Self-cleaning bionic anti-drag film based on sharkskin surface structure and preparation process of self-cleaning bionic anti-drag film
By introducing antistatic polyurethane coating and photocuring technology onto the drag-reducing membrane, combined with the microstructure of shark skin surface, a self-cleaning biomimetic drag-reducing membrane was prepared, which solved the problem of contaminant accumulation in complex environments and improved the membrane's durability and drag-reducing effect.
Patent Information
- Application Number
- CN202511564959.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-10-30
- Publication Date
- 2026-01-06
AI Technical Summary
Existing drag-reducing membranes tend to accumulate pollutants in complex environments, increasing drag and accelerating corrosion and aging, thus affecting service life and drag reduction effect.
A self-cleaning biomimetic drag-reducing membrane fabrication process based on the surface structure of shark skin was adopted. By coating an antistatic polyurethane coating on a high-temperature resistant thermoplastic polyurethane film and performing thermo-curing and photo-curing to form a microstructure, the microstructure was then laminated with a release film and laser-perforated to prepare a biomimetic drag-reducing membrane with self-cleaning effect.
It achieves a self-cleaning effect for the drag-reducing membrane, improves its heat resistance, thermal conductivity and corrosion resistance, extends its service life and maintains its drag-reducing performance.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of biomimetic drag-reducing membrane preparation technology, specifically to a self-cleaning biomimetic drag-reducing membrane based on the surface structure of shark skin and its preparation process. Background Technology
[0002] The drag-reducing membrane has a fine microstructure on its surface, inspired by the biomimetic structure of shark skin. Shark skin has tiny ribs on its surface, which can effectively reduce water resistance. Based on this, a biomimetic drag-reducing membrane was designed and applied to modern transportation vehicles, such as airplanes and high-speed trains, to change the friction between airflow and the fuselage, thereby achieving drag reduction.
[0003] However, due to long-term exposure to complex environments such as rain and sun, various pollutants easily accumulate on the surface of the drag-reducing membrane, which not only increases the drag resistance but also accelerates the corrosion and aging of the drag-reducing membrane, affecting its service life and drag reduction effect.
[0004] Therefore, we propose a self-cleaning biomimetic drag-reducing membrane based on the surface structure of shark skin and its preparation process. By introducing titanium dioxide with photodegradable self-cleaning effect into a polyurethane coating and curing it to form a coating, a self-cleaning effect is achieved. Summary of the Invention
[0005] The purpose of this invention is to provide a self-cleaning biomimetic drag-reducing membrane based on the surface structure of shark skin and its preparation process, so as to solve the problems raised in the prior art.
[0006] To achieve the above objectives, the present invention provides the following technical solution: a preparation process for a self-cleaning biomimetic drag-reducing membrane based on the surface structure of shark skin, comprising the following steps: Step A: Take a high-temperature resistant thermoplastic polyurethane film, coat one side with an antistatic polyurethane coating, heat cure it, then emboss and light cure it to obtain a drag-reducing layer with a microstructure. Step B: Coat the side of the high-temperature resistant thermoplastic polyurethane film away from the drag-reducing layer with polyurethane adhesive, and bond it with the release film. Then, perform laser perforation and cutting to obtain a self-cleaning biomimetic drag-reducing film.
[0007] Furthermore, in step A, the thickness of the high-temperature resistant thermoplastic polyurethane film is 20~30μm; In step A, the coating thickness of the antistatic polyurethane coating is 40~60μm; In step A, the microstructure is grooved, and the groove is V-shaped or U-shaped; The height of the trench is 20~40μm; the width of the trench is 10~20μm; When the trench is V-shaped, the apex angle of the trench is 50~60°.
[0008] Furthermore, in step A, the thermosetting process conditions are: temperature 110~120℃, time 2~3min; In step A, the photocuring process conditions are as follows: irradiation with a UV lamp at an intensity of 60~80 mW / cm². 2 Irradiation time: 10-20 minutes.
[0009] Furthermore, in step B, the coating thickness of the polyurethane adhesive is 5~15μm.
[0010] Furthermore, in step B, the release film is either a PET (polyethylene terephthalate) release film or a PC (polycarbonate) release film.
[0011] Furthermore, in step B, the diameter of the holes formed by laser perforation is 0.5~0.7mm, and the spacing between the holes is 5~7mm.
[0012] Furthermore, in step A, the high-temperature resistant thermoplastic polyurethane film is prepared by the following process: Step 1: Resorcinol di(2-hydroxyethyl) ether, dodecanediol, 3,3',4,4'-benzophenone tetracarboxylic dianhydride and catalyst 1 are mixed and heated under nitrogen atmosphere. After the reaction is completed, dehydration is carried out under vacuum. Chain extender and 11-hydroxyundecanoic acid are added and mixed. The temperature is increased and the reaction is carried out under vacuum to obtain polyol. Step 2: Mix the polyol, 4,4-diisocyanate dicyclohexylmethane, and catalyst 2 evenly, heat and react to obtain a high-temperature resistant polyurethane prepolymer, then add a chain extender, melt extrude through a screw extruder, cast and molded, and cooled to obtain a high-temperature resistant thermoplastic polyurethane film.
[0013] Furthermore, in step 1, the mass ratio of resorcinol di(2-hydroxyethyl) ether, dodecyl glycol, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, catalyst 1, chain extender, and 11-hydroxyundecanoic acid is (25~35):(15~25):(50~70):(0.05~0.09):(1~3):(1.5~3.5).
