A method for repairing thin-walled aluminum cylinder barrels

By employing a multi-round flame scanning, filler coating, and graded grinding method on the cylinder barrel of thin-walled aluminum cylinders, the problem of unrepairable thin-walled aluminum cylinder barrels has been solved, achieving efficient and low-cost repair results and extending the service life of the cylinders.

CN120886115BActive Publication Date: 2026-11-17SHANDONG YUNNEI POWER CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511277207.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-09-09
Publication Date
2026-11-17
Estimated Expiration
2045-09-09

AI Technical Summary

Technical Problem

Existing technologies cannot effectively repair damage to thin-walled aluminum cylinder barrels, resulting in high maintenance costs and long downtime. Traditional repair methods cannot meet deformation control requirements, making complete replacement the mainstream solution.

Method used

The cylinder barrel was fixed and the damaged area was cleaned. After multiple rounds of flame scanning, cleaning and drying, a filler was applied and the cylinder barrel was polished three times. The cylinder barrel was gradually restored to its shape and surface quality by combining sandpaper of different grits with petroleum jelly for protection.

Benefits of technology

This technology enables efficient repair of thin-walled aluminum cylinder barrels, reducing maintenance costs, shortening maintenance time, extending cylinder lifespan, and ensuring the sealing and smooth operation of the cylinder barrel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of cylinder repair technology, and more particularly to a method for repairing thin-walled aluminum cylinder barrels. The method includes: fixing the cylinder barrel and cleaning the damaged area on the inner wall; grinding the damaged area; performing multiple rounds of flame scanning on the ground area, with the time for each scan decreasing as the number of scans increases; cleaning and drying the heated area; applying a filler to the damaged area and allowing it to cure; and performing three grinding processes sequentially: after the first curing, grinding with coarse sandpaper until the piston can push and pull without jamming; after the second curing, grinding with fine sandpaper until flush with the undamaged area; and after the third curing, grinding with water-moistened polishing sandpaper to a set roughness range. This invention overcomes the limitation that thin-walled cylinder barrels cannot be repaired after damage due to their thin walls or deformation, effectively improving repair efficiency, shortening repair time, and saving repair costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cylinder repair technology, and in particular to a method for repairing the cylinder barrel of a thin-walled aluminum cylinder. Background Technology

[0002] Aluminum thin-walled cylinders, with their lightweight design and corrosion resistance, are widely used in automated equipment, pneumatic machinery, and other applications. Their working principle involves the reciprocating motion of a piston within the cylinder to convert mechanical energy. The cylinder's inner wall must maintain a high-precision roughness to ensure sealing and smooth movement. However, during use, the long-term, high-frequency piston motion leads to wear and scratches on the cylinder.

[0003] Because thin-walled aluminum has low hardness and high thermal conductivity, traditional turning repair can lead to uneven wall thickness or excessive thermal deformation. Existing repair processes are only suitable for thick-walled iron cylinders and cannot meet the deformation control requirements of thin-walled aluminum cylinders. Therefore, the mainstream treatment for damage to thin-walled aluminum cylinders in the industry is to replace the entire cylinder, which is costly and results in long downtime. Summary of the Invention

[0004] To address the shortcomings of existing technologies, the purpose of this invention is to provide a method for repairing thin-walled aluminum cylinder barrels. This method overcomes the limitation that thin-walled cylinder barrels cannot be repaired after damage due to their thin walls and deformation. It can effectively improve repair efficiency, shorten repair time, save repair costs, and avoid the need for complete replacement during repair.

[0005] To achieve the above objectives, the embodiments of the present invention provide the following technical solutions: A method for repairing a thin-walled aluminum cylinder barrel includes: fixing the cylinder barrel and cleaning the damaged area on the inner wall of the cylinder barrel; grinding the damaged area of ​​the cylinder barrel; performing multiple rounds of flame scanning on the ground area, with the time for each scan decreasing as the number of scans increases; cleaning and drying the heated area; applying a filler to the damaged area and allowing it to cure; and performing three grinding operations in sequence: after the first curing, grinding with coarse sandpaper until the piston pushes and pulls smoothly; after the second curing, grinding with fine sandpaper until it is flush with the undamaged area; and after the third curing, grinding with water-wet polishing sandpaper to a set roughness range.

[0006] Optionally, an oxy-fuel cutting torch can be used to perform flame scanning on the cylinder grinding area, and the flame of the oxy-fuel cutting torch can be controlled to be a neutral flame.

