High-temperature-erosion-resistant Fe-based amorphous coating welding wire and preparation method

A high-amorphous-content amorphous-nanocrystalline composite structure was prepared using Fe-Cr-Nb-BW-Si-Mo amorphous alloy welding wire, which solved the problem of low bonding strength of traditional welding wires under extreme environments, and achieved improved high-temperature erosion resistance and industrial application.

CN121245306APending Publication Date: 2026-01-02XIAN THERMAL POWER RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511210830.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-27
Publication Date
2026-01-02

AI Technical Summary

Technical Problem

Most existing welding wires are crystalline alloys, which are prone to forming coarse grains and brittle phases during non-equilibrium solidification, resulting in low coating bonding strength and poor crack resistance, making it difficult to meet the durability requirements of extreme environments such as water-cooled walls in thermal power plants.

Method used

Using Fe-Cr-Nb-BW-Si-Mo amorphous alloy welding wire, an amorphous-nanocrystalline composite structure with high amorphous content was prepared by optimizing the proportion of multi-component components. Nanocrystalline phases such as Fe2Nb, FeCr, FeMo, and Fe13Mo2B5 were used to improve wear resistance and erosion resistance.

Benefits of technology

It achieves high-efficiency high-temperature abrasion resistance, reduces raw material costs and production complexity, is suitable for industrial mass production, and is applicable to the high-efficiency protection of water-cooled wall surfaces in thermal power plants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121245306A_ABST
    Figure CN121245306A_ABST
Patent Text Reader

Abstract

The invention provides a high-temperature-erosion-resistant Fe-based amorphous coating welding wire and a preparation method, and belongs to the technical field of metal materials. The welding wire comprises a flux core and a welding skin. Wherein the flux core comprises 25%-28% of Cr powder, 23%-25% of Nb powder, 8%-10% of B powder, 8%-10% of Si powder, 15%-17% of Mo powder, 8%-10% of W powder and the balance Fe powder; and the welding skin is a Fe60Cr40 steel strip. According to the novel Fe-Cr-Nb-B-W-Si-Mo series amorphous alloy welding wire, by optimizing the proportion of multiple components, the coating is endowed with excellent wear resistance, high temperature corrosion resistance and erosion resistance while the high amorphous content is ensured. The welding wire can adopt a conventional electric arc surfacing process, efficient protection of the surface of the water cooling wall is achieved under the low-cost condition, and an innovative solution is provided for long-acting protection of key components of a power plant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure belongs to the field of metallic materials technology, specifically relating to a high-temperature erosion resistant Fe-based amorphous coated welding wire and its preparation method. Background Technology

[0002] Water-cooled walls in boiler systems of thermal power plants operate under extreme environments of high temperature, high pressure, high corrosion, and high wear for extended periods. Their failure significantly impacts the safety and operational efficiency of the power plant. Common failure modes include high-temperature oxidation, sulfide / chloride corrosion, and erosion wear from coal ash particles. These factors collectively lead to wall thinning and can even cause tube rupture accidents. Currently, traditional protective methods such as thermal spraying and welding with corrosion-resistant alloys can partially alleviate corrosion and wear problems. However, due to inherent defects in crystalline materials, such as grain boundaries, dislocations, and compositional segregation, their long-term protective performance remains significantly insufficient, making it difficult to meet the durability requirements under complex operating conditions.

[0003] In recent years, amorphous alloys have attracted much attention in the field of materials science due to their unique short-range ordered and long-range disordered atomic structure. Compared with traditional crystalline alloys, amorphous alloys are free of grain boundaries and precipitates, exhibiting isotropic characteristics and displaying ultra-high strength, high hardness, and excellent wear resistance and corrosion resistance. These properties make amorphous alloy coatings show great potential in the field of surface protection in extreme environments. Although amorphous coating preparation technologies such as laser cladding and cold spraying have made some progress, there is still a lack of amorphous alloy welding wires suitable for industrial surfacing. Most existing welding wires are crystalline alloys, which are prone to forming coarse grains and brittle phases during non-equilibrium solidification, resulting in low coating bonding strength and poor crack resistance. In addition, the composition design of traditional welding wires is difficult to simultaneously meet the requirements of high amorphous formation capability and service performance, limiting the engineering application of amorphous coatings. Summary of the Invention

[0004] This disclosure aims to at least solve one of the technical problems existing in the prior art, and to provide a high-temperature erosion resistant Fe-based amorphous coated welding wire and its preparation method.

