpiece forming process.

[0029] Furthermore, the roller motion grooves are provided on the top surface and the side surfaces of the furnace body to ensure that the roller assembly can independently and freely move in the radial and axial directions of the blank.

[0030] As a preferred embodiment of the present invention, the furnace body includes furnace body one and furnace body two, and the furnace body one and the furnace body two are arranged opposite to each other, and furnace cavity one is formed in the furnace body one, and furnace cavity two is formed in the furnace body two, and furnace cavity one and furnace cavity two form a furnace cavity of the furnace body, and the furnace body one and the furnace body two can be close to or away from the workbench. After the furnace body one and the furnace body two are close to each other, they form a furnace cavity, so that the blank is located in the effective temperature compensation zone; a first rotary wheel motion groove is provided on the furnace body one, and a second rotary wheel motion groove is provided on the furnace body two, and the first rotary wheel motion groove and the second rotary wheel motion groove form the rotary wheel motion groove.

[0031] In the above technical solution, the furnace body structure of the heat supplement system is a semi-closed movable split structure; the furnace body one and the furnace body two can be close to or away from the workbench, which is convenient for taking or placing the workpiece blank; when the blank is to be placed on the workbench or the blank is to be taken out of the workbench after spinning is completed, the furnace body one and the furnace body two are away from the workbench, and the furnace body is in an open state at this time; when the blank is fixed on the workbench of the spinning equipment, the furnace body one and the furnace body two are close to the workbench, and the furnace body is in a closed state, the furnace cavity one and the furnace cavity two form a furnace cavity, the first rotary wheel motion groove and the second rotary wheel motion groove form the rotary wheel motion groove, the rotary wheel assembly passes through the rotary wheel motion groove and is located in the rotary wheel motion groove, and an effective temperature supplement zone is provided in the furnace cavity. When the furnace body is closed, the blank is located in the effective temperature supplement zone, and the heat supplement system can accurately monitor and adjust the temperature of the effective temperature supplement zone through closed-loop control between the furnace body temperature measurement module, the heating module and the control module of the temperature control system, so that the effective temperature supplement zone provides a uniform temperature field to heat the blank.

[0032] As a more preferred embodiment of the present invention, the furnace body of the supplementary heat system is closed by the first and second furnace bodies approaching the workbench; and the furnace body of the supplementary heat system is opened by the first and second furnace bodies moving away from the workbench. The time taken for the furnace body to complete closing is controlled within 15 seconds, and the time taken for the furnace body to complete opening is controlled within 15 seconds. The furnace body structure of the supplementary heat system is a semi-enclosed movable split structure. The closing or opening of the furnace body is achieved by the first and second furnace bodies respectively moving closer to or away from the workbench. During the process of approaching or moving away from the workbench, the effective heating area is open, which will cause heat loss in the effective heating area. Therefore, the time to complete closing or opening needs to be strictly controlled to avoid excessive loss of ambient temperature in the effective heating area due to the opening of the furnace body.

[0033] As a more preferred embodiment of the present invention, the maximum target temperature of the supplemental heating system after the furnace is closed is consistent with the pre-spinning temperature required by the process. The set target temperature should fully account for the temperature rise effect caused by heat generated during the spinning deformation zone. The sum of the set spinning temperature and the temperature rise caused by heat generated during the deformation is the actual measured spinning temperature during the workpiece deformation process.

[0034] As a more preferred embodiment of the present invention, the first furnace body or the second furnace body is connected to the spinning equipment body via a sliding component or a hinged component, so that the first furnace body and the second furnace body can slide toward or away from the workbench, or the first furnace body and the second furnace body can rotate toward or away from the workbench. Through the above arrangement, a semi-enclosed effective temperature compensation zone is formed in the first furnace body and the second furnace body. Before the blank is transferred and clamped on the workbench, the first furnace body and the second furnace body are away from the workbench. After the blank is fixed, the first furnace body and the second furnace body are close to the workbench, forming an effective temperature compensation zone, and the blank is heated and compensated by the heating system until the blank reaches the spinning temperature.

[0035] As a more preferred embodiment of the present invention, the furnace body 1 and the furnace body 2 are semi-cylindrical cavity structures with a wall thickness of 50-100 mm.

[0036] As a preferred embodiment of the present invention, the blank temperature T is measured after the blank is clamped and fixed. 坯 and the temperature before spinning required by the process Contrast; if Start the supplementary heating system to heat the blank. The supplementary heating system will increase the heating power of the heating element, increase the temperature rise rate of the supplementary heating, and actively compensate the heating of the blank during the supplementary heating time to make the blank temperature reach the temperature before spinning. Then start the spinning equipment to start spinning the workpiece according to the predetermined spinning program; if The supplementary heating system is started to supplement the temperature of the blank, and at the same time, the spinning equipment is started to start spinning the workpiece according to the predetermined spinning program. The supplementary heating system will maintain the heating power of the heating element to keep the blank temperature within the spinning temperature range.

[0037] In the above technical solution, the heat of the blank heated to the spinning preheating temperature will be lost during the transfer process and the process of fixing it to the workbench, causing the blank temperature to drop, so that the blank temperature cannot reach the pre-spinning temperature. It is impossible to achieve near-isothermal hot spinning. By measuring the blank temperature T 坯 and the temperature before spinning required by the process Compare the results to determine whether to start spinning immediately or wait for the heating system to replenish the billet temperature to the pre-spinning temperature before starting spinning. 坯 Lower than the temperature before spinning required by the process The temperature of the blank decreases greatly during the transferring process and the process of being fixed to the workbench, and the temperature of the blank cannot meet the requirement of the start spinning temperature, so the heating system increases the heating power of the heating element, increases the temperature rising rate of the compensation heating, actively and quickly compensates and heats the blank within the specified compensation heating time, so as to offset the heat loss of the blank, and the temperature of the blank reaches the pre-spinning temperature. 坯 The temperature of the blank is higher than the pre-spinning temperature required by the process The temperature of the blank decreases slightly during the transferring process and the process of being fixed to the workbench, and the temperature of the blank can meet the requirement of the start spinning temperature, so the heating system maintains the heating power of the heating element, maintains the spinning temperature, and prevents the temperature of the blank from decreasing during the spinning process. At the same time when the heating system starts to compensate and heat the blank, the spinning equipment starts to spin the workpiece according to the predetermined spinning program.

