Vanadium battery key material and preparation method and preparation system thereof

High-purity vanadium pentoxide is prepared from alkaline vanadium-containing leachate by vanadium precipitation with weakly acidic ammonium salt and sodium ammonium substitution reaction in solid phase transformation. This solves the problems of complex process, high cost and environmental pollution in the existing technology, and realizes the preparation of high-purity vanadium pentoxide and simplified production of key materials for vanadium batteries.

CN121292514APending Publication Date: 2026-01-09CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD

Patent Information

Application Number
CN202511876775.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-12-12
Publication Date
2026-01-09

AI Technical Summary

Technical Problem

Existing technologies for preparing high-purity vanadium pentoxide suffer from problems such as long process flow, high cost, serious environmental pollution, and harsh operating conditions. In particular, when using alkaline vanadium-containing leachate as raw material, there is a lack of simple and efficient impurity removal methods.

Method used

High-purity ammonium vanadate was prepared from alkaline vanadium-containing leachate by vanadium precipitation with weakly acidic ammonium salt and sodium ammonium substitution reaction in solid phase transformation. High-purity vanadium pentoxide was obtained by calcination and used to prepare key materials for vanadium batteries.

Benefits of technology

It achieves the complete removal of major impurities such as K, Na, Si, and Cr, and produces high-purity vanadium pentoxide. This simplifies the process, reduces costs, minimizes environmental pollution, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121292514A_ABST
    Figure CN121292514A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of vanadium batteries, and particularly discloses a vanadium battery key material as well as a preparation method and a preparation system thereof. The method comprises the following steps: adding ammonium salt and acid into an alkaline vanadium-containing leaching solution, and carrying out weak acid ammonium salt vanadium precipitation reaction under the conditions that the pH is 4-6 and the temperature is 20-85 DEG C to obtain a sodium ammonium decavanadate solid; the method comprises the following steps: mixing a sodium ammonium decavanadate solid with a solution containing ammonium ions, and carrying out solid-phase crystal transformation ammonium sodium replacement reaction at the temperature of 90-100 DEG C to obtain high-purity ammonium vanadate; directly calcining the high-purity ammonium vanadate or calcining the high-purity ammonium vanadate after re-dissolution recrystallization to obtain high-purity vanadium pentoxide; the high-purity vanadium pentoxide is used for preparing a vanadium battery key material. According to the scheme, the alkaline vanadium-containing leachate serves as the raw material, deep removal of impurities is achieved through weak acid ammonium salt vanadium precipitation and solid-phase crystal transformation ammonium sodium replacement, high-purity ammonium vanadate is prepared, high-purity vanadium pentoxide is further prepared, and the high-performance vanadium battery key material is prepared with the high-purity vanadium pentoxide serving as the raw material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of vanadium batteries, specifically relating to a key material for vanadium batteries and its preparation method and system. Background Technology

[0002] Vanadium redox flow battery (VRFB) is a type of flow energy storage battery that uses vanadium ions as the only active electrochemical reactant. Its core advantages are "capacity and power separation, long lifespan, and high safety". It is particularly suitable for large-scale, long-term energy storage scenarios (such as wind power / solar power consumption and grid peak shaving) and is one of the key energy storage technologies in the current new power system.

[0003] Vanadium pentoxide (V₂O₅), as a core raw material for preparing vanadium battery electrolytes, is converted into vanadium ion active components in the electrolyte through chemical or electrochemical methods, forming the basis for energy storage and conversion in vanadium batteries. The vanadium electrolyte is not only a core material of the vanadium battery system but also an energy carrier, and its performance is directly constrained by the purity level of vanadium pentoxide.

[0004] Currently, the main methods for preparing high-purity vanadium pentoxide include multi-stage precipitation, chemical purification, extraction, ion exchange, and chlorination. However, these methods generally suffer from problems such as long process flows, high preparation costs, environmental pollution, and harsh operating conditions.

[0005] Multi-stage precipitation involves repeatedly precipitating, dissolving, and reprecipitating vanadium raw materials to separate impurities. For example, Chinese patent CN119683681A proposes a closed-loop method for preparing high-purity vanadium pentoxide from ammonium metavanadate. Its core process consists of three steps: First, crude ammonium metavanadate from the Bayer process alumina is converted into ammonium polyvanadate precipitate in an acidic system (pH=2.5~3.5, 95~99℃ for 30~60 min). During this process, ammonium metavanadate dissolves and then precipitates as ammonium polyvanadate. Second, ammonium polyvanadate is recrystallized into high-purity ammonium metavanadate in an alkaline system (adjusted with ammonia, pH=8.5~9.5, dissolved at 85~95℃ and then cooled to 20~40℃ for crystallization, utilizing the difference in solubility of ammonium metavanadate at high and low temperatures). Finally, vanadium pentoxide is obtained through calcination. The vanadium pentoxide product prepared by this process achieves a purity of over 99.9% and realizes resource recycling and zero emissions. However, the vanadium precipitate product requires several precipitation-dissolution-reprecipitation processes, resulting in a long process flow and high costs. Furthermore, impurities gradually accumulate in the mother liquor during long-term circulation, potentially affecting the purity of the final product. Chinese patent CN106044853B proposes a similar process, dissolving crude ammonium metavanadate in water, acidifying it to generate ammonium polyvanadate, and then dissolving it with ammonia and recrystallizing it to obtain high-purity ammonium metavanadate. In addition, Chinese patents CN102603000A and CN102730757A both disclose technical routes for preparing high-purity vanadium pentoxide using crude sodium metavanadate as raw material. This involves alkali dissolving crude sodium metavanadate, adding magnesium salts and other impurity removal agents for liquid-phase purification, and then reprecipitating the purified liquid to obtain high-purity ammonium metavanadate. The introduction of magnesium ions during the impurity removal process may affect the purity of the final product. All of the above-mentioned patents on the preparation of high-purity vanadium pentoxide through multi-stage precipitation have the problems of high raw material costs, lengthy process flow, and high preparation costs.

[0006] Chemical purification utilizes the differences in chemical properties between substances (such as solubility, acidity / alkalinity, redox properties, and complexing ability) to transform impurities in vanadium raw materials into easily separable forms (such as precipitates, gases, water, or the target substance itself) through specific chemical reactions, thereby achieving vanadium purification. For example, Chinese patents CN114480883B and CN114477283B both employ a "metal ion synergistic precipitation method" to remove silicon (Si) and chromium (Cr) impurities from vanadium solutions. First, a reducing agent is used to reduce hexavalent chromium to trivalent chromium, and then a metal ion source (Ni) is added under alkaline conditions. 2+ and Zn 2+ At high temperatures, it reacts with silicate ions to form NiSiO3 / ZnSiO3 precipitates, and simultaneously reacts with Cr... 3+Co-precipitation generates a complex hydroxide, achieving simultaneous and deep removal of silicon and chromium. This method utilizes the principle of chemical impurity removal, producing vanadium pentoxide with a purity of 99.99%. However, the reduction process requires precise control of pH and reducing agent dosage. Incomplete reduction leads to a significant increase in chromium residue, affecting product stability. Furthermore, the resulting silicon-chromium slag is difficult to treat, resulting in a waste of chromium resources.

[0007] The core principle of extraction is to utilize the selective complexation or ion exchange between vanadium ions and specific organic extractants to achieve the directional migration of vanadium from the aqueous phase to the organic phase. Then, back-extraction efficiently transfers the vanadium back to the aqueous phase, ultimately achieving the separation of impurities and deep purification. It is generally divided into cationic extraction (VO2+ extraction). 2+ ) and anion extraction (V 10 O 28 6- For example, Chinese patent CN111057876B proposes a method for preparing high-purity vanadium pentoxide using microemulsion extraction. First, the sodium vanadium solution undergoes pre-desiliconization treatment, while the pH of the desilicon solution is adjusted to 3.0. Pentavalent vanadate ions are extracted using a microemulsion extraction system (Aliquat336 (quaternary ammonium salt, 25%), isoamyl alcohol (20%), n-heptane (51%), and 0.5 mol / L NaOH-NaCl internal aqueous phase). Then, the extract is obtained through organic phase washing and back-extraction. Finally, ammonium salt is added to precipitate vanadium to obtain high-purity ammonium metavanadate. Chinese patent CN201310377023 discloses a method for preparing high-purity vanadium pentoxide using amine extraction of heteropolyacid impurities. This method employs a completely opposite approach, extracting impurity ions from a mixed solution, leaving vanadium in the raffinate, thus achieving separation of vanadium and impurities. Although extraction methods have advantages such as good selectivity, high product purity, no impurity introduction, and recyclable extractant, multi-stage extraction and back-extraction make the process complex and extend the cycle. They also have disadvantages such as expensive and easily degraded extractants, flammable and toxic organic solvents, environmental pollution, and harsh operating conditions.

[0008] The chlorination process for preparing high-purity vanadium pentoxide uses vanadium slag, vanadium intermediates, or vanadium-based catalysts as raw materials. A chlorination reaction produces crude vanadium oxychloride (VOCl3), which is then purified by distillation to separate its boiling point from that of impurity chlorides. High-purity vanadium oxychloride is converted into the final product through hydrolysis or ammonium salt precipitation followed by calcination, or directly produced as high-purity vanadium pentoxide powder after dust removal, washing, sedimentation, and distillation under oxygen-enriched air and a catalyst. This method offers advantages such as thorough impurity separation, no ammonia nitrogen wastewater, high product purity, and low vanadium loss rate. However, it places stringent safety requirements on equipment and is currently mainly in the laboratory research and development stage. Published related patents include: CN109835949A, CN110683580A, and CN106676289A.

[0009] Furthermore, Chinese patent CN117682557A discloses a method for preparing vanadium pentoxide using sodium vanadium chloride solution containing silicon and chromium. This patent relates to the idea of ​​preparing high-purity vanadium pentoxide from sodium ammonium vanadate (SAV) through both alkali precipitation and acid precipitation, both processes involving the dissolution and recrystallization of sodium ammonium vanadate. Specifically, sodium ammonium vanadate (SAV) is obtained by two-stage pH precipitation after removing silicon from sodium vanadium chloride solution with aluminum sulfate. Then, it is obtained by hot dissolution (dissolving at 80-95℃, cooling to ≤70℃, adding ammonium sulfate, and crystallizing at 20-50℃) to obtain ammonium metavanadate, or by acid dissolution (dissolving at pH=1.8-2.5, adding ammonium sulfate, and crystallizing at 80-95℃) to obtain ammonium polyvanadate. Finally, calcination yields high-purity vanadium pentoxide. This method suffers from serious drawbacks, including high residual Si and Cr impurities (0.01-0.03%), low efficiency due to silicon removal and standing for ≥48 hours, complex multi-stage filtrate circulation operation making industrialization difficult, and high cost due to large volumes of ammonia nitrogen wastewater.

[0010] Currently, there is still a lack of a simple, efficient, and cost-effective industrial-scale process for directly preparing high-purity vanadium pentoxide (purity ≥99.9%) from alkaline vanadium-containing leachate. Summary of the Invention

[0011] The main objective of this invention is to address the shortcomings of the existing technology by providing a method for preparing high-purity vanadium pentoxide using alkaline vanadium-containing leachate as a raw material and using this as a raw material to prepare key materials for vanadium batteries.

