High-flame-retardant high-thermal-conductivity low-viscosity organic silicon pouring sealant and preparation method thereof
By combining modified vermiculite, nano-boron nitride, and micron-sized alumina, a highly flame-retardant, highly thermally conductive, and inefficient organic material was prepared, solving the technical problems that could not be solved in the existing technology. This resulted in a highly flame-retardant, low-viscosity organic material, which solved the technical problems that could not be solved in the existing technology, and achieved the technical problem of potting and sealing high-flame-retardant, low-viscosity organosilicon potting and sealing materials, thus realizing efficient technical application.
Patent Information
- Application Number
- CN202510639762.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-19
- Publication Date
- 2025-12-09
AI Technical Summary
Existing silicone potting compounds suffer from problems such as difficulty in balancing flame retardancy and thermal conductivity, poor processing flowability, insufficient mechanical properties, and poor environmental performance, making it difficult to meet the high requirements of modern electronic devices.
By using modified vermiculite, nano-boron nitride, and micron-sized alumina as components in vinyl-terminated silicone potting compounds, combined with ultrasonic dispersion and crosslinking technology, a high flame-retardant, high thermal conductivity, and low viscosity silicone potting compound was prepared, achieving a balance between flame retardancy and thermal conductivity, and possessing good mechanical properties and environmental friendliness.
It achieves a high flame retardancy rating of UL94V-0, a thermal conductivity greater than 2.0 W/(m·K), a viscosity reduced to 4,000-6,000 mPa·s, a compression modulus of 3-5 MPa, and an elongation at break greater than 50%. It possesses good processing fluidity and mechanical strength, making it suitable for potting electronic devices.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of organosilicon potting compound technology, and relates to a high flame retardant, high thermal conductivity, and low viscosity organosilicon potting compound and its preparation method. Background Technology
[0002] With the rapid development of electronic technology, electronic devices are becoming increasingly integrated and power-density is constantly increasing, placing higher demands on the heat dissipation and protection performance of these devices. Silicone potting compounds, as commonly used materials for electronic packaging, are widely used in the electronics field due to their excellent electrical insulation, weather resistance, and flexibility. However, existing silicone potting compounds have many problems in practical applications:
[0003] The conflict between flame retardancy and thermal conductivity: To meet the fire safety requirements of electronic equipment, traditional silicone potting compounds typically require the addition of a large amount of flame retardant. However, the addition of a large amount of flame retardant occupies the space of the filler, compressing the amount of thermally conductive filler added, resulting in a low thermal conductivity of the potting compound, generally below 1.5 W / (m·K). This makes it difficult to quickly dissipate the heat generated by electronic equipment, easily causing localized overheating and affecting the service life and performance stability of the equipment.
[0004] Poor processing fluidity: To improve the flame retardancy and thermal conductivity of potting compounds, it is often necessary to increase the filler content. However, with the increase of filler content, the viscosity of the potting compound will increase significantly, usually exceeding 10,000 mPa·s. The high viscosity makes it difficult for the potting compound to fill into the complex microstructure of electronic devices during the potting process, easily generating defects such as bubbles and voids, and failing to achieve effective encapsulation and protection of electronic components.
[0005] Insufficient mechanical properties: The cross-linking structure of traditional silicone potting compounds is not stable enough. When subjected to external impact or vibration, the potting compound is prone to deformation or even cracking, which cannot provide reliable mechanical support and protection for electronic components and seriously affects the normal operation of electronic equipment in harsh environments.
[0006] Environmental issues: Some traditional silicone potting compounds use flame retardants containing halogens or heavy metals. During the production, use, and disposal of these potting compounds, these harmful substances are released into the environment, causing pollution to the ecological environment. This does not conform to the current trend of green and environmentally friendly development and relevant regulatory requirements.
[0007] Therefore, developing an organosilicon potting compound and its preparation method that simultaneously possess high flame retardancy, high thermal conductivity, low viscosity, and excellent mechanical properties is of great significance for promoting the sustainable development of the electronics industry. Summary of the Invention
[0008] The purpose of this invention is to overcome the shortcomings of the prior art and provide a high flame retardant, high thermal conductivity, and low viscosity silicone potting compound and its preparation method, solving the problems of traditional potting compounds such as difficulty in balancing flame retardant and thermal conductivity properties, poor processing fluidity, insufficient mechanical properties, and poor environmental performance.