[0038] As a more preferred scheme of the present application, the temperature of the effective compensation heating area of the heating system is not higher than the pre-heating temperature of spinning; if The heating system compensates and heats the blank, and the compensation heating time of the heating system is not more than 5 minutes. The spinning temperature of the workpiece made of different metal materials is different, and the corresponding compensation heating time is different. The compensation heating time is determined according to the processed metal material, so as to control the heating system. In the present application, the fixed blank is located in the effective compensation heating area of the heating system, and the holding temperature of the effective compensation heating area before the heating system is turned on should be lower than the pre-heating temperature of spinning, so as to prevent the temperature of the blank from increasing and causing microstructure defects, and the compensation heating time is controlled to be not more than 5 minutes. Therefore, the temperature rising rate of the heating compensation should be as fast as possible.

[0039] As a preferred scheme of the present application, the spinning equipment is further provided with a blank temperature measuring module for detecting the temperature of the blank located in the effective compensation heating area, so as to obtain the temperature T 坯 or the spinning temperature T 旋 of the blank.

[0040] In the above technical scheme, after the clamping is completed, the temperature of the blank is detected by the blank temperature measuring module, and the detected temperature of the blank is fed back to the heating system, so as to control the heating system to compensate and heat the blank. In addition, when the heating system comprises a furnace body and a temperature control system, the temperature control system comprises a furnace body temperature measuring module, a control module and a heating module, the furnace body temperature measuring module is used for detecting the temperature of the effective compensation heating area, and the furnace body temperature measuring module and the blank temperature measuring module cooperate to test the effective heating area and the temperature of the blank respectively, so as to obtain the real-time temperature of the effective compensation heating area for compensating and heating the blank, provide a basis for parameter adjustment of the heating system, stabilize the adjustment range of the heating system, and improve the stability and reliability of the heating system.

[0041] As a more preferred embodiment of the present invention, the blank temperature measurement module includes at least one infrared temperature measurement sensor, which is non-contact with the target blank. The infrared temperature measurement sensor is located between the blank and the heating element, and the infrared temperature measurement sensor always points to the blank. The installation of the infrared temperature measurement sensor will not affect the movement of the spinning assembly.

[0042] As a preferred embodiment of the present invention, the spinning temperature for a high-temperature alloy billet is 900-1150°C. The high-temperature alloy billet includes, but is not limited to, one of Waspaloy, GH4169, IN718, GH3536, IN783, IN625, and GH4698. The spinning temperature varies for different types of high-temperature alloys, and the spinning temperature range is determined by the specific material grade, but is generally within the range of 900-1150°C.

[0043] When spinning high-temperature alloy materials, as they are difficult-to-deform alloy materials, it is necessary to pay attention to avoid grain growth caused by excessively high temperatures, which will affect the mechanical properties of the material. At the same time, too low a forging temperature will increase the difficulty of spinning deformation and cause cracks in the workpiece. Therefore, in the present invention, a near-isothermal hot spinning process is adopted for the high-temperature alloy material. During the spinning forming, a heating system is used to heat the blank so that the spinning temperature fluctuation range of the blank is controlled within the range of ±20°C. The maximum and minimum values ​​of the spinning temperature are both within the spinning temperature range required by the process. Such a setting can ensure that the metal material has better deformation ability during the spinning process, reduce deformation resistance, improve forming quality and forming efficiency, and meet the workpiece manufacturing requirements. Accurately controlling the temperature during the spinning process is the key to ensuring the quality of high-temperature alloy forgings.

[0044] During the spinning process, the forming performance and final microstructure of the workpiece are optimized by controlling the spinning process parameters. In addition, after forming, the cooling rate of the workpiece has a significant impact on the final microstructure and performance.

[0045] As a preferred embodiment of the present invention, the spinning temperature for titanium alloy blanks is 700-900°C. The titanium-based alloy blanks include, but are not limited to, one of Ti6242, Ti64, TC11, TC4, TA12A, TA7, and TA15. The spinning temperature varies for different types of titanium alloys and is adjusted based on the phase transition temperature of the specific material grade to ensure high plasticity and low deformation resistance at the spinning temperature.

[0046] During the spinning process, the spinning temperature of the titanium alloy material at the beginning of spinning is usually higher than its β transformation temperature to ensure that the titanium alloy has good plasticity in the β phase region. At the same time, the spinning temperature before the end of spinning should be controlled within the α+β two-phase region to ensure the microstructure and mechanical properties of the forging. In addition, the spinning temperature range of titanium alloy is relatively narrow, which requires strict control of the heating time of the blank by the heating system during the spinning manufacturing process, so that the fluctuation range of the blank spinning temperature is controlled within the range of ±20℃ to avoid grain growth or the formation of other unfavorable microstructures.

[0047] As a preferred embodiment of the present invention, during near-isothermal hot spinning, a supplemental heating system is used to heat the blank, ensuring that the spinning temperature fluctuates within ±10°C from the start to the end of the spinning process. This more precise control of the spinning temperature reduces the deformation coefficient of the metal material and improves the consistency of the formed workpiece.

