Method for manufacturing raw glass sheet and method for manufacturing product glass sheet

By detecting and identifying frequent defect areas and setting exclusion areas, the problem of concentrated defects in the manufacture of original glass plates affecting the quality of electronic equipment is solved, and the reliability and quality of the product glass plates are improved.

CN120774638APending Publication Date: 2025-10-14NIPPON ELECTRIC GLASS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510327340.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-03
Filing Date
2025-03-19
Publication Date
2025-10-14

AI Technical Summary

Technical Problem

During the manufacturing process of glass original plates, when defects are concentrated along a specific direction, the product glass plates will affect the quality of electronic equipment. Existing technology cannot effectively suppress this problem.

Method used

Through the inspection process, defect information is recorded, frequent areas are identified and excluded areas are set, and product glass sheets that do not contain frequent areas are cut out. Frequent areas are set and removed using a combination of automation and manual methods to ensure the quality of product glass sheets.

Benefits of technology

It effectively suppresses the deterioration of the quality of electronic equipment caused by the product glass plate, improves the reliability and quality of the product glass plate, and reduces process time and material waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120774638A_ABST
    Figure CN120774638A_ABST
Patent Text Reader

Abstract

The invention provides a method for manufacturing a glass plate and a method for manufacturing a product glass plate, which can reliably suppress deterioration of quality of an electronic device due to a product glass plate cut from the glass plate. The method for manufacturing a glass sheet comprises: a detection step (S3) for detecting defects included in each continuously obtained glass sheet and recording defect information of the defects; and a determination step (S4) for determining, on the basis of the defect information, a cut-out pattern of a product glass plate that can be cut out from the raw glass plate. The determination step (S4) includes: a frequent occurrence determination step (S9) for determining, on the basis of the defect information, whether or not there is a frequent occurrence region in which defects occur frequently in the plurality of glass raw sheets; and an exclusion region setting step (S10) for setting a region including the frequent occurrence region as an exclusion region in which the product glass plate cannot be cut when the frequent occurrence region is generated. In a determination step (S4), the cut-out pattern excluding the region not included in the product glass plate is determined.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to a manufacturing method of a glass raw sheet and a manufacturing method of a product glass sheet. BACKGROUND

[0002] A glass sheet is used as a glass substrate, a cover glass in electronic devices such as displays. As such a glass sheet, a product glass sheet cut out from a glass raw sheet (also referred to as a mother glass) is generally used.

[0003] In addition, defects such as foreign matter, bubbles, and the like are sometimes contained in the glass raw sheet. Therefore, for example, Patent Literature 1 discloses that a defective defect having a high possibility of causing a fatal failure in an electronic device among defects contained in a glass raw sheet is not contained in a cut-out pattern of a product glass sheet.

[0004] In addition, in this document, it is disclosed that a judgment criterion of a pass defect and a fail defect is changed based on the number of one equivalent of a pass defect having a low possibility of causing a fatal failure in an electronic device among defects contained in a defective glass raw sheet.

[0005] PRIOR ART DOCUMENTS

[0006] PATENT LITERATURE

[0007] Patent Literature 1: Japanese Patent Application Publication No. 2020-121911 SUMMARY

[0008] PROBLEMS TO BE SOLVED BY THE INVENTION

[0009] In addition, a glass raw sheet is manufactured by cutting out a single sheet from a long glass ribbon continuously formed by a down-draw method, a float method, or the like. Defects are sometimes distributed in a specific direction such as a sheet drawing direction in a glass raw sheet thus manufactured. When such defects are distributed in a specific direction, even if the number of defects (for example, pass defects) equivalent to one sheet is not a problem, in a case where product glasses cut out from the glass raw sheet are assembled to electronic devices, the quality of the electronic devices is sometimes negatively affected.

[0010] The present application relates to a manufacturing method of a glass raw sheet and a manufacturing method of a product glass sheet. The present application relates to a manufacturing method of a glass raw sheet and a manufacturing method of a product glass sheet.

[0011] MEANS FOR SOLVING THE PROBLEMS

[0012] (1) To solve the above problems, the present application is a method for manufacturing a glass substrate, including: a cutting step of continuously cutting glass substrates from a glass ribbon; a detection step of detecting defects included in each of the cut glass substrates and recording defect information of the defects; and a determination step of determining a cutting pattern of a product glass sheet that can be cut from the glass substrates based on the defect information, by repeatedly performing the cutting step, the detection step, and the determination step, thereby determining the cutting pattern for each of a plurality of glass substrates that are continuously obtained, characterized in that the determination step includes: a frequency occurrence determination step of determining whether a frequency occurrence region in which defects frequently occur is generated in the plurality of glass substrates based on the defect information; and an exclusion region setting step of setting a region including the frequency occurrence region as an exclusion region in which the product glass sheet cannot be cut in a case where the frequency occurrence region is generated, and in the determination step, the exclusion region is determined not to be included in the cutting pattern of the product glass sheet.

[0013] In this way, the exclusion region including the frequency occurrence region in which defects frequently occur in the plurality of glass substrates is determined not to be included in the cutting pattern of the product glass sheet. Therefore, if the glass substrates are cut based on the determined cutting pattern, the product glass sheet in which defects that frequently occur in the plurality of glass substrates are not included can be obtained. Thus, if an electronic device is manufactured using the thus obtained product glass sheet, it is possible to reliably suppress a case where the quality of the electronic device is deteriorated due to the product glass sheet.

[0014] (2) In the structure of the above (1), it is preferable that the method for manufacturing a glass substrate include a forming step of forming a glass ribbon from molten glass, and the frequency occurrence region and the exclusion region are set as regions having a long strip shape extending in a drawing direction of the glass substrate.