[0005] In one aspect, this disclosure provides a high-temperature erosion-resistant Fe-based amorphous coated welding wire, the welding wire comprising: a flux core and a welding sheath; wherein,

[0006] The core comprises 25-28% Cr powder, 23-25% Nb powder, 8-10% B powder, 8-10% Si powder, 15-17% Mo powder, 8-10% W powder, and the balance Fe powder.

[0007] The weld bead is Fe60Cr40 steel strip.

[0008] Optionally, the thickness of the solder skin is 0.2-0.4 mm and the width is 6-8 mm.

[0009] Optionally, the filler amount of welding wire is controlled at 22-25 wt%.

[0010] In another aspect of this disclosure, a method for preparing the high-temperature erosion-resistant Fe-based amorphous coated welding wire described above is provided, the method comprising:

[0011] Weigh out 25-28% Cr powder, 23-25% Nb powder, 8-10% B powder, 8-10% Si powder, 15-17% Mo powder, 8-10% W powder, and the remainder Fe powder as the pharmaceutical powder.

[0012] The powder is placed in a vacuum furnace for heating treatment, and the dried powder is then mixed.

[0013] The welding wire is pretreated and then drawn by wrapping the flux powder inside the welding wire.

[0014] Optionally, the particle size of the powder is 100-200 mesh.

[0015] Optionally, the heat treatment temperature is 220–260℃, and the holding time is 1–3 hours.

[0016] Optionally, the mixing time for the dried powder is 1 to 3 hours.

[0017] Optionally, in the drawing process, the diameter of the first drawing die is 2.6 mm.

[0018] Optionally, the diameter of the welding wire is 1-1.5 mm.

[0019] This disclosure presents a high-temperature erosion-resistant Fe-based amorphous coating welding wire and its preparation method. The welding wire comprises a flux core and a welding sheath; wherein the flux core comprises 25-28% Cr powder, 23-25% Nb powder, 8-10% B powder, 8-10% Si powder, 15-17% Mo powder, 8-10% W powder, and the balance being Fe powder; the welding sheath is Fe60Cr40 steel strip. This disclosure proposes a novel Fe-Cr-Nb-BW-Si-Mo amorphous alloy welding wire, which, through optimized multi-component ratio, ensures high amorphous content while imparting excellent wear resistance, high-temperature corrosion resistance, and erosion resistance to the coating. This welding wire can be used with conventional arc welding processes to achieve efficient protection of water-cooled wall surfaces under low-cost conditions, providing an innovative solution for the long-term protection of critical components in power plants. Attached Figure Description

[0020] Figure 1 This is a flowchart illustrating the method for preparing high-temperature erosion resistant Fe-based amorphous coated welding wire according to a specific embodiment of this disclosure.

[0021] Figure 2This is a scanning electron microscope image of the amorphous weld overlay layer prepared in Example 2 of this disclosure;

[0022] Figure 3 The scanning electron microscope morphology of the amorphous weld overlay prepared in Example 2 of this disclosure after 15 minutes of high-temperature erosion. Detailed Implementation

[0023] To enable those skilled in the art to better understand the technical solutions of this disclosure, the disclosure will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain this disclosure and represent a part of the embodiments of this disclosure, not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this disclosure without creative effort are within the protection scope of this disclosure.

[0024] One aspect of this disclosure provides a high-temperature erosion resistant Fe-based amorphous coated welding wire, comprising: a flux core and a welding sheath; wherein the flux core comprises 25-28% Cr powder, 23-25% Nb powder, 8-10% B powder, 8-10% Si powder, 15-17% Mo powder, 8-10% W powder, and the balance being Fe powder; the welding sheath is Fe60Cr40 steel strip.