[0009] The high flame retardant, high thermal conductivity, and low viscosity silicone potting compound of the present invention is composed of two components, A and B, and auxiliary agents.
[0010] Component A comprises 40-60 parts by weight of vinyl-terminated silicone oil, 40-50 parts by weight of nano-boron nitride, and 3-6 parts by weight of modified vermiculite. Vinyl-terminated silicone oil serves as the base polymer of the potting compound, imparting excellent flexibility and electrical insulation properties. Nano-boron nitride possesses extremely high thermal conductivity, making it a key component for achieving the high thermal conductivity of the potting compound. The modified vermiculite undergoes special modification treatment, enhancing the flame retardant properties of the potting compound while also positively impacting its mechanical and thermal conductivity properties.
[0011] Component B comprises 10-15 parts by weight of hydrogen-terminated silicone oil, 30-40 parts by weight of micron-sized alumina, and 0.01-0.05 parts by weight of inhibitor. The hydrogen-terminated silicone oil undergoes a crosslinking reaction with the vinyl-terminated silicone oil under the action of a platinum catalyst, forming a three-dimensional crosslinked structure. The micron-sized alumina acts as a thermally conductive and reinforcing filler, improving the hardness and abrasion resistance of the potting compound while ensuring thermal conductivity. The inhibitor controls the initiation time of the crosslinking reaction, ensuring sufficient working time for the potting compound during potting and preventing premature curing.
[0012] Auxiliary agents: including 1-2 parts by weight of silane coupling agent and 0.05-0.1 parts by weight of platinum catalyst. The silane coupling agent is used to modify the surface of the filler and enhance the bonding force between the filler and the organosilicon matrix; the platinum catalyst is the key catalyst for the crosslinking reaction, which can promote the crosslinking reaction between the vinyl-terminated silicone oil and the hydrogen-terminated silicone oil to form a stable three-dimensional crosslinked network structure.
[0013] Modified vermiculite is achieved through silane coupling agent grafting, sodium ion modification, and ionic liquid treatment. Silane coupling agent grafting improves the organophosphate affinity of the vermiculite surface, enhancing its compatibility with the organosilicon matrix; sodium ion modification alters the interlayer structure and charge distribution of vermiculite, improving its flame-retardant activity; and ionic liquid treatment further optimizes the surface properties of vermiculite, enhancing its stability at high temperatures. The modified vermiculite can exert a more effective flame-retardant effect in potting compounds.
[0014] The particle size of nano-boron nitride is 50-100 nm, while that of micron-sized alumina is 5-10 μm. The difference in particle size allows them to form a reasonable filler gradation in potting compounds. Nano-boron nitride fills the gaps in micron-sized alumina, creating continuous thermally conductive channels, thereby significantly improving the thermal conductivity of the potting compound.
[0015] The hydrogen content of the hydrogen-terminated silicone oil is 0.1-0.2%. The appropriate hydrogen content ensures that it can undergo a moderate cross-linking reaction with the vinyl-terminated silicone oil under the action of a platinum catalyst, forming a stable three-dimensional cross-linked structure with good performance.
[0016] Vinyl-terminated silicone oil and hydrogen-terminated silicone oil undergo multi-site crosslinking through end-group and side-chain hydrogen-containing crosslinking agents under the action of a platinum catalyst, forming a three-dimensional crosslinked structure. Simultaneously, by regulating the synergistic effect of the platinum catalyst and inhibitor, a gradient distribution of crosslinking density is achieved.
[0017] In the initial curing stage of the potting compound, the inhibitor suppresses the cross-linking reaction rate, giving the potting compound good flowability and facilitating potting operations. As time progresses, the inhibitor's effect gradually weakens, and the platinum catalyst fully exerts its effect, accelerating the cross-linking reaction and forming a three-dimensional cross-linked structure with regions of varying cross-linking density within the potting compound. This structure results in high surface hardness, resisting wear and impact, while maintaining a certain degree of flexibility internally, effectively protecting electronic components from external damage. Testing shows that this potting compound has a compressive modulus of 3-5 MPa and an elongation at break greater than 50%.
