Method for improving volcanic ash activity of water-quenched copper slag through synergistic modification of magnetic separation iron removal

By adding CaO for chemical modification during copper smelting and combining it with magnetic separation for iron removal, the amorphous network structure of water-quenched copper slag was adjusted, solving the problem of low activity of volcanic ash in water-quenched copper slag and realizing efficient resource recycling and iron resource recovery.

CN121135175APending Publication Date: 2025-12-16CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511389940.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-09-26
Publication Date
2025-12-16

AI Technical Summary

Technical Problem

Water-quenched copper slag has low pozzolanic activity, making it difficult to use directly as a cementing material. Furthermore, its high iron content leads to excessive polymerization of the amorphous network structure and insufficient active components, which limits its resource utilization.

Method used

By adding CaO for chemical modification during copper smelting and combining it with magnetic separation for iron removal, the amorphous network structure is adjusted to form non-magnetic tailings, thereby improving the activity of pozzolanic ash and realizing the recycling of iron resources.

Benefits of technology

It significantly improved the pozzolanic activity of water-quenched copper slag, broadened its application scenarios, achieved efficient resource recycling, reduced energy consumption, and improved the recovery rate of iron resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121135175A_ABST
    Figure CN121135175A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of industrial solid waste recycling and filling materials, and particularly discloses a method for improving pozzolanic activity of water-quenched copper slag through synergistic modification of magnetic separation iron removal, which comprises the following steps: adding CaO into molten copper slag discharged in a copper smelting process, uniformly mixing, reacting in an oxygen-containing atmosphere, and then carrying out water quenching and quenching to obtain the pozzolanic activity of the water-quenched copper slag. Modified copper slag particles are obtained; the modified copper slag particles are subjected to wet grinding and drying, and modified copper slag powder is obtained; and the modified copper slag powder is subjected to magnetic separation, and magnetic iron ore concentrate and non-magnetic tailings are obtained. The prepared non-magnetic tailings replace part of cement to prepare the auxiliary cementing material with high pozzolanic activity. Through the synergistic effect of CaO modification and a magnetic separation iron removal process, the pozzolanic activity of the water-quenched copper slag is remarkably improved. The method is simple and convenient in process, the high value-added application way of the water-quenched copper slag is effectively widened, the resource utilization rate is increased, and the method has important significance on promoting comprehensive utilization of solid waste and environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of industrial solid waste resource utilization and filling materials, and particularly relates to a method for improving the pozzolanic activity of water-quenched copper slag by magnetic separation and iron removal. BACKGROUND

[0002] Copper slag is the main industrial solid waste generated in the process of copper smelting. Its main disposal method is direct stockpiling, which not only occupies valuable land resources, but also poses a potential threat to the surrounding atmosphere, soil and groundwater due to its content of heavy metals and other components. Given that water-quenched copper slag is rich in SiO2 and glass phase content and has a certain pozzolanic activity, it shows application potential as an auxiliary cementitious material and can partially replace cement as a cementitious material to realize the resource utilization of copper slag. However, its pozzolanic activity is low and it is difficult to directly prepare alkali-activated cementitious materials as a precursor.

[0003] Previous studies have shown that the pozzolanic activity can be effectively improved by mechanical activation, chemical activation, thermodynamic activation and other means. Mechanical activation is to convert mechanical energy into surface energy of slag by grinding; chemical activation is to stimulate the potential activity of the material by using alkaline or sulfate chemicals; thermodynamic activation is to improve the activity by increasing the curing temperature and high-temperature treatment. However, due to the excessively high iron content in water-quenched copper slag, the polymerization degree of the amorphous network structure is too high, and the content of active components such as calcium and aluminum is significantly insufficient, resulting in low overall reaction activity. Therefore, it is necessary to improve the pozzolanic activity from the source. For this purpose, the present application reconstructs the glass phase of copper slag by chemical melting-water quenching-quick cooling-grinding-magnetic separation and other multi-process composite modification methods, realizes the activity enhancement of copper slag after impurity removal, and realizes the secondary recycling of iron phase. Not only greatly improves the application of copper slag in the field of cementitious materials, promotes the carbon emission reduction of cement industry, but also radiates the resource utilization of other bulk smelting solid wastes. SUMMARY

[0004] In view of the above problems, the present application provides a method for improving the pozzolanic activity of water-quenched copper slag by magnetic separation and iron removal. The non-magnetic tailings prepared by the present application replace part of the cement to prepare an auxiliary cementitious material with high pozzolanic activity. The present application significantly improves the pozzolanic activity of water-quenched copper slag by introducing CaO modification and the synergistic effect of magnetic separation and iron removal process. The method is simple and effective, which widens the high-value-added application of water-quenched copper slag, improves the resource utilization rate, and has important significance for promoting the comprehensive utilization of solid waste and environmental protection.