[0012] To achieve the above objectives, the present invention adopts the following technical solution: According to a first aspect of the present invention, a method for preparing a key material for vanadium batteries is provided, comprising the following steps: S1: Add ammonium salt and acid to alkaline vanadium-containing leachate, and carry out weakly acidic ammonium salt precipitation reaction under the conditions of pH 4~6 and temperature 20~85℃ to obtain sodium decavanadate solid. S2: The sodium decavanadate solid is mixed with a solution containing ammonium ions, and a solid-phase crystallization sodium ammonium substitution reaction is carried out at a temperature of 90~100℃ to obtain high-purity ammonium vanadate. S3: The high-purity ammonium vanadate is directly calcined or calcined after recrystallization to obtain high-purity vanadium pentoxide; S4: Use the high-purity vanadium pentoxide to prepare key materials for vanadium batteries.

[0013] As a further embodiment, in step S1, the ammonium salt is at least one of ammonium sulfate, ammonium chloride, and ammonium nitrate.

[0014] As a further embodiment, in step S1, the amount of ammonium salt added is (0.22~0.41):1, calculated as the mass ratio of ammonium ions to V in the alkaline vanadium-containing leachate.

[0015] As a further embodiment, in step S1, the amount of ammonium salt added is (0.27~0.33):1, calculated as the mass ratio of ammonium ions to V in the alkaline vanadium-containing leachate.

[0016] As a further embodiment, in step S1, the acid is at least one of sulfuric acid, hydrochloric acid, and nitric acid.

[0017] As a further implementation, in step S1, the pH is 5 to 5.5.

[0018] As a further implementation method, in step S1, the reaction temperature is 20~40°C.

[0019] As a further embodiment, in step S1, the reaction time is 30-90 minutes. Preferably, the reaction time is 60 minutes.

[0020] As a further embodiment, in step S2, the solution containing ammonium ions is at least one of ammonium sulfate solution, ammonium chloride solution, and ammonium nitrate solution.

[0021] As a further embodiment, in step S2, the concentration of ammonium ions in the solution containing ammonium ions is 6~48 g / L, and the amount of sodium decavanadate solid added is 1:(5~8) based on the solid-liquid ratio of sodium decavanadate solid to the solution containing ammonium ions.

[0022] As a further embodiment, in step S2, the concentration of ammonium ions in the solution containing ammonium ions is 36~48 g / L, and the amount of sodium decavanadate solid added is 1:6 based on the solid-liquid ratio of sodium decavanadate solid to the solution containing ammonium ions.

[0023] As a further implementation method, in step S2, the reaction time is 60~120 min.

[0024] As a further implementation, in step S2, the reaction temperature is 100°C and the reaction time is 90 min.

[0025] As a further implementation method, in step S3, the calcination temperature is 500~600℃ and the calcination time is 1~3h.

[0026] As a further implementation method, in step S3, the back dissolution and recrystallization is carried out in the following manner: first, the high-purity ammonium vanadate, water, and alkali are mixed, the pH of the solution is controlled to be 9-10, and back dissolution is carried out. After the solid is completely dissolved, ammonium salt is added and recrystallization is carried out. The amount of ammonium salt added is (0.54~1.09)∶1 based on the mass ratio of ammonium ions to V in the back solution, and the recrystallization time is 60~90 min.

[0027] As a further implementation method, the pH is controlled at 9-9.5 during resolution, the amount of ammonium salt added during recrystallization is 0.82:1 based on the mass ratio of ammonium ions to V in the resolution solution, and the recrystallization time is 60 min.

[0028] As a further embodiment, in step S3, the alkali is at least one of sodium hydroxide and potassium hydroxide.

[0029] As a further embodiment, in step S3, the ammonium salt is at least one of ammonium sulfate, ammonium chloride, and ammonium nitrate.

[0030] As a further embodiment, step S4 includes: placing the mixture of high-purity vanadium pentoxide and sulfuric acid solution into the negative electrode storage tank of the electrolysis device, adjusting the total vanadium concentration to 1.5~1.7 mol / L, adding sulfuric acid solution with the same acidity as the negative electrode to the positive electrode storage tank, and applying the solution at a current density of 100~500 mA / cm². 2 Under constant current electrolysis conditions, vanadium battery electrolyte is prepared by vanadium-ion battery electrolyte.

[0031] As a further implementation, in step S4, the total vanadium concentration in the negative electrode storage tank is adjusted to 1.6 mol / L, and the current density is 200 mA / cm². 2 Under constant current electrolysis conditions, the oxidation state is reduced to 3.5.

[0032] According to a second aspect of the present invention, a key material for vanadium batteries is provided, which is prepared by the above-described method for preparing key materials for vanadium batteries.

[0033] According to a third aspect of the present invention, a preparation system for a key vanadium battery material is provided, which is used to implement the above-described method for preparing the key vanadium battery material, the preparation system comprising: The ammonium salt vanadium precipitation subsystem includes: a vanadium precipitation reaction tank for carrying out a weakly acidic ammonium salt vanadium precipitation reaction; an ammonium salt storage tank for adding ammonium salt to the vanadium precipitation reaction tank; an acid storage tank for adding acid to the vanadium precipitation reaction tank; a pH meter for detecting the pH of the slurry in the vanadium precipitation reaction tank; a vanadium precipitation temperature control device for controlling the temperature of the slurry in the vanadium precipitation reaction tank; and a vanadium precipitation solid-liquid separation device fluidly connected to the vanadium precipitation reaction tank for solid-liquid separation of the products after the vanadium precipitation reaction. A solid-phase crystallization sodium ammonium substitution subsystem includes: a crystallization reaction tank for receiving solid sodium decavanadate obtained after solid-liquid separation from the vanadium precipitation solid-liquid separation device and performing a solid-phase crystallization sodium ammonium substitution reaction on it; an ammonium solution storage tank for preparing a solution containing ammonium ions and adding the solution containing ammonium ions to the crystallization reaction tank; a pH meter for detecting the pH of the slurry in the crystallization reaction tank; a crystallization temperature control device for controlling the temperature of the slurry in the crystallization reaction tank; and a crystallization solid-liquid separation device fluidly connected to the crystallization reaction tank for solid-liquid separation of the product after the substitution reaction. A vanadium pentoxide preparation subsystem includes: a first drying device for receiving and drying high-purity ammonium vanadate obtained after solid-liquid separation from the crystallization solid-liquid separation device; a first calcination device for receiving and calcining the dried high-purity ammonium vanadate from the first drying device; and a first vanadium pentoxide storage silo for receiving high-purity vanadium pentoxide produced after calcination from the first calcination device; and / or includes: a recrystallization reaction tank for receiving and recrystallizing high-purity ammonium vanadate obtained after solid-liquid separation from the crystallization solid-liquid separation device; an alkali storage silo for adding alkali to the recrystallization reaction tank; a pH meter for detecting the pH of the slurry in the recrystallization reaction tank; and a alkali storage silo for adding alkali to the recrystallization reaction tank. The system includes an ammonium salt storage silo for ammonium salt, a recrystallization solid-liquid separation device fluidly connected to the recrystallization reaction tank for solid-liquid separation of the product after recrystallization reaction, a second drying device for receiving and drying the high-purity ammonium metavanadate product obtained after solid-liquid separation from the recrystallization solid-liquid separation device, a second calcination device for receiving and calcining the dried high-purity ammonium metavanadate product from the second drying device, and a second vanadium pentoxide storage silo for receiving the high-purity vanadium pentoxide produced after calcination from the second calcination device. The recrystallization solid-liquid separation device is fluidly connected to the ammonium solution storage tank in the solid-phase crystallization ammonium sodium replacement subsystem to supply it with the filtrate and washing water produced after solid-liquid separation. A vanadium battery key material preparation subsystem receives high-purity vanadium pentoxide from a first vanadium pentoxide storage silo or a second vanadium pentoxide storage silo and uses the high-purity vanadium pentoxide to prepare key materials for vanadium batteries. A pure water supply subsystem, connected to the ammonium salt vanadium precipitation subsystem, the solid-phase crystallization ammonium sodium substitution subsystem, and the vanadium pentoxide preparation subsystem, is used to supply pure water to the vanadium precipitation solid-liquid separation device of the ammonium salt vanadium precipitation subsystem, the crystallization reaction tank and the crystallization solid-liquid separation device of the solid-phase crystallization ammonium sodium substitution subsystem, and the recrystallization reaction tank and the recrystallization solid-liquid separation device of the vanadium pentoxide preparation subsystem.

[0034] As a further embodiment, the preparation system further includes: a raw material pretreatment subsystem, which is used to pretreat the crude alkaline vanadium-containing leachate and supply the pretreated alkaline vanadium-containing leachate to the ammonium salt precipitation subsystem. The raw material pretreatment subsystem includes: a storage tank for storing the crude alkaline vanadium-containing leachate, a filter device for filtering the crude alkaline vanadium-containing leachate to remove suspended solids, and a buffer tank for storing the filtered alkaline vanadium-containing leachate. The buffer tank is in fluid communication with the precipitation reaction tank of the ammonium salt precipitation subsystem to supply the alkaline vanadium-containing leachate to it.

[0035] As a further embodiment, the preparation system further includes a vanadium slag leaching subsystem, which is used to leach vanadium slag to obtain the alkaline vanadium-containing crude leachate. The solid-liquid separation device of the solid-phase crystallization sodium ammonium substitution subsystem is connected to the vanadium slag leaching subsystem and is used to supply the filtrate and washing water generated after solid-liquid separation to it for leaching vanadium slag.

[0036] As a further embodiment, the vanadium battery key material preparation subsystem includes: an electrolysis device with a positive electrode storage tank and a negative electrode storage tank, wherein the negative electrode storage tank is used to store a mixture of high-purity vanadium pentoxide and sulfuric acid solution received from a first vanadium pentoxide storage silo or a second vanadium pentoxide storage silo, and the positive electrode storage tank is used to store a sulfuric acid solution with the same acidity as the negative electrode storage tank, and the electrolysis device prepares vanadium electrolyte by electrolysis.

[0037] As a further embodiment, the preparation system further includes: a steam injection subsystem connected to the ammonium salt vanadium precipitation subsystem and the solid-phase crystallization ammonium sodium substitution subsystem, for injecting steam into the vanadium precipitation reactor of the ammonium salt vanadium precipitation subsystem and the crystallization reactor of the solid-phase crystallization ammonium sodium substitution subsystem to control the reaction temperature.

[0038] As a further embodiment, the preparation system further includes a wastewater treatment subsystem, which is connected to the vanadium precipitation solid-liquid separation device of the ammonium salt vanadium precipitation subsystem, for receiving and treating the filtrate and washing water generated after solid-liquid separation.

[0039] By adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art: The present invention uses alkaline vanadium-containing leachate as raw material, and achieves comprehensive removal of major impurity elements such as K, Na, Si, and Cr through vanadium precipitation with weakly acidic ammonium salt and solid-phase crystallization sodium ammonium replacement, thereby achieving the purpose of deep impurity removal, thus preparing high-purity ammonium vanadate, and then preparing high-purity vanadium pentoxide, and using this high-purity vanadium pentoxide as raw material to prepare key materials for high-performance vanadium batteries. Attached Figure Description

[0040] To more clearly illustrate the technical solution of the present invention, the accompanying drawings used in the description of the present invention will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other embodiments can be obtained based on these drawings without creative effort.