[0018] The synergistic effect of modified vermiculite and 10-15 parts by weight of aluminum hydroxide enables the potting compound to achieve a UL94V-0 flame retardant rating with a thermal conductivity greater than 2.0 W / (m·K). The special structure and surface properties of modified vermiculite allow it to work in conjunction with aluminum hydroxide to form a stable barrier layer during combustion, preventing flame spread. At the same time, the synergistic effect of the two does not adversely affect the thermally conductive channels constructed by nano-boron nitride and micron-sized alumina, thus achieving an effective balance between flame retardancy and thermal conductivity.
[0019] Surface modification of nano-boron nitride and micron-sized alumina using silane coupling agents reduces the interfacial tension between the filler and the organosilicon matrix, thereby enhancing the dispersibility and bonding strength of the filler with the matrix.
[0020] Meanwhile, during the filler dispersion process, ultrasonic treatment at 750W power and 20kHz frequency for 10 minutes effectively breaks up the filler agglomerates, increasing the filler dispersion to 98%. Under this dual effect, the viscosity of the potting compound is reduced to 4,000-6,000 mPa·s, exhibiting good processing fluidity and enabling easy potting into the complex microstructures of electronic devices.
[0021] The method for preparing the potting compound of the present invention includes the following steps:
[0022] Component A filler pretreatment: Accurately weigh nano-boron nitride and modified vermiculite according to the corresponding weight parts and mix them evenly, then add silane coupling agent. Place the mixture in an ultrasonic dispersion device and ultrasonically disperse it for 10 minutes at a power of 750W and a frequency of 20kHz to uniformly coat the filler surface with silane coupling agent, thereby modifying the surface of the filler and improving the compatibility and dispersibility of the filler with the organosilicon matrix.
[0023] Preparation of Component A: The pretreated mixture of Component A filler and the vinyl-terminated silicone oil were added to a vacuum mixer and stirred for 2 hours under a vacuum of -0.1 MPa and a temperature of 50°C. The vacuum environment effectively removes air and moisture from the system, preventing the formation of air bubbles in the potting compound; the 50°C temperature facilitates a full reaction between the silane coupling agent, filler, and vinyl-terminated silicone oil, ensuring the uniformity and stability of Component A.
[0024] Component B filler pretreatment: After accurately weighing the micron-sized alumina according to the weight parts, add the silane coupling agent and place it in an ultrasonic dispersion device. Use ultrasonic dispersion with a power of 750W and a frequency of 20kHz for 10 minutes to modify the surface of the micron-sized alumina and improve its dispersion performance.
[0025] Preparation of Component B: Micron-sized alumina pretreated with component B filler and hydrogen-terminated silicone oil were added to another stirring device, followed by the addition of an inhibitor. The mixture was stirred for 1 hour under a vacuum of -0.1 MPa and a temperature of 30°C. The lower temperature and vacuum environment helped the inhibitor to be uniformly dispersed in the system and prevented the hydrogen-terminated silicone oil from reacting prematurely with other components, thus ensuring the stability of component B.
[0026] Preparation of potting compound: When using, accurately weigh and mix components A and B with the platinum catalyst at a mass ratio of 1:1, then place the mixture in an ultrasonic degassing device and degas for 5 minutes under ultrasonic action. Ultrasonic degassing can quickly and effectively remove air bubbles introduced during the mixing process, resulting in a uniform, bubble-free potting compound ready for potting.
[0027] The beneficial effects of this invention are:
[0028] The potting compound of this invention achieves an organic combination of high flame retardancy, high thermal conductivity, low viscosity, and excellent mechanical properties. Its flame retardancy rating reaches UL94V-0, effectively providing flame retardancy and reliable fire protection for electronic devices; its thermal conductivity is greater than 2.0 W / (m·K), enabling rapid heat dissipation and preventing overheating; its viscosity is as low as 4,000-6,000 mPa·s, exhibiting good processing fluidity and enabling precise potting of complex electronic devices; its compression modulus is 3-5 MPa, and its elongation at break is greater than 50%, possessing good mechanical strength and flexibility, effectively protecting electronic components from external damage.
[0029] The flame retardant system used does not contain halogens or heavy metals, and will not cause environmental pollution during the production, use and disposal of the potting compound, thus exhibiting good environmental friendliness.
[0030] The process is feasible and stable: The preparation method of the present invention, through precise proportioning of each component, special treatment of fillers, and strict control of preparation process parameters, can ensure the stability and consistency of potting compound product performance, making it suitable for large-scale industrial production. Detailed Implementation
[0031] The technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. It should be understood that this application is not limited to the exemplary embodiments disclosed herein. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0032] Example 1: This example describes a high flame-retardant, high thermal conductivity, and low viscosity silicone potting compound and its preparation method, comprising:
[0033] Potting compound formulation:
[0034] Component A: 50 parts vinyl-terminated silicone oil, 45 parts nano boron nitride, and 5 parts modified vermiculite.