[0015] As a result of the intensive research by the present inventors, it was known that the frequency occurrence region is generated in the drawing direction of the glass substrate more often due to the forming step or the like. Therefore, if the frequency occurrence region and the exclusion region are set as regions having a long strip shape extending in the drawing direction of the glass substrate, it is possible to reliably exclude defects that frequently occur in the plurality of glass substrates from the cutting pattern.

[0016] (3) In the structure of the above (2), it can also be that, with respect to a plurality of glass substrates for which the detection step is continuously performed, a plurality of small regions arranged in the drawing direction are set for each of the glass substrates, the number of defects included in a small region group composed of the corresponding small regions of each of the glass substrates is accumulated in the drawing direction for each position in a width direction orthogonal to the drawing direction, an accumulated defect distribution in which the position in the width direction in which the accumulated number of defects becomes equal to or greater than a set threshold value is found for each small region group, and the frequency occurrence region is set in the position in the width direction along the drawing direction in a case where the position in the width direction is consistent in each of the accumulated defect distributions.

[0017] Thus, the setting of the frequent area can be automated.

[0018] (4) In the structure of the above (2) or (3), it is preferable that, in the exclusion area setting step, a band-shaped area including the frequent area and larger than the frequent area on both sides in a width direction orthogonal to the pulling direction be set as the exclusion area.

[0019] Thus, the frequent area can be simply and reliably included in the exclusion area.

[0020] (5) In any one of the structures of the above (1) to (4), it can also be that, in a case where it is determined in the frequent area determination step that different multiple frequent areas are generated, multiple exclusion areas corresponding to the multiple frequent areas are set in the exclusion area setting step.

[0021] Thus, even in a case where different multiple frequent areas are generated, the exclusion area taking into account each frequent area can be set.

[0022] (6) In any one of the structures of the above (2) to (5), it can also be that, with respect to multiple glass substrates on which the detection step is continuously performed, multiple small areas arranged in the pulling direction are set for each glass substrate, the number of defects included in a group of small areas composed of the corresponding small areas of each glass substrate in the pulling direction is accumulated for each position in the width direction orthogonal to the pulling direction, an accumulated defect distribution in which the positions in the width direction are associated with each other is calculated for each group of small areas, and the manufacturing method of the glass substrate further includes a step of canceling the setting of the frequent area in a case where the accumulated number of defects at the position in the width direction corresponding to the frequent area in at least one accumulated defect distribution becomes below the cancellation threshold.

[0023] Thus, the cancellation of the frequent area can be automated.

[0024] (7) In the structure of the above (6), it is preferable that the manufacturing method of the glass substrate further include a step of canceling the setting of the exclusion area including the frequent area in a case where the setting of the frequent area is canceled.

[0025] Thus, the cancellation of the exclusion area can be automated.

[0026] (8) In any of the structures described in (1) to (7) above, preferably, the defect information includes the kind of defect and the position coordinates of the glass original plate in which the defect is detected, and further includes: a cumulative defect map production process of producing a cumulative defect map in which the kinds of defects are cumulatively produced in a form corresponding to the position coordinates of the defects, in a plurality of glass original plates in which the detection process is continuously performed; and a process of displaying the cumulative defect map using an image in which the defects are indicated with different marks for each kind of defect.

[0027] In this way, it is easy to confirm the state of defects that frequently occur in a plurality of glass original plates.

[0028] (9) In any of the structures described in (1) to (8) above, preferably, the defect information includes the kind of defect, and in the frequency occurrence determination process, the generation of the frequency occurrence region is determined based on the generation state of defects of which the kind is bubbles and foreign matter.

[0029] The kind of defects that are generated in a specific direction such as the drawing direction is frequently bubbles and foreign matter. Therefore, if the generation of the frequency occurrence region is determined based on these specific defects, the generation of the frequency occurrence region can be accurately detected.

[0030] (10) In any of the structures described in (1) to (9) above, preferably, the determination process further includes a defect classification process of classifying defects into acceptable defects or unacceptable defects, and in the determination process, with respect to the glass original plate that does not contain unacceptable defects, only the frequency occurrence determination process and the exclusion region setting process are performed based on acceptable defects.

[0031] In this way, it is possible to limit the object to which the frequency occurrence determination process and the exclusion region setting process are performed to the glass original plate that does not contain unacceptable defects, and thus it is possible to reduce the working hours required for these processes.

[0032] (11) In any of the structures described in (1) to (10) above, it can also be that the determination process further includes a defect classification process of classifying defects into acceptable defects or unacceptable defects, and in the frequency occurrence determination process, the generation of the frequency occurrence region is determined based on both acceptable defects and unacceptable defects.

[0033] In this way, the number of defects used to determine the generation of the frequency occurrence region increases, and thus it is possible to more accurately determine the generation of the frequency occurrence region.

[0034] (12) In any of the structures described in (1) to (11) above, preferably, the manufacturing method of the glass original plate includes a storage process of storing each cutout pattern classified by the case where the exclusion region is included in the cutout pattern of the product glass plate, in the determination process.

[0035] In this manner, the defects that frequently occur in the plurality of original glass plates can be taken into consideration, and the original glass plates can be classified and stored so that product glass plates can be easily cut out from the original glass plates.

[0036] (13) In any one of the above structures (1) to (12), it is preferred that the method for manufacturing the glass original plate includes a discarding step of discarding the glass original plate when it is determined in the judging step that the excluded area does not exist and is not included in the cut-out pattern of the product glass plate.

[0037] In this manner, the glass original plates can be discarded in consideration of the state in which defects frequently occur in the plurality of glass original plates.