[0025] It should be noted that the sum of the percentages of the various powder components included in the core is 100%, and the particle size of each powder is preferably 100-200 mesh, and the purity of the powder is ≥99.90%.

[0026] It should be further noted that, due to the high Fe content in the steel strip, the overall Fe content of the welding wire is high, forming an Fe-based amorphous coating welding wire.

[0027] The roles and functions of each alloy component in the amorphous welding wire disclosed herein are as follows:

[0028] (1) Fe element: In this disclosure, the Fe element is transferred into the weld metal through the weld skin, and its mechanism of action is mainly reflected in the following aspects:

[0029] 1) As the main component of Fe-based amorphous alloys, Fe not only endows materials with excellent comprehensive properties (including outstanding mechanical properties, good soft magnetic properties and excellent corrosion resistance), but also has a cost advantage compared with other amorphous alloy systems, which is conducive to industrial applications.

[0030] 2) In terms of microstructure regulation, Fe plays multiple roles: some Fe forms a solid solution phase with Cr, effectively improving the ductility and toughness of the amorphous weld overlay and significantly reducing the risk of cracking due to material brittleness; at the same time, it participates in the formation process of nanocrystalline phases, reacting with alloying elements such as Nb, Mo, and B to generate Fe2Nb, FeCr, and Fe... 13Multiple reinforcing phases such as Mo2B5.

[0031] 3) This multi-scale microstructure design achieves synergistic reinforcement of the amorphous matrix and the nanocrystalline phase, enabling the weld overlay to possess both high strength and high toughness.

[0032] (2) Cr element: In this disclosure, the Cr element is introduced into the weld metal through the weld skin and flux powder. Its main functions can be summarized into the following four aspects:

[0033] 1) Structural formation role: As a key alloying element, it participates in the formation of Fe-based amorphous structure; some Cr reacts with Fe to form FeCr nanocrystalline phase, which is distributed in the amorphous matrix in a dispersed strengthening manner;

[0034] 2) High-temperature protection mechanism: preferentially reacts with oxygen to form a dense Cr2O3 protective film; significantly improves the stability of the weld overlay in high-temperature corrosive environments;

[0035] 3) Mechanical property optimization: It forms a solid solution phase with Fe, which improves the material's plastic deformation ability; and enhances high-temperature erosion resistance through the synergistic effect of solid solution strengthening and nano-phase strengthening.

[0036] 4) Multi-scale synergistic effect: It participates in the construction of amorphous structures at the atomic scale; forms a reinforcing phase at the nanoscale; and achieves performance optimization at the macroscale.

[0037] (3) Nb element: In this disclosure, Nb element is introduced into the weld metal system through flux powder, and its key role is reflected in the following two aspects:

[0038] 1) Amorphous formation and microstructure regulation: As an important metalloid element, it significantly enhances the amorphous formation ability of Fe-based alloys; by inhibiting grain nucleation and growth, it promotes the stable formation of amorphous structures;

[0039] 2) Nano-strengthening and performance improvement mechanism: Fe2Nb nanocrystalline phase is generated in situ by reacting with Fe; these nanocrystalline phases are uniformly dispersed in the amorphous matrix to form a unique "amorphous-nanocrystalline" composite structure; this special microstructure can simultaneously improve the corrosion resistance and high-temperature erosion resistance of the material.

[0040] (4) Mo element: In this invention, the Mo element is introduced into the weld overlay metal system through flux powder, and its core functions are reflected in the following two aspects:

[0041] 1) Amorphous formation and structural stabilization: As an important transition element, Mo significantly improves the amorphous formation ability of Fe-based alloys; by inhibiting grain boundary migration and grain growth, it maintains the long-term stability of the amorphous structure.