[0005] In order to solve the above problems, the present application provides a method for improving the pozzolanic activity of water-quenched copper slag by magnetic separation and iron removal, which comprises the following steps:

[0006] S1, CaO is added to molten copper slag discharged from a copper smelting process and mixed uniformly, and then water quenching is performed after reaction in an oxygen-containing atmosphere to obtain modified copper slag particles;

[0007] S2, the modified copper slag particles are wet ground and dried to obtain modified copper slag powder;

[0008] S3, the modified copper slag powder is subjected to magnetic separation to obtain magnetic iron concentrate and non-magnetic tailings.

[0009] Preferably, in step S1, the CaO is added to the copper slag at a binary basicity of 0.6-0.9.

[0010] Preferably, in step S1, the copper smelting process is carried out in a conditioning furnace, and the temperature of the conditioning furnace is 1200-1300℃.

[0011] Preferably, in step S1, the reaction time is 15-60min.

[0012] Preferably, in step S1, the oxygen-containing atmosphere includes at least one of pure oxygen and air.

[0013] Preferably, in step S1, the oxygen-containing atmosphere is introduced at a rate of 50-120L / min.

[0014] Preferably, in step S2, the wet grinding specifically includes adding water to the modified copper slag particles and grinding at a grinding concentration of 45-55wt% to pass 98wt% of the modified copper slag through a 325 mesh screen.

[0015] Preferably, in step S3, the magnetic field strength for the magnetic separation is 800-1000GS.

[0016] Principle of the present application:

[0017] (1) The present application introduces CaO network modifier oxide into the silicate glass phase structure, which can promote the rupture of the silicon (aluminum) oxygen tetrahedral network composed of bridging oxygen and covalent bonds, forming non-bridging oxygen with negative charge, and combining with metal elements in the form of ionic bonds. This network breaking effect can increase the number of network modifiers and ionic bonds in the silicate glass phase structure, thereby reducing the polymerization degree of the material, which can improve the pozzolanic activity of the copper slag;

[0018] (2) The CaO of the present application is added in a molten state, and the Ca 2+ can be replaced by Fe 2+ in the iron silicate, and Fe 3+and further form Fe3O4 crystals. Therefore, the air inlet can provide an oxidation atmosphere, so that Fe is enriched in Fe3O4, and the iron grade of the non-magnetic tailings after magnetic separation is effectively reduced.

[0019] Compared with the prior art, the present application has the following advantages:

[0020] (1) The present application utilizes the heat energy of liquid copper slag discharged in the copper smelting process to directly mix with CaO for modification, avoiding additional costs of secondary repeated calcination, and having the advantages of low energy consumption and low cost.

[0021] (2) The iron concentrate obtained by magnetic separation has a total iron (TFe) content of >85wt%, which is significantly higher than the industrial grade of ironmaking raw materials (≥55wt%), and can be directly recycled as high-quality ironmaking raw materials. The process improves the pozzolanic activity of copper slag while achieving efficient recovery of iron resources;

[0022] (3) The present application utilizes a relatively simple method to improve the pozzolanic activity of copper slag, broadens the utilization scenarios of copper slag, and realizes higher utilization, which has the significance of resource recycling and environmental protection. BRIEF DESCRIPTION OF DRAWINGS

[0023] Figure 1 The process flow chart of the method for improving the pozzolanic activity of water-quenched copper slag by magnetic separation and iron removal and modification is described in the embodiments of the present application.

[0024] Figure 2 The Fourier transform infrared spectroscopy (FTIR) and X-ray photoelectron spectroscopy (XPS) diagrams of the CaO modified copper slag of embodiments 1-4 and the CaO unmodified copper slag of comparative example 1 are shown in the present application; wherein (a) is the FTIR diagram; (b) is the XPS diagram.

[0025] Figure 3 The O1s peak fitting diagram of X-ray photoelectron spectroscopy (XPS) of embodiments 1-4 and comparative example 1 is shown in the present application; wherein (a) is comparative example 1; (b) is embodiment 1; (c) is embodiment 2; (d) is embodiment 3; (e) is embodiment 4. DETAILED DESCRIPTION

[0026] In order to make the present application more easily understood, the present application is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present application and are not used to limit the scope of the present application. Obviously, the described examples are only a part of the examples of the present application, but not all the examples. Based on the examples in the present application, all other examples obtained by those skilled in the art without creative labor are within the scope of protection of the present application. Unless otherwise defined, the professional terms used below are consistent with the meanings understood by those skilled in the art; unless otherwise specified, the raw materials and reagents involved in the present application can be purchased from the market or prepared by known methods.