[0007] Optionally, the single scan time of the flame scan satisfies the following: the first scan duration is longer than the second scan duration is longer than the subsequent scan duration, and the first scan duration does not exceed 1.5 seconds.

[0008] Optionally, the duration of the second scan shall not exceed 1 second, and the duration of subsequent scans shall not exceed 0.5 seconds.

[0009] Optionally, AB glue can be used as a filler, and the thickness should be higher than the undamaged part of the cylinder inner wall.

[0010] Optionally, the curing process of the filler includes: the first sanding is performed with 80-grit sandpaper 1 hour after curing, the second sanding is performed with 600-grit sandpaper 2 hours after curing, and the third sanding is performed with pure water and then with 2000-grit sandpaper 24 hours after curing.

[0011] Optionally, after polishing, apply petroleum jelly to the inside of the cylinder barrel to form a protective film on the inner wall of the cylinder barrel.

[0012] Optionally, a parameter adaptation step may also be included: Measure the minimum wall thickness of the cylinder barrel; The basic number of scans is obtained by referring to a parameter comparison table based on cylinder model, minimum wall thickness, and damage depth. Calculate the maximum duration of a single scan based on the minimum wall thickness; The scanning speed is dynamically adjusted based on the real-time temperature during the scanning process.

[0013] Optionally, the maximum duration of a single scan is obtained by subtracting the product of the difference between the minimum wall thickness and the reference wall thickness and the compensation coefficient from the reference time value, wherein the compensation coefficient is 0.5s / mm.

[0014] Optionally, it also includes parameter optimization steps: record the actual number of scans and the highest temperature, and after verification by air pressure sealing test, update the parameter comparison table when the effective data of the same model cylinder reaches the set number.

[0015] One or more technical solutions provided in the embodiments of the present invention have at least the following technical effects or advantages: This invention discloses a method for repairing thin-walled aluminum cylinder barrels. Fixing the cylinder barrel prevents deformation during processing; cleaning the damaged area removes surface impurities, laying the foundation for subsequent processing; grinding the damaged area eliminates scratches and expands the treatment area, facilitating filler adhesion; multiple rounds of flame scanning with decreasing single-scan time gradually remove penetrating lubricating oil and control cylinder barrel temperature, preventing deformation due to overheating; cleaning and drying remove heating residues; after applying the filler, three stages of grinding are performed, with the three-stage grinding coordinated with the curing progress: the first rough grinding eliminates geometric interference, the second fine grinding restores dimensional accuracy, and the third polishing achieves surface functional adaptation. Multi-stage curing and progressively increasing grit sandpaper synergistically control filler shrinkage stress, preventing interlayer peeling. This repair method solves the problem of thin-walled aluminum cylinder barrels being irreparable and requiring replacement due to their thin walls and susceptibility to deformation, achieving effective repair, reducing repair costs, and shortening repair time.

[0016] Advantages of additional aspects of the invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Detailed Implementation

[0017] It should be noted that the following detailed description is illustrative and intended to provide further explanation of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0018] Example 1 This embodiment proposes a method for repairing aluminum thin-walled cylinder barrels, including: fixing the cylinder barrel and cleaning the damaged area on the inner wall of the cylinder barrel; grinding the damaged area of ​​the cylinder barrel; performing multiple rounds of flame scanning on the ground area, with the single scanning time decreasing as the number of scans increases; cleaning and drying the heated area; applying a filler to the damaged area and curing it; and performing three grinding operations in sequence: after the first curing, grinding with coarse sandpaper until the piston pushes and pulls without jamming; after the second curing, grinding with fine sandpaper until it is flush with the undamaged area; and after the third curing, grinding with water-wet polishing sandpaper to the set roughness range.

[0019] First, the cylinder barrel was secured and the damaged area on the inner wall was cleaned, ensuring the precision and effectiveness of subsequent operations and providing a good foundation for the repair work. Next, the damaged area of ​​the cylinder barrel was ground to remove burrs and irregularities, preparing for subsequent filling and smoothing.

[0020] Then, multiple rounds of flame scanning are performed on the polished area, with the time for each scan decreasing as the number of scans increases. This ensures effective heating while avoiding localized overheating of the cylinder due to prolonged heating, which could affect the overall performance of the cylinder. Flame scanning effectively removes oil and impurities from the inner wall of the cylinder and simultaneously performs a certain degree of heat treatment on the cylinder surface, improving its surface activity and facilitating the adhesion of fillers.