[0014] Furthermore, in step 1, the process conditions for the heating reaction are: temperature 130~140℃, time 2.0~2.2h; In step 1, the process conditions for vacuum dehydration are: temperature 210~250℃, time 4~6h, and vacuum degree -0.08~-0.10MPa.
[0015] Furthermore, in step 1, the heating reaction is divided into three stages. The process conditions for the first stage heating reaction are: temperature 155~165℃, time 1.8~2.0h. The process conditions for the second stage of heating reaction are: temperature 170~180℃, time 0.8~1.0h; The process conditions for the third stage heating reaction are: temperature 200~205℃, time 0.8~1.0h.
[0016] Furthermore, in step 2, the mass ratio of polyol, 4,4-diisocyanate dicyclohexylmethane, catalyst 2, and chain extender is 10:(6~8):(0.10~0.15):(0.5~1.5).
[0017] Furthermore, in step 2, the process conditions for the heating reaction are: temperature 85~95℃, time 2.5~3.0h; In step 2, the process conditions for melt extrusion are: temperature 205~215℃, rotation speed 45~55r / min, and extrusion pressure 9~11MPa.
[0018] Furthermore, the catalyst 1 is tetraisopropyl titanate; The catalyst 2 is stannous octoate; The chain extender is 1,4-butanediol.
[0019] In the above technical solution, the hydroxyl groups of resorcinol di(2-hydroxyethyl) ether and dodecanediol undergo ring-opening esterification with the anhydride of 3,3',4,4'-benzophenone tetracarboxylic dianhydride to generate a prepolymer of ester and carboxyl groups. Then, a chain extender and 11-hydroxyundecanoic acid are added, and esterification polycondensation continues under the action of catalyst 1 to form a polyol. This polyol is then mixed and reacted with 4,4-diisocyanate dicyclohexylmethane, and then melt-extruded to obtain a high-temperature resistant thermoplastic polyurethane film. The structure of resorcinol di(2-hydroxyethyl) ether contains both benzene rings and ether bonds, combining rigidity and flexibility, resulting in good mechanical properties. The hydroxyl groups on it react with 3,3',4,4'-benzophenone tetracarboxylic dianhydride to form ester bonds. The resulting polyol contains both ester and ether bonds, which compensates for the performance shortcomings of single polyethers or polyesters. The ester bonds provide polar sites, enhance intermolecular interactions, and improve the mechanical properties of the film. The ether bonds have excellent hydrolysis resistance and good molecular chain flexibility, which compensates for the problem of excessive rigidity causing the film to be prone to breakage.
[0020] Furthermore, in step A, the preparation process of the antistatic polyurethane coating is as follows: S1: 11-hydroxyundecanoic acid, methanol, and 3-buten-1-amine are mixed, heated under reflux, rotary evaporated, and dried under vacuum. Then, 1-vinylimidazolium, methacryloyloxyethyltrimethylammonium chloride, styrene, and anhydrous ethanol are mixed. Under nitrogen atmosphere, initiator 1 is added, the mixture is heated and stirred, cooled, and then precipitated in n-hexane and dried to obtain the modified quaternary ammonium salt. S2: The modified quaternary ammonium salt, 4,4-diisocyanate dicyclohexylmethane, and pentamethyldiethylenetriamine are mixed and heated to react, thereby obtaining the isocyanate prepolymer; S3: Mix polyol, isocyanate prepolymer, mercaptolated titanium dioxide, dibutyltin dilaurate, and solvent, heat and stir to react, then add caprolactone acrylate and tripropylene glycol methyl ether and continue stirring to react for 2.0~2.5h. Cool down to 50℃, add initiator 2, and stir for 20~40min to obtain antistatic polyurethane coating.
[0021] Furthermore, in S1, the mass ratio of 11-hydroxyundecanoic acid, methanol, 3-buten-1-amine, 1-vinylimidazole, methacryloyloxyethyltrimethylammonium chloride, styrene, anhydrous ethanol, and initiator 1 is 1:(5~10):(1.1~1.3):(0.2~0.4):(0.4~0.6):(0.1~0.3):(20~30):(0.1~0.3). The initiator 1 is benzoyl peroxide.
[0022] Furthermore, in S1, the process conditions for the heating reflux reaction are: temperature 150~170℃, time 20~24h; In S1, the process conditions for heating and stirring reaction are: temperature 80~90℃, time 4~6h; In S1, the drying process conditions are: temperature 75~85℃, time 8~12h.
[0023] Furthermore, in S2, the mass ratio of modified quaternary ammonium salt, 4,4-diisocyanate dicyclohexylmethane, and pentamethyldiethylenetriamine is (10~30):(5~15):(0.01~0.03).
[0024] Furthermore, in S2, the process conditions for the heating reaction are: temperature 80~90℃, time 0.5~1.0h.
[0025] Furthermore, in S3, the mass ratio of polyol, isocyanate prepolymer, mercaptolated titanium dioxide, dibutyltin dilaurate, solvent, caprolactone acrylate, tripropylene glycol methyl ether, and initiator 2 is (20~25):(30~40):(2.5~4.5):(0.02~0.06):50:(8~10):(1~3):(0.5~0.7); The solvent is one or a mixture of two of N,N-dimethylformamide and toluene; The initiator 2 is 1-hydroxycyclohexylphenyl ketone.