[0041] Figure 1 A flowchart illustrating the preparation method of key vanadium battery materials provided by this invention; Figure 2 This is a process flow diagram of a method for preparing key materials for vanadium batteries provided in one embodiment of the present invention; Figure 3 This is a block diagram of the preparation system for key vanadium battery materials provided by the present invention; Figure 4 This is a configuration diagram of a part of the vanadium battery key material preparation system provided in one embodiment of the present invention; Figure 5 XRD patterns of the products obtained from the solid-phase crystallization sodium ammonium substitution reaction under different ammonium ion concentrations; Figure 6 The XRD patterns of the products obtained from the solid-phase crystallization sodium ammonium substitution reaction under different ammonium ion concentrations are magnified in the 2θ range of 14.5~16. Figure 7 The total vanadium content and overall yield of the products obtained from the solid-phase crystallization sodium ammonium substitution reaction under different ammonium ion concentrations are shown. Figure 8 The XRD pattern of the high-purity ammonium vanadate solid obtained in step (2) of Example 2 is shown below. Figure 9 The XRD pattern of calcined product 1# in step (3) of Example 2; Figure 10 The XRD pattern of product 2# calcined in step (5) of Example 2 is shown. Detailed Implementation

[0042] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0043] Specific embodiments of the invention are disclosed herein as needed; however, it should be understood that the embodiments disclosed herein are merely examples of the invention that may be implemented in various alternative forms. In the following description, various operating parameters and components are described in several contemplated embodiments. These specific parameters and components are provided as examples only and are not intended to be limiting.

[0044] The endpoints and any values ​​of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.

[0045] Vanadium leaching solution is an aqueous solution containing soluble vanadium compounds obtained from vanadium-containing raw materials through a leaching process. This solution is generally alkaline and typically rich in anionic impurities such as silicon (Si), chromium (Cr), and phosphorus (P). These impurities significantly increase the difficulty of vanadium product purification and refining, severely restricting the quality of subsequent vanadium products and limiting its application in high-end fields. Currently, although the steel industry remains the main consumer of vanadium globally (approximately 85%), emerging application areas are rapidly rising. Vanadium shows enormous development potential as a high-performance catalyst, a colorant for glass and ceramics, and especially as an electrolyte for all-vanadium redox flow batteries and the matrix for vanadium dioxide (VO2) phase change materials for intelligent temperature control. These high-tech fields place almost stringent requirements on the purity of vanadium products and the content of key impurities such as silicon and chromium; the cost of impurity removal in existing processes is too high.

[0046] Against this backdrop, the strategic advantages and product value of exploring innovative methods to directly prepare high-purity vanadium pentoxide from primary raw materials—alkaline vanadium-containing leachate—are becoming increasingly prominent, abandoning the traditional and cumbersome multi-step purification and conversion process.

[0047] To achieve the aforementioned objectives, the first aspect of this invention provides a method for preparing key materials for vanadium batteries, such as... Figure 1 As shown, the method includes the following steps: S1: Add ammonium salt and acid to an alkaline vanadium-containing leaching solution, and carry out a weakly acidic ammonium salt precipitation reaction under conditions of pH 4-6 and temperature 20-85℃. After solid-liquid separation, sodium decavanadate solid is obtained; S2: Mix the sodium decavanadate solid with a solution containing ammonium ions, and carry out a solid-phase crystallization sodium ammonium substitution reaction at a temperature of 90-100℃. After solid-liquid separation, high-purity ammonium vanadate solid is obtained; S3: Calcinate the high-purity ammonium vanadate solid directly or after recrystallization to obtain high-purity vanadium pentoxide; S4: Use high-purity vanadium pentoxide to prepare key materials for vanadium batteries.

[0048] The preparation method of this invention uses alkaline vanadium-containing leachate as raw material. Through weakly acidic ammonium salt precipitation and solid-phase crystallization with sodium ammonium vanadate, the main impurity elements such as K, Na, Si, and Cr are comprehensively removed, achieving deep impurity removal. This yields high-purity ammonium vanadate, which in turn yields high-purity vanadium pentoxide. This high-purity vanadium pentoxide is then used as a raw material to prepare key materials for high-performance vanadium batteries. Specifically, the preparation method uses alkaline vanadium-containing leachate as raw material. Through a weakly acidic ammonium salt precipitation reaction, vanadium is separated from impurities such as Si and Cr in the solution. Vanadium precipitates as solid sodium decavanadate, while most Si and Cr impurities remain in the solution, and a small amount of Si and Cr impurities are adsorbed on the surface of the solid sodium decavanadate. Through a solid-phase crystallization with sodium ammonium vanadate substitution reaction, sodium decavanadate is converted into ammonium vanadate. This not only eliminates the contamination of the final product by potassium and sodium ions but also, because ammonium vanadate is more crystalline than sodium decavanadate... Sodium ammonium vanadate, with its reduced degree of polymerization, has a weaker adsorption capacity for Si and Cr impurities, which facilitates further removal of Si and Cr impurities and further improves product purity, thus producing high-purity ammonium vanadate. Direct calcination of high-purity ammonium vanadate yields vanadium pentoxide with a purity greater than 99.9%. Further calcination after recrystallization of high-purity ammonium vanadate yields vanadium pentoxide with a purity greater than 99.99%. Using this high-purity vanadium pentoxide as raw material, high-performance key materials for vanadium batteries can be produced.

[0049] The preparation method of this invention highly integrates impurity removal with the core steps of product preparation, significantly reducing intermediate steps and operating units, and substantially shortening the process flow. This not only means faster production cycles and response speeds, but also reduces the complexity of process control and equipment investment. The preparation method of this invention eliminates the chlorination, ion exchange, extraction, and chemical impurity removal steps in the conventional high-purity vanadium pentoxide preparation process. The process introduces no impurity ions, generates no new solid waste, and completely avoids chlorine and organic pollution. The entire process is simple, requires minimal equipment, is environmentally friendly, and highly meets the requirements of industrial production.

[0050] Alkaline vanadium-containing leachate is a core intermediate product in the vanadium smelting industry chain, connecting "vanadium-containing raw materials" with "vanadium products (such as vanadium pentoxide, ferrovanadium, and vanadium electrolyte)." The preparation method of this invention uses alkaline vanadium-containing leachate as raw material. Compared to using other vanadium intermediates or crude products to prepare high-purity vanadium pentoxide, using the most basic primary raw material in the vanadium smelting industry chain not only significantly reduces production costs but also has broad adaptability to raw materials, contributing to the rapid development of the vanadium industry. This invention does not specify requirements for the composition of the alkaline vanadium-containing leachate.

[0051] In some embodiments, the alkaline vanadium-containing leachate is specifically a sodium vanadium solution, i.e., the leachate obtained from vanadium slag through a sodium roasting-water leaching process. This solution is alkaline and rich in anionic impurities such as silicon (Si), Cr, and P.

[0052] The preparation method of the present invention will be further described below for each step.

[0053] In step S1, the pH range is 4 to 6. A pH that is too low or too high will affect the vanadium precipitation yield. The pH can typically, but not exclusively, be set to 4, 4.5, 5, 5.5, or 6. Preferably, the pH is 5 to 5.5.

[0054] In step S1, the reaction temperature is 20~85℃. At higher temperatures, not only is the target product unobtainable, but the product yield is also low. The reaction temperature can typically, but not limitedly, be set to 20℃, 25℃, 30℃, 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃, 75℃, 80℃, or 85℃. Preferably, the reaction temperature is 20~40℃.

[0055] In step S1, the ammonium salt is at least one selected from ammonium sulfate, ammonium chloride, and ammonium nitrate. Preferably, the ammonium salt is ammonium sulfate.

[0056] In step S1, the amount of ammonium salt added (also known as the ammonium addition coefficient) is calculated as (0.22~0.41)∶1 by the mass ratio of ammonium ions to V in the alkaline vanadium-containing leachate.

[0057] The ammonium addition coefficient ranges from (0.22 to 0.41):1. An excessively high coefficient leads to wasted ammonium salts and increased preparation costs; an excessively low coefficient affects the vanadium precipitation yield. Typical, but not limited, values ​​for the ammonium addition coefficient can be 0.22:1, 0.25:1, 0.27:1, 0.30:1, 0.33:1, 0.35:1, 0.38:1, and 0.41:1. Preferably, the ammonium addition coefficient, calculated as the mass ratio of ammonium ions to V in the alkaline vanadium-containing leachate, is (0.27 to 0.33):1. In step S1, the reaction time is 30-90 min. If the reaction time is too short, the reaction is not complete, resulting in a low yield of sodium decavanadate; if the reaction time is too long, the yield remains unchanged, reducing production efficiency. The reaction time can typically, but is not limited to, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, or 90 min. Preferably, the reaction time is 60 min.

[0058] In step S1, the acid is at least one selected from sulfuric acid, hydrochloric acid, and nitric acid. Preferably, the acid is sulfuric acid.

[0059] In step S2, the reaction temperature is 90-100℃, under which the crystallization reaction rate is fast and the vanadium yield is high. The reaction temperature can typically, but not limitedly, be set to 90℃, 92℃, 94℃, 96℃, 98℃, or 100℃. Preferably, the reaction temperature is 100℃.

[0060] In step S2, the reaction time is 60-120 min. If the reaction time is too short, the vanadium precipitation reaction is not complete, resulting in a low vanadium yield; if the reaction time is too long, the yield remains unchanged, but the process energy consumption increases. The reaction time can typically, but is not limited to, be 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, or 120 min. Preferably, the reaction time is 90 min.

[0061] In step S2, the solution containing ammonium ions is at least one of ammonium sulfate solution, ammonium chloride solution, and ammonium nitrate solution. Preferably, the solution containing ammonium ions is an ammonium sulfate solution.

[0062] Preferably, the solution containing ammonium ions used in step S2 corresponds to the ammonium salt used in step S1, in order to minimize the introduction of impurities.

[0063] In step S2, the concentration of ammonium ions in the solution containing ammonium ions is 6~48 g / L, and the amount of sodium decavanadate solid added is 1:(5~8) based on the solid-liquid ratio of sodium decavanadate solid to the solution containing ammonium ions.

[0064] In this solution containing ammonium ions, the concentration of ammonium ions is 6-48 g / L. Too low a concentration affects the vanadium yield; too high a concentration leads to waste of ammonium salt and increased preparation costs. Typical, but not limited, ammonium ion concentrations can be set to 6 g / L, 12 g / L, 18 g / L, 24 g / L, 30 g / L, 36 g / L, 42 g / L, and 48 g / L. The amount of sodium decavanadate added is based on a solid-liquid ratio S(t):L(m). 3 If the ratio of pure water to vanadium is 1:(5~8), excessively high pure water volume results in a large filtrate treatment volume, high cost, and high vanadium loss rate; excessively low pure water volume affects the transformation of the product crystal form and the removal of impurities. The addition of sodium decavanadate is typically, but not limited to, 1:5, 1:6, 1:7, or 1:8. Preferably, the concentration of ammonium ions in the solution containing ammonium ions is 36~48 g / L, and the addition of solid sodium decavanadate is based on a solid-liquid ratio of 1:6 between the solid sodium decavanadate and the solution containing ammonium ions.

[0065] In step S3, the calcination temperature is 500~600℃ and the calcination time is 1~3h.