[0027] It should be noted that the present application Figure 2 B1 represents a basicity of 0.1 (the basicity of the unmodified copper slag is 0.1); B6 represents a basicity of 0.6, B7 represents a basicity of 0.7, B8 represents a basicity of 0.8, and B9 represents a basicity of 0.9; GCS represents granular copper slag (i.e. unmodified copper slag).

[0028] In view of the problem that water-quenched copper slag has the potential of auxiliary cementitious material, but is difficult to be efficiently recycled due to its low inherent reactivity, the present application provides a method for improving the pozzolanic activity of water-quenched copper slag by magnetic separation and iron removal. The present application introduces CaO into molten copper slag for chemical modification, simultaneously combines with the process of magnetic separation and iron removal, effectively regulates the amorphous network structure and enriches the active components, thereby greatly improves the utilization efficiency of copper slag in the cementitious system.

[0029] The present application is further described below in conjunction with specific examples and comparative examples.

[0030] Example 1

[0031] A method for improving the pozzolanic activity of water-quenched copper slag by magnetic separation and iron removal, as shown in Figure 1 , comprises the following steps:

[0032] (1) A certain amount of CaO is added to the discharged liquid copper slag, so that the binary basicity (SiO2 / CaO) of the mixed copper slag is 0.6, and then air is introduced for 30 min to make it fully react;

[0033] (2) The molten copper slag is poured into water for water quenching and rapid cooling, and the modified copper slag particles after cooling are collected;

[0034] (3) The collected modified copper slag particles are ground to 98wt% or more passing through a 325 mesh sieve at a grinding concentration of 50wt%, and then put into a drying oven at 105℃ for drying;

[0035] (4) The modified copper slag after drying is subjected to magnetic separation at a magnetic field strength of 900GS to obtain magnetic concentrate and non-magnetic tailings.

[0036] The non-magnetic tailings prepared above replace part of the cement, and standard sand and other materials are used to prepare cement mortar test blocks (raw materials include non-magnetic tailings, cement, standard sand, and water). According to GB / T 17671-2021, the modified copper slag content is 30% of the mass of the cement, the water-binder ratio is 0.5, and the mortar-sand ratio is 1:3. After curing for 3, 7, and 28 days, uniaxial compressive strength experiments are performed. The results are shown in Table 1.

[0037] Example 2

[0038] The difference between this example and Example 1 is that the binary alkalinity (SiO2 / CaO) is 0.7. The other steps and parameters are the same as those of Example 1.

[0039] The non-magnetic tailings prepared above replace part of the cement, and standard sand and other materials are used to prepare cement mortar test blocks (raw materials include non-magnetic tailings, cement, standard sand, and water). According to GB / T 17671-2021, the modified copper slag content is 30% of the mass of the cement, the water-binder ratio is 0.5, and the mortar-sand ratio is 1:3. After curing for 3, 7, and 28 days, uniaxial compressive strength experiments are performed. The results are shown in Table 1.

[0040] Example 3

[0041] The difference between this example and Example 1 is that the binary alkalinity (SiO2 / CaO) is 0.8. The other steps and parameters are the same as those of Example 1.

[0042] The non-magnetic tailings prepared above replace part of the cement, and standard sand and other materials are used to prepare cement mortar test blocks (raw materials include non-magnetic tailings, cement, standard sand, and water). According to GB / T 17671-2021, the modified copper slag content is 30% of the mass of the cement, the water-binder ratio is 0.5, and the mortar-sand ratio is 1:3. After curing for 3, 7, and 28 days, uniaxial compressive strength experiments are performed. The results are shown in Table 1.

[0043] Example 4

[0044] The difference between this example and Example 1 is that the binary alkalinity (SiO2 / CaO) is 0.9. The other steps and parameters are the same as those of Example 1.

[0045] The non-magnetic tailings prepared above replace part of the cement, and standard sand and other materials are used to prepare cement mortar test blocks (raw materials include non-magnetic tailings, cement, standard sand, and water). According to GB / T 17671-2021, the modified copper slag content is 30% of the mass of the cement, the water-binder ratio is 0.5, and the mortar-sand ratio is 1:3. After curing for 3, 7, and 28 days, uniaxial compressive strength experiments are performed. The results are shown in Table 1.

[0046] Comparative Example 1

[0047] The difference between this embodiment and Example 1 is that the binary alkalinity (SiO2 / CaO) is 0.9. Other steps and parameters are the same as those in Example 1.

[0048] The non-magnetic tailings prepared above are used to replace part of the cement, and standard sand and other materials are used to prepare cement mortar test blocks (raw materials include non-magnetic tailings, cement, standard sand, and water). According to GB / T 17671-2021, the modified copper slag content is 30% of the mass of the cement, the water-binder ratio is 0.5, and the mortar-sand ratio is 1:3. After curing for 3, 7, and 28 days, uniaxial compressive strength tests are performed. The results are shown in Table 1.