[0026] Furthermore, in S3, the process conditions for heating and stirring reaction are: temperature 80~85℃, time 0.3~0.5h, and stirring speed 200~300r / min.
[0027] Furthermore, in S3, the thiolized titanium dioxide is prepared by the following process: Under a nitrogen atmosphere, γ-mercaptopropyltriethoxysilane and a 50-60% (w / w) aqueous ethanol solution were mixed, and nano-titanium dioxide was added while stirring. The mixture was heated to 35-45℃ and stirred for 2-4 hours. After washing, centrifugation at 5000-7000 r / min and drying, mercapto-modified titanium dioxide was obtained.
[0028] Furthermore, the ratio of γ-mercaptopropyltriethoxysilane, aqueous ethanol solution, and nano-titanium dioxide is 10 mL: (15~25) mL: (4~6) g.
[0029] Furthermore, the drying process conditions are: temperature 70~80℃, time 6~8h.
[0030] In the above technical solution, the carboxyl group of 11-hydroxyundecanoic acid first undergoes an amidation reaction with the amino group of 3-buten-1-amine to generate an amide bond, retaining the hydroxyl group and double bond. Then, it is copolymerized with 1-vinylimidazole and methacryloyloxyethyltrimethylammonium chloride to obtain a modified quaternary ammonium salt containing amide bonds, hydroxyl groups, and imidazole groups. Next, the isocyanate group is reacted with the hydroxyl group to form an isocyanate group from the reaction of 4,4-diisocyanate dicyclohexylmethane to obtain an isocyanate prepolymer. Finally, it is reacted with a polyol, mercaptolated titanium dioxide, and caprolactone acrylate to obtain an antistatic polyurethane. Ester coatings; Titanium dioxide has good photodegradation and self-cleaning effects. Modification of nano-titanium dioxide with γ-mercaptopropyltriethoxysilane ensures uniform dispersion of titanium dioxide in the system and provides thiol groups for subsequent reactions with double bonds. The modified quaternary ammonium salt contains amide bonds and imidazole groups, exhibiting good high-temperature stability and antistatic properties. The hydroxyl groups provide conditions for subsequent prepolymerization reactions. The added caprolactone acrylate crosslinks with the thiolized titanium dioxide during photocuring, improving the heat resistance, thermal conductivity, and corrosion resistance of the antistatic polyurethane coating.
[0031] Compared with the prior art, the beneficial effects of the present invention are: 1. The structure of resorcinol di(2-hydroxyethyl) ether contains both benzene rings and ether bonds, combining rigidity and flexibility, and exhibiting good mechanical properties. The hydroxyl groups on it react with 3,3',4,4'-benzophenone tetracarboxylic dianhydride to form ester bonds. The resulting polyol contains both ester and ether bonds, which compensates for the performance shortcomings of single polyethers or polyesters. The ester bonds provide polar sites, enhance intermolecular interactions, and improve the mechanical properties of the film. The ether bonds have excellent hydrolysis resistance and good molecular chain flexibility, which compensates for the problem of excessive rigidity causing the film to be prone to breakage.
[0032] 2. Titanium dioxide exhibits good photodegradation and self-cleaning properties. Modification of nano-titanium dioxide with γ-mercaptopropyltriethoxysilane ensures uniform dispersion of titanium dioxide in the system and provides thiol groups to facilitate subsequent reactions with double bonds. The modified quaternary ammonium salt contains amide bonds and imidazole groups, exhibiting good high-temperature stability and antistatic properties. The hydroxyl groups provide conditions for subsequent prepolymerization reactions. The added caprolactone acrylate crosslinks with the thiolized titanium dioxide during photocuring, improving the heat resistance, thermal conductivity, and corrosion resistance of the antistatic polyurethane coating. Detailed Implementation
[0033] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0034] In the following specific implementation, Polyurethane adhesive, model JA-2018R; The release film is a PET release film with a thickness of 12~14μm; Nano-sized titanium dioxide, with an average diameter of 20 nm and a length of 2~10 μm; Initiator 1 is benzoyl peroxide; Initiator 2 is 1-hydroxycyclohexylphenyl ketone; The solvent is N,N-dimethylformamide; Catalyst 1 is tetraisopropyl titanate; Catalyst 2 is stannous octoate; The chain extender is 1,4-butanediol; TPU film, 50μm thick.