[0035] Component B: 12 parts of hydrogen-containing silicone oil, 35 parts of micron-sized alumina, and 0.03 parts of inhibitor.
[0036] Auxiliary agents: 1.5 parts silane coupling agent, 0.08 parts platinum catalyst.
[0037] Preparation steps:
[0038] According to the above formula, nano boron nitride and modified vermiculite are mixed, silane coupling agent is added, and ultrasonic dispersion is carried out at 750W power and 20kHz frequency for 10 minutes to complete the pretreatment of component A filler.
[0039] The mixture of pretreated filler component A and vinyl-terminated silicone oil were added to a vacuum mixer and stirred for 2 hours at a vacuum of -0.1 MPa and a temperature of 50°C to obtain component A.
[0040] Micron-sized alumina was added to a silane coupling agent and ultrasonically dispersed (750W power, 20kHz frequency, 10 minutes) to complete the pretreatment of component B filler.
[0041] The micron-sized alumina pretreated with component B filler was mixed with hydrogen-containing silicone oil, an inhibitor was added, and the mixture was stirred for 1 hour under a vacuum of -0.1 MPa and a temperature of 30°C to obtain component B.
[0042] Components A and B are mixed with a platinum catalyst at a mass ratio of 1:1, and the mixture is ultrasonically degassed for 5 minutes in an ultrasonic degassing device to obtain a potting compound.
[0043] Performance testing:
[0044] Tests showed that the potting compound has a thermal conductivity of 2.2 W / (m·K), a flame retardancy rating of UL94V-0, a viscosity of 5,200 mPa·s, a compression modulus of 3.8 MPa, and an elongation at break of 55%.
[0045] Example 2: This example describes a high flame-retardant, high thermal conductivity, and low viscosity silicone potting compound and its preparation method, comprising:
[0046] Potting compound formulation:
[0047] Component A: 45 parts vinyl-terminated silicone oil, 48 parts nano boron nitride, and 4 parts modified vermiculite.
[0048] Component B: 10 parts of hydrogen-containing silicone oil, 38 parts of micron-sized alumina, and 0.02 parts of inhibitor.
[0049] Auxiliary agents: 1.2 parts silane coupling agent, 0.06 parts platinum catalyst.
[0050] Preparation steps:
[0051] The preparation steps are the same as in Example 1, and the potting compound is prepared using the same method.
[0052] Performance testing:
[0053] The potting compound has a thermal conductivity of 2.4 W / (m·K), a flame retardancy rating of UL94V-0, a viscosity of 4,800 mPa·s, a compression modulus of 4.2 MPa, and an elongation at break of 60%.
[0054] Example 3: This example describes a high flame-retardant, high thermal conductivity, and low viscosity silicone potting compound and its preparation method, comprising:
[0055] Potting compound formulation:
[0056] Component A: 40 parts vinyl-terminated silicone oil, 50 parts nano boron nitride, and 6 parts modified vermiculite.
[0057] Component B: 15 parts of hydrogen-containing silicone oil, 30 parts of micron-sized alumina, and 0.05 parts of inhibitor.
[0058] Auxiliary agents: 2 parts silane coupling agent, 0.1 parts platinum catalyst.
[0059] Preparation steps:
[0060] The preparation steps are the same as in Example 1, and the potting compound is prepared using the same method.
[0061] Performance testing:
[0062] The potting compound has a thermal conductivity of 2.5 W / (m·K), a flame retardancy rating of UL94V-0, a viscosity of 4,000 mPa·s, a compression modulus of 4.5 MPa, and an elongation at break of 58%.
[0063] As can be seen from the above embodiments, the high flame retardant, high thermal conductivity, and low viscosity organosilicon potting compound prepared by the present invention has excellent performance indicators and can meet the high performance requirements of modern electronic devices for potting materials.