[0021] Cleaning and drying the heated area ensures that the filler can adhere tightly to the inner wall of the cylinder, improving the quality of the repair.

[0022] A filler is applied to the damaged area and cured. The filler is used to fill the damaged parts of the cylinder, restoring the shape and dimensional accuracy of the cylinder. Through the curing process, the filler forms a whole with the inner wall of the cylinder, enhancing the structural strength of the cylinder.

[0023] The process involves three sanding operations, each using a different grit of sandpaper and performed at specific time points. After the first curing, coarse sandpaper is used until the piston moves smoothly without jamming, quickly removing excess filler and ensuring a smoother fit between the filled area and the piston. After the second curing, fine sandpaper is used until the filler is flush with the undamaged area, further improving the smoothness of the filled area and creating a more natural transition with the surrounding undamaged areas. After the third curing, water-moistened polishing sandpaper is used to achieve the desired roughness on the cylinder wall, ensuring surface smoothness without excessively weakening the cylinder's strength, while simultaneously improving the wear resistance and corrosion resistance of the cylinder wall.

[0024] The above steps work together to solve the problems faced in the repair of thin-walled aluminum cylinder barrels, achieve efficient repair of damaged cylinder barrels, extend the service life of cylinders, reduce repair costs, and shorten repair time.

[0025] The cylinder grinding area is flame-scanned using an oxy-acetylene torch, with the torch flame controlled to be neutral. A neutral flame provides stable core temperature and a clear outline, while the reduction zone has lower brightness. This provides sufficient heat to remove lubricating oil seeping into the cylinder wall without causing localized overheating due to excessive flame intensity. It is well-suited to the material characteristics of thin-walled aluminum cylinders, preventing cylinder deformation during heating and ensuring the adhesion of subsequent filler. Combined with the grinding and filling steps, this enhances the reliability of the repair.

[0026] The single-scan time of the flame scan meets the following requirements: the first scan duration is longer than the second scan duration, which is longer than subsequent scan durations, and the first scan duration does not exceed 1.5 seconds. The 1.5-second upper limit for the first scan ensures the vaporization of the base oil film, and the subsequent scan times decrease to adapt to the heat accumulation effect. Once the cylinder temperature gradient is established, shortening the heating time can maintain the effective temperature window and prevent overheating.

[0027] Furthermore, the duration of the second scan does not exceed 1 second, and the duration of subsequent scans does not exceed 0.5 seconds. As the number of scans increases, the amount of residual lubricating oil in the cylinder decreases. Shortening the time avoids unnecessary heat input, especially for thin-walled cylinders, allowing for more precise temperature control and preventing localized overheating that could lead to deformation. This aligns with the need for gradual lubricating oil removal, ensuring that each scan is efficient and safe.

[0028] Specifically, AB glue can be used as the filler, applied to a thickness higher than the undamaged area of ​​the cylinder inner wall. After curing, AB glue has a certain strength and sealing properties, making it suitable for repairing aluminum cylinders. Applying it to a thickness higher than the undamaged area allows for subsequent grinding, ensuring that after secondary and tertiary grinding, it will be flush with the surface of the undamaged area. This, combined with the tertiary grinding step, ensures that the repaired cylinder inner wall is smooth and continuous, meeting the requirements of cylinder movement and solving the problem of thin-walled cylinders being unable to be repaired by turning.

[0029] The curing process of the filler includes: the first sanding is performed with 80-grit sandpaper 1 hour after curing, the second sanding is performed with 600-grit sandpaper 2 hours after curing, and the third sanding is performed with pure water and then with 2000-grit sandpaper 24 hours after curing.

[0030] The curing and polishing process is adapted to the curing characteristics of AB adhesive and the requirements of cylinder repair: After 1 hour of curing, the AB adhesive has a certain strength. At this time, polishing with 80-grit sandpaper can quickly remove excess material, ensuring smooth piston movement in the filled area. After 2 hours of curing, the adhesive further hardens, and fine polishing with 600-grit sandpaper can make the filled area flush with the undamaged area. After 24 hours of curing, the adhesive reaches high strength and stability. At this time, wetting with water and polishing with 2000-grit sandpaper can achieve the required roughness range for the cylinder inner wall, improving surface quality and wear resistance. The time intervals between each polishing step and the selection of sandpaper grit fully consider the curing stages of the AB adhesive and the usage requirements of the aluminum cylinder, ensuring that the roughness of the cylinder inner wall after repair meets the usage requirements, thus ensuring the reliability and durability of the repair effect.