[0035] Example 1: The fabrication process of a self-cleaning biomimetic drag-reducing membrane based on shark skin surface structure includes the following steps: (1) Preparation of antistatic polyurethane coating: Under a nitrogen atmosphere, γ-mercaptopropyltriethoxysilane and a 60% (w / w) aqueous ethanol solution were mixed, and nano-titanium dioxide was added while stirring. The mixture was heated to 45°C and stirred for 4 hours. After washing, centrifugation at 7000 r / min, and drying, mercapto-titrated titanium dioxide was obtained. The ratio of γ-mercaptopropyltriethoxysilane, aqueous ethanol solution, and nano-titanium dioxide was 10 mL: 25 mL: 6 g. The drying conditions were: temperature 80°C, time 8 hours. S1: 11-Hydroxyundecanoic acid, methanol, and 3-buten-1-amine are mixed and heated under reflux. The mixture is then rotary evaporated, dried under vacuum, and mixed with 1-vinylimidazolium, methacryloyloxyethyltrimethylammonium chloride, styrene, and anhydrous ethanol. Benzoyl peroxide is added under a nitrogen atmosphere, and the mixture is heated and stirred. After cooling, the mixture is precipitated in n-hexane and dried to obtain the modified quaternary ammonium salt. S2: The modified quaternary ammonium salt, 4,4-diisocyanate dicyclohexylmethane, and pentamethyldiethylenetriamine are mixed and heated to obtain the isocyanate. Prepolymer; S3: Polyol, isocyanate prepolymer, mercaptolated titanium dioxide, dibutyltin dilaurate, and N,N-dimethylformamide are mixed, heated and stirred to react, then caprolactone acrylate and tripropylene glycol methyl ether are added and stirred for another 2.5 h. The mixture is then cooled to 50 °C, 1-hydroxycyclohexylphenyl ketone is added, and stirred for 40 min to obtain an antistatic polyurethane coating; In S1, 11-hydroxyundecanoic acid, methanol, 3-buten-1-amine, 1-vinylimidazolium, methacryloyloxyethyltrimethylammonium chloride, and styrene are present. The mass ratio of anhydrous ethanol and benzoyl peroxide is 1:10:1.3:0.4:0.6:0.3:30:0.3; In S1, the process conditions for the heating and reflux reaction are: temperature 170℃, time 24h; In S1, the process conditions for the heating and stirring reaction are: temperature 90℃, time 6h; In S1, the process conditions for drying are: temperature 85℃, time 12h; In S2, the mass ratio of modified quaternary ammonium salt, 4,4-diisocyanate dicyclohexylmethane, and pentamethyldiethylenetriamine is 30:15:0. 03; In S2, the process conditions for the heating reaction are: temperature 90℃, time 1.0h; In S3, the mass ratio of polyol, isocyanate prepolymer, mercaptolated titanium dioxide, dibutyltin dilaurate, N,N-dimethylformamide, caprolactone acrylate, tripropylene glycol methyl ether, and 1-hydroxycyclohexylphenyl ketone is 25:40:4.5:0.06:50:10:3:0.7; In S3, the process conditions for the heating and stirring reaction are: temperature 85℃, time 0.5h, and stirring speed 300r / min; (2) Preparation of high-temperature resistant thermoplastic polyurethane film: Step 1: Resorcinol di(2-hydroxyethyl) ether, dodecyl glycol, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, and tetraisopropyl titanate are mixed and heated under a nitrogen atmosphere. After the reaction is complete, dehydration is carried out under vacuum. 1,4-Butanediol and 11-hydroxyundecanoic acid are added and mixed. The reaction is continued at a higher temperature and dehydrated under vacuum to obtain a polyol. Step 2: The polyol, 4,4-diisocyanate dicyclohexylmethane, and stannous octoate are mixed. The mixture is stirred until homogeneous, heated to react, and a high-temperature resistant polyurethane prepolymer is obtained. Then, 1,4-butanediol is added, and the mixture is melt-extruded, cast, and cooled using a screw extruder to obtain a high-temperature resistant thermoplastic polyurethane film. In step 1, the mass ratio of resorcinol di(2-hydroxyethyl) ether, dodecyl glycol, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, tetraisopropyl titanate, 1,4-butanediol, and 11-hydroxyundecanoic acid is 35:25:70:0.0 9:3:3.5; In step 1, the heating reaction conditions are: temperature 140℃, time 2.2h; In step 1, the vacuum dehydration process conditions are: temperature 250℃, time 6h, vacuum degree -0.10MPa; In step 1, the heating reaction is divided into three stages. The process conditions for the first stage heating reaction are: temperature 165℃, time 2.0h; The process conditions for the second stage heating reaction are: temperature 180℃, time 1.0h; The third stage... The process conditions for the heating reaction are: temperature 205℃, time 1.0h; in step 2, the mass ratio of polyol, 4,4-diisocyanate dicyclohexylmethane, stannous octoate, and 1,4-butanediol is 10:8:0.15:1.5; in step 2, the process conditions for the heating reaction are: temperature 95℃, time 3.0h; in step 2, the process conditions for melt extrusion are: temperature 215℃, rotation speed 55r / min, and extrusion pressure 11MPa. (3) Preparation of self-cleaning biomimetic drag-reducing membrane: Step A: Take a high-temperature resistant thermoplastic polyurethane film, coat one side with an antistatic polyurethane coating, perform thermosetting, then emboss and photocur, to obtain a drag-reducing layer with a microstructure; Step B: Coat the side of the high-temperature resistant thermoplastic polyurethane film away from the drag-reducing layer with polyurethane adhesive, and bond it with a PET release film, then perform laser perforation and cutting to obtain a self-cleaning biomimetic drag-reducing membrane; In Step A, the thickness of the high-temperature resistant thermoplastic polyurethane film is 30μm; In Step A, the coating thickness of the antistatic polyurethane coating is 60μm; In Step A, the microstructure is grooved, the grooves are V-shaped, the apex angle of the groove is 60°, the height of the groove is 40μm, and the width of the groove is 20μm; In Step A, the thermosetting process conditions are: temperature 120℃, time 3min; In Step A, the photocuring process conditions are: irradiation with a UV lamp, irradiation intensity of 80mW / cm². 2The irradiation time is 20 min; in step B, the coating thickness of the polyurethane adhesive is 15 μm; in step B, the diameter of the small hole formed by laser perforation is 0.7 mm, and the hole spacing is 7 mm.