[0066] The calcination temperature is 500-600℃. At lower temperatures, calcination is incomplete, resulting in the formation of low-valent vanadium oxide byproducts; at higher temperatures, energy consumption increases significantly. Typical, but not limited, calcination temperatures can be set to 500℃, 520℃, 540℃, 560℃, 580℃, and 600℃. The calcination time is 1-3 hours. Too short a time results in incomplete reduction; too long a time increases energy consumption. Typical, but not limited, calcination times can be set to 1 hour, 1.5 hours, 2 hours, 2.5 hours, and 3 hours. Preferably, the calcination temperature is 550℃, and the calcination time is 2 hours.

[0067] Note: The calcination parameters for direct calcination of high-purity ammonium vanadate solid are the same as those for calcination after recrystallization of high-purity ammonium vanadate solid.

[0068] In step S3, the back dissolution and recrystallization are carried out as follows: First, high-purity ammonium vanadate, water, and alkali are mixed, and the pH of the solution is controlled at 9-10. Back dissolution is then performed. After all the solid has dissolved, ammonium salt is added, and recrystallization is carried out. The amount of ammonium salt added is calculated based on the mass ratio of ammonium ions to V in the back solution as (0.54~1.09):1. The recrystallization time is 60~90 minutes. Here, "back solution" refers to the solution obtained after back dissolution of high-purity ammonium vanadate, water, and alkali.

[0069] During the re-dissolution process, the pH is controlled at 9-10, preferably 9-9.5. If the pH is too low, the reaction product will not dissolve completely; if the pH is too high, the amount of ammonium salt used in subsequent vanadium precipitation will increase, leading to higher costs. The re-dissolution pH can typically, but is not limited to, 9.0, 9.2, 9.4, 9.6, 9.8, or 10.0. During recrystallization, the ammonium salt addition ratio is (0.54-1.09):1. A too high addition ratio results in wasted ammonium salt and increased preparation costs; a too low addition ratio affects the vanadium precipitation yield. The ammonium salt addition ratio can typically, but is not limited to, 0.54:1, 0.68:1, 0.82:1, 0.95:1, or 1.09:1. Preferably, the ammonium salt addition ratio is 3:1. The recrystallization time is 60-90 minutes. Too short a time results in incomplete reaction; too long a time increases energy consumption. The recrystallization time can typically, but not limited to, be set to 60 min, 70 min, 80 min, or 90 min. Preferably, the recrystallization time is 60 min.

[0070] In step S3, the alkali used for dissolution is at least one of sodium hydroxide and potassium hydroxide. Preferably, the alkali used for dissolution is sodium hydroxide.

[0071] In step S3, the ammonium salt used during recrystallization is at least one of ammonium sulfate, ammonium chloride, and ammonium nitrate. Preferably, the ammonium salt is ammonium sulfate.

[0072] In step S4, the key material for vanadium batteries is prepared using high-purity vanadium pentoxide, mainly by preparing the vanadium battery electrolyte. The preparation of the vanadium battery electrolyte includes: placing a mixture of high-purity vanadium pentoxide and sulfuric acid in the negative electrode storage tank of the electrolysis device, and placing a sulfuric acid solution of the same acidity in the positive electrode storage tank of the electrolysis device; and then obtaining the vanadium battery electrolyte through constant current electrolysis.

[0073] Specifically, a mixture of high-purity vanadium pentoxide and sulfuric acid solution is placed in the negative electrode storage tank of the electrolysis device, and the total vanadium concentration is adjusted to 1.5~1.7 mol / L. A sulfuric acid solution with the same acidity as the negative electrode is added to the positive electrode storage tank, and the current density is 100~500 mA / cm². 2 Vanadium battery electrolyte is prepared by constant current electrolysis to a valence state of 3.5 under specific conditions. Preferably, the total vanadium concentration is adjusted to 1.6 mol / L, and the electrolyte is prepared at a current density of 200 mA / cm². 2 Under constant current electrolysis conditions.

[0074] In some embodiments, the preparation method further includes: returning the filtrate and washing water generated during the solid-liquid separation process after the solid-phase crystallization sodium ammonium displacement reaction to the vanadium slag leaching process for leaching the vanadium slag to obtain an alkaline vanadium-containing crude leachate. The filtrate and washing water generated during the solid-liquid separation process after the solid-phase crystallization sodium ammonium displacement reaction have low impurity content and can be directly reused in the vanadium slag leaching process of large-scale production. This not only recovers residual V and ammonium ions but also reduces the wastewater treatment volume of the entire large-scale production system, resulting in significant economic and social benefits.

[0075] In some embodiments, the preparation method further includes: returning the filtrate and washing water generated after solid-liquid separation following remelting and recrystallization to the solid-phase conversion sodium ammonium ion replacement process for use as a solution containing ammonium ions. The filtrate and washing water generated after solid-liquid separation following remelting and recrystallization have extremely low impurity content and are directly reused in the solid-phase conversion sodium ammonium ion replacement process, recovering residual V and ammonium ions, reducing the wastewater treatment volume and ammonium salt usage of the entire process, and significantly reducing the cost of vanadium pentoxide products.

[0076] The following combination Figure 2 Further explanation is provided regarding the preparation method of the key vanadium battery material provided in one embodiment of the present invention. For example... Figure 2As shown, this method uses sodium vanadium chloride solution as raw material. Vanadium is precipitated with ammonium salts at low temperature, and after solid-liquid separation, sodium decavanadate and filtrate are obtained. The filtrate can be treated in a wastewater treatment process. The obtained sodium decavanadate is replaced by solid-phase crystallization with sodium ammonium chloride, and after solid-liquid separation, high-purity ammonium vanadate and filtrate are obtained. The filtrate can be used in a vanadium slag leaching process. The obtained high-purity ammonium vanadate can be dried and calcined via route one to obtain 99.9% grade vanadium pentoxide, or via route two through alkali dissolution and alkaline ammonium salt precipitation, and after solid-liquid separation, ammonium metavanadate (AMV) and filtrate are obtained. The filtrate can be recycled to the solid-phase crystallization with sodium ammonium chloride replacement process. The obtained ammonium metavanadate is dried and calcined to obtain 99.99% grade vanadium pentoxide. The obtained 99.9% grade vanadium pentoxide and 99.99% grade vanadium pentoxide can be electrolyzed to prepare vanadium battery electrolyte.

[0077] The specific steps of this method and the main chemical reactions involved are described below: (1) Low-temperature ammonium salt precipitation of vanadium Using sodium vanadium solution as raw material, ammonium salt is added at low temperature to produce sodium ammonium decavanadate (NH4)4Na2V. 10 O 28 The reaction formula is as follows: NH 4+ +Na + +V 10 O 28 6- →3(NH4)4Na2V 10 O 28 ↓ (20~85℃) Formula (1) (2) Solid-phase conversion to crystalline sodium ammonium substitution Adding ammonium salt to pure water creates a solution containing a certain concentration of ammonium ions (NH4+). + The solution of sodium decavanadate (1) is prepared without pH adjustment. After stirring and heating for a set time, the solution is filtered, washed, and dried to obtain high-purity ammonium vanadate (pure phase NH4V3O8 or a mixture of NH4V3O8 and NH4VO3). The reaction formula is as follows: 3(NH4)4Na2V 10 O 28 +8H + →10NH4V3O8↓+6Na + +2NH4 + +4H2O (90~100℃) formula (2) NH4V3O8+2OH - +2NH4 + →3NH4VO3↓+H2O formula (3) 3(NH4)4Na2V 10 O 28 +2OH- +8NH4 + →5NH4V3O8↓+15NH4VO3↓+H2O+6Na + Equation (4) During the reaction, as H + As the solution's pH gradually increases due to the consumption of H, the reaction proceeds sequentially according to equation (2) → equation (3), with the overall reaction being equation (4). + The H remaining from the previous low-temperature ammonium salt precipitation of vanadium + At the beginning of the crystallization process, the pH of the slurry is less than 6. As the reaction proceeds, the pH value gradually increases. After the reaction is completed, the pH of the slurry is around 7.0.

[0078] (3) Preparation of 99.9% grade vanadium pentoxide A mixture of high-purity ammonium vanadate was calcined to obtain 99.9% high-purity vanadium pentoxide. The reaction formula is as follows: 2xNH4V3O8+2yNH4VO3→(3x+y)V2O5+2(x+y)NH3↑+(x+y)H2O↑Equation (5) (4) Redissolution and recrystallization xNH4V3O8+yNH4VO3+(x+3y)NaOH→(x+3y)NaVO3+(x+y)NH3↑+(x+2y)H2O Formula (6) 2NaVO3 + (NH4)2SO4 → 2NH4VO3↓ + Na2SO4 (Equation 7) (5) Preparation of 99.99% grade vanadium pentoxide The NH4VO3 obtained by the recrystallization reaction of (4) was calcined to obtain 99.99% vanadium pentoxide.

[0079] 2NH4VO3→V2O5+2NH3↑+H2O↑ Equation (8) The core principles of this method include the following aspects: (1) The precipitation reaction of sodium decavanadate, also known as weakly acidic ammonium salt precipitation of vanadium, is highly effective in removing impurities such as silicon (Si) and chromium (Cr). A single precipitation process can reduce the Si and Cr content in the product to below 0.005%. The key to this process is to add sodium decavanadate to a solution containing ammonium ions (NH4+). + The solution of sodium decavanadate was used to suppress the dissolution of sodium decavanadate by means of the common ion effect (because it has a high solubility in pure water), that is, the reverse dissolution process of formula (1). This suppression effect ensures the efficient removal of impurities silicon and chromium. The main reason is that once sodium decavanadate dissolves, it will release Si and Cr ions back into the solution, which will affect the impurity removal effect and yield of subsequent precipitation steps.

[0080] (2) When sodium decavanadate is added to a solution containing ammonium ions, the pH of the solution is in the range of 5-6. Upon heating, ammonium ions redistribute and sodium ions are released. This process leads to the decavanadate (V) group in its macromolecular structure being reduced. 10 O 28 6- The groups depolymerize to form trivanadate (V3O8), which has a lower degree of polymerization. - It is worth noting that sodium decavanadate did not undergo significant dissolution at this stage, but its internal crystal structure underwent a significant transformation. Therefore, this step is called solid-phase transformation, i.e., the chemical process represented by formula (2). As the reaction continues, hydrogen ions are continuously consumed, causing the pH of the solution to slowly rise to around 7.0. At this point, trivanadate (V3O8) - It undergoes another solid-state transformation, converting into metavanadate (VO3), which has a lower degree of polymerization. - The chemical process is represented by equation (3). The overall reaction of the entire process is shown in equation (4), which realizes the replacement of sodium ions in sodium decavanadate with sodium ions by ammonium ions in the solution, generating ammonium vanadate. The research of this invention shows that the final replacement product may be a single-phase ammonium trivanadate, or it may be a mixture of ammonium trivanadate and ammonium metavanadate, and the ratio of the two will change dynamically with the adjustment of reaction parameters. Even the mixed-phase ammonium vanadate has no adverse effect on the subsequent preparation of vanadium pentoxide. Therefore, in actual operation, the reaction parameters should be optimized by comprehensively considering factors such as material consumption, energy consumption and production efficiency.