[0049] Performance testing and result analysis:

[0050] The samples obtained after modification in Examples 1-4 and Comparative Example 1 are subjected to XPS and FTIR testing, and the results are shown in Figures 2-3 As can be seen from Figure 2 (a), when the binary alkalinity is controlled at 0.6-0.9, the bridge oxygen bonds can be broken, generating non-bridge oxygen bonds, i.e., the silicate network is effectively destroyed, the polymerization degree of the silicate network is reduced, and the pozzolanic activity is improved. As can be seen from Figure 2 (b), the Ca 2+ peak of the present application proves that the Ca 2+ enters the silicate network in the form of Si-O-Ca 2+ . As can be seen from Figure 3 , it is further proved that the increase in alkalinity has a depolymerization effect on the silicate network in the copper slag. This proves that the modification effect of CaO on the copper slag is irreplaceable by Al2O3.

[0051] The different age compressive strength tests of the concrete test blocks prepared from the non-magnetic tailings obtained in Examples 1-4 and Comparative Example 1 are shown in Table 1 below:

[0052] Table 1:

[0053] As can be seen from Table 1, by comparing Examples 1-4 with Comparative Example 1, it is found that after adding CaO to the copper slag, the strength at different curing ages is enhanced, the strength of Examples 1-4 at 3d age is increased by 22.6%, 30.6%, 41.9%, and 38.7%, respectively; the strength of Examples at 7d age is increased by 18.3%, 41.3%, 51.9%, and 27.9%, respectively; and the strength of Examples 1-4 at 28d age is increased by 18.9%, 37.8%, 46.8%, and 34.8%, respectively.

[0054] The different age compressive strength of the embodiment 1-4 shows that the compressive strength of each age increases first and then decreases with the increase of alkalinity, and the maximum value is obtained when the alkalinity is 0.8. This shows that in a certain range, the increase of alkalinity has a positive promoting effect on the pozzolanic activity of copper slag, and beyond this range, not only the activity is reduced, but also the resources are wasted.

[0055] The above examples only express several embodiments of the present application, and the description is more specific and detailed, but it cannot be understood as limiting the scope of the application patent application. It should be pointed out that for ordinary skilled in the art, without departing from the inventive concept of the present application, a number of modifications and improvements can be made, which all belong to the protection scope of the present application. Therefore, the protection scope of the present application patent should be subject to the appended claims.

Claims

1. A method for improving the activity of water-quenched copper slag pozzolan by magnetic separation and iron removal and synergistic modification, characterized in that, The method comprises the following steps: S1, adding CaO into molten copper slag discharged from a copper smelting process and mixing uniformly, then performing reaction under an oxygen-containing atmosphere and water quenching to obtain modified copper slag particles; S2, wet grinding and drying the modified copper slag particles to obtain modified copper slag powder; S3, performing magnetic separation on the modified copper slag powder to obtain magnetic iron concentrate and non-magnetic tailings.

2. The method for improving the activity of the copper slag volcanic ash by magnetic separation and iron removal and synergistic modification according to claim 1, characterized in that, In step S1, the binary basicity of the CaO added to the copper slag is 0.6-0.

9.

3. The method for improving the activity of the copper slag volcanic ash by magnetic separation and iron removal and synergistic modification according to claim 1, characterized in that, In step S1, the copper smelting process is performed in a conditioning furnace, and the temperature of the conditioning furnace is 1200-1300℃.

4. The method for improving the activity of the copper slag volcanic ash by magnetic separation and iron removal and synergistic modification according to claim 1, characterized in that, In step S1, the reaction time is 15-60 min.

5. The method for improving the activity of the copper slag volcanic ash by magnetic separation and iron removal and synergistic modification according to claim 1, characterized in that, In step S1, the oxygen-containing atmosphere comprises at least one of pure oxygen and air.

6. The method for improving the activity of the copper slag volcanic ash by magnetic separation and iron removal and synergistic modification according to claim 1, characterized in that, In step S1, the oxygen-containing atmosphere is introduced at a rate of 50-120 L / min.

7. The method for improving the activity of the copper slag volcanic ash by magnetic separation and iron removal and synergistic modification according to claim 1, characterized in that, In step S2, the wet grinding is specifically adding water to the modified copper slag particles and grinding at a grinding concentration of 45-55 wt% to 98 wt% or more of the modified copper slag passing through a 325 mesh sieve.

8. The method for improving the activity of the copper slag volcanic ash by magnetic separation and iron removal and synergistic modification according to claim 1, characterized in that, In step S3, the magnetic field strength of the magnetic separation is 800-1000 GS.