[0042] 2) High-temperature strengthening and performance optimization mechanism: FeMo and Fe are generated in situ by reacting with elements such as Fe and B.13 Mo2B5 nano-reinforcing phases; these nanocrystalline phases are uniformly distributed in the amorphous matrix, forming a unique "amorphous matrix-nanoprecipitated phase" composite structure; this special microstructure enables the weld overlay to exhibit excellent wear resistance under high-temperature erosion environment.

[0043] (5) Botanical element: Botanical element enters the weld metal through the flux powder. Botanical element has two main functions: forming Fe-based amorphous structures; and reacting with Fe to form Fe. 13 Mo2B5 nanocrystals are dispersed in the amorphous matrix, which improves the matrix's resistance to high-temperature erosion.

[0044] (6) Si element: Si element enters the weld metal through the flux powder. The main role of Si element is to form Fe-based amorphous structure.

[0045] (7) W element: In this invention, the W element is introduced into the weld metal system through a flux powder, and its core functions are mainly reflected in the following aspects:

[0046] 1) Amorphous formation promoting effect: As a high-melting-point transition metal element, W significantly enhances the amorphous formation ability of Fe-based alloys; by inhibiting grain boundary migration and crystal nucleation, it promotes the stable formation of amorphous structures;

[0047] 2) High-temperature stability strengthening mechanism: W significantly improves the structural stability of amorphous structures under high-temperature environments; enhances the resistance of the weld overlay to high-temperature softening.

[0048] In some preferred embodiments, the filler wire content is controlled at 22-25 wt%.

[0049] In some other preferred embodiments, the thickness of the solder skin is 0.2-0.4 mm, for example, 0.3 mm, and the width is 6-8 mm, for example, 7 mm.

[0050] This disclosure innovatively designs an Fe-Cr-Nb-BW-Si-Mo amorphous alloy welding wire. By optimizing the alloy composition and process parameters, a high-performance weld overlay with an amorphous content ≥44% was successfully prepared. This weld overlay exhibits a uniform distribution of Fe2Nb, FeCr, FeMo, and Fe within an amorphous matrix. 13 The presence of nanocrystalline phases such as Mo2B5 forms a unique amorphous-nanocrystalline composite structure. This special microstructure significantly enhances the high-temperature erosion resistance of the weld overlay, enabling it to exhibit excellent service performance under harsh conditions such as high temperature and high wear.

[0051] like Figure 1 As shown, another aspect of this disclosure proposes a method S100 for preparing a high-temperature erosion-resistant Fe-based amorphous coated welding wire, specifically including the following steps S110 to S130:

[0052] S110. Weigh out 25-28% Cr powder, 23-25% Nb powder, 8-10% B powder, 8-10% Si powder, 15-17% Mo powder, 8-10% W powder, and the balance Fe powder according to the following mass percentages. The sum of the mass percentages of the above components is 100%, which is used as the pharmaceutical powder.

[0053] It should be noted that the particle size, purity, and function of the powder in step S110 are described in the previous text and will not be repeated here.

[0054] S120. The powder is placed in a vacuum furnace for heating treatment, and the dried powder is mixed.

[0055] In step S120, the powder weighed in step S110 is placed in a vacuum heating furnace and heated at a temperature of 220-260°C for 1-3 hours to remove the water of crystallization from the powder. The dried powder is then placed in a powder mixer for thorough mixing for 1-3 hours.

[0056] S130. The welding skin is pretreated, and the flux powder is wrapped inside the welding skin and then drawn to obtain the welding wire.

[0057] In step S130, the pretreatment of the weld skin includes: using Fe60Cr40 steel strip as the weld skin, removing the grease from the surface of the Fe60Cr40 steel strip with alcohol, and then wrapping the flux powder prepared in step S120 inside the Fe60Cr40 steel strip using a flux-cored wire drawing device. The diameter of the first drawing die is 2.6mm. After the first drawing process is completed, the die diameter is reduced sequentially to finally obtain a flux-cored wire with a diameter of 1-1.5mm.