[0048] As a preferred embodiment of the present invention, during the process of spinning the blank using a near-isothermal hot spinning process, the blank rotation speed is 50 to 300 r / min; the spinning wheel feed ratio is 0.1 to 3 cm / r; the spinning wheel fillet radius is 0.3t to 2.5t, where t is the blank wall thickness, mm; the thinning rate per pass is 10 to 40%, and the thinning rate per pass should not be greater than the limit thinning rate of the metal material.

[0049] In the above technical solution, in order to ensure the mechanical properties and processing accuracy of the workpiece, the spinning process parameters are controlled during the spinning process. The spindle of the spinning equipment drives the workbench and the blank to rotate. The speed of the blank rotation is reasonably selected within the range of 50 to 300 rpm, and the feed ratio of the spinning wheel is reasonably selected within the range of 0.1 to 3 mm / rev. The radius of the spinning wheel corner is reasonably selected within the range of 0.3t to 2.5t. The thinning rate of each pass should not be greater than the limit thinning rate, and is generally selected within the range of 10 to 40%. After at least one spinning pass, the blank is spun to the design requirements of the workpiece. If the thinning rate does not exceed the limit thinning rate of the material in one spinning pass, If a single-pass spinning is used, the blank can meet the wall thickness and size requirements of the ring, and the spinning forming is completed; if the thinning rate of a single pass exceeds the limit thinning rate The spinning should be carried out in two passes, and the thinning rate of the first pass can be set as the limit thinning rate. If the second pass thinning rate also exceeds the limit thinning rate If the workpiece still does not reach the required thickness, it should be divided into three spinning passes, and so on, until the thickness of the workpiece meets the process requirements after the last spinning pass. During the spinning process, the forming performance and final microstructure of the workpiece are optimized by controlling the spinning process parameters.

[0050] As a preferred scheme of the present application, the spinning wheel assembly of the spinning equipment adopts staggered or non-staggered distance, when the staggered distance is adopted, the radial and axial staggered distances are selected according to the spinning process and the material of the workpiece; the spinning wheel mode adopts positive spinning or reverse spinning.

[0051] The present application also provides a metal workpiece, which is prepared by the near-isothermal hot spinning forming method.

[0052] As a preferred scheme of the present application, the workpiece cross section includes but is not limited to one suitable for the spinning process in rectangular workpieces, flange workpieces, I-shaped workpieces, L-shaped workpieces, long cylindrical workpieces, conical workpieces, special-shaped workpieces, etc.

[0053] The present application also provides a heating method for a heating system in near-isothermal hot spinning forming, which comprises the following steps: after the heated blank is transferred and clamped on the workbench rotating with the main shaft of the spinning equipment, the blank is located in the effective heating area of the heating system, the blank is heated and tempered by the heating system, the heating target temperature T 补 and the heating rate v of the heating system are set, so that the blank temperature T 坯 of the blank reaches the spinning pre-temperature required by the process The spinning pre-temperature is calculated according to the following formula:

[0054]

[0055] Wherein T 旋 is the measured spinning temperature in the spinning deformation zone during the spinning process of the workpiece, in ℃; ΔT is the temperature rise caused by the spinning deformation heat, in ℃;

[0056] After the blank temperature T 坯 of the blank reaches the spinning pre-temperature required by the process , the spinning equipment is started to spin according to the predetermined spinning program, and the blank is heated and tempered by the heating system to control the spinning temperature within the range required by the process, and the fluctuation range is not more than ±20℃ during the spinning deformation process.

[0057] As a preferred scheme of the present application, the calculation formula of ΔT is as follows:

[0058]

[0059] Wherein Q is the heat generated by plastic deformation, in J; m is the mass of the blank, in kg; C is the specific heat capacity of the blank material, in J / (kg·℃).

[0060] As a preferred scheme of the present application, the calculation formula of the heat Q generated by plastic deformation is as follows:

[0061]

[0062] Where θ is the thermal effect coefficient of deformation, which is generally taken as 0.9 in metal plastic deformation; is the equivalent stress at the deformation temperature. For the convenience of calculation, the yield strength σs of the material at the deformation temperature can be taken; is the equivalent strain rate of spinning deformation; the calculation formula of the equivalent strain rate is as follows:

[0063]

[0064] Where n is the spinning spindle speed, unit is r / min; is the spinning reduction rate, t0 and tf are the thickness of the blank before and after spinning, respectively, in mm.

[0065] Compared with the prior art, the present invention has the following beneficial effects:

[0066] 1. The hot spinning forming method provided by the present invention places the blank in the effective temperature compensation zone, measures the temperature of the blank after clamping and fixing before spinning, and judges whether the blank temperature meets the blank pre-spinning temperature required by the spinning process. If the blank temperature meets the blank pre-spinning temperature required by the process at this time, the spinning equipment is started for spinning; if the blank temperature is lower than the blank pre-spinning temperature required by the process at this time, the heating system is waited for to heat the blank to the blank pre-spinning temperature before spinning is started again. By starting the heating system to quickly heat up, the effective temperature compensation zone of the heating system continuously heats the blank to prevent the blank temperature from continuing to lose, so that the blank temperature reaches the spinning condition required by the process, that is, reaches the pre-spinning temperature, and at the blank temperature Spinning begins when the temperature reaches the temperature of the blank before spinning; during the spinning process, the heating system is continued to be used to heat the blank so that the temperature fluctuation range of the blank's spinning temperature from the beginning to the end of spinning does not exceed ±20°C, that is, the deformation temperature of the metal material during the forming process is maintained within a smaller fluctuation range by using a measurable and controllable heating system. Such a setting can ensure that the metal material has better deformation ability during the spinning process, reduce deformation resistance, improve forming quality and forming efficiency, and the consistency of the formed workpiece product is very good, which can meet the manufacturing requirements of high-precision workpieces. The technical solution of the present invention is suitable for difficult-to-deform metals with a narrow forming temperature range, and is also applicable to non-difficult-to-deform metals.