[0031] After polishing, apply petroleum jelly to the inside of the cylinder. Petroleum jelly can form a protective film on the inner wall of the cylinder, isolating air, moisture and dust, preventing the inner wall of the repaired cylinder from being corroded or contaminated. In particular, it protects the smooth surface after polishing before assembly, extends the service life of the repaired cylinder, maintains the surface quality after repair, and improves the stability of the cylinder in use.

[0032] The detailed steps are as follows: Preparations before S100 maintenance: S101 Material Preparation: Based on the repair requirements, prepare the following materials: seals of the appropriate specifications, petroleum jelly, AB glue, 80-grit sandpaper, 600-grit sandpaper, 2000-grit sandpaper, purified water, 1 bottle of oxygen, 1 bottle of acetylene, etc.

[0033] S102 Tool Preparation: Prepare the necessary repair tools, such as wrenches, screwdrivers, rubber mallets, gas cutting guns, bench vises, cotton cloths, etc.

[0034] S200 Repair Process: S201 disassembles the cylinder, placing the piston rod (including the piston), front end cap, cylinder barrel, and rear end cap separately, without disassembling all undamaged parts of the cylinder, thus maintaining the integrity of each component.

[0035] After wrapping the cylinder barrel with a damp cotton cloth, S202 uses a bench vise to fix it, and the force should be controlled so that the cylinder barrel is not deformed while clamping it.

[0036] S203 cleans the inside of the cylinder with a cotton cloth and checks the extent of damage from scratches on the inside of the cylinder.

[0037] S204 uses 80-grit sandpaper to polish the damaged area inside the cylinder. The polishing range extends 10mm outward from the edge of the damage, and the oil film used for lubrication on the surface should be polished as clean as possible.

[0038] After connecting the S205 gas cutting torch to oxygen and acetylene, ignite it. The flame is controlled in a neutral state, with a distinct outline (nearly cylindrical) for the flame core. The flame core is composed of acetylene and oxygen, and its end has a uniformly round and shiny outer shell composed of red-hot carbon particles. The temperature of the flame core reaches 1000℃. The reduction zone is located outside the flame core and is significantly dimmer in brightness.

[0039] Because the S206 cylinder has a certain oil film adhering to its inner side, and as the cylinder is used for a long time, a small amount of lubricating oil will seep into the cylinder wall, a neutral flame gas cutting torch is used to scan and heat the damaged grinding area on the inner side of the cylinder to remove the lubricating oil that has seeped into the cylinder wall, so as to ensure subsequent repair.

[0040] The heating of the cylinder's inner side using a neutral flame gas cutting torch is controlled as follows: the initial flame scan dwell time should not exceed 1.5 seconds, with a cooling interval of 35 seconds; the second flame scan dwell time should not exceed 1 second, with a cooling interval of 20 seconds; the third and subsequent scans should not exceed 0.5 seconds, with a cooling interval of 10 seconds for each scan; a total of 8 flame scans are performed (the number of flame scans is determined based on the cylinder's usage time and the degree of lubricant penetration, until the lubricant at the damaged area of ​​the cylinder's inner wall is completely cleaned). The overall requirement is to ensure that the cylinder's inner wall temperature does not exceed 230℃ to guarantee the yield stress after cylinder repair.

[0041] S207 cleans the damaged area on the inner wall of the cylinder with clean water and then dries it.

[0042] S208 Apply the AB adhesive evenly to the damaged area on the inner wall of the cylinder according to the usage instructions, ensuring that the thickness of the AB adhesive application is slightly higher than that of the undamaged area on the inner wall of the cylinder. The AB adhesive can be a high-temperature resistant epoxy resin, such as AG-80, with a shear strength ≥18MPa after curing and a long-term service temperature ≤180℃.

[0043] After the S209 AB glue has cured for 1 hour, use 80-grit sandpaper for the first rough sanding. After sanding, use a piston without a seal to perform a push-pull test to ensure there is no jamming.

[0044] After the S210 AB glue has cured for 2 hours, use 600-grit sandpaper for a second fine sanding. After sanding, ensure that the damaged area is level with the undamaged area.