[0036] Example 2: The preparation process of a self-cleaning biomimetic drag-reducing membrane based on shark skin surface structure includes the following steps: (1) Preparation of antistatic polyurethane coating: Under a nitrogen atmosphere, γ-mercaptopropyltriethoxysilane and a 55% (w / w) aqueous ethanol solution were mixed, and nano-titanium dioxide was added while stirring. The mixture was heated to 40°C and stirred for 3 hours. After washing, centrifugation at 6000 r / min, and drying, mercapto-titrated titanium dioxide was obtained. The ratio of γ-mercaptopropyltriethoxysilane, aqueous ethanol solution, and nano-titanium dioxide was 10 mL: 20 mL: 5 g. The drying conditions were: temperature 75°C, time 7 hours. S1: 11-Hydroxyundecanoic acid, methanol, and 3-buten-1-amine are mixed and heated under reflux. The mixture is then rotary evaporated, dried under vacuum, and mixed with 1-vinylimidazolium, methacryloyloxyethyltrimethylammonium chloride, styrene, and anhydrous ethanol. Benzoyl peroxide is added under a nitrogen atmosphere, and the mixture is heated and stirred. After cooling, the mixture is precipitated in n-hexane and dried to obtain the modified quaternary ammonium salt. S2: The modified quaternary ammonium salt, 4,4-diisocyanate dicyclohexylmethane, and pentamethyldiethylenetriamine are mixed and heated to obtain the isocyanate. Prepolymer; S3: Polyol, isocyanate prepolymer, mercaptolated titanium dioxide, dibutyltin dilaurate, and N,N-dimethylformamide are mixed, heated and stirred to react, then caprolactone acrylate and tripropylene glycol methyl ether are added and the reaction is continued for 2.3 h. The mixture is cooled to 50 °C, 1-hydroxycyclohexylphenyl ketone is added, and the mixture is stirred for 30 min to obtain an antistatic polyurethane coating; In S1, 11-hydroxyundecanoic acid, methanol, 3-buten-1-amine, 1-vinylimidazolium, methacryloyloxyethyltrimethylammonium chloride, and styrene are present. The mass ratio of alkene, anhydrous ethanol, and benzoyl peroxide is 1:8:1.2:0.3:0.5:0.2:25:0.2; In S1, the reflux reaction conditions are: temperature 160℃, time 22h; In S1, the stirring reaction conditions are: temperature 85℃, time 5h; In S1, the drying conditions are: temperature 80℃, time 10h; In S2, the mass ratio of modified quaternary ammonium salt, 4,4-diisocyanate dicyclohexylmethane, and pentamethyldiethylenetriamine is 20:10:0. .02; In S2, the process conditions for the heating reaction are: temperature 85℃, time 0.8h; In S3, the mass ratio of polyol, isocyanate prepolymer, mercaptolated titanium dioxide, dibutyltin dilaurate, N,N-dimethylformamide, caprolactone acrylate, tripropylene glycol methyl ether, and 1-hydroxycyclohexylphenyl ketone is 22:35:3.5:0.04:50:9:2:0.6; In S3, the process conditions for the heating and stirring reaction are: temperature 83℃, time 0.4h, and stirring speed 250r / min; (2) Preparation of high-temperature resistant thermoplastic polyurethane film: Step 1: Resorcinol di(2-hydroxyethyl) ether, dodecyl glycol, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, and tetraisopropyl titanate are mixed and heated under a nitrogen atmosphere. After the reaction is complete, dehydration is carried out under vacuum. 1,4-Butanediol and 11-hydroxyundecanoic acid are added and mixed. The reaction is continued at a higher temperature and dehydrated under vacuum to obtain a polyol. Step 2: The polyol, 4,4-diisocyanate dicyclohexylmethane, and stannous octoate are mixed. The mixture is stirred until homogeneous, heated to react, and a high-temperature resistant polyurethane prepolymer is obtained. Then, 1,4-butanediol is added, and the mixture is melt-extruded using a screw extruder, cast, and cooled to obtain a high-temperature resistant thermoplastic polyurethane film. In step 1, the mass ratio of resorcinol di(2-hydroxyethyl) ether, dodecyl glycol, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, tetraisopropyl titanate, 1,4-butanediol, and 11-hydroxyundecanoic acid is 30:20:60:0.0 8:2:2.5; In step 1, the heating reaction conditions are: temperature 135℃, time 2.1h; In step 1, the vacuum dehydration process conditions are: temperature 230℃, time 5h, vacuum degree -0.09MPa; In step 1, the heating reaction is divided into three stages. The process conditions for the first stage heating reaction are: temperature 160℃, time 1.9h; The process conditions for the second stage heating reaction are: temperature 175℃, time 0.9h; The third stage... The process conditions for the heating reaction are: temperature 203℃, time 0.9h; in step 2, the mass ratio of polyol, 4,4-diisocyanate dicyclohexylmethane, stannous octoate, and 1,4-butanediol is 10:7:0.13:1.0; in step 2, the process conditions for the heating reaction are: temperature 90℃, time 2.8h; in step 2, the process conditions for melt extrusion are: temperature 210℃, rotation speed 50r / min, and extrusion pressure 10MPa. (3) Preparation of self-cleaning biomimetic drag-reducing membrane: Step A: Take a high-temperature resistant thermoplastic polyurethane film, coat one side with an antistatic polyurethane coating, perform thermosetting, then emboss and photocur, to obtain a drag-reducing layer with a microstructure; Step B: Coat the side of the high-temperature resistant thermoplastic polyurethane film away from the drag-reducing layer with polyurethane adhesive, and bond it with a PET release film, then perform laser perforation and cutting to obtain a self-cleaning biomimetic drag-reducing membrane; In Step A, the thickness of the high-temperature resistant thermoplastic polyurethane film is 25μm; In Step A, the coating thickness of the antistatic polyurethane coating is 50μm; In Step A, the microstructure is grooved, the grooves are V-shaped, the apex angle of the groove is 55°, the height of the groove is 30μm, and the width of the groove is 15μm; In Step A, the thermosetting process conditions are: temperature 115℃, time 2.5min; In Step A, the photocuring process conditions are: irradiation with a UV lamp, irradiation intensity of 70mW / cm². 2The irradiation time is 15 min; in step B, the coating thickness of the polyurethane adhesive is 10 μm; in step B, the diameter of the small hole formed by laser perforation is 0.6 mm, and the hole spacing is 6 mm.