[0038] (14) The present invention made to solve the above-mentioned problems is a method for manufacturing a product glass plate, characterized in that the method for manufacturing the product glass plate includes a process of executing a method for manufacturing a glass original plate having any one of the structures in (1) to (13) above, and the method for manufacturing the product glass plate also includes a precision cutting process of cutting the product glass plate from the glass original plate based on the cutting pattern when there is an excluded area not included in the cutting pattern of the product glass plate in the judgment process.

[0039] In this manner, product glass plates can be cut out from the glass original plates in consideration of the state of defects that frequently occur in the plurality of glass original plates.

[0040] Effects of the Invention

[0041] According to the present invention, it is possible to reliably suppress deterioration in the quality of electronic devices due to a product glass plate cut out from an original glass plate. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a flowchart showing a method for producing a glass original plate according to an embodiment of the present invention.

[0043] Figure 2 It is a perspective view showing a part of the manufacturing method of the glass original plate of this embodiment.

[0044] Figure 3 This is a conceptual diagram showing an example of a cumulative defect map.

[0045] Figure 4 This is a conceptual diagram showing an example of cumulative defect distribution in the width direction when a frequent occurrence region is set.

[0046] Figure 5 This is a conceptual diagram showing an example of cumulative defect distribution in the width direction when the setting of the frequent occurrence region is canceled.

[0047] Figure 6 This is a flowchart showing a method for producing a glass plate product according to another embodiment of the present invention.

[0048] Reference Signs List

[0049] 1 shaped body

[0050] 4 scribing tool

[0051] 7 conveying device

[0052] 8 scribing tool

[0053] 10 defect inspection device

[0054] 11 cumulative defect map

[0055] 13, 14 cumulative defect distribution

[0056] G1 first glass substrate

[0057] G2 second glass substrate

[0058] GM molten glass

[0059] GR glass ribbon

[0060] R1 frequent area

[0061] R2 exclusion area

[0062] S1 shaping step

[0063] S2 cutting step

[0064] S3 detecting step

[0065] S4 discriminating step

[0066] S7 cumulative defect map making step

[0067] S8 defect classifying step

[0068] S9 frequency determining step

[0069] S10 exclusion area setting step

[0070] S22, S25 disposal step

[0071] S23, S24, S26 storage step

[0072] S27, S28, S29 precision cutting step

[0073] X width direction

[0074] Y pulling direction DETAILED DESCRIPTION

[0075] Embodiments of the present application will be described below with reference to the accompanying drawings.

[0076] As Figure 1 shown, the manufacturing method of the glass raw plate of the present embodiment includes a forming step S1, a cutting step S2, a detecting step S3, and a discriminating step S4.

[0077] As Figure 2 shown, the forming step S1 is a step of forming a glass ribbon GR from a molten glass GM. In the forming step S1, the molten glass GM is supplied to a top portion of a wedge-shaped forming body 1 and is caused to overflow. After the overflowed molten glass GM flows down along side surface portions of the forming body 1, respectively, the molten glass GM is fused and integrated at a lower end portion of the forming body 1.

[0078] Thereby, the glass ribbon GR in a plate shape is formed. After that, the formed glass ribbon GR is drawn downward in a state of being sandwiched from both a front surface and a back surface by a pair of rollers (omitted from illustration) arranged in a plurality of stages in the vertical direction. A pair of cooling rollers (also referred to as edge rollers) is arranged at the uppermost stage of the pair of rollers arranged in a plurality of stages in the vertical direction. In the present embodiment, a drawing direction Y in the forming step S1 is set to be along the vertical direction.

[0079] The formed glass ribbon GR has a first main surface 2 and a second main surface 3. In the present embodiment, the glass ribbon GR is exemplified in which the first main surface 2 is a non-guaranteed surface and the second main surface 3 is a guaranteed surface. Here, the guaranteed surface is a surface in a product glass plate finally obtained from the glass ribbon GR, which is formed into an element or the like, and is a surface of which surface properties are guaranteed. The non-guaranteed surface is a surface of which surface properties can not be guaranteed to the extent of the guaranteed surface.

[0080] Ear portions having a larger thickness than a central portion in the width direction are formed at both end portions Ga of the glass ribbon GR, respectively. The thickness of the central portion in the width direction of the glass ribbon GR is 1000 μm or less, preferably 700 μm or less, and a lower limit value thereof is, for example, 50 μm or more.

[0081] The cutting step S2 includes a first cutting step S5 and a second cutting step S6.

[0082] The first cutting step S5 is a step of cutting out a first glass raw plate G1 from the glass ribbon GR formed in the forming step S1 by scribing in the width direction X. The first cutting step S5 includes a scribing step of forming a scribe line SL1 in the glass ribbon GR using a scribing tool 4, and a breaking step of imparting a bending stress to the glass ribbon GR on which the scribe line SL1 is formed and breaking it.

[0083] The first glass raw plate G1 is carried by a carrying device 7 to a position at which the second cutting step S6 can be performed (carrying step). The carrying device 7 is configured to carry the first glass raw plate G1 in a state in which the first glass raw plate G1 is held in a vertical attitude. The carrying device 7 has a holding portion 7a that holds an upper portion of the first glass raw plate G1.

[0084] The second cutting step S6 is a step of cutting both widthwise end portions Ga of the first glass original sheet G1 to obtain a second glass original sheet G2 without ear portions. The second cutting step S6 includes a scoring step of forming a score line SL2 on the first glass original sheet G1 using a scoring tool 8, and a breaking step of applying bending stress to the first glass original sheet G1 with the score line SL2 formed thereon to break the sheet.