[0081] (3) Highly polymerized decavanadates, due to their large molecular size and numerous unsaturated coordination sites (such as exposed VO bonds), are more likely to adsorb a large number of impurity ions through strong electrostatic interactions and coordination exchange. In contrast, lowly polymerized ammonium trivanadate and ammonium metavanadate have simple structures and limited adsorption capacity for impurities. This phase transition crystallization process not only eliminates sodium ion contamination of the final product, but the structural simplification itself also helps to improve the purity of the precipitate, thereby obtaining high-purity ammonium vanadate. A second aspect of this invention provides a key vanadium battery material prepared using the above-described preparation method.

[0082] Based on the same concept, a third aspect of the present invention provides a preparation system for key vanadium battery materials used in implementing the above-described preparation method, such as... Figure 3 and Figure 4 As shown, the preparation system includes an ammonium salt vanadium precipitation subsystem 2, a solid-phase crystallization ammonium sodium substitution subsystem 3, a vanadium pentoxide preparation subsystem 4, a vanadium battery key material preparation subsystem 7, and a pure water supply subsystem 8.

[0083] The ammonium salt vanadium precipitation subsystem 2 is used to prepare sodium decavanadate via a weakly acidic ammonium salt vanadium precipitation reaction. The ammonium salt vanadium precipitation subsystem 2 includes: a vanadium precipitation reaction vessel 2-6 for carrying out the weakly acidic ammonium salt vanadium precipitation reaction; an ammonium salt storage silo 2-4 for adding ammonium salt to the vanadium precipitation reaction vessel 2-6; an acid storage tank 2-5 for adding acid to the vanadium precipitation reaction vessel 2-6; a pH meter 2-2 for detecting the pH of the slurry in the vanadium precipitation reaction vessel 2-6; a vanadium precipitation temperature control device for controlling the temperature of the slurry in the vanadium precipitation reaction vessel 2-6; and a vanadium precipitation solid-liquid separation device 2-8, fluidly connected to the vanadium precipitation reaction vessel 2-6, for solid-liquid separation of the products after the vanadium precipitation reaction.

[0084] Specifically, the electrode of pH meter 2-2 is in contact with the slurry in vanadium precipitation reaction tank 2-6; the vanadium precipitation temperature control device includes a thermometer 2-3 for detecting the slurry temperature, which is in contact with the slurry in vanadium precipitation reaction tank 2-6; the outlet of ammonium salt storage silo 2-4 is connected to the inlet of vanadium precipitation reaction tank 2-6; the outlet pipe of acid storage tank 2-5 is connected to the inlet pipe of vanadium precipitation reaction tank 2-6; the outlet pipe of vanadium precipitation reaction tank 2-6 is connected to the inlet pipe of vanadium precipitation solid-liquid separation device 2-8 via slurry pump 2-7. The vanadium precipitation solid-liquid separation device 2-8 can be configured as a filter centrifuge.

[0085] The solid-phase crystallization sodium ammonium substitution subsystem 3 is used to prepare high-purity ammonium vanadate via a solid-phase crystallization sodium ammonium substitution reaction. The solid-phase crystallization sodium ammonium substitution subsystem 3 includes: a crystallization reaction tank 3-6 that receives the solid ammonium decavanadate obtained after solid-liquid separation from the vanadium precipitation solid-liquid separation device 2-8 of the ammonium salt precipitation subsystem 2 and performs a solid-phase crystallization sodium ammonium substitution reaction on it; an ammonium solution storage tank 3-7 for preparing a solution containing ammonium ions and adding the solution containing ammonium ions to the crystallization reaction tank 3-6; a pH meter 3-4 for detecting the pH of the slurry in the crystallization reaction tank 3-6; a crystallization temperature control device for controlling the temperature of the slurry in the crystallization reaction tank 3-6; and a crystallization solid-liquid separation device 3-9, fluidly connected to the crystallization reaction tank 3-6, for solid-liquid separation of the product after the substitution reaction.

[0086] Specifically, the discharge port of the vanadium precipitation solid-liquid separation device 2-8 is connected to the inlet of the crystallization reaction tank 3-6 via the feed belt 3-1; the electrode of the pH meter 3-4 is in contact with the slurry in the crystallization reaction tank 3-6; the crystallization temperature control device includes a thermometer 3-5 for detecting the slurry temperature, which is in contact with the slurry in the crystallization reaction tank 3-6; the outlet pipe of the ammonium solution storage tank 3-7 is connected to the inlet pipe of the crystallization reaction tank 3-6; the outlet pipe of the crystallization reaction tank 3-6 is connected to the inlet pipe of the crystallization solid-liquid separation device 3-9 via the slurry pump 3-8. The crystallization solid-liquid separation device 3-9 can be configured as a filter centrifuge.

[0087] Vanadium pentoxide preparation subsystem 4 is used to prepare vanadium pentoxide from high-purity ammonium vanadate. Vanadium pentoxide preparation subsystem 4 includes: a first drying device 4-1 that receives and dries the high-purity ammonium vanadate solid obtained after solid-liquid separation from the solid-liquid separation device 3-9 of the solid-phase crystallization ammonium sodium substitution subsystem 3; a first calcining device 4-4 that receives and calcines the dried high-purity ammonium vanadate solid from the first drying device 4-1; and a first vanadium pentoxide storage silo 4-5 that receives the high-purity vanadium pentoxide produced after calcination from the first calcining device 4-4; and / or includes: a recrystallization reaction tank 5-5 that receives and recrystallizes the high-purity ammonium vanadate solid obtained after solid-liquid separation from the solid-liquid separation device 3-9 of the solid-phase crystallization ammonium sodium substitution subsystem 3; an alkali storage silo 5-2 for adding alkali to the recrystallization reaction tank 5-5; and a pH meter for detecting the pH of the slurry in the recrystallization reaction tank 5-5. The system comprises: 5-3, an ammonium salt storage silo 5-1 for adding ammonium salt to the recrystallization reaction tank 5-5, a recrystallization solid-liquid separation device 5-7 connected in fluid to the recrystallization reaction tank 5-5 for solid-liquid separation of the product after recrystallization, a second drying device 6-1 for receiving and drying the high-purity ammonium metavanadate product obtained after solid-liquid separation from the recrystallization solid-liquid separation device 5-7, a second calcination device 6-4 for calcining the dried high-purity ammonium metavanadate product from the second drying device 6-1, and a second vanadium pentoxide storage silo 6-3 for receiving the high-purity vanadium pentoxide produced after calcination from the second calcination device 6-4. The recrystallization solid-liquid separation device 5-7 is in fluid communication with the ammonium solution storage tank 3-7 of the solid-phase crystallization ammonium sodium substitution subsystem 3 to supply it with the filtrate and washing water produced after solid-liquid separation.

[0088] The "and / or" mentioned above refers to the following: the vanadium pentoxide preparation subsystem 4 may include only the first drying device 4-1, the first calcining device 4-4, and the first vanadium pentoxide storage silo 4-5; it may also include only the remelting and recrystallization related components, the second drying device 6-1, the second calcining device 6-4, and the second vanadium pentoxide storage silo 6-3; or it may include both. The first vanadium pentoxide storage silo 4-5 is a 99.9% grade vanadium pentoxide storage silo, and the second vanadium pentoxide storage silo 6-3 is a 99.99% grade vanadium pentoxide storage silo. In the first case, the vanadium pentoxide preparation subsystem 4 can only prepare 99.9% grade vanadium pentoxide; in the second case, the vanadium pentoxide preparation subsystem 4 can only prepare 99.99% grade vanadium pentoxide; and in the third case, the vanadium pentoxide preparation subsystem 4 can selectively prepare either 99.9% grade vanadium pentoxide or 99.99% grade vanadium pentoxide.

[0089] exist Figure 4In the illustrated embodiment, the preparation system falls under the third category described above, and can selectively prepare 99.9% or 99.99% vanadium pentoxide. For this purpose, a converter 3-12 is provided for switching between the two processes. Specifically, the discharge port of the crystallization solid-liquid separation device 3-9 is connected to the converter 3-12 via a feed belt 3-11, and the converter 3-12 has two discharge ports for connecting to the two processes respectively.

[0090] Specifically, one outlet of converter 3-12 is connected to the inlet of the first drying device 4-1; the outlet of the first drying device 4-1 is connected to the inlet of the storage silo 4-3 via the feeding belt 4-2; the outlet of the storage silo 4-3 is connected to the inlet of the first calcining device 4-4; the first calcining device 4-4 has a ventilation and negative pressure device; the outlet of the first calcining device 4-4 is connected to the inlet of the first vanadium pentoxide storage silo 4-5; and the outlet of the first vanadium pentoxide storage silo 4-5 is connected to the inlet of the 99.9% grade vanadium pentoxide packaging drum 4-6.

[0091] Another outlet of converter 3-12 is connected to the inlet of recrystallization reactor 5-5; the outlet of ammonium salt storage silo 5-1 is connected to the inlet of recrystallization reactor 5-5; the outlet of alkali storage silo 5-2 is connected to the inlet of recrystallization reactor 5-5; the electrode of pH meter 5-3 is in contact with the slurry in recrystallization reactor 5-5; a thermometer 5-4 is also installed in recrystallization reactor 5-5, and the thermometer 5-4 is in contact with the slurry in recrystallization reactor 5-5; recrystallization reactor 5-5 is connected to the inlet pipe of recrystallization solid-liquid separation device 5-7 via slurry pump 5-6; the discharge port of recrystallization solid-liquid separation device 5-7 is connected via... The feeding belt 5-8 is connected to the inlet of the second drying device 6-1; the outlet pipe of the recrystallization solid-liquid separation device 5-7 is connected to the inlet of the ammonium solution storage tank 3-7; the outlet of the second drying device 6-1 is connected to the inlet of the storage silo 6-3 via the feeding belt 6-2; the outlet of the storage silo 6-3 is connected to the inlet of the second calcining device 6-4; the second calcining device 6-4 has a ventilation and negative pressure device; the outlet of the second calcining device 6-4 is connected to the inlet of the second vanadium pentoxide storage silo 6-5; the outlet of the second vanadium pentoxide storage silo 6-5 is connected to the inlet of the 99.99% grade vanadium pentoxide packaging drum 6-6. The first drying device 4-1 and the second drying device 6-1 can be configured as microwave dryers. The first calcining device 4-4 and the second calcining device 6-4 can be configured as rotary kilns.

[0092] The pure water supply subsystem 8 is connected to the ammonium salt vanadium precipitation subsystem 2, the solid-phase crystallization ammonium sodium replacement subsystem 3, and the vanadium pentoxide preparation subsystem 4, and is used to supply pure water to the vanadium precipitation solid-liquid separation device 2-8 of the ammonium salt vanadium precipitation subsystem 2, the crystallization reaction tank 3-6 and the crystallization solid-liquid separation device 3-9 of the solid-phase crystallization ammonium sodium replacement subsystem 3, and the recrystallization reaction tank 5-5 and the recrystallization solid-liquid separation device 5-7 of the vanadium pentoxide preparation subsystem 4.

[0093] Specifically, the pure water supply subsystem 8 includes a pure water pipeline, which is connected to the inlet pipeline of the vanadium precipitation solid-liquid separation device 2-8 via a pure water valve 2-9; the pure water pipeline is connected to the inlet pipeline of the crystallization reaction tank 3-6 via a pure water valve 3-2; the pure water pipeline is connected to the inlet pipeline of the crystallization solid-liquid separation device 3-9 via a pure water valve 3-3; the pure water pipeline is connected to the inlet pipeline of the recrystallization reaction tank 5-5 via a pure water valve 5-9; and the pure water pipeline is connected to the inlet pipeline of the recrystallization solid-liquid separation device 5-7 via a pure water valve 5-10.