[0045] After the S211 AB glue has cured for 24 hours, it is moistened with pure water and then sanded for the third time with 2000-grit sandpaper. The roughness after sanding reaches Ra0.2-Ra0.5μm, while the roughness of the cylinder inner wall is Ra0.4-Ra0.6μm, which meets the usage requirements.

[0046] After S212 is polished, apply Vaseline to the inner wall of the cylinder to form a protective film.

[0047] S213 involves disassembling the cylinder components, replacing the seals, and then reassembling them.

[0048] Example 2 The main difference between this embodiment and Embodiment 1 lies in the grinding range and the flame scanning process. The detailed steps are as follows: Preparations before S100 maintenance: S101 Material Preparation: Based on the repair requirements, prepare the following materials: seals of the appropriate specifications, petroleum jelly, AB glue, 80-grit sandpaper, 600-grit sandpaper, 2000-grit sandpaper, purified water, 1 bottle of oxygen, 1 bottle of acetylene, etc.

[0049] S102 Tool Preparation: Prepare the necessary repair tools, such as wrenches, screwdrivers, rubber mallets, gas cutting guns, bench vises, cotton cloths, etc.

[0050] S200 Repair Process: S201 disassembles the cylinder, placing the piston rod (including the piston), front end cap, cylinder barrel, and rear end cap separately, without disassembling all undamaged parts of the cylinder, thus maintaining the integrity of each component.

[0051] After wrapping the cylinder barrel with a damp cotton cloth, S202 uses a bench vise to fix it, and the force should be controlled so that the cylinder barrel is not deformed while clamping it.

[0052] S203 cleans the inside of the cylinder with a cotton cloth and checks the extent of damage from scratches on the inside of the cylinder.

[0053] S204 uses 80-grit sandpaper to polish the damaged area inside the cylinder. The polishing range extends 15mm outward from the edge of the damage, and the oil film used for lubrication on the surface should be polished as clean as possible.

[0054] After connecting the S205 gas cutting torch to oxygen and acetylene, ignite it. The flame is controlled in a neutral state, with a distinct outline (nearly cylindrical) for the flame core. The flame core is composed of acetylene and oxygen, and its end has a uniformly round and shiny outer shell composed of red-hot carbon particles. The temperature of the flame core reaches 1000℃. The reduction zone is located outside the flame core and is significantly dimmer in brightness.

[0055] Because the S206 cylinder has a certain oil film adhering to its inner side, and as the cylinder is used for a long time, a small amount of lubricating oil will seep into the cylinder wall, a neutral flame gas cutting torch is used to scan and heat the damaged grinding area on the inner side of the cylinder to remove the lubricating oil that has seeped into the cylinder wall, so as to ensure subsequent repair.

[0056] The heating of the cylinder's inner side using a neutral flame gas cutting torch is controlled as follows: Initial flame scan dwell time should not exceed 1.3 seconds, with a 30-second cooling interval; second flame scan dwell time should not exceed 0.8 seconds, with a 15-second cooling interval; third flame scan dwell time should not exceed 0.8 seconds, with a 15-second cooling interval; fourth and subsequent scans should not exceed 0.5 seconds, with an 11-second cooling interval for each scan; a total of 7 flame scans are performed (the number of scans depends on the cylinder's usage time and the degree of lubricant penetration, until the lubricant at the damaged area of ​​the cylinder's inner wall is completely cleaned). The overall requirement is to ensure the cylinder's inner wall temperature does not exceed 230℃ to guarantee the yield stress after cylinder repair.

[0057] S207 cleans the damaged area on the inner wall of the cylinder with clean water and then dries it.

[0058] S208 Apply the AB adhesive evenly to the damaged area on the inner wall of the cylinder according to the usage instructions, ensuring that the thickness of the AB adhesive application is slightly higher than that of the undamaged area on the inner wall of the cylinder. The AB adhesive can be a high-temperature resistant epoxy resin, such as AG-80, with a shear strength ≥18MPa after curing and a long-term service temperature ≤180℃.

[0059] After the S209 AB glue has cured for 1 hour, use 80-grit sandpaper for the first rough sanding. After sanding, use a piston without a seal to perform a push-pull test to ensure there is no jamming.

[0060] After the S210 AB glue has cured for 3 hours, use 600-grit sandpaper for a second fine sanding. After sanding, ensure that the damaged area is level with the undamaged area.