[0085] The width dimension of the second original glass sheet G2 is, for example, 1500 mm or greater, preferably 2000 mm or greater, and more preferably 3000 mm or greater. Meanwhile, the upper limit can be, for example, 4000 mm or less. Furthermore, the width dimension of the second original glass sheet G2 in the drawing direction is, for example, 1500 mm or greater, preferably 2000 mm or greater, and more preferably 3000 mm or greater. Meanwhile, the upper limit can be, for example, 4000 mm or less.

[0086] The detection step S3 detects defects in each of the second original glass sheets G2 continuously cut from the glass ribbon GR and records defect information related to the defects. In the detection step S3, the defect inspection device 10 acquires defect information related to the defects in the second original glass sheets G2, including the type (bubbles, foreign matter, scratches, etc.), number, location coordinates, and size. This defect information is transmitted to a control device (not shown) along with identification information for the second original glass sheets G2.

[0087] The control device stores the defect information acquired by the defect inspection device 10 and, in the identification step S4 described below, performs various calculations based on the defect information to identify a cutout pattern for a product glass sheet that can be cut out from the second original glass sheet G2. The control device comprises, for example, a computer (e.g., a PC or control panel) equipped with various hardware components, such as a CPU, ROM, RAM, HDD, display device, and input / output interfaces.

[0088] The inspection step S3 is performed while the second glass original plate G2 is supported in a vertical position by the conveying device 7, but the present invention is not limited thereto. For example, the inspection step S3 may be performed while the second glass original plate G2 is supported in a horizontal position by another conveying device.

[0089] like Figure 1 As shown, the determination step S4 is a step of determining a cutout pattern of a product glass plate that can be cut out from the second glass original plate G2 based on the defect information obtained in the detection step S3. The determination step S4 is automatically performed by a computer, but at least a part of the step may be performed manually.

[0090] The discrimination process S4 is performed while the second glass substrate G2 is supported in the vertical attitude by the conveyance device 7, but is not limited thereto and can be performed while the second glass substrate G2 is supported in the horizontal attitude by another conveyance device.

[0091] In the discrimination process S4, the defect information of the one second glass substrate G2 on which the cutout pattern is discriminated and the defect information of the plurality of second glass substrates G2 continuously manufactured therebefore are used.

[0092] In detail, the discrimination process S4 includes an accumulated defect map creation process S7, a defect classification process S8, a frequency determination process S9, and an exclusion region setting process S10.

[0093] In the accumulated defect map creation process S7, an accumulated defect map in which the kinds of defects (bubbles, foreign matters, damages, and the like) are accumulated in a form in which the position coordinates (the coordinate in the drawing direction Y, the coordinate in the width direction X) in the second glass substrate G2 are associated with each defect is created from the plurality of second glass substrates G2 on which the detection process S3 is continuously performed. The number of second glass substrates G2 accumulated for creating the accumulated defect map is preferably, for example, 30 or more, and more preferably 50 or more. Thereby, the tendency of concentration of defects is easily expressed in the accumulated defect map. The number of second glass substrates G2 accumulated for creating the accumulated defect map is preferably, for example, 200 or less, and more preferably 150 or less. Thereby, the tendency of concentration of defects can be grasped as early as possible. The amount of defect information of the number of second glass substrates G2 accumulated can be accumulated when the accumulated defect map is created, but is not limited thereto. The defect information of the newest second glass substrate G2 can be added to the accumulated defect map, and the defect information of the oldest second glass substrate G2 included in the accumulated defect map can be removed from the accumulated defect map. The created accumulated defect map is displayed as an image on a display device (for example, a display) of a control device, for example.

[0094] In Figure 3An example of a cumulative defect map 11 is shown in FIG. The cumulative defect map 11 shows an area that reproduces the size of a second glass plate G2. In the cumulative defect map 11, for example, the position coordinates of each defect contained in the accumulated second glass plate G2 display a mark 12 of varying shapes depending on the defect type (e.g., a circular mark 12a for bubbles, a triangular mark 12b for foreign matter, etc.). Furthermore, in the cumulative defect map 11, the size of the defect is indicated by, for example, the color of the mark 12 (e.g., red for large sizes, yellow for medium sizes, blue for small sizes, etc.). In other words, the cumulative defect map 11 allows visual identification of the defect type, location, and size. In the illustrated cumulative defect map 11, the marks 12 representing bubbles or foreign matter within the defect are shown as concentrated along the sheet pulling direction Y. It should be noted that the cumulative defect map 11 may also include marks 12 representing defects other than bubbles and foreign matter.

[0095] like Figure 1 As shown, in the defect classification step S8, the defects detected in the inspection step S3 are classified as acceptable defects or unacceptable defects. Here, an acceptable defect is a defect that is determined to be acceptable based on a predetermined criterion and has a low probability of causing a fatal failure in the electronic device. An unacceptable defect is a defect that is determined to be unacceptable based on a predetermined criterion and has a high probability of causing a fatal failure in the electronic device. The predetermined criterion may also be different for each defect type.

[0096] In this embodiment, the predetermined criterion for determination is the size of the defect. Defects smaller than the predetermined determination size are considered acceptable defects, while defects larger than the predetermined determination size are considered unacceptable defects. The determination size is appropriately set based on the size and intended use of the final glass sheet. For example, if the defect is a bubble, the determination size is set within the range of 50 μm to 1000 μm, while if the defect is foreign matter, the determination size is set within the range of 20 μm to 500 μm. It should be noted that in the defect classification step S8, defects other than bubbles and foreign matter are also classified as acceptable or unacceptable defects.