[0094] In some embodiments, the preparation system further includes a raw material pretreatment subsystem 1, which is used to pretreat the crude alkaline vanadium-containing leachate and supply the pretreated alkaline vanadium-containing leachate to the ammonium salt vanadium precipitation subsystem 2. The raw material pretreatment subsystem 1 includes: a storage tank 1-1 for storing the crude alkaline vanadium-containing leachate; a filter device 1-3 for filtering the crude alkaline vanadium-containing leachate to remove suspended solids; and a buffer tank 1-4 for storing the filtered alkaline vanadium-containing leachate. The buffer tank 1-4 is in fluid communication with the vanadium precipitation reaction tank 2-6 of the ammonium salt vanadium precipitation subsystem 2 to supply it with the alkaline vanadium-containing leachate.

[0095] Specifically, the outlet pipe of the storage tank 1-1 is connected to the inlet pipe of the filter device 1-3 via the centrifugal pump 1-2; the outlet pipe of the filter device 1-3 is connected to the inlet pipe of the buffer tank 1-4; and the outlet pipe of the buffer tank 1-4 is connected to the inlet pipe of the vanadium precipitation reaction tank 2-6 via the centrifugal pump 2-1. The filter device 1-3 can be configured as a precision filter.

[0096] In some embodiments, the preparation system further includes a vanadium slag leaching subsystem, which is used to leach vanadium slag to obtain a crude alkaline vanadium-containing leachate. The vanadium slag leaching subsystem is connected to the raw material pretreatment subsystem 1 to supply it with the crude alkaline vanadium-containing leachate. Preferably, the solid-liquid separation device 3-9 of the solid-phase crystallization sodium ammonium substitution subsystem 3 is connected to the vanadium slag leaching subsystem to supply it with the filtrate and washing water generated after solid-liquid separation for leaching the vanadium slag. Specifically, the outlet pipe of the solid-liquid separation device 3-9 is connected to the vanadium slag leaching subsystem via a centrifugal pump 3-10.

[0097] In some embodiments, the preparation system further includes a steam injection subsystem connected to the ammonium salt vanadium precipitation subsystem 2 and the solid-phase crystallization ammonium sodium substitution subsystem 3. This steam injection subsystem injects steam into the vanadium precipitation reaction vessel 2-6 of the ammonium salt vanadium precipitation subsystem 2 and the crystallization reaction vessel 3-6 of the solid-phase crystallization ammonium sodium substitution subsystem 3 to control the reaction temperature. Specifically, the steam injection subsystem includes a medium-pressure steam pipeline connected to the inlet pipe of the vanadium precipitation reaction vessel 2-6 via a steam valve 2-11, and connected to the inlet pipe of the crystallization reaction vessel 3-6 via a steam valve 3-13.

[0098] In some embodiments, the preparation system further includes a wastewater treatment subsystem connected to the vanadium precipitation solid-liquid separation device 2-8 of the ammonium salt vanadium precipitation subsystem 2. This wastewater treatment subsystem receives and treats the filtrate and wash water generated after solid-liquid separation to recover residual V and Cr. Specifically, the effluent pipe of the vanadium precipitation solid-liquid separation device 2-8 is connected to the wastewater treatment subsystem via a centrifugal pump 2-10.

[0099] The following combination Figure 4 The specific operation steps of the vanadium battery key material preparation system provided in one embodiment of the present invention are further explained.

[0100] (1) Raw material preparation process: Use centrifugal pump 1-2 to pump the crude alkaline vanadium-containing leachate from storage tank 1-1 into filter device 1-3. The solid suspended matter in the solution is removed by filtration through the filter device. The filtered alkaline vanadium-containing leachate is then pumped into buffer tank 1-4 for later use.

[0101] (2) Low-temperature ammonium salt precipitation process: A certain volume of alkaline vanadium-containing leaching solution is pumped from buffer tank 1-4 into vanadium precipitation reaction tank 2-6. Ammonium salt (e.g., ammonium sulfate) and acid (e.g., sulfuric acid) are added from ammonium salt storage silo 2-4 and acid storage tank 2-5 to vanadium precipitation reaction tank 2-6 respectively. The amount of ammonium salt is controlled to be m(NH4) + The solution pH is controlled at 4-6 using pH meter 2-2, and the temperature is controlled at 20-85℃ using thermometer 2-3 and steam valve 2-11. Stirring is continued for 30-90 minutes. After stirring, the slurry from vanadium precipitation tank 2-6 is pumped into solid-liquid separation device 2-8 via slurry pump 2-7 for solid-liquid separation. The filtrate from solid-liquid separation device 2-8 is pumped into the wastewater treatment process via centrifugal pump 2-10 to recover residual V and Cr. After filtration, pure water valve 2-9 is opened to wash the solid product in solid-liquid separation device 2-8 with pure water. The wash water from solid-liquid separation device 2-8 is also pumped into the wastewater treatment process via centrifugal pump 2-10 to recover residual V and Cr. After washing, sodium decavanadate (NH4)4Na2V is obtained. 10 O 28 .

[0102] (3) Solid-phase crystallization sodium ammonia replacement process: The sodium decavanadate reaction product in the solid-liquid separation device 2-8 is added to the crystallization reaction tank 3-6 via the feeding belt 3-1. An ammonium sulfate solution with an ammonium ion concentration of 6~48 g / L is prepared in the ammonium solution storage tank 3-7. The prepared ammonium sulfate solution is added to the crystallization reaction tank 3-6. The amount of sodium decavanadate added is based on the solid-liquid ratio L (m 3 S(t) = (5~8):1, the weight of sodium decavanadate needs to be reduced by the water content. After stirring evenly, the solution temperature is controlled at 90~100℃ by thermometer 3-5 and steam valve 3-13, and stirring is continued for 60~120min. After stirring is completed, the slurry in the crystallization reaction tank 3-6 is pumped into the solid-liquid separation device 3-9 through slurry pump 3-8 for solid-liquid separation. The filtrate produced in the solid-liquid separation device 3-9 is pumped into the vanadium slag leaching process by centrifugal pump 3-10 to recover the residual V and ammonium ions. After filtration, the pure water valve 3-3 is opened, and the solid product in the solid-liquid separation device 3-9 is washed with pure water. The washing water produced in the solid-liquid separation device 3-9 is also pumped into the vanadium slag leaching process by centrifugal pump 3-3 to recover the residual V and ammonium ions. After washing, high-purity ammonium vanadate product is obtained.

[0103] (4) Drying and calcining process of 99.9% grade vanadium pentoxide: The high-purity ammonium vanadate product in the filter centrifuge 3-9 is fed through the feed belt 3-11 and then connected to the feed inlet of the first drying device 4-1 via the converter 3-12. The dried ammonium vanadate product is fed through the discharge port of the microwave dryer 4-1 and into the storage silo 4-3 via the feed belt 4-2. Then, it is sent from the storage silo 4-3 into the first calcining device 4-4 for calcination at a temperature of 500~600℃ for 1~3 hours. After calcination, vanadium pentoxide is fed through the discharge port of the first calcining device 4-4 into the first vanadium pentoxide storage silo 4-5. Then, it is loaded from the first vanadium pentoxide storage silo 4-5 into the 99.9% grade vanadium pentoxide packaging barrel 4-6 to complete the packaging work, and finally obtain vanadium pentoxide with a purity greater than 99.9%.

[0104] The following steps (5) and (6) are additional steps required to produce 99.99% vanadium pentoxide.

[0105] (5) Re-dissolution and recrystallization process: The high-purity ammonium vanadate product in the solid-liquid separation device 3-9 is fed into the recrystallization reaction tank 5-5 via the feed belt 3-11 and then the converter 3-12. Pure water of the same volume as the alkaline vanadium-containing leachate is added through the pure water valve 5-9 and stirred evenly. Then, alkali (e.g., solid sodium hydroxide) is added to the recrystallization reaction tank 5-5 through the alkali storage silo 5-2. The pH of the solution is controlled to 9-10 according to the pH meter 5-3. After continuous stirring until all the solid is dissolved, ammonium salt is added to the recrystallization reaction tank 5-5 from the ammonium salt storage silo 5-1, controlling m(NH4)2. + With a concentration of m(V) = (0.22~0.41):1, after stirring for 60~90 min, the slurry in recrystallization reactor 5-5 is pumped into solid-liquid separation device 5-7 via slurry pump 5-6 for solid-liquid separation. The filtrate produced in solid-liquid separation device 5-7 is returned to ammonium solution storage tank 3-7 for circulation and used in the solid-phase crystallization sodium ammonium replacement reaction. After filtration, pure water valve 5-10 is opened to wash the reaction product in solid-liquid separation device 5-7 with pure water. The washing water produced in solid-liquid separation device 5-7 is also returned to ammonium solution storage tank 3-7 for recycling. After washing, high-purity ammonium metavanadate product is obtained.

[0106] (6) 99.99% Vanadium Pentoxide Drying and Calcination Process: The high-purity ammonium metavanadate product in the solid-liquid separation device 5-7 is added to the second drying device 6-1 via the feeding belt 5-8. The dried ammonium metavanadate product is discharged from the outlet of the second drying device 6-1 and fed into the storage silo 6-3 via the feeding belt 6-2. Then, it is sent from the storage silo 6-3 to the second calcination device 6-4 for calcination at a temperature of 500~600℃ for 1~3 hours. After calcination, vanadium pentoxide is sent from the second calcination device 6-4 to the second vanadium pentoxide storage silo 6-5, and then from the second vanadium pentoxide storage silo 6-5 into 99.99% vanadium pentoxide packaging barrels 6-6 to complete the packaging. Finally, vanadium pentoxide with a purity greater than 99.99% is obtained.

[0107] The following describes the process methods mentioned in this invention with specific embodiments, but this invention is not limited to the following embodiments.

[0108] The vanadium sodium solution used in the following examples came from the Panzhihua Vanadium Products Branch of Panzhihua Iron and Steel Group. The vanadium raw material was obtained by sodium roasting and water leaching of vanadium slag. First, the initial vanadium sodium solution in the storage tank 1-1 was pumped into the filter device 1-3 using centrifugal pump 1-2. The solid suspended matter in the solution was removed by filtration through the filter device 1-3. The filtered vanadium sodium solution was then pumped into the buffer tank 1-4 for later use. The specific composition was tested and found to be: K - 0.63 g / L, Na - 43.60 g / L, Si - 0.94 g / L, Ca - 0.15 g / L, Cr - 2.97 g / L, and TV - 52.39 g / L.