[0067] 2. The spinning equipment of the present invention integrates a heat supplement system and a rotary wheel system, which are arranged on the machine body. The rotary wheel assembly of the rotary wheel system locally pressurizes the blank, which can form the shape and size of the workpiece; the furnace body of the heat supplement system is a semi-closed structure, and a furnace cavity is formed in the furnace body, and heating elements are arranged in the furnace cavity. The arrangement of the heating elements forms an effective temperature supplement zone in the furnace body, and the blank is located in the effective temperature supplement zone, which can heat and supplement the temperature of the blank; at the same time, the furnace body of the heat supplement system is provided with a rotary wheel movement groove, and the rotary wheel assembly passes through the rotary wheel movement groove and is located in the rotary wheel movement groove, ensuring that the rotary wheel assembly can move independently in the radial and axial directions of the worktable, and the spinning process and the heat supplement process do not interfere with each other, thereby ensuring the realization of spinning and heating and supplementing temperature during the workpiece forming process.

[0068] 3. The furnace body and temperature control system of the heat supplement system of the present invention, the temperature control system includes a furnace body temperature measuring module, a control module and a heating module. The connection between the furnace body temperature measuring module, the heating module and the control module of the temperature control system constitutes a closed-loop temperature control system. Through the precise temperature measurement of the furnace body temperature measuring module, the temperature control of the control module and the precise regulation of the heating module, the temperature uniformity of the effective temperature supplement zone is achieved to be ±15°C, and the temperature control accuracy is ±1°C, which provides an equipment foundation for realizing precise control of the spinning temperature during the spinning process.

[0069] 4. The present invention adopts a heating system to heat and compensate the temperature of the blank during the spinning process, realizing a near-isothermal hot spinning process, which can improve the deformation coordination of the blank, and improve the forming quality and production efficiency of the workpiece. The results of the embodiment show that the near-isothermal hot spinning method of the present invention is used to spin-form high-temperature alloys or titanium alloys, and the resulting spun workpiece has uniform wall thickness, avoiding cracking of the workpiece during multiple spinning passes, and has good forming quality. Defects such as instability and wrinkling will not occur during the spinning process, and the risk of crack generation and grinding is also reduced. The mechanical properties of the workpiece obtained by spinning meet the performance requirements of the parts, while improving the organizational uniformity of the workpiece, and the grain size can reach level 7-9.

[0070] 5. The near-isothermal hot spinning forming method of the present invention can realize the forming of thin-walled workpieces by controlling the temperature and spinning process parameters. The process flow is simple and feasible, saving materials and reducing processing costs. At the same time, the temperature during the spinning deformation process is controllable and measurable, effectively improving the quality consistency and stability of the workpiece. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] Figure 1 This is a schematic cross-sectional view of the blank prepared in Example 1.

[0072] Figure 2 Schematic diagram of the cross section of the workpiece prepared in Example 1.

[0073] Figure 3It is a structural schematic diagram of the heat supplement system and the spinning wheel system of the spinning equipment of the present invention.

[0074] Figure 4 It is a cross-sectional schematic diagram of the opening and closing states of the heat supplement system of the spinning equipment of the present invention.

[0075] Figure 5 It is a top view schematic diagram of the heat supplement system and the spinning wheel system of the spinning equipment of the present invention.

[0076] Figure 6 This is a schematic cross-sectional view of the blank prepared in Example 2.

[0077] Figure 7 Schematic diagram of the cross section of the workpiece prepared in Example 2.

[0078] Figure numerals: 1-machine body, 2-workbench, 31-furnace body 1, 32-furnace body 2, 41-extrorotating wheel, 42-introrotating wheel, 5-blank, 6-workpiece. DETAILED DESCRIPTION

[0079] In order to more clearly describe the invention purpose, technical solutions and technical effect advantages in the specific implementation cases of the present invention, the solutions in the specific embodiments will be described in detail in conjunction with the drawings of the specification of the present invention. The specific technical solutions involved in the following specific embodiments are only for the purpose of clearly and completely describing the innovative technical solutions of the present invention. They themselves are only part of the specific implementation plans that can be adopted by the present invention, not all embodiments, and should not be understood as limiting the innovative solutions of the present invention. Any solution that adopts the same inventive concept of the present invention should be included in the scope of protection of the present invention.

[0080] Secondly, the descriptions of the drawings in the specific embodiments of the present invention are only for the purpose of facilitating technical personnel's understanding of the present invention. The details in the drawings are for the purpose of clearly presenting the technical solution. It should not be assumed that all technical features in the drawings must be included in the specific implementation cases, nor should the details in the drawings be considered as additional limitations on the innovative technical solution of the present invention. The components in the various embodiments described and shown in the drawings can be combined and arranged in different configurations. These changes in combination and arrangement should be considered as part of the entire embodiment of the innovative solution of the present invention and included in the scope of protection of the present invention.

[0081] In summary, the solutions or descriptions presented in the specific embodiments and drawings of the present invention are not intended to limit the scope of protection claimed, but merely represent selected embodiments / cases to help technicians understand the relevant innovative solutions. Based on these embodiments, all other equivalent or parallel embodiments obtained by those skilled in the art without inventive effort are also within the scope of protection claimed by the present invention.