[0097] In the frequent occurrence determination step S9, the presence or absence of defects (hereinafter referred to as specific defects) such as bubbles or foreign matter in the plurality of second glass original sheets G2 is determined based on the defect information. Figure 3 ) occurs. Specific defects often occur along the drawing direction Y when forming the glass ribbon GR using a downdraw method such as the overflow method or the float method. Therefore, in the frequent occurrence determination step S9, it is determined that the frequent occurrence region R1 often occurs along the drawing direction Y.

[0098] Here, the reason why the frequent occurrence region R1 is generated along the sheet drawing direction Y is considered to be that when a glass ribbon is formed by a down-draw method such as an overflow method or a float method, when an abnormality occurs in a portion of the width direction of the molten glass or the glass ribbon conveying path, a specific defect is likely to occur frequently along the sheet drawing direction in the portion of the glass ribbon that passes through the abnormal portion. Specifically, for example, Figure 2 In the overflow downdraw method shown, when a portion of the side surface of the forming body 1 where the molten glass GM flows in the width direction X is damaged or foreign matter is attached, a specific defect-prone region R1 may be generated along the drawing direction Y.

[0099] The presence or absence of the frequent occurrence region R1 and the position of the frequent occurrence region R1 may be determined manually by an operator based on the accumulated defect map 11 displayed on the display device of the control device, but in this embodiment, the determination is made automatically as follows.

[0100] First, for each of the plurality of second glass sheets G2 that have been continuously subjected to the inspection step S3, two small areas are set along the sheet pulling direction Y. Next, for each position in the width direction X, the number of specific defects contained in the small area group consisting of the corresponding small areas of each second glass sheet G2 is accumulated in the sheet pulling direction Y. For each small area group, a cumulative defect distribution corresponding to the position in the width direction X is calculated.

[0101] In this embodiment, as the same process as this, Figure 3 As shown, the cumulative defect map 11 is set with two small areas 11a and 11b arranged along the plate pulling direction Y. These small areas 11a and 11b correspond to the small area group mentioned above. Next, for each position in the width direction X, the number of specific defects (marks 12a and 12b) consisting of qualified defects contained in each small area 11a and 11b in the plate pulling direction Y is accumulated, as shown in FIG. Figure 4 As shown, cumulative defect distributions 13 and 14 are calculated for each of the small areas 11a and 11b, corresponding to the position in the width direction X. Specifically, a frequency curve is created for each of the small areas 11a and 11b, with the horizontal axis representing the position in the width direction X and the vertical axis representing the cumulative number of specific defects. The range of the levels can be, for example, set to be between 1 mm and 100 mm. Figure 4The illustrated cumulative defect distributions 13, 14 are obtained by linking the cumulative number of specific defects in each grade. Note that in this figure, the cumulative defect distribution 13 illustrates the cumulative defect distribution of the small region 11a, and the cumulative defect distribution 14 illustrates the cumulative defect distribution of the small region lib. The size of the draw direction Y of each small region 11a, lib is preferably the same. It is also possible to set three or more small regions arranged along the draw direction Y for the cumulative defect map 11, and to obtain the cumulative defect distribution of each small region.

[0102] Also, as illustrated in Figure 4 the cumulative defect distributions 13, 14, in a case where the position in the width direction X at which the cumulative number of specific defects composed of acceptable defects becomes equal to or greater than the set threshold value Tl coincides, it is automatically determined that the frequent region Rl is generated. Here, the case where the position in the width direction at which the cumulative number of specific defects becomes equal to or greater than the set threshold value Tl coincides in each cumulative defect distribution 13, 14 means a case where the range Xa in the width direction X at which the cumulative number of specific defects becomes equal to or greater than the set threshold value Tl in the cumulative defect distribution 13 and the range Xb in the width direction X at which the cumulative number of specific defects becomes equal to or greater than the set threshold value Tl in the cumulative defect distribution 14 overlap at least in part. The frequent region Rl is set to a range Xc common to the range Xa and the range Xb. Also, as illustrated in Figure 3 the range Xc, the frequent region Rl is automatically set in a strip shape along the draw direction Y. That is, the frequent region Rl is set to a region having an elongated shape extending in the length direction along the draw direction Y. Note that the frequent region Rl can also be set to a range Xd included in either of the range Xa and the range Xb. In addition, in a case where three or more small regions arranged along the draw direction Y are set for the cumulative defect map 11, the set conditions of the frequent region Rl are determined based on three or more cumulative defect distributions.

[0103] In the exclusion region setting process S10, in a case where the frequent region Rl is generated, a region including the frequent region Rl is set as the exclusion region R2 in which the product glass sheet cannot be cut out. In the present embodiment, as illustrated in Figure 3 the exclusion region R2 is set to a strip-shaped region including the frequent region Rl and larger than the frequent region Rl on both sides in the width direction X. The width ΔW by which the exclusion region R2 extends from one side in the width direction X of the frequent region Rl is, for example, 50 mm to 200 mm.

[0104] The exclusion region R2 can also be set manually in a case where the frequent region Rl is set, but in the present embodiment, it is automatically set in conjunction with the setting of the frequent region Rl.

[0105] Note that the frequent area R1 and the exclusion area R2 can be set in multiple numbers within the range of the second glass raw plate G2.

[0106] As shown in FIG. 6, in the determination step S4, the second glass raw plate G2 not including the unqualified defect is determined not to include the exclusion area R2 in the cutout pattern of the product glass plate in the determination step S4. Figure 1

[0107] In detail, in the determination step S4, first, based on the result of the defect classification step S8, it is determined whether the unqualified defect is included in the second glass raw plate G2 (step Sll).

[0108] As for the second glass raw plate G2 determined not to include the unqualified defect by the step Sll, it is determined whether the set condition of the frequent area Rl is satisfied (frequent determination step S9).