[0109] Example 1: (1) Pump 10m³ of vanadium precipitation solution from buffer tank 1-4 into vanadium precipitation reaction tank 2-6. 3 Vanadium sodium chloride solution was prepared by stirring and adding 629 kg of ammonium sulfate (ammonium addition ratio 0.33:1) from ammonium salt storage tank 2-4 to vanadium precipitation tank 2-6. After the ammonium sulfate was completely dissolved, sulfuric acid was added from acid storage tank 2-5 to vanadium precipitation tank 2-6. The pH of the solution was controlled at 5.5 using pH meter 2-2, and the solution temperature was controlled at 20°C using thermometer 2-3. Stirring was continued for 70 minutes. After stirring, the slurry in vanadium precipitation tank 2-6 was pumped into solid-liquid separation device 2-8 via slurry pump 2-7 for solid-liquid separation to obtain sodium decavanadate (NH4)4Na2V. 10 O 28 The solids, filtrate, and washings produced during the process are fed into the wastewater treatment process. Testing revealed that the sodium decavanadate solid contained 9.6% water and 40.11% vanadium.

[0110] (2) Mix 880 kg of ammonium sulfate with 5 m 3 Pure water was added to the ammonium solution storage tank 3-7 to prepare an ammonium sulfate solution with an ammonium ion concentration of 47.95 g / L, which was then added to the crystallization reaction tank 3-6. Next, 790 kg of sodium decavanadate solid was added to the crystallization reaction tank 3-6 via the feed belt 3-1 (liquid-to-solid ratio 7:1). The mixture was stirred until homogeneous, and the material was heated by opening the steam valve 3-13. The solution temperature was controlled at 96℃ using a thermometer 3-5, and stirring was continued for 80 minutes. After stirring, the slurry in the crystallization reaction tank 3-6 was pumped into the solid-liquid separation device 3-9 via the slurry pump 3-8 for solid-liquid separation to obtain high-purity ammonium vanadate solid. The filtrate and washing liquid generated during the process were sent to the vanadium slag leaching process. Testing revealed that the high-purity ammonium vanadate solid contained 26.1% water and 47.52% vanadium.

[0111] (3) The high-purity ammonium vanadate product in the solid-liquid separation device 3-9 is fed into the first drying device 4-1 through the feeding belt 3-11 for drying. After drying, the product is sent from the storage bin 4-3 to the first calcination device 4-4 for calcination. The calcination temperature is 550℃ and the time is 2h. After calcination, the calcined product 1# is subjected to chemical detection and analysis.

[0112]

[0113] (unit:%) (4) Take 500 kg of high-purity ammonium vanadate solid from step (2) and add it to recrystallization reactor 5-5. Open pure water valve 5-9 and add 5 ml of water. 3Pure water is stirred until homogeneous, then solid sodium hydroxide is added to recrystallization reactor 5-5 through alkali storage silo 5-2. The pH of the solution is controlled to 9.5 using pH meter 5-3. After continuous stirring until the solid is completely dissolved, 351 kg of ammonium sulfate (ammonium addition coefficient of 0.54) is added to recrystallization reactor 5-5 from ammonium sulfate storage silo 5-1. After stirring for 60 minutes, the slurry in recrystallization reactor 5-5 is pumped into solid-liquid separation device 5-7 through slurry pump 5-6 for solid-liquid separation to obtain high-purity ammonium metavanadate solid. The filtrate and washing liquid produced in solid-liquid separation device 5-7 are returned to ammonium solution storage tank 3-7 for later use.

[0114] (5) The high-purity ammonium vanadate product in the solid-liquid separation device 5-7 is fed into the second drying device 6-1 through the feeding belt 5-8 for drying. After drying, the product is sent from the storage bin 6-3 to the second calcination device 6-4 for calcination. The calcination temperature is 550℃ and the time is 2h. After calcination, the calcined product 2# is subjected to chemical detection and analysis.

[0115]

[0116] (unit:%) (6) The calcined products obtained in steps (3) and (5) are electrolyzed in an electrolysis system to obtain vanadium electrolyte. After testing, the quality of the obtained electrolyte meets the requirements of Grade I of the national standard GB / T 37204-2018 "Electrolytes for Vanadium Redox Flow Batteries".

[0117] Comparative Example 1: (1) Pump 10m into vanadium precipitation reaction tank 2-6 3 Vanadium sodium chloride solution was prepared by stirring and adding 629 kg of ammonium sulfate to the vanadium precipitation reaction tank 2-6. After the ammonium sulfate was completely dissolved, sulfuric acid was added from the acid storage tank 2-5 to the vanadium precipitation reaction tank 2-6. The pH of the solution was controlled at 5.5 using pH meter 2-2, and the solution temperature was controlled at 20°C using thermometer 2-3. Stirring was continued for 70 minutes. After stirring, the slurry in the vanadium precipitation reaction tank 2-6 was subjected to solid-liquid separation in the solid-liquid separation device 2-8 to obtain sodium ammonium decavanadate (NH4)4Na2V. 10 O 28 Solid. Analysis showed that the sodium decavanadate solid contained 9.6% water and 40.11% vanadium.

[0118] (2) Open the pure water valve 3-2 and add 5m to the crystallization reaction vessel 3-6. 3Pure water is used to feed 790 kg of sodium decavanadate solid into the crystallization reaction tank 3-6 via feed belt 3-1. Sodium hydroxide is then added and the pH is adjusted to 9.0 using pH meter 3-4. At the same time, steam valve 3-13 is opened, and the mixture is heated and stirred until the solid is completely dissolved. Then, 880 kg of ammonium sulfate is added, and the mixture is stirred and cooled to 30°C. Stirring is continued for 80 minutes. After the reaction is completed, the slurry in the crystallization reaction tank 3-6 is subjected to solid-liquid separation in solid-liquid separation device 3-9 to obtain high-purity ammonium metavanadate solid.

[0119] (3) Ammonium metavanadate was dried in the first drying device 4-1 and calcined in the first calcination device 4-4 at a temperature of 550℃ for 2 hours. After calcination, the calcined product 3# was subjected to chemical analysis.

[0120]

[0121] (unit:%) (4) The calcined product obtained in step (3) is electrolyzed in an electrolysis system to obtain vanadium electrolyte. After testing, the quality of the obtained electrolyte does not meet the requirements of the national standard GB / T 37204-2018 "Electrolytes for Vanadium Redox Flow Batteries".

[0122] Comparative Example 2: (1) Pump 10m into vanadium precipitation reaction tank 2-6 3 Vanadium sodium chloride solution was prepared by stirring and adding 629 kg of ammonium sulfate to the vanadium precipitation reaction tank 2-6. After the ammonium sulfate was completely dissolved, sulfuric acid was added from the acid storage tank 2-5 to the vanadium precipitation reaction tank 2-6. The pH of the solution was controlled at 5.5 using pH meter 2-2, and the solution temperature was controlled at 20°C using thermometer 2-3. Stirring was continued for 70 minutes. After stirring, the slurry in the vanadium precipitation reaction tank 2-6 was subjected to solid-liquid separation in the solid-liquid separation device 2-8 to obtain sodium ammonium decavanadate (NH4)4Na2V. 10 O 28 Solid. Analysis showed that the sodium decavanadate solid contained 9.6% water and 40.11% vanadium.

[0123] (2) Open the pure water valve 3-2 and add 5m to the crystallization reaction vessel 3-6. 3 Pure water is fed into the crystallization reaction tank 3-6 via feed belt 3-1 with 790 kg of sodium polyvanadate solid. Then, 880 kg of ammonium sulfate is added, and sulfuric acid solution is added. The pH is adjusted to 2.5 using pH meter 3-4. At the same time, steam valve 3-13 is opened, and the mixture is heated to 96°C and stirred continuously for 80 min. After the reaction is completed, the slurry in the crystallization reaction tank 3-6 is separated into solid and liquid components in solid-liquid separation device 3-9 to obtain high-purity APV solid (ammonium polyvanadate).

[0124] (3) The APV was dried in the first drying device 4-1 and calcined in the first calcining device 4-4 at a temperature of 550℃ for 2 hours. After calcination, the calcined product 4# was subjected to chemical analysis.

[0125]

[0126] (unit:%) (4) The calcined product obtained in step (3) is electrolyzed in an electrolysis system to obtain vanadium electrolyte. After testing, the quality of the obtained electrolyte does not meet the requirements of the national standard GB / T 37204-2018 "Electrolytes for Vanadium Redox Flow Batteries".

[0127] Example 2: (1) Pump 10m into vanadium precipitation reaction tank 2-6 3 In a sodium vanadium chloride solution, stirring is started, and 419 kg of ammonium sulfate (with an ammonium addition coefficient of 0.22) is added to the vanadium precipitation reaction tank 2-6. After the ammonium sulfate is completely dissolved, sulfuric acid is added from the acid storage tank 2-5 to the vanadium precipitation reaction tank 2-6. The pH of the solution is controlled to 6.0 using pH meter 2-2. Steam valve 2-11 is opened, and the solution temperature is controlled to 85°C using thermometer 2-3. Stirring is continued for 90 minutes. After stirring is complete, the slurry in the vanadium precipitation reaction tank 2-6 is subjected to solid-liquid separation in solid-liquid separation device 2-8 to obtain sodium ammonium decavanadate (NH4)4Na2V. 10 O 28 Solid. Testing revealed that the sodium decavanadate solid contained 10.5% water and 41.05% vanadium.

[0128] (2) Mix 660 kg of ammonium sulfate with 5 m 3 Pure water was added to the ammonium solution storage tank 3-7 to prepare an ammonium sulfate solution with an ammonium ion concentration of 35.96 g / L, which was then added to the crystallization reaction tank 3-6. 930 kg of sodium decavanadate solid was added to the crystallization reaction tank 3-6 via the feed belt 3-1 (liquid-to-solid ratio 6:1). The mixture was stirred until homogeneous, and the material was heated by opening the steam valve 3-13. The solution temperature was controlled at 94℃ using a thermometer 3-5, and stirring was continued for 60 minutes. After stirring, the slurry in the crystallization reaction tank 3-6 was pumped into the solid-liquid separation device 3-9 via the slurry pump 3-8 for solid-liquid separation to obtain high-purity ammonium vanadate solid. The filtrate and washing liquid generated during the process were sent to the vanadium slag leaching process. Testing revealed that the high-purity ammonium vanadate solid contained 25.5% water and 48.42% vanadium.

[0129] (3) The high-purity ammonium vanadate solid was dried in the first drying device 4-1 and calcined in the first calcination device 4-4 at a temperature of 600℃ for 1 hour. After calcination, the calcined product 1# was subjected to chemical analysis.

[0130]

[0131] (unit:%) (4) Take 500 kg of high-purity ammonium vanadate solid from step (2) and add it to recrystallization reactor 5-5, then add 5m 3 After purifying the water, solid sodium hydroxide is added while stirring, and the pH of the solution is controlled to 9.0 according to pH meter 5-3. After continuous stirring until the solid is completely dissolved, 541 kg of ammonium sulfate (ammonium addition coefficient of 0.82) is added to the recrystallization reaction tank 5-5. After stirring for 90 min, the slurry in the recrystallization reaction tank 5-5 is subjected to solid-liquid separation in the solid-liquid separation device 5-7 to obtain high-purity ammonium metavanadate solid. The filtrate and washing liquid produced in the solid-liquid separation device 5-7 are returned to the ammonium solution storage tank 3-7 for later use.

[0132] (5) The high-purity ammonium metavanadate solid was dried in the second drying device 6-1 and calcined in the rotary kiln 6-4 of the second calcination device at a temperature of 600℃ for 1 hour. After calcination, the calcined product 2# was subjected to chemical analysis.