[0082] It should be noted that, unless otherwise specified, in the description of the specific embodiments of the present invention, the terms indicating the orientation or positional relationship, such as "up", "down", "left", "right", "center", "inside", "outside", etc., are all based on the expression of the orientation or positional relationship shown in the accompanying drawings, or are the orientation or positional relationship in which the invented product / device / apparatus is placed when it is conventionally used. These terms of orientation or positional relationship are merely for the purpose of facilitating the description of the scheme of the present invention or simplifying the description in the specific embodiments to facilitate the rapid understanding of the scheme by technicians, and do not indicate or imply that a specific device / component / element must have a specific orientation, or be constructed and operated in a specific positional relationship, and therefore should not be understood as limiting the present invention.

[0083] Furthermore, in the description of the technical solutions of the present invention, unless otherwise expressly specified, defined, or limited, the terms "disposed," "installed," "connected," and "connected" should be understood broadly. For example, they may refer to fixed connections, detachable connections, or integral connections. They may be welded, riveted, bolted, threaded, or other commonly used connection methods in the art. Such connections may be mechanical or electrical, direct or indirect through an intermediate medium, or internally connected between two components.

[0084] Example 1

[0085] The blank material is high temperature alloy GH4169, and the initial wall thickness of blank 5 before spinning is 15 mm. Figure 1 As shown, the minimum wall thickness of the workpiece 6 after spinning is designed to be 10.5 mm. Figure 2 As shown, the spinning thinning rate is 30%. According to the production experience of hot spinning of nickel-based high-temperature alloys, the single-pass limit thinning rate is generally 50-60%. The maximum thinning rate of the workpiece is less than the limit thinning rate, and single-pass spinning can be used. The spinning design adopts one-pass spinning to 10.5mm, the deformation is 30%, and the spinning section length is increased from 145mm to 200mm. The workpiece spinning adopts near-isothermal hot spinning, and the spinning is carried out in the spinning equipment.

[0086] like Figure 3 、 Figure 4As shown, the spinning equipment integrates a heat supplement system and a rotary wheel system. A workbench 2 is installed on the main shaft of the spinning equipment body 1, and the main shaft can drive the workbench 2 to rotate. The heat supplement system includes a furnace body and a temperature control system. The temperature control system includes a furnace body temperature measuring module, a control module and a heating module. The heating module includes several heating rods; the furnace body structure is a semi-closed movable split structure, a furnace cavity is formed in the furnace body, and heating rods are arranged on the inner wall of the furnace cavity to form an effective temperature supplement zone in the furnace cavity. The furnace body includes furnace body 1 31 and furnace body 2 32, which are semi-cylindrical cavity structures. Furnace body 1 31 and furnace body 2 32 are arranged relative to each other. Furnace body 1 31 and furnace body 2 32 can be close to or away from the workbench 2, furnace cavity 1 is formed in furnace body 1 31, and furnace cavity 2 is formed in furnace body 2 32. When furnace body 1 31 and furnace body 2 32 are close to the workbench 1, the blank 5 is located in the effective temperature supplement zone; a first rotary wheel movement groove is provided on furnace body 1 31, The second rotary wheel groove is provided on the furnace body 32, and the first rotary wheel groove and the second rotary wheel groove form a rotary wheel groove. The rotary wheel system includes an inner rotary wheel 42 and an outer rotary wheel 41. When the rotary wheel assembly is working, the entire structure of the inner rotary wheel 42 and a partial structure of the outer rotary wheel 41 are in the effective temperature compensation area of ​​the heating system. The inner rotary wheel 42 is located on the inner side of the blank 5 and can abut the inner wall of the workpiece blank 5. The outer rotary wheel 41 is located on the outer side of the blank 5 and the outer rotary wheel 41 can abut the outer wall of the workpiece blank 5. The inner rotary wheel 42 and the outer rotary wheel 41 pass through the rotary wheel groove and are located in the rotary wheel groove. The inner rotary wheel 42 and the outer rotary wheel 41 can move freely in the radial and axial directions of the blank. The radial direction of the blank refers to the direction perpendicular to the central axis of the blank; the axial direction of the blank refers to the direction parallel to the central axis of the blank workpiece. The diameter and width of the rotary wheel groove should be larger than the diameters of the inner and outer rotary wheels. The rotary wheel groove is C-shaped, such as Figure 5 As shown, to prevent interference in the spinning process.

[0087] The spinning equipment is equipped with a control system for controlling the operation of the heating system and the spinning system. The spinning equipment is also equipped with a blank temperature measurement module, which is external to the heating system. The blank temperature measurement module is an infrared temperature sensor, which is used to detect the temperature of the blank in the effective heating zone and obtain the blank temperature T 坯 Or spinning temperature T 旋 .

[0088] During the spinning process, the billet temperature must reach the pre-spinning temperature required by the process before spinning can be started. The pre-spinning temperature is obtained based on experience or by using a calculation formula. The calculation formula is as follows:

[0089]

[0090] Where T 旋The spinning temperature is the measured spinning temperature in the spinning deformation zone during the workpiece spinning process, in °C. The spinning temperature can be obtained based on the thermal processing diagram corresponding to the workpiece material. The spinning temperature range for a specific metal material can be obtained from the material manual or thermal simulation test. ΔT is the temperature rise caused by the heat generated by spinning deformation, in °C. The calculation formula for ΔT is as follows:

[0091]

[0092] Where Q is the heat generated by plastic deformation, in J; m is the mass of the blank, in kg; C is the specific heat capacity of the blank material, in J / (kg·℃). The calculation formula for the heat Q generated by plastic deformation is as follows:

[0093]

[0094] Where θ is the thermal effect coefficient of deformation, which is generally taken as 0.9 in metal plastic deformation; is the equivalent stress at the deformation temperature. For the convenience of calculation, the yield strength σs of the material at the deformation temperature can be taken; is the equivalent strain rate of spinning deformation;

[0095]

[0096] Where n is the spinning spindle speed, unit is r / min; is the spinning reduction rate, t0 and tf are the thickness of the blank before and after spinning, respectively, in mm.