[0037] Example 3: The preparation process of a self-cleaning biomimetic drag-reducing membrane based on shark skin surface structure includes the following steps: (1) Preparation of antistatic polyurethane coating: Under a nitrogen atmosphere, γ-mercaptopropyltriethoxysilane and a 50% (w / w) aqueous ethanol solution were mixed, and nano-titanium dioxide was added while stirring. The mixture was heated to 35°C and stirred for 2 hours. After washing, centrifugation at 5000 r / min, and drying, mercapto-titrated titanium dioxide was obtained. The ratio of γ-mercaptopropyltriethoxysilane, aqueous ethanol solution, and nano-titanium dioxide was 10 mL: 15 mL: 4 g. The drying conditions were: temperature 70°C, time 6 hours. S1: 11-Hydroxyundecanoic acid, methanol, and 3-buten-1-amine are mixed and heated under reflux. The mixture is then rotary evaporated, dried under vacuum, and mixed with 1-vinylimidazolium, methacryloyloxyethyltrimethylammonium chloride, styrene, and anhydrous ethanol. Benzoyl peroxide is added under a nitrogen atmosphere, and the mixture is heated and stirred. After cooling, the mixture is precipitated in n-hexane and dried to obtain the modified quaternary ammonium salt. S2: The modified quaternary ammonium salt, 4,4-diisocyanate dicyclohexylmethane, and pentamethyldiethylenetriamine are mixed and heated to obtain isocyanic acid. Ester prepolymer; S3: Polyol, isocyanate prepolymer, mercaptolated titanium dioxide, dibutyltin dilaurate, and N,N-dimethylformamide are mixed, heated and stirred to react, then caprolactone acrylate and tripropylene glycol methyl ether are added and stirred for another 2.0 h. The mixture is then cooled to 50 °C, 1-hydroxycyclohexylphenyl ketone is added, and stirred for 20 min to obtain an antistatic polyurethane coating; In S1, 11-hydroxyundecanoic acid, methanol, 3-buten-1-amine, 1-vinylimidazolium, methacryloyloxyethyltrimethylammonium chloride, and benzene are present. The mass ratio of ethylene, anhydrous ethanol, and benzoyl peroxide is 1:5:1.1:0.2:0.4:0.1:20:0.1; In S1, the process conditions for the reflux reaction are: temperature 150℃, time 20h; In S1, the process conditions for the stirring reaction are: temperature 80℃, time 4h; In S1, the drying process conditions are: temperature 75℃, time 8h; In S2, the mass ratio of modified quaternary ammonium salt, 4,4-diisocyanate dicyclohexylmethane, and pentamethyldiethylenetriamine is 10:5:0. In S1; the process conditions for the heating reaction are: temperature 80℃, time 0.5h; in S3, the mass ratio of polyol, isocyanate prepolymer, mercaptolated titanium dioxide, dibutyltin dilaurate, N,N-dimethylformamide, caprolactone acrylate, tripropylene glycol methyl ether, and 1-hydroxycyclohexylphenyl ketone is 20:30:2.5:0.02:50:8:1:0.5; in S3, the process conditions for the heating and stirring reaction are: temperature 80℃, time 0.3h, and stirring speed 200r / min. (2) Preparation of high-temperature resistant thermoplastic polyurethane film: Step 1: Resorcinol di(2-hydroxyethyl) ether, dodecyl glycol, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, and tetraisopropyl titanate are mixed and heated under a nitrogen atmosphere. After the reaction is complete, dehydration is carried out under vacuum. 1,4-Butanediol and 11-hydroxyundecanoic acid are added and mixed. The temperature is raised and the reaction is continued. Dehydration is carried out under vacuum to obtain a polyol. Step 2: The polyol, 4,4-diisocyanate dicyclohexylmethane, and stannous octoate are mixed... The mixture is stirred evenly and heated to react, yielding a high-temperature resistant polyurethane prepolymer. Then, 1,4-butanediol is added, and the mixture is melt-extruded, cast, and cooled using a screw extruder to obtain a high-temperature resistant thermoplastic polyurethane film. In step 1, the mass ratio of resorcinol di(2-hydroxyethyl) ether, dodecyl glycol, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, tetraisopropyl titanate, 1,4-butanediol, and 11-hydroxyundecanoic acid is 25:15:50:0. 05:1:1.5; In step 1, the heating reaction conditions are: temperature 130℃, time 2.0h; In step 1, the vacuum dehydration process conditions are: temperature 210℃, time 4h, vacuum degree -0.08MPa; In step 1, the heating reaction is divided into three stages. The process conditions for the first stage heating reaction are: temperature 155℃, time 1.8h; The process conditions for the second stage heating reaction are: temperature 170℃, time 0.8h; The third... The process conditions for the first heating reaction are: temperature 200℃, time 0.8h; in step 2, the mass ratio of polyol, 4,4-diisocyanate dicyclohexylmethane, stannous octoate, and 1,4-butanediol is 10:6:0.10:0.5; the process conditions for the second heating reaction are: temperature 