[0109] In the case where it is determined by the frequent determination step S9 that the set condition of the frequent area Rl is satisfied, the exclusion area R2 including the area is set (exclusion area setting step S10). Also, it is determined whether there is the cutout pattern of the second glass raw plate G2 not including the exclusion area R2 (step S12).

[0110] In the case where it is determined by the step S12 that there is the cutout pattern, the second glass raw plate G2 is rated based on the cutout pattern (step S13). In the present embodiment, a case where the second glass raw plate G2 is rated in three levels of, for example, a first grade, a second grade, and a third grade in order from a high quality for the variety of the second glass raw plate G2 will be described. In this case, as for the second glass raw plate G2 of the second glass raw plate G2 in which the exclusion area R2 is set and in which there is the cutout pattern, it is determined to be the second grade (step S13). The second glass raw plate G2 determined to be the second grade by the step S13 is subjected to the storage step S23 described later. Note that the quality of the second glass raw plate G2 belonging to the upper grade is better than the quality of the second glass raw plate G2 belonging to the lower grade, and substantially the same post-processing (for example, precision cutting) can be performed on the second glass raw plate G2 belonging to the same grade.

[0111] In the case where it is determined by the step S12 that there is no cutout pattern, the second glass raw plate G2 is determined to be the third grade (step S14). The second glass raw plate G2 determined to be the third grade by the step S14 is subjected to the disposal step S22 described later.

[0112] Also, in the case where it is determined by the frequent determination step S9 that the set condition of the frequent area Rl is not satisfied, it is determined whether another exclusion area R2 has been set (step S15).

[0113] ​In a case where it is determined in the step S15 that the other exclusion area R2 is not set, the second glass substrate G2 is determined as the first variety (step S16). In the second glass substrate G2 determined as the first variety, there is no unqualified defect, and there is also no frequent area R1 in which the specific defects frequently occur. The second glass substrate G2 determined as the first variety in the step S16 is subjected to the storage step S24 described later.

[0114] In a case where it is determined in the step S15 that the other exclusion area R2 is set, it is determined whether the release condition of the exclusion area R2 is satisfied (step S17).

[0115] In a case where it is determined in the step S17 that the release condition of the exclusion area R2 is satisfied, the setting of the exclusion area R2 is released (step S18), and the second glass substrate G2 is determined as the first variety (step S16).

[0116] In a case where it is determined in the step S17 that the release condition of the exclusion area R2 is not satisfied, it is determined whether the cutout pattern of the second glass substrate G2 excluding the exclusion area R2 exists (step S12). Based on the result, the second glass substrate G2 is determined as the second variety (step S13) or as the third variety (step S14) in the same manner as described above.

[0117] Here, the setting of the exclusion area R2 can be manually released in a case where the setting of the frequent area R1 included in the exclusion area R2 is released, but in the present embodiment, the setting of the exclusion area R2 is automatically released in conjunction with the release of the setting of the frequent area R1 included in the exclusion area R2. The setting of the frequent area R1 can be manually released in a case where the cumulative defect map 11 is displayed on the display device of the control device and the frequent area R1 is not considered as the specific defect, but in the present embodiment, the setting of the frequent area R1 is automatically released as follows.

[0118] First, with respect to a plurality of second glass substrates G2 for which the detection step S3 is continuously performed, two small areas arranged in the pull direction Y are set for each of the second glass substrates G2. Next, the number of the specific defects (bubbles, foreign matters) included in the small area group composed of the corresponding small areas of each of the second glass substrates G2 is accumulated in the pull direction Y for each position in the width direction X, and the cumulative defect distribution in which the position in the width direction X is associated is calculated for each of the small area groups.

[0119] In the present embodiment, as the same processing as this, as Figure 3As shown, two small regions 11a, 11b arranged in the pull tab direction Y are set to the cumulative defect map 11. The small regions 11a, 11b correspond to the above-described small region group. Next, the number of specific defects (marks 12a, 12b) included in each small region 11a, 11b is cumulated in the pull tab direction Y for each position in the width direction X, as shown in Figure 5 As shown, the cumulative defect distributions 13, 14 in which the positions in the width direction X are associated are obtained for each small region 11a, 11b. Note that, instead of two small regions 11a, 11b arranged in the pull tab direction Y, three or more small regions arranged in the pull tab direction Y can be set to the cumulative defect map 11, and the cumulative defect distributions of the small regions can be obtained.

[0120] Further, as shown in Figure 5 In the case where the cumulative number of specific defects of the position in the width direction X corresponding to the frequent region R1 in at least one of the cumulative defect distributions 13, 14 becomes equal to or less than the release threshold T2, the setting of the frequent region R1 is released. Note that, in the illustrated example, the case where the cumulative number of specific defects of the position in the width direction X corresponding to the frequent region R1 in both of the cumulative defect distributions 13, 14 becomes equal to or less than the release threshold T2 is illustrated. In the case where three or more small regions arranged in the pull tab direction Y are set to the cumulative defect map 11, the release condition of the setting of the frequent region R1 is determined based on the three or more cumulative defect distributions. Note that the release threshold T2 is set to a value smaller than the setting threshold T1.

[0121] As shown in Figure 1 In the discrimination process S4 of the present embodiment, in the case where it is determined that the second glass substrate G2 contains a defective defect (process S11), it is also determined whether there is a cutout pattern not containing the defective defect with respect to the second glass substrate G2 containing the defective defect (process S19). In the case where there is a cutout pattern, the second glass substrate G2 is determined to be a second variety (process S20). The second glass substrate G2 determined to be the second variety by the process S20 is subjected to the storage process S26 described later. On the other hand, in the case where there is no cutout pattern, the second glass substrate G2 is determined to be a third variety (process S21). The second glass substrate G2 determined to be the third variety by the process S21 is subjected to the disposal process S25 described later.