[0097] The near-isothermal hot spinning method includes the following steps:

[0098] (1) Use a heating device to heat the blank to the spinning preheating temperature of 1000°C. During the heating process, the set heating temperature of the heating device is 1000°C. The blank needs to be kept warm after being placed in the heating device. The holding time is calculated based on the wall thickness of the blank at 0.4 to 0.8 min / mm, so that the blank temperature reaches 1000°C;

[0099] (2) The target temperature of the heating system after the furnace body is closed is consistent with the spinning temperature required by the process. Before the blank is placed on the workbench, the furnace body 1 and the furnace body 2 of the heating system are moved away from the workbench to a certain distance so that the furnace body is opened. The time for opening the furnace body is controlled within 15 seconds.

[0100] The robotic arm quickly transfers the heated blank and clamps it on the workbench of the spinning equipment. After clamping, the furnace bodies 1 and 2 of the heating system are moved close to the workbench and the furnace bodies are quickly closed. The closing time of the furnace bodies is controlled within 15 seconds.

[0101] (3) The infrared temperature sensor detects the temperature of the blank at this time, and the control system sets the blank temperature T 坯 and the calculated temperature before spinning In contrast, if Start the supplementary heating system to heat the blank. The supplementary heating system will increase the heating power of the heating element, increase the temperature rise rate of the supplementary heating, increase the ambient temperature in the effective temperature zone of the supplementary heating system, and actively compensate for the blank heating during the supplementary heating time to make up for the temperature loss of the workpiece. If The heating system is started to heat the blank, and at the same time the spinning equipment is started to spin the workpiece according to the predetermined spinning program.

[0102] (4) The billet is spun into shape using a near-isothermal hot spinning process in the spinning equipment. The inner and outer spinning wheels spin the starting point of the spinning process according to the preset motion trajectory through the prefabricated groove motion knife on the furnace body of the supplementary heating system, and then start hot spinning according to the preset spinning trajectory. During the spinning process, the supplementary heating system is continued to heat the billet, and the deformation temperature in the spinning deformation zone of the billet, i.e., the spinning temperature, is monitored and recorded in real time, so that the spinning temperature fluctuates no more than ±20°C from the beginning to the end of spinning. The spinning process parameters are: the speed of the worktable driving the billet is 100 rpm; the feed ratio of the spinning wheel is 0.5-0.8 mm / rev; the radius of the spinning wheel corner is 1t; the pass thinning rate is 30%, and the spinning method adopts positive spinning.

[0103] Inspection of the formed parts revealed uniform wall thickness and no cracking defects. Mechanical properties of high-temperature alloy workpieces, as tested according to mechanical property testing standards, met the requirements in multiple test results. Furthermore, the grain size of the formed workpieces reached levels 7-9, demonstrating the high precision of the forming method, ensuring workpiece quality and meeting the reliability and durability requirements for various engineering applications.

[0104] Example 2

[0105] The blank material is Ti64 titanium alloy, and the initial wall thickness of the blank 5 before spinning is 26 mm. Figure 6 As shown, the wall thickness of the workpiece 6 after spinning is designed to be 15 mm, and the workpiece is a flanged workpiece, as shown in FIG. Figure 7 As shown, the spinning thinning amount is 42%, and the spinning design adopts two passes to spin to 15mm. The spinning of the workpiece adopts near-isothermal hot spinning, and the spinning of this embodiment is carried out in the spinning equipment of Example 1.

[0106] The temperature of Ti64 titanium alloy billet before spinning is obtained based on experience or calculated based on the relationship between spinning deformation temperature and deformation temperature rise. In this implementation, the spinning temperature T is obtained by referring to the Ti64 alloy thermal processing diagram and combining production experience. 旋 30-50℃ below the phase transition point, this embodiment selects T旋 is 900℃, so calculate the temperature of the blank before spinning The near-isothermal hot spinning method at about 870°C includes the following steps:

[0107] (1) The blank is heated to the spinning preheating temperature of 900°C using a heating device. During the heating process, the set heating temperature of the heating device is 900°C. The blank needs to be kept warm in the heating device. The holding time is calculated based on the wall thickness of the blank at 0.6 to 0.8 min / mm.

[0108] (2) The target temperature of the heating system after the furnace body is closed is consistent with the spinning temperature required by the process. Before the blank is placed on the workbench, the furnace body 1 and the furnace body 2 of the heating system are moved away from the workbench to a certain distance so that the furnace body is opened. The time for opening the furnace body is controlled within 15 seconds.

[0109] The robotic arm quickly transfers the heated blank and clamps it on the workbench of the spinning equipment. After clamping, the furnace bodies 1 and 2 of the heating system are moved close to the workbench and the furnace bodies are quickly closed. The closing time of the furnace bodies is controlled within 15 seconds.

[0110] (3) The infrared temperature sensor detects the temperature of the blank at this time, and the control system sets the blank temperature T 坯 and the calculated temperature before spinning In contrast, if Start the supplementary heating system to heat the blank. The supplementary heating system will increase the heating power of the heating element, increase the temperature rise rate of the supplementary heating, increase the ambient temperature in the effective temperature zone of the supplementary heating system, and actively compensate for the blank heating during the supplementary heating time to make up for the temperature loss of the workpiece. If The heating system is started to heat the blank, and at the same time the spinning equipment is started to spin the workpiece according to the predetermined spinning program.