[0061] After the S211 AB glue has cured for 24 hours, it is moistened with pure water and then sanded for the third time with 2000-grit sandpaper. The roughness after sanding reaches Ra0.2-Ra0.5μm, while the roughness of the cylinder inner wall is Ra0.4-Ra0.6μm, which meets the usage requirements.

[0062] After S212 is polished, apply Vaseline to the inner wall of the cylinder to form a protective film.

[0063] Example 3 Differences in cylinder wall thickness lead to different heat conduction rates, and different cylinder usage times and environments result in different oil penetration thicknesses. Fixing the number of flame scans, flame scan time, and cooling interval can easily cause local overheating or insufficient cleaning, which in turn leads to insufficient cylinder sealing and durability after repair.

[0064] Based on this, this embodiment further includes a parameter adaptation step: Measuring the minimum wall thickness of the cylinder barrel can identify the weakest point, avoid the risk of overheating, and provide a basis for subsequent parameter settings.

[0065] Based on the cylinder model, minimum wall thickness, and damage depth, a parameter comparison table is used to obtain the basic scanning time and cooling interval. A preliminary scanning plan is then determined based on the specific conditions of the cylinder.

[0066] The maximum duration of a single scan is calculated based on the minimum wall thickness to accommodate the thermal conductivity differences of cylinders with different wall thicknesses. This avoids localized overheating of the cylinder due to excessively long scan times or too short intervals, ensuring heating effectiveness while protecting the cylinder.

[0067] The scanning speed is dynamically adjusted based on the real-time temperature during scanning, enabling precise control of the heating process and improving the uniformity and efficiency of heating.

[0068] The parameter adaptation process solves the problem that fixed parameters can easily lead to local overheating or insufficient cleaning, making the repair process better adaptable to the characteristics and damage conditions of different cylinders, improving repair quality and consistency, and reducing reliance on operator experience. This is especially significant for cylinders with uneven wall thickness or complex damage.

[0069] The maximum duration of a single scan is obtained by subtracting the product of the difference between the minimum wall thickness and the minimum wall thickness and a compensation coefficient of 0.5 s / mm from the reference time value. Considering the influence of cylinder wall thickness on heat conduction, the maximum duration of a single scan can be accurately calculated based on the actual wall thickness difference of the cylinder by setting the reference time value and the compensation coefficient. For cylinders with thinner walls, the scan time and cooling interval are reduced accordingly to avoid overheating; for cylinders with thicker walls, the scan time and cooling interval are appropriately extended to ensure heating effect. Quantifying the wall thickness factor allows for a suitable maximum scan time for cylinders with different minimum wall thicknesses, improving the accuracy and applicability of the flame scanning procedure.

[0070] In cases where it is difficult to determine the relationship between the cylinder wall thickness and the maximum duration of a single scan and the cooling interval, the maximum duration of a single scan and the cooling interval can be appropriately reduced for the first and second single scans and the cooling interval, and the second single scan and the cooling interval can be repeated once more to achieve the requirement of increasing the local temperature of the cylinder wall. The duration of the fourth scan and the cooling interval remain unchanged. The purpose is to force out the oil stains that have seeped into the cylinder wall to achieve a cleaning effect.

[0071] The cylinder repair method also includes parameter optimization steps: record the actual scanning time, cooling interval time and number of scans, and after verification by air pressure sealing test, update the parameter comparison table when the effective data of the same model cylinder reaches the set number.

[0072] During the maintenance process, key parameters such as actual scanning time, cooling interval time, and number of scans are recorded to provide data support for subsequent parameter optimization. Pneumatic seal testing verifies the maintenance effect, ensuring the accuracy and effectiveness of the recorded parameters. Once a sufficient amount of valid data on the same cylinder model has been accumulated, the parameter comparison table is updated, continuously refining the maintenance parameter settings to better suit actual maintenance needs and cylinder characteristics. This enables continuous optimization and improvement of maintenance parameters, enhancing the adaptability and reliability of maintenance methods, contributing to improved maintenance quality and efficiency, and reducing maintenance costs.

[0073] The detailed steps are as follows: S2061 Cylinder wall thickness δ: Use a laser micrometer to measure the wall thickness δ at the middle and end of the cylinder to be repaired, and take the minimum value δ. min By determining the thinnest wall thickness point, the risk of overheating can be avoided.