[0058] It should be understood that after the flux-cored welding wire is drawn, the wire is wound onto the wire spool by a wire winding machine and finally sealed in a vacuum packaging bag for later use.

[0059] The welding wire formulation disclosed herein is simple, reducing raw material costs and production process complexity, making it suitable for industrial mass production. It has strong process compatibility, and the diameter of the welding wire combines good wire feeding stability and deposition efficiency.

[0060] This disclosure describes the use of high-temperature erosion resistant Fe-based amorphous coated welding wire for welding protection on the fire-facing surface of water-cooled walls in thermal power plants. The resulting weld overlay is mainly composed of an amorphous phase, a partial solid solution, and a partial nanocrystalline phase, exhibiting excellent high-temperature erosion and corrosion resistance.

[0061] It should be noted that the amorphous alloy welding wire provided in this disclosure can directly prepare a high-amorphous-content weld overlay layer using conventional arc welding processes, breaking through the limitations of traditional amorphous material preparation methods that rely on rapid cooling techniques (such as the strip spinning method). Compared with existing amorphous material preparation processes, this invention simplifies the process, reduces costs, and is easier to industrialize, demonstrating significant engineering application value.

[0062] The following will further illustrate the preparation method and application of high-temperature erosion-resistant Fe-based amorphous coated welding wire with specific embodiments:

[0063] Example 1

[0064] Step 1: Weigh out the following powders by mass percentage: Cr powder 25%, Nb powder 23%, B powder 8%, Si powder 8%, Mo powder 15%, W powder 8%, and the remainder is Fe powder. The sum of the mass percentages of the above components is 100%.

[0065] Step 2: Place the weighed powder from Step 1 into a vacuum heating furnace and heat it at 220℃ for 1 hour to remove the water of crystallization from the powder; place the dried powder into a powder mixer for thorough mixing for 1 hour.

[0066] Step 3: Using Fe60Cr40 steel strip as the welding layer, the grease on the surface of the Fe60Cr40 steel strip is removed with alcohol. The flux-cored wire drawing equipment is used to wrap the flux powder prepared in step 2 inside the Fe60Cr40 steel strip. The diameter of the first drawing die is 2.6mm.

[0067] Step 4: After the first drawing process is completed, the die hole diameter is reduced one by one to finally obtain a flux-cored wire with a diameter of 1.2mm;

[0068] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0069] Arc welding was performed on the surface of the water-cooled wall tube using the amorphous coated welding wire provided in Implementation Case 1. The results are as follows:

[0070] (1) The arc is stable during the welding process, with less spatter, and the weld layer is aesthetically pleasing with no visible defects such as cracks or pores.

[0071] (2) XRD test results of the weld overlay showed that the amorphous structure accounted for 45.7%;

[0072] (3) The Brinell hardness of the weld overlay is 695 HBW;

[0073] (4) The high-temperature erosion performance of the weld overlay at 600℃ is 5.6 times that of the water-cooled wall tube substrate.

[0074] Example 2

[0075] Step 1: Weigh out the following powders by mass percentage: Cr powder 28%, Nb powder 25%, B powder 10%, Si powder 10%, Mo powder 17%, W powder 10%, and the remainder is Fe powder. The sum of the mass percentages of the above components is 100%.

[0076] Step 2: Place the weighed powder from Step 1 into a vacuum heating furnace and heat it at 260℃ for 3 hours to remove the water of crystallization from the powder; place the dried powder into a powder mixer for thorough mixing for 3 hours.

[0077] Step 3: Using Fe60Cr40 steel strip as the welding layer, the grease on the surface of the Fe60Cr40 steel strip is removed with alcohol. The flux-cored wire drawing equipment is used to wrap the flux powder prepared in step 2 inside the Fe60Cr40 steel strip. The diameter of the first drawing die is 2.6mm.

[0078] Step 4: After the first drawing process is completed, the die hole diameter is reduced one by one to finally obtain a flux-cored wire with a diameter of 1.2mm;

[0079] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0080] Arc welding was performed on the surface of the water-cooled wall tube using the amorphous coated welding wire provided in Implementation Case 2. The results are as follows:

[0081] (1) The arc is stable during the welding process, with less spatter, and the weld layer is aesthetically pleasing with no visible defects such as cracks or pores.