[0122] The glass substrate manufacturing method of the present embodiment further includes the storage processes S23, S24, S26 and the disposal processes S22, S25 after the discrimination process S4.

[0123] In the storage processes S23, S24, S26, the tray for the first variety, the tray for the second variety are prepared, respectively, and the second glass substrates G2 determined to be of the respective varieties by the determination process S4 are bundled in the trays corresponding to the respective varieties and stored. That is, the second glass substrates G2 bundled in the same tray and belonging to the same grade are subjected to substantially the same processing (for example, precision cutting) after the storage processes S23, S24, S26.

[0124] In the disposal processes S22, S25, the second glass substrates G2 determined to be of the third variety by the determination process S4 are disposed of. Note that the disposal processes S22, S25 can also be performed by causing the second glass substrates G2 to fall from the conveyance device 7 to the recovery chamber provided on the lower layer on the conveyance path of the conveyance device 7, or can also be performed by placing the disposed second glass substrates G2 on the tray prepared for recovery.

[0125] The present application is not limited to the structures of the above-described embodiments, nor to the above-described effects. The present application can be modified in various ways without departing from the gist thereof.

[0126] In the above-described embodiments, the case where it is determined in the frequent occurrence determination process S9 whether the frequent occurrence region R1 is generated based on only the specific defects (bubbles, foreign matter) composed of the acceptable defects has been described, but the kind of defects used to determine whether the frequent occurrence region R1 is generated is not limited thereto. For example, it can also be that it is determined whether the frequent occurrence region R1 is generated based on at least one defect selected from the specific defects composed of the acceptable defects, the specific defects composed of the unqualified defects, the defects other than the specific defects composed of the acceptable defects (damage, etc.), and the defects other than the specific defects composed of the unqualified defects. If it is determined whether the frequent occurrence region R1 is generated based on the specific defects composed of the acceptable defects and the specific defects composed of the unqualified defects among them, it is easy to detect the generation of the frequent occurrence region R1 along the pull plate direction Y as early as possible.

[0127] In the above-described embodiments, the case where it is determined in the determination process S4 whether the second glass substrate G2 has the unqualified defect (process S11) after the determination (processes S9, S10, S12, etc.) based on the exclusion region R2 is performed on the second glass substrate G2 has been described, but it is not limited thereto. For example, it can also be that it is determined whether the second glass substrate G2 has the unqualified defect (process S11) after the determination (processes S9, S10, S12, etc.) based on the exclusion region R2 is performed on the second glass substrate G2 in the determination process S4. In this case, in the determination process S4, the cutout pattern that does not contain both the unqualified defect and the exclusion region is determined.

[0128] In the above-described embodiment, a case where the second glass sheet G2 in which a defective defect exists is not subjected to the determination based on the exclusion area R2 (processes S9, S10, S12, etc.) is described, but the determination based on the exclusion area R2 can be performed on the second glass sheet G2 in which a defective defect exists in addition to the second glass sheet G2 in which a defective defect does not exist. In this case, in the determination process S4, the second glass sheet G2 in which a defective defect exists is determined not to include the cutout pattern of both the defective defect and the exclusion area.

[0129] In the above-described embodiment, a case where the frequent area Rl and the exclusion area R2 are set along the drawing direction Y of the second glass sheet G2 is described, but the frequent area Rl and the exclusion area R2 can be set along a specific direction other than the drawing direction Y such as the width direction X in a case where defects frequently occur along the specific direction in a plurality of second glass sheets G2. As a case where the frequent area Rl is generated along the width direction X, for example, a case where a cutting failure in the first cutting process S5 is caused by deterioration of the scribing tool 4 or the like can be cited.

[0130] In the above-described embodiment, the second glass sheets G2 of a prescribed number are accumulated when the cumulative defect map is created, but the present application is not limited thereto. The second glass sheets G2 produced within a prescribed time can be accumulated. The prescribed time can be, for example, 15 minutes or more and 90 minutes or less.

[0131] In the above-described embodiment, the second glass sheet G2 determined to be the first variety or the second variety by the determination process S4 is subjected to the storage processes S23, S24, S26, but the present application is not limited thereto. As shown in FIG. 6, instead of the storage processes S23, S24, S26, the precision cutting processes S27, S28, S29 can be performed. Figure 6

[0132] In the above-described embodiment, after the glass ribbon GR is formed from the molten glass GM in the forming process S l, the glass sheet is cut out from the glass ribbon GR by the cutting process S2, but the present application is not limited thereto. The glass sheet can be cut out from the glass ribbon GR after the glass ribbon GR is drawn from a glass roll wound in a roll shape.

[0133] In the above-described embodiment, in the exclusion area setting process S10, in a case where the frequent area Rl is generated, the exclusion area R2 is set as an area including the frequent area Rl and extending by a width ΔW on both sides of the frequent area Rl in the width direction X, but the present application is not limited thereto. The width ΔW by which the exclusion area R2 extends compared to the frequent area Rl can be different on the left and right of the frequent area Rl. That is, as long as the frequent area Rl is included, the position of the exclusion area R2 can be arbitrarily set.

[0134] ​Also, in a case where it is determined in the exclusion region setting step S10 that different multiple frequent-occurrence regions R1 are generated, a single exclusion region R2 is set in a manner that includes each of the frequent-occurrence regions R1 when the distance between the respective frequent-occurrence regions R1 is close.