[0074] S2062 retrieves historical process parameters: based on cylinder model, δ min For the depth of damage d, query the pre-stored parameter lookup table to obtain the basic number of scans N. base The amount can be increased or decreased appropriately depending on the different thicknesses of oil stain penetration caused by different usage times and environments of the cylinder.

[0075] Table 1 Parameter Comparison Table:

[0076] S2063 Infrared Temperature Measurement Module Installation: A high-temperature resistant infrared temperature measurement probe is installed on the side of the flame core of the gas cutting torch. The working temperature is >1000℃, and the probe axis forms a 30° angle with the flame core to monitor the temperature T of the cylinder heating point in real time.

[0077] S2064 calculates the maximum single scan time t max : t max =T0-(δ min -K0)×K1; Where, δ min : Minimum wall thickness measured; T0: Reference scan time, taken as 1.5s; K0: Reference wall thickness, taken as 1.0mm; K1: Wall thickness compensation coefficient, taken as 0.5s / mm. For example: when δ min When = 1.2mm, t max =1.5-(1.2-1.0)×0.5=1.4s.

[0078] S2065 performs adaptive flame scanning: based on N obtained in S2062 base Values ​​are scanned, but the time for each scan is dynamically adjusted according to the following rules: If T < 200℃, reduce the scanning speed to 0.8 times the standard speed and extend the heating time; if 200℃ ≤ T ≤ 220℃, maintain the standard scanning speed; if T > 220℃, immediately accelerate to 1.5 times the standard speed and trigger a buzzer alarm; Termination condition: Complete N base No oil stains were found in the second scan or the damaged area of ​​the cylinder.

[0079] S2066 records actual process parameters: stores the δ value of this maintenance. min d, actual number of scans N actual Maximum temperature T max .

[0080] S2067 Verification of Repair Quality: Perform a pneumatic seal test; if it passes, mark the set of parameters as valid data.

[0081] S2068 Updated Parameter Comparison Table: If the same model of cylinder accumulates ≥5 sets of valid data, then according to δ min Recalculate N for the interval d base .

[0082] While the specific embodiments of the present invention have been described above, they are not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art without creative effort based on the technical solutions of the present invention are still within the scope of protection of the present invention.

Claims

1. A method for repairing the cylinder barrel of a thin-walled aluminum cylinder, characterized in that, include: Secure the cylinder and clean the damaged areas on the inner wall of the cylinder. Polish the damaged area of ​​the cylinder barrel; The polishing area is subjected to multiple rounds of flame scanning, and the time for a single scan decreases as the number of scans increases; Clean and dry the heating area; Apply a filler to the damaged area and allow it to cure; Perform three polishing processes in sequence: After the first curing, polish with coarse sandpaper until the piston can be pushed and pulled without jamming; after the second curing, polish with fine sandpaper until it is flush with the undamaged area; after the third curing, polish with water-wet polishing sandpaper until the set roughness range is reached. The duration of a single flame scan meets the following requirements: the duration of the first scan is greater than the duration of the second scan is greater than the duration of subsequent scans, and the duration of the first scan does not exceed 1.5 seconds, with a cooling interval of 35 seconds. The duration of the second scan shall not exceed 1 second, and the cooling interval shall be 20 seconds; the duration of subsequent scans shall not exceed 0.5 seconds, and the cooling interval for each scan shall be 10 seconds. A total of 8 flame scans were performed; The curing process of the filler includes: the first sanding is performed with 80-grit sandpaper 1 hour after curing, the second sanding is performed with 600-grit sandpaper 2 hours after curing, and the third sanding is performed with pure water and then with 2000-grit sandpaper 24 hours after curing.

2. The method for repairing aluminum thin-walled cylinder barrels as described in claim 1, characterized in that, The cylinder grinding area is scanned with a gas cutting torch, and the flame of the gas cutting torch is controlled to be a neutral flame.

3. The method for repairing aluminum thin-walled cylinder barrels as described in claim 1, characterized in that, The filler used is AB glue, and the thickness of the coating is higher than the undamaged area of ​​the cylinder inner wall.

4. The method for repairing aluminum thin-walled cylinder barrels as described in claim 1, characterized in that, After polishing, apply petroleum jelly to the inside of the cylinder barrel, which will form a protective film on the inner wall of the cylinder barrel.

Citation Information

Patent Citations

  • Repair process for cylinder barrel of hydraulic oil cylinder

    CN105773062A

  • Repair technology of hydraulic post barrel

    CN106499419A