[0082] (2) XRD test results of the weld overlay showed that the amorphous structure accounted for 47.1%;

[0083] (3) The Brinell hardness of the weld overlay is 689 HBW;

[0084] (4) The high-temperature erosion performance of the weld overlay at 600℃ is 5.7 times that of the water-cooled wall tube substrate.

[0085] Figure 2 This is a scanning electron microscope (SEM) image of the amorphous weld overlay layer prepared in Example 2. As can be seen from the image, the nanocrystalline phases (Fe₂Nb, FeCr, FeMo, Fe) are present. 13 Nanocrystalline phases such as Mo2B5 are distributed on an amorphous matrix.

[0086] Figure 3 The image shows the scanning electron microscope (SEM) morphology of the amorphous weld overlay prepared in Example 2 after 15 minutes of high-temperature erosion. As can be seen from the image, no bulk metal fragments have detached from the weld overlay surface, indicating excellent erosion resistance.

[0087] Example 3

[0088] Step 1: Weigh out the following powders by mass percentage: Cr powder 26%, Nb powder 24%, B powder 9%, Si powder 9%, Mo powder 16%, W powder 9%, and the remainder is Fe powder. The sum of the mass percentages of the above components is 100%.

[0089] Step 2: Place the weighed powder from Step 1 into a vacuum heating furnace and heat it at 240℃ for 2 hours to remove the water of crystallization from the powder; place the dried powder into a powder mixer for thorough mixing for 2 hours.

[0090] Step 3: Using Fe60Cr40 steel strip as the welding layer, the grease on the surface of the Fe60Cr40 steel strip is removed with alcohol. The flux-cored wire drawing equipment is used to wrap the flux powder prepared in step 2 inside the Fe60Cr40 steel strip. The diameter of the first drawing die is 2.6mm.

[0091] Step 4: After the first drawing process is completed, the die hole diameter is reduced one by one to finally obtain a flux-cored wire with a diameter of 1.2mm;

[0092] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0093] Arc welding was performed on the surface of the water-cooled wall tube using the amorphous coated welding wire provided in Example 3, and the results are as follows:

[0094] (1) The arc is stable during the welding process, with less spatter, and the weld layer is aesthetically pleasing with no visible defects such as cracks or pores.

[0095] (2) XRD test results of the weld overlay showed that the amorphous structure accounted for 47.2%;

[0096] (3) The Brinell hardness of the weld overlay is 699 HBW;

[0097] (4) The high-temperature erosion performance of the weld overlay at 600℃ is 5.77 times that of the water-cooled wall tube substrate.

[0098] Example 4

[0099] Step 1: Weigh out the following powders by mass percentage: Cr powder 26%, Nb powder 24.5%, B powder 9.5%, Si powder 9.5%, Mo powder 16.5%, W powder 9.5%, and the remainder is Fe powder. The sum of the mass percentages of the above components is 100%.

[0100] Step 2: Place the weighed powder from Step 1 into a vacuum heating furnace and heat it at 245℃ for 1.3 hours to remove the water of crystallization from the powder. After drying, place the powder into a powder mixer for thorough mixing for 1.3 hours.

[0101] Step 3: Using Fe60Cr40 steel strip as the welding layer, the grease on the surface of the Fe60Cr40 steel strip is removed with alcohol. The flux-cored wire drawing equipment is used to wrap the flux powder prepared in step 2 inside the Fe60Cr40 steel strip. The diameter of the first drawing die is 2.6mm.

[0102] Step 4: After the first drawing process is completed, the die hole diameter is reduced one by one to finally obtain a flux-cored wire with a diameter of 1.2mm;

[0103] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0104] Arc welding was performed on the surface of the water-cooled wall tube using the amorphous coated welding wire provided in Example 4, and the results are as follows:

[0105] (1) The arc is stable during the welding process, with less spatter, and the weld layer is aesthetically pleasing with no visible defects such as cracks or pores.