85℃, time 2.5h; the process conditions for the third melt extrusion are: temperature 205℃, rotation speed 45r / min, and extrusion pressure 9MPa. (3) Preparation of self-cleaning biomimetic drag-reducing membrane: Step A: Take a high-temperature resistant thermoplastic polyurethane film, coat one side with an antistatic polyurethane coating, perform thermosetting, then emboss and photocur, to obtain a drag-reducing layer with a microstructure; Step B: Coat the side of the high-temperature resistant thermoplastic polyurethane film away from the drag-reducing layer with polyurethane adhesive, and bond it with a PET release film, then perform laser perforation and cutting to obtain a self-cleaning biomimetic drag-reducing membrane; In Step A, the thickness of the high-temperature resistant thermoplastic polyurethane film is 20μm; In Step A, the coating thickness of the antistatic polyurethane coating is 40μm; In Step A, the microstructure is grooved, the grooves are V-shaped, the apex angle of the groove is 50°, the height of the groove is 20μm, and the width of the groove is 10μm; In Step A, the photocuring process conditions are: irradiation with a UV lamp, the irradiation intensity is 60mW / cm². 2 The irradiation time is 10 min; in step B, the coating thickness of the polyurethane adhesive is 5 μm; in step B, the diameter of the small hole formed by laser perforation is 0.5 mm, and the hole spacing is 5 mm.
[0038] Comparative Example 1: Compared with Example 1, the high-temperature resistant thermoplastic polyurethane film was replaced with a commercially available TPU film, while all other conditions remained unchanged.
[0039] Comparative Example 2: Compared with Example 1, no modified quaternary ammonium salt was added to the antistatic polyurethane coating, and all other conditions remained the same.
[0040] Comparative Example 3: Compared with Example 1, the high-temperature resistant thermoplastic polyurethane film was replaced with a commercially available TPU film, and no modified quaternary ammonium salt was added to the antistatic polyurethane coating, while the other conditions remained unchanged.
[0041] Experiment: The self-cleaning biomimetic drag-reducing membranes obtained in the examples and comparative examples were tested for various properties; Thermal shrinkage rate: The self-cleaning biomimetic drag-reducing membrane was cut into 10×10cm samples and divided into 6 groups of 3 samples each. The samples were placed in vacuum ovens at 110℃, 125℃ and 150℃ for 2 hours, respectively, and then taken out and cooled. The transverse length and longitudinal length were measured and the thermal shrinkage rate was calculated to characterize the heat resistance of the self-cleaning biomimetic drag-reducing membrane. Antistatic performance test: The self-cleaning bionic drag-reducing film was cut into 2×2cm samples, and the surface resistance of the self-cleaning bionic drag-reducing film was tested using a high resistance meter SME-8310 to characterize its antistatic performance. ;
[0042] Based on the data in the table above, the following conclusions can be drawn: Compared with Example 1, Comparative Example 1 replaced the high-temperature resistant thermoplastic polyurethane film with a commercially available TPU film. The heat shrinkage rate of the resulting self-cleaning biomimetic drag-reducing film increased, indicating that the heat resistance of the self-cleaning biomimetic drag-reducing film decreased. This is because the high-temperature resistant thermoplastic polyurethane film in this invention uses resorcinol di(2-hydroxyethyl) ether, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, etc. as raw materials, and its molecular structure contains benzene rings and ether bonds, which have both flexibility and heat resistance. Compared with Example 1, Comparative Example 2 did not add modified quaternary ammonium salt to the antistatic polyurethane coating, and the surface resistance of the resulting self-cleaning biomimetic drag-reducing film increased, indicating that its antistatic performance decreased. Compared with Example 1, Comparative Example 3 replaced the high-temperature resistant thermoplastic polyurethane film with a commercially available TPU film, and did not add modified quaternary ammonium salt to the antistatic polyurethane coating. Both heat resistance and antistatic properties decreased. It can be seen that the selection of raw materials for the antistatic polyurethane coating and the high-temperature resistant thermoplastic polyurethane film in this invention can promote the comprehensive improvement of the heat resistance and antistatic properties of the self-cleaning biomimetic drag-reducing film.
[0043] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.