[0111] (4) The billet is spun into shape using a near-isothermal hot spinning process in the spinning equipment. The inner and outer spinning wheels spin the starting point of the spinning process according to the preset motion trajectory through the prefabricated groove motion knife on the furnace body of the supplementary heating system, and then start hot spinning according to the preset spinning trajectory. During the spinning process, the supplementary heating system is continued to heat the billet, and the deformation temperature in the spinning deformation zone of the billet, i.e., the spinning temperature, is monitored and recorded in real time, so that the spinning temperature fluctuates no more than ±20°C from the beginning to the end of spinning. The spinning process parameters are: the speed of the worktable driving the billet is 180 rpm; the feed ratio of the spinning wheel is 1 to 1.2 mm / rev; the radius of the spinning wheel corner is 1t, the thinning rate per pass is 20 to 25%, and the spinning method adopts positive spinning.

[0112] Repeat the above steps and complete two spinning passes until the blank reaches the designed dimensions of the workpiece. According to the mechanical properties test standards of the titanium alloy workpiece, the mechanical properties of the workpiece meet the requirements in multiple test results, and the grain size of the formed workpiece can reach 7-9 levels.

[0113] For those skilled in the art, when understanding the solutions described in the specific embodiments of the present invention, they can refer to conventional technical manuals in the field. At the same time, for the places where the above-mentioned terms appear, they can make appropriate understanding or adjustments for reference, and deduce the implementation of the same or similar technical solutions without paying any creative work.

[0114] The above embodiments describe only the basic principles, main features and / or advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and the invention content of the specification only describe the principles or specific cases of the present invention. Without departing from the essence of the innovative ideas of the present invention, the innovative solutions of the present invention may be subject to various changes and improvements, and these changes and improvements all fall within the scope of protection claimed by the present invention.

Claims

1. A near-isothermal hot spinning method for a metal workpiece, characterized in that: The following steps are involved: Heat the blank to the spinning preheating temperature; The heated blank is transferred and clamped on a workbench that rotates with the main shaft of the spinning equipment. A supplementary heating system is installed on the periphery of the workbench, and the blank is located in an effective supplementary heating zone set by the supplementary heating system; Measure the temperature of the blank after clamping and determine the blank temperature T 坯 Whether the blank temperature before spinning T meets the process requirements b旋 , if T 坯 ≥T b旋 , then start the spinning equipment to start spinning; if T 坯 <T b旋 , the heating system is used to heat the blank to meet the temperature T 坯 ≥T b旋 , then start the spinning equipment to carry out spinning; In the spinning equipment, a near-isothermal hot spinning process is used to spin the blank. During near-isothermal hot spinning, a heating system is used to actively heat the blank and monitor the spinning temperature of the blank's spinning deformation zone in real time to ensure that the fluctuation range of the spinning temperature does not exceed ±20°C from the start to the end of the spinning deformation process.

2. The near-isothermal hot spinning method for a metal workpiece according to claim 1, characterized in that: The time taken to transfer the heated blank and clamp it on the workbench of the spinning equipment is taken as the transfer time, which is required to be no more than 90s.

3. The near-isothermal hot spinning method of a metal workpiece according to claim 1, characterized in that: The spinning equipment includes a machine body, a heat supplement system and a rotary wheel system. A workbench is installed on the main shaft of the machine body. The rotary wheel system includes a rotary wheel assembly. The heat supplement system includes a furnace body and a temperature control system. The temperature control system includes a furnace body temperature measuring module, a control module and a heating module. The heating module includes several heating elements. A furnace cavity is formed in the furnace body, and the heating elements are arranged on the inner wall of the furnace cavity to form an effective temperature supplement zone in the furnace cavity. A rotary wheel movement groove is provided on the furnace body, and the rotary wheel assembly passes through the rotary wheel movement groove to ensure that the rotary wheel assembly can move freely in the radial and axial directions of the blank. The furnace body temperature measuring module is used to detect the temperature of the effective temperature supplement zone. The furnace body temperature measuring module and the heating module are both electrically connected to the control module.

4. The near-isothermal hot spinning method of a metal workpiece according to claim 3, characterized in that: The roller assembly includes an inner roller and an outer roller. When the roller assembly is working, the entire structure of the inner roller and a partial structure of the outer roller are in the effective temperature compensation zone of the heat compensation system. The inner roller is located on the inner side of the blank and can abut the inner wall of the workpiece blank. The outer roller is located on the outer side of the blank and can abut the outer wall of the workpiece blank. The inner roller and the outer roller pass through the roller motion groove and are located in the roller motion groove, ensuring that the inner roller and the outer roller can move independently and freely in the radial and axial directions of the blank.

5. The near-isothermal hot spinning method of a metal workpiece according to claim 3, characterized in that: The furnace body includes furnace body one and furnace body two, and the furnace body one and furnace body two are arranged opposite to each other. The furnace body one and furnace body two can be close to or away from the workbench. When the furnace body one and the furnace body two are close to each other, they are closed to form a furnace cavity, so that the blank is located in the effective temperature compensation area of ​​the furnace cavity; the furnace body one is provided with a first rotary wheel motion groove, and the furnace body two is provided with a second rotary wheel motion groove, and the first rotary wheel motion groove and the second rotary wheel motion groove form the rotary wheel motion groove.