[0106] (2) XRD test results of the weld overlay showed that the amorphous structure accounted for 47.8%;

[0107] (3) The Brinell hardness of the weld overlay is 690 HBW;

[0108] (4) The high-temperature erosion performance of the weld overlay at 600℃ is 5.68 times that of the water-cooled wall tube substrate.

[0109] Example 5

[0110] Step 1: Weigh out the following powders by mass percentage: Cr powder 25.5%, Nb powder 23.5%, B powder 8.5%, Si powder 8.5%, Mo powder 15.5%, W powder 8.5%, and the remainder is Fe powder. The sum of the mass percentages of the above components is 100%.

[0111] Step 2: Place the powder weighed in Step 1 into a vacuum heating furnace and heat it at 225℃ for 1.1 hours to remove the water of crystallization from the powder; place the dried powder into a powder mixer for thorough mixing for 1.1 hours.

[0112] Step 3: Using Fe60Cr40 steel strip as the welding layer, the grease on the surface of the Fe60Cr40 steel strip is removed with alcohol. The flux-cored wire drawing equipment is used to wrap the flux powder prepared in step 2 inside the Fe60Cr40 steel strip. The diameter of the first drawing die is 2.6mm.

[0113] Step 4: After the first drawing process is completed, the die hole diameter is reduced one by one to finally obtain a flux-cored wire with a diameter of 1.2mm;

[0114] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0115] Arc welding was performed on the surface of the water-cooled wall tube using the amorphous coated welding wire provided in Example 5, and the results are as follows:

[0116] (1) The arc is stable during the welding process, with less spatter, and the weld layer is aesthetically pleasing with no visible defects such as cracks or pores.

[0117] (2) XRD test results of the weld overlay showed that the amorphous structure accounted for 47.9%;

[0118] (3) The Brinell hardness of the weld overlay is 686 HBW;

[0119] (4) The high-temperature erosion performance of the weld overlay at 600℃ is 5.66 times that of the water-cooled wall tube substrate.

[0120] Example 6

[0121] Step 1: Weigh out the following powders by mass percentage: Cr powder 27.8%, Nb powder 24.8%, B powder 9.9%, Si powder 9.9%, Mo powder 16.8%, W powder 9.8%, and the remainder is Fe powder. The sum of the mass percentages of the above components is 100%.

[0122] Step 2: Place the weighed powder from Step 1 into a vacuum heating furnace and heat it at 255℃ for 2.8 hours to remove the water of crystallization from the powder. After drying, place the powder into a powder mixer for thorough mixing for 2.7 hours.

[0123] Step 3: Using Fe60Cr40 steel strip as the welding layer, the grease on the surface of the Fe60Cr40 steel strip is removed with alcohol. The flux-cored wire drawing equipment is used to wrap the flux powder prepared in step 2 inside the Fe60Cr40 steel strip. The diameter of the first drawing die is 2.6mm.

[0124] Step 4: After the first drawing process is completed, the die hole diameter is reduced one by one to finally obtain a flux-cored wire with a diameter of 1.2mm;

[0125] Step 5: After the flux-cored welding wire is drawn, it is wound onto the welding wire spool by a wire winding machine and finally sealed in a flux-cored welding wire vacuum packaging bag for later use.

[0126] Arc welding was performed on the surface of the water-cooled wall tube using the amorphous coated welding wire provided in Example 6, and the results are as follows:

[0127] (1) The arc is stable during the welding process, with less spatter, and the weld layer is aesthetically pleasing with no visible defects such as cracks or pores.

[0128] (2) XRD test results of the weld overlay showed that the amorphous structure accounted for 45.5%;

[0129] (3) The Brinell hardness of the weld overlay is 683 HBW;

[0130] (4) The high-temperature erosion performance of the weld overlay at 600℃ is 5.98 times that of the water-cooled wall tube substrate.