Claims
1. A preparation process of self-cleaning biomimetic drag-reducing film based on shark skin surface structure, characterized in that: The method comprises the following steps: Step A: mixing polyol, isocyanate prepolymer, mercapto titanium dioxide, dibutyl tin dilaurate and solvent, heating and stirring to react, then adding caprolactone acrylate and tripropylene glycol methyl ether to continue stirring for 2.0-2.5 hours, cooling to 50 DEG C, adding initiator 2, stirring for 20-40 minutes to obtain antistatic polyurethane coating; Step B: taking high-temperature-resistant thermoplastic polyurethane film, coating the antistatic polyurethane coating on one side of the film, performing heat curing, then performing embossing and light curing to obtain a micro-structured drag-reducing layer; Step C: coating polyurethane adhesive on the side of the high-temperature-resistant thermoplastic polyurethane film away from the drag-reducing layer, and bonding with a release film, then performing laser perforation and cutting to obtain a self-cleaning biomimetic drag-reducing film; In step A, the isocyanate prepolymer is prepared by the following process: S1: mixing 11-hydroxyundecanoic acid, methanol and 3-buten-1-amine, heating and refluxing to react, rotary evaporation, vacuum drying, then mixing with 1-vinylimidazole, methyl acryloyloxyethyl trimethyl ammonium chloride, styrene and anhydrous ethanol, adding initiator 1 under nitrogen atmosphere, heating and stirring to react, cooling, then precipitating in n-hexane, drying to obtain modified quaternary ammonium salt; S2: mixing the modified quaternary ammonium salt, 4,4-diisocyanate dicyclohexyl methane and pentamethyldiethylene triamine, heating to react to obtain isocyanate prepolymer; In step B, the microstructure is in the form of grooves, the microstructure is in the form of grooves, and the grooves are in the form of V-shape or U-shape; The height of the grooves is 20-40 microns, and the width of the grooves is 10-20 microns; When the grooves are in the form of V-shape, the top angle of the grooves is 50-60 DEG.
2. The process for the preparation of sharkskin surface structure based self-cleaning biomimetic drag reducing film as claimed in claim 1, wherein: In step B, the high-temperature-resistant thermoplastic polyurethane film is prepared by the following process: Step 1: mixing resorcinol di(2-hydroxyethyl) ether, dodecanediol, 3,3',4,4'-benzophenone tetracarboxylic dianhydride and catalyst 1, heating to react under nitrogen atmosphere, vacuum and pressure reduction dehydration after reaction; mixing with chain extender and 11-hydroxyundecanoic acid, continuing to heat to react, vacuum and pressure reduction dehydration to obtain polyol; Step 2: mixing the polyol, 4,4-diisocyanate dicyclohexyl methane and catalyst 2, stirring uniformly, heating to react to obtain high-temperature-resistant polyurethane prepolymer, then adding chain extender, melt extruding through screw extruder, casting molding and cooling to obtain high-temperature-resistant thermoplastic polyurethane film.
3. The process for the preparation of sharkskin surface structure based self-cleaning biomimetic drag reducing film as claimed in claim 1, wherein: In step A, the mercapto titanium dioxide is prepared by the following process: Mixing gamma-mercaptopropyl triethoxysilane and 50-60% ethanol aqueous solution under nitrogen atmosphere, adding nano titanium dioxide while stirring, heating to 35-45 DEG C and stirring for 2-4 hours, washing, centrifuging at 5000-7000 r / min and drying to obtain mercapto titanium dioxide.
4. The process for the preparation of sharkskin surface structure based self-cleaning biomimetic drag reducing film as claimed in claim 1, wherein: In S1, the mass ratio of 11-hydroxyundecanoic acid, methanol, 3-buten-1-amine, 1-vinylimidazole, methacryloyloxyethyltrimethylammonium chloride, styrene, anhydrous ethanol, initiator 1 is 1: (5-10): (1.1-1.3): (0.2-0.4): (0.4-0.6): (0.1-0.3): (20-30): (0.1-0.3). The initiator 1 is dibenzoyl peroxide.
5. The process for the preparation of sharkskin surface structure based self-cleaning biomimetic drag reducing film as claimed in claim 1, wherein: In S2, the mass ratio of modified quaternary ammonium salt, 4, 4-diisocyanate dicyclohexyl methane, pentamethyl diethylene triamine is (10-30): (5-15): (0.01-0.03).
6. The process for the preparation of sharkskin surface structure based self-cleaning biomimetic drag reducing film as claimed in claim 1, wherein: In step A, the mass ratio of polyol, isocyanate prepolymer, mercapto titanium dioxide, dibutyl tin dilaurate, solvent, caprolactone acrylate, tripropylene glycol methyl ether, initiator 2 is (20-25): (30-40): (2.5-4.5): (0.02-0.06): 50: (8-10): (1-3): (0.5-0.7).
7. The process for the preparation of sharkskin surface structure based self-cleaning drag reducing biomimetic film as claimed in claim 2, wherein said process comprises of the steps of: In step 1, the mass ratio of resorcinol di(2-hydroxyethyl) ether, dodecanediol, 3, 3', 4, 4'-benzophenone tetracarboxylic dianhydride, catalyst 1, chain extender, 11-hydroxyundecanoic acid is (25-35): (15-25): (50-70): (0.05-0.09): (1-3): (1.5-3.5).
8. The process for the preparation of sharkskin surface structure based self-cleaning biomimetic drag reducing film as claimed in claim 2, wherein: In step 2, the mass ratio of polyol, 4, 4-diisocyanate dicyclohexyl methane, catalyst 2, chain extender is 10: (6-8): (0.10-0.15): (0.5-1.5).
9. The process for the preparation of sharkskin surface structure based self-cleaning drag reducing biomimetic film as claimed in claim 1, wherein: The solvent is one or a mixture of two of N, N-dimethylformamide and toluene; The initiator 2 is 1-hydroxycyclohexyl phenyl ketone.
10. A self-cleaning biomimetic drag-reducing film based on the surface structure of shark skin, characterized in that: The preparation process according to any one of claims 1-9 is obtained. The preparation process according to any one of claims 1-9 is obtained.