6. The near-isothermal hot spinning method of a metal workpiece according to claim 5, characterized in that: The furnace body 1 and the furnace body 2 close the furnace body of the supplementary heat system by approaching the workbench; the furnace body 1 and the furnace body 2 open the furnace body of the supplementary heat system by moving away from the workbench. The time taken for the furnace body to complete closing is controlled within 15 seconds, and the time taken for the furnace body to complete opening is controlled within 15 seconds.

7. The near-isothermal hot spinning method of a metal workpiece according to claim 1, characterized in that: Measure the blank temperature T after clamping and fixing the blank 坯 and the temperature before spinning T required by the process b旋 Contrast; if T 坯 <T b旋 , start and wait for the supplementary heating system to heat the blank. The supplementary heating system will increase the heating power of the heating element, increase the temperature rise rate of the supplementary heating, and actively compensate the blank for heating within the supplementary heating time specified in the process, so that the blank temperature reaches the pre-spinning temperature, and then start the spinning equipment to start spinning the workpiece according to the predetermined spinning program; if T 坯 ≥T b旋 , start the supplementary heating system to supplement the temperature of the blank, and at the same time start the spinning equipment to start spinning according to the predetermined spinning program. The supplementary heating system will maintain the heating power of the heating element to keep the blank temperature within the spinning temperature range.

8. The near-isothermal hot spinning method for a metal workpiece according to claim 7, characterized in that: The temperature of the effective heating zone of the heating system is not higher than the spinning preheating temperature; if T 坯 <T b旋 , start the supplementary heating system to heat the blank, and the supplementary heating time of the supplementary heating system does not exceed 5 minutes.

9. The near-isothermal hot spinning method for a metal workpiece according to claim 1, characterized in that: The spinning equipment is also provided with a blank temperature measuring module for detecting the temperature of the blank in the effective heating zone to obtain the blank temperature or the spinning temperature; the blank temperature measuring module is externally mounted on the heating system or the body of the spinning equipment.

10. The near-isothermal hot spinning method of a metal workpiece according to claim 1, characterized in that: During near-isothermal hot spinning, a supplementary heating system is used to heat the blank to ensure that the fluctuation range of the spinning temperature does not exceed ±10°C from the beginning to the end of the spinning deformation.

11. A near-isothermal hot spinning method for a metal workpiece according to any one of claims 1 to 10, characterized in that: For the blank of high temperature alloy material, the spinning temperature is 900~1150℃.

12. A near-isothermal hot spinning method for a metal workpiece according to any one of claims 1 to 10, characterized in that: For titanium alloy blanks, the spinning temperature is 700-900°C.

13. A near-isothermal hot spinning method for a metal workpiece according to any one of claims 1 to 10, characterized in that: During the process of spinning the blank using a near-isothermal hot spinning process, the blank rotation speed is 50 to 300 r / min; the spinning wheel feed ratio is 0.1 to 3 mm / r; the spinning wheel fillet radius is 0.3t to 2.5t, where t is the blank wall thickness; the thinning rate of each pass does not exceed the limit thinning rate of the blank material, and the thinning rate of each pass is 10 to 40%.

14. A metal workpiece, characterized in that: The workpiece is prepared by using a near-isothermal hot spinning method for a metal workpiece as described in any one of claims 1-13.

15. A metal workpiece according to claim 14, characterized in that: The workpiece is one of a rectangular workpiece, a flange workpiece, an I-shaped workpiece, an L-shaped workpiece, a long cylindrical workpiece, a tapered workpiece, and a special-shaped workpiece.

16. A method for replenishing heat in a heat replenishing system in near-isothermal hot spinning, characterized in that: The heat supplementation method comprises: After the heated blank is transferred and clamped on the workbench rotating with the main shaft of the spinning equipment, the blank is located in the effective heating zone of the heating system. The heating system is used to heat the blank. By setting the heating target temperature and heating rate of the heating system, the blank temperature T 坯 The temperature before spinning T that meets the process requirements b旋 , temperature before spinning T b旋 The calculation formula is as follows: T b旋 =T 旋 -ΔT Where T 旋 is the spinning temperature measured in the spinning deformation zone during the workpiece spinning process; ΔT is the temperature rise caused by the heat generated by spinning deformation; Billet temperature T 坯 The temperature before spinning T that meets the process requirements b旋 After that, start the spinning equipment and start spinning according to the predetermined spinning program. At the same time, start the heating system to heat the blank to make the spinning temperature within the range required by the process, and the fluctuation range does not exceed ±20℃ during the process from the beginning to the end of the spinning deformation.

17. The method for replenishing heat of a heat replenishing system in near-isothermal hot spinning according to claim 16, characterized in that: The calculation formula for ΔT is as follows: Where Q is the heat generated by plastic deformation; m is the mass of the blank; and C is the specific heat capacity of the blank material.

18. The method for replenishing heat of a heat replenishing system in near-isothermal hot spinning according to claim 17, characterized in that: The calculation formula for the heat Q generated by plastic deformation is as follows: Where θ is the deformation thermal effect coefficient; is the equivalent stress at deformation temperature; is the equivalent strain rate of spinning deformation.

Citation Information

Patent Citations

  • A precise temperature control method for hot spinning of thin-walled titanium alloy components

    CN103706716B

  • A Spin Forming Method for Titanium-Based Alloy Materials Based on Composite Heating

    CN109108139B

  • Precision temperature control system and precision temperature control spinning method for heating and spinning of metal materials

    CN111842603B

  • High-temperature thermal power spinning heating method and device

    CN106964682A

  • Titanium-based alloy material spinning forming method based on composite heating

    CN109108139A

Cited By

  • Spinning control method and system for magnesium alloy hot spinning three-wheel powerful spinning machine

    CN121696289A

  • Near-isothermal hot spin forming method and heat complementing method for metal workpiece

    EP4703057A1