[0131] This disclosure presents a high-temperature erosion-resistant Fe-based amorphous coating welding wire and its preparation method, which has the following advantages compared to the prior art:

[0132] (1) The welding wire formulation disclosed herein is simplified, requiring only a small amount of powder components, which greatly reduces raw material costs and production complexity, making it particularly suitable for industrial mass production; and the welding wire diameter is optimized to 1.2 mm, which has both good wire feeding stability and deposition efficiency.

[0133] (2) This disclosure innovatively designs an Fe-Cr-Nb-BW-Si-Mo amorphous alloy welding wire, and successfully prepares a high-performance weld overlay with an amorphous content ≥44% by optimizing the alloy composition and process parameters. This weld overlay has Fe2Nb, FeCr, FeMo, and Fe atoms uniformly distributed in the amorphous matrix. 13 The presence of nanocrystalline phases such as Mo2B5 forms a unique amorphous-nanocrystalline composite structure. This special microstructure significantly enhances the high-temperature erosion resistance of the weld overlay, enabling it to exhibit excellent service performance under harsh conditions such as high temperature and high wear.

[0134] (3) The welding wire disclosed herein can be used for welding protection of the fire-facing surface of the water-cooled wall in thermal power plants. The weld overlay is mainly composed of amorphous phase + part solid solution + part nanocrystalline phase, and has excellent high-temperature erosion and high-temperature corrosion performance.

[0135] (4) The amorphous alloy welding wire provided in this disclosure can directly prepare a high-amorphous-content weld overlay using conventional arc welding processes. It exhibits strong process compatibility, enabling efficient automated operations using MIG welding as well as precision operations using TIG welding, meeting the needs of different application scenarios and overcoming the limitations of traditional amorphous material preparation methods that rely on rapid cooling techniques (such as the strip-spinning method). Compared to existing amorphous material preparation processes, this invention simplifies the process, reduces costs, and is easier to industrialize, demonstrating significant engineering application value.

[0136] It is understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of this disclosure, and this disclosure is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the spirit and substance of this disclosure, and these modifications and improvements are also considered to be within the scope of protection of this disclosure.

Claims

1. A high-temperature erosion-resistant Fe-based amorphous coated welding wire, characterized in that, The welding wire comprises: a flux core and a welding sheath; wherein... The core comprises 25-28% Cr powder, 23-25% Nb powder, 8-10% B powder, 8-10% Si powder, 15-17% Mo powder, 8-10% W powder, and the balance Fe powder. The weld bead is made of Fe60Cr40 steel strip.

2. The high-temperature erosion-resistant Fe-based amorphous coated welding wire according to claim 1, characterized in that, The thickness of the weld bead is 0.2-0.4 mm, and the width is 6-8 mm.

3. The high-temperature erosion-resistant Fe-based amorphous coated welding wire according to claim 1, characterized in that, The filler content of the welding wire should be controlled between 22 and 25 wt%.

4. A method for preparing a high-temperature erosion-resistant Fe-based amorphous coated welding wire as described in any one of claims 1 to 3, characterized in that, The method includes: Weigh out 25-28% Cr powder, 23-25% Nb powder, 8-10% B powder, 8-10% Si powder, 15-17% Mo powder, 8-10% W powder, and the remainder Fe powder as the pharmaceutical powder. The powder is placed in a vacuum furnace for heating treatment, and the dried powder is then mixed. The welding wire is pretreated and then drawn by wrapping the flux powder inside the welding wire.

5. The method according to claim 4, characterized in that, The particle size of the powder is 100-200 mesh.

6. The method according to claim 4, characterized in that, The heat treatment temperature is 220–260℃, and the holding time is 1–3 hours.

7. The method according to claim 4, characterized in that, The mixing time for the dried medicinal powder is 1 to 3 hours.

8. The method according to claim 4, characterized in that, In the drawing process, the diameter of the first drawing die is 2.6 mm.

9. The method according to claim 4, characterized in that, The diameter of the welding wire is 1-1.5 mm.