Claims

1. A method for manufacturing a glass base plate, comprising: Cutting process: continuously cutting out glass sheets from the glass ribbon; An inspection step of inspecting defects contained in each of the cut glass original plates and recording defect information of the defects; and a determination step of determining a cutout pattern of a product glass plate that can be cut out from the original glass plate based on the defect information, By repeatedly performing the cutting step, the detecting step, and the distinguishing step, the cutout pattern is distinguished for each of the plurality of glass original plates obtained continuously. The method for manufacturing the glass original plate is characterized in that: The discrimination process includes: a frequency determination step of determining whether a frequent occurrence region where the defect frequently occurs occurs in the plurality of glass original plates based on the defect information; as well as an exclusion area setting step of, when the frequent occurrence area is generated, setting an area including the frequent occurrence area as an exclusion area from which the product glass sheet cannot be cut; In the judging step, it is judged that the excluded area is not included in the cutout pattern of the product glass sheet.

2. The method for producing a glass original plate according to claim 1, wherein: The method for manufacturing the glass raw plate includes a forming step of forming the glass ribbon from molten glass. The frequent occurrence area and the exclusion area are set as areas having a long strip shape extending along the pulling direction of the glass original plate.

3. The method for manufacturing a glass plate according to claim 2, wherein: For the plurality of glass original plates on which the inspection process is continuously performed, a plurality of small areas arranged along the pulling direction are set for each glass original plate. For each position in the width direction perpendicular to the plate pulling direction, the number of defects contained in the small area group consisting of the corresponding small areas of each glass original plate is accumulated in the plate pulling direction, and for each small area group, a cumulative defect distribution corresponding to the position in the width direction is calculated. When the positions in the width direction where the cumulative number of defects in each of the cumulative defect distributions becomes equal to or greater than a set threshold value are identical, the frequent occurrence region is set along the sheet pulling direction at the position in the width direction.

4. The method for producing a glass original plate according to claim 2 or 3, wherein: In the exclusion region setting step, a band-shaped region including the frequent occurrence region and larger than the frequent occurrence region on both sides in a width direction perpendicular to the pulling direction is set as the exclusion region.

5. The method for producing a glass original plate according to any one of claims 1 to 3, wherein When it is determined in the frequent occurrence determination step that a plurality of different frequent occurrence areas are generated, in the exclusion area setting step, a plurality of the exclusion areas corresponding to the plurality of frequent occurrence areas are set.

6. The method for manufacturing a glass plate according to claim 2, wherein: For the plurality of glass original plates on which the inspection process is continuously performed, a plurality of small areas arranged along the pulling direction are set for each glass original plate. For each position in the width direction perpendicular to the plate pulling direction, the number of defects contained in the small area group consisting of the corresponding small areas of each glass original plate is accumulated in the plate pulling direction, and for each small area group, a cumulative defect distribution corresponding to the position in the width direction is calculated. The method for manufacturing a glass original plate further includes the step of canceling the setting of the frequent occurrence region when the cumulative number of defects at positions in the width direction corresponding to the frequent occurrence region in at least one of the cumulative defect distributions becomes equal to or smaller than a cancellation threshold.

7. The method for producing a glass original plate according to claim 6, wherein: The method for manufacturing the glass original plate further includes a step of canceling the setting of the exclusion area that was set to include the frequent occurrence area when the setting of the frequent occurrence area is canceled.

8. The method for producing a glass original plate according to any one of claims 1 to 3, wherein The defect information includes the type of the defect and the coordinates of the position of the defect in the original glass plate where the defect is detected. The discrimination process further comprises: a cumulative defect map creating step of creating a cumulative defect map by accumulating the types of defects in a form corresponding to the position coordinates of the defects in the plurality of glass original plates that have been continuously subjected to the inspection step; and and displaying the cumulative defect map using an image in which the defects are represented by different marks for each type of the defects.

9. The method for producing a glass original plate according to any one of claims 1 to 3, wherein The defect information includes the type of the defect, In the frequent occurrence determination step, the occurrence of the frequent occurrence region is determined based on the occurrence status of the defect, namely, bubbles and foreign matter.

10. The method for producing a glass original plate according to any one of claims 1 to 3, wherein The determination step further includes a defect classification step of classifying the defect as a qualified defect or a failed defect. In the determination step, the frequent occurrence determination step and the exclusion area setting step are performed on the glass original plate that does not include the unacceptable defect based only on the acceptable defect.

11. The method for producing a glass base plate according to any one of claims 1 to 3, wherein: The determination step further includes a defect classification step of classifying the defect as a qualified defect or a failed defect. In the frequent occurrence determination step, the presence or absence of the frequent occurrence region is determined based on both the acceptable defect and the unacceptable defect.

12. The method for producing a glass original plate according to any one of claims 1 to 3, wherein: The method for manufacturing a glass original plate includes a storing step of classifying and storing the product glass plate for each cutout pattern when the excluded region is not included in the cutout pattern in the determination step.

13. The method for producing a glass original plate according to any one of claims 1 to 3, wherein: The method for manufacturing a glass original plate includes a discarding step of discarding the glass original plate when the excluded region is not included in the cutout pattern of the product glass plate in the determining step.

14. A method for manufacturing a glass plate product, characterized in that: The method for manufacturing the product glass plate comprises the steps of performing the method for manufacturing the original glass plate according to any one of claims 1 to 3, The method for manufacturing a product glass sheet further includes a precision cutting step of cutting the product glass sheet from the original glass sheet based on the cutting pattern when the exclusion area is not included in the cutting pattern of the product glass sheet in the determining step.

Citation Information

Patent Citations

  • Method of manufacturing glass substrate

    JP2020121911A