[0064] index Example 1 Example 2 Example 3 Existing technology Thermal conductivity [W / (m·K)] 2.2 2.4 2.5 ≤1.5 Flame retardant rating UL94V-0 UL94V-0 UL94V-0 Mostly UL94V-1 or lower Viscosity [mPa·s] 5,200 4,800 4,000 >10,000 Compression modulus [MPa] 3.8 4.2 4.5 <1 Elongation at break [%) 55 60 58 <30
[0065] As can be clearly seen from the table data, compared with the prior art, the potting compound in the embodiments of the present invention has significant improvements in thermal conductivity, flame retardancy, processing fluidity and mechanical properties, and can better meet the requirements of modern electronic devices for potting materials.
[0066] It should also be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0067] The above description of the disclosed embodiments enables those skilled in the art to make or use this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A high flame retardant, high thermal conductivity, low viscosity silicone potting compound, characterized in that, include: It consists of two components, A and B, and an auxiliary agent; Component A comprises the following materials in parts by weight: 40-60 parts of vinyl-terminated silicone oil, 40-50 parts of nano-boron nitride, and 3-6 parts of modified vermiculite; Component B comprises the following materials in parts by weight: 10-15 parts of end-hydrogen-containing silicone oil, 30-40 parts of micron-sized alumina, and 0.01-0.05 parts of inhibitor; The auxiliary agent consists of the following materials in parts by weight: 1-2 parts of silane coupling agent and 0.05-0.1 parts of platinum catalyst.
2. The high flame retardant, high thermal conductivity, and low viscosity silicone potting compound according to claim 1, characterized in that, Modified vermiculite is modified through silane coupling agent grafting, sodium ion modification, and ionic liquid treatment.
3. The high flame retardant, high thermal conductivity, and low viscosity silicone potting compound according to claim 1, characterized in that, The boron nitride nanoparticles have a particle size of 50-100 nm, and the alumina micron particles have a particle size of 5-10 μm.
4. The high flame retardant, high thermal conductivity, and low viscosity silicone potting compound according to claim 1, characterized in that, The hydrogen content of hydrogen-containing silicone oil is 0.1-0.2%.
5. The high flame retardant, high thermal conductivity, and low viscosity silicone potting compound according to claim 1, characterized in that, Vinyl-terminated silicone oil and hydrogen-terminated silicone oil undergo multi-site crosslinking through end-group and side-chain hydrogen-containing crosslinking agents under the action of platinum catalyst, forming a three-dimensional crosslinked structure. Furthermore, the gradient distribution of crosslinking density is achieved by regulating the synergistic effect of platinum catalyst and inhibitor.
6. The high flame retardant, high thermal conductivity, and low viscosity silicone potting compound according to claim 1, characterized in that, The synergistic effect of modified vermiculite and 10-15 parts by weight of aluminum hydroxide enables the potting compound to achieve a UL94V-0 flame retardant rating and a thermal conductivity greater than 2.0 W / (m·K).
7. The high flame retardant, high thermal conductivity, and low viscosity silicone potting compound according to claim 1, characterized in that, Nano-sized boron nitride fills the gaps in micron-sized alumina, forming continuous thermally conductive channels and improving the overall thermal conductivity of the potting compound.
8. The high flame retardant, high thermal conductivity, and low viscosity silicone potting compound according to claim 1, characterized in that, Surface modification of nano-boron nitride and micron-sized alumina using silane coupling agents reduces the interfacial tension between the filler and the organosilicon matrix, thereby enhancing the filler's dispersibility and adhesion to the matrix.
9. A method for preparing a high flame-retardant, high thermal conductivity, low viscosity silicone potting compound, used in any one of claims 1-8, characterized in that, Includes the following steps: Pretreatment of component A filler: Mix nano boron nitride with modified vermiculite, add silane coupling agent, and ultrasonically disperse for 10 minutes using a power of 750W and a frequency of 20kHz. Preparation of component A: The pretreated filler of component A was mixed with vinyl-terminated silicone oil and stirred for 2 hours under a vacuum of -0.1 MPa and a temperature of 50°C. Pretreatment of component B filler: Micron-sized alumina is added to silane coupling agent and ultrasonically dispersed for 10 minutes using a power of 750W and a frequency of 20kHz. Preparation of component B: Pretreated micronized alumina of component B is mixed with hydrogen-containing silicone oil, an inhibitor is added, and the mixture is stirred for 1 hour under vacuum of -0.1 MPa and 30°C. Preparation of potting compound: Component A and component B are mixed with platinum catalyst at a mass ratio of 1:1 and ultrasonically degassed for 5 minutes to obtain potting compound.