[0133]

[0134] (unit:%) (6) The calcined products obtained in steps (3) and (5) are electrolyzed in an electrolysis system to obtain vanadium electrolyte. After testing, the quality of the obtained electrolyte meets the requirements of Grade I of the national standard GB / T 37204-2018 "Electrolytes for Vanadium Redox Flow Batteries".

[0135] Example 3: (1) Pump 10m into vanadium precipitation reaction tank 2-6 3 In a sodium vanadium chloride solution, stirring is started, and 424 kg of ammonium chloride (ammonium addition coefficient of 0.27) is added to the vanadium precipitation reaction tank 2-6. After stirring until the ammonium chloride is completely dissolved, hydrochloric acid is added to the vanadium precipitation reaction tank 2-6 from the acid storage tank 2-5. The pH of the solution is controlled to 5.5 using pH meter 2-2. Steam valve 2-11 is opened, and the solution temperature is controlled to 40℃ using thermometer 2-3. Stirring is continued for 30 minutes. After stirring is completed, the slurry in the vanadium precipitation reaction tank 2-6 is subjected to solid-liquid separation device 2-8 to obtain sodium ammonium decavanadate (NH4)4Na2V. 10 O 28 Solid. Analysis showed that the sodium decavanadate solid contained 9.8% water and 41.21% vanadium.

[0136] (2) Mix 267 kg of ammonium chloride with 5 m 3Pure water was added to the ammonium solution storage tank 3-7 to prepare an ammonium chloride solution with an ammonium ion concentration of 17.97 g / L, which was then added to the crystallization reaction tank 3-6. 1110 kg of sodium decanvanadate solid was added to the crystallization reaction tank 3-6 via the feed belt 3-1 (liquid-to-solid ratio 5:1). The mixture was stirred until homogeneous, and the material was heated by opening the steam valve 3-13. The solution temperature was controlled at 100℃ using a thermometer 3-5, and stirring was continued for 100 minutes. After stirring, the slurry in the crystallization reaction tank 3-6 was pumped into the solid-liquid separation device 3-9 via the slurry pump 3-8 for solid-liquid separation to obtain high-purity ammonium vanadate solid. The filtrate and washing liquid generated during the process were sent to the vanadium slag leaching process. Testing revealed that the high-purity ammonium vanadate solid contained 24.7% water and 48.71% vanadium.

[0137] (3) The high-purity ammonium vanadate solid was dried in the first drying device 4-1 and calcined in the first calcination device 4-4 at a temperature of 570℃ for 1.5h. After calcination, the calcined product 1# was subjected to chemical analysis.

[0138]

[0139] (unit:%) (4) Take 500 kg of high-purity ammonium vanadate solid from step (2) and add it to recrystallization reactor 5-5, then add 5m 3 After purifying the water, solid potassium hydroxide is added while stirring, and the pH of the solution is controlled to 10.0 according to pH meter 5-3. After continuous stirring until the solid is completely dissolved, 405 kg of ammonium chloride (ammonium addition coefficient of 0.74) is added to the recrystallization reaction tank 5-5. After stirring for 70 min, the slurry in the recrystallization reaction tank 5-5 is subjected to solid-liquid separation in the solid-liquid separation device 5-7 to obtain high-purity ammonium metavanadate solid. The filtrate and washing liquid produced in the solid-liquid separation device 5-7 are returned to the ammonium solution storage tank 3-7 for later use.

[0140] (5) The high-purity ammonium metavanadate solid was dried in the second drying device 6-1 and calcined in the second calcination device 6-4 at a temperature of 570℃ for 1.5h. After calcination, the calcined product 2# was subjected to chemical analysis.

[0141]

[0142] (unit:%) (6) The calcined products obtained in steps (3) and (5) are electrolyzed in an electrolysis system to obtain vanadium electrolyte. After testing, the quality of the obtained electrolyte meets the requirements of Grade I of the national standard GB / T 37204-2018 "Electrolytes for Vanadium Redox Flow Batteries".

[0143] Example 4: (1) Pump 10m into vanadium precipitation reaction tank 2-6 3 Vanadium sodium chloride solution (ammonium addition coefficient 0.41) was stirred, and 952 kg of ammonium nitrate was added to vanadium precipitation tank 2-6. After the ammonium nitrate was completely dissolved, nitric acid was added to vanadium precipitation tank 2-6 from acid storage tank 2-5. The pH of the solution was controlled to 4.0 using pH meter 2-2. Steam valve 2-11 was opened, and the solution temperature was controlled to 60℃ using thermometer 2-3. Stirring was continued for 50 minutes. After stirring was completed, the slurry in vanadium precipitation tank 2-6 was subjected to solid-liquid separation device 2-8 to obtain sodium decavanadate (NH4)4Na2V. 10 O 28 Solid. Analysis showed that the sodium decavanadate solid contained 10.0% water and 40.09% vanadium.

[0144] (2) Mix 133 kg of ammonium nitrate with 5 m 3 Pure water was added to the ammonium solution storage tank 3-7 to prepare an ammonium nitrate solution with an ammonium ion concentration of 5.99 g / L, which was then added to the crystallization reaction tank 3-6. 694 kg of sodium decavanadate solid was added to the crystallization reaction tank 3-6 via the feed belt 3-1 (liquid-to-solid ratio 8:1). The mixture was stirred until homogeneous, and the material was heated by opening the steam valve 3-13. The solution temperature was controlled at 90℃ using a thermometer 3-5, and stirring was continued for 120 minutes. After stirring, the slurry in the crystallization reaction tank 3-6 was pumped into a filter centrifuge 3-9 via a slurry pump 3-8 for solid-liquid separation to obtain high-purity ammonium vanadate solid. The filtrate and washing liquid generated during the process were sent to the vanadium slag leaching process. Testing revealed that the high-purity ammonium vanadate solid contained 25.9% water and 47.66% vanadium.

[0145] (3) The high-purity ammonium vanadate solid was dried in the first drying device 4-1 and calcined in the first calcination device 4-4 at a temperature of 500℃ for 3 hours. After calcination, the calcined product 1# was subjected to chemical analysis.

[0146]

[0147] (unit:%) (4) Take 500 kg of high-purity ammonium vanadate solid from step (2) and add it to recrystallization reactor 5-5, then add 5m 3 After purifying the water, solid potassium hydroxide is added while stirring, and the pH of the solution is controlled to 9.7 according to pH meter 5-3. After the solid is completely dissolved, 855 kg of ammonium nitrate (ammonium addition coefficient of 1.09) is added to the recrystallization reaction tank 5-5. After stirring for 80 minutes, the slurry in the recrystallization reaction tank 5-5 is subjected to solid-liquid separation in the solid-liquid separation device 5-7 to obtain high-purity ammonium metavanadate solid. The filtrate and washing liquid produced in the solid-liquid separation device 5-7 are returned to the ammonium solution storage tank 3-7 for later use.

[0148] (5) The high-purity ammonium metavanadate solid was dried in the second drying device 6-1 and calcined in the second calcination device 6-4 at a temperature of 500℃ for 3 hours. After calcination, the calcined product 2# was subjected to chemical analysis.

[0149]

[0150] (unit:%) (6) The calcined products obtained in steps (3) and (5) are electrolyzed in an electrolysis system to obtain vanadium electrolyte. After testing, the quality of the obtained electrolyte meets the requirements of Grade I of the national standard GB / T 37204-2018 "Electrolytes for Vanadium Redox Flow Batteries".

[0151] The results of Example 1 and Comparative Examples 1 and 2 show that the solid-phase crystallization sodium ammonium substitution process (without using acid or alkali to adjust pH) helps to obtain vanadium pentoxide with higher purity.

[0152] The high-purity ammonium vanadate solid in step (2) of Example 2 was subjected to XRD refinement analysis, see... Figure 8 This shows that high-purity ammonium vanadate solid is a mixture of ammonium trivanadate and ammonium metavanadate. In high-purity ammonium vanadate solid, NH4V3O8 accounts for 63.19% and NH4VO3 accounts for 36.81%.

[0153] XRD analysis was performed on calcined product 1# in step (3) of Example 2, see... Figure 9 This shows that the calcination product is pure vanadium pentoxide, indicating that the high-purity ammonium vanadate mixture does not affect the phase of the final product.

[0154] XRD analysis was performed on calcined product 2# in step (5) of Example 2, see... Figure 10 This shows that the calcination product is pure vanadium pentoxide, indicating that the high-purity ammonium vanadate mixture does not affect the phase of the final product.

[0155] also, Figure 7 The XRD patterns of the products obtained from the solid-phase crystallization sodium ammonium substitution reaction under different ammonium ion concentrations are shown, along with magnified peak spectra of the characteristic peaks in the 2θ range of 14.5–16, as well as the total vanadium content and overall yield. Figure 5 and Figure 6 It can be seen that when the ammonium ion concentration is less than or equal to 18 g / L, the solid-state crystallization product is the pure phase NH4V3O8; when the ammonium ion concentration is greater than or equal to 24 g / L, the characteristic peak of NH4VO3 appears, and the product is a mixture of NH4V3O8 and NH4VO3. This indicates that the solid-state crystallization pattern is (NH4)4Na2V 10 O 28→NH4V3O8→NH4VO3. From Figure 7 It can be seen that when the ammonium ion concentration is greater than 36 g / L, the overall yield reaches its maximum. Further increasing the ammonium ion concentration does not significantly increase the yield. Considering industrial production costs, the ammonium ion concentration should be controlled below 48 g / L. Therefore, it is unnecessary to convert all NH4V3O8 to NH4VO3, and in practice, it is difficult to achieve complete conversion without pH adjustment. Furthermore, when the ammonium ion concentration is between 6 and 48 g / L, the total vanadium content of the product ranges from 47.74% to 51.21%. Calculations show that the theoretical vanadium content of NH4V3O8 is 51.17%, and the theoretical vanadium content of NH4VO3 is 43.59%. This also indirectly indicates that when the ammonium ion concentration is greater than or equal to 24 g / L, the product is a mixture of NH4V3O8 and NH4VO3.

[0156] In summary, the present invention innovatively uses sodium vanadium precipitate as raw material to prepare vanadium pentoxide with a purity greater than 99.9% through a one-step vanadium precipitation process and to prepare vanadium pentoxide with a purity greater than 99.99% through a two-step vanadium precipitation process. Its significant advantage is that it eliminates the chlorination, ion exchange, extraction, and chemical impurity removal steps in conventional high-purity vanadium preparation processes. The process introduces no impurity ions, generates no new solid waste, and completely avoids chlorine and organic pollution. The entire process is simple, requires minimal equipment, is environmentally friendly, and highly meets the requirements of industrial production.

[0157] Finally, it should be noted that the embodiments described above are only some, not all, of the embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

Claims

1. A method for preparing a key material for vanadium batteries, characterized in that, Includes the following steps: S1: Add ammonium salt and acid to alkaline vanadium-containing leachate, and carry out weakly acidic ammonium salt precipitation reaction under the conditions of pH 4~6 and temperature 20~85℃ to obtain sodium decavanadate solid. S2: The sodium decavanadate solid is mixed with a solution containing ammonium ions, and a solid-phase crystallization sodium ammonium substitution reaction is carried out at a temperature of 90~100℃ to obtain high-purity ammonium vanadate. S3: The high-purity ammonium vanadate is directly calcined or calcined after recrystallization to obtain high-purity vanadium pentoxide; S4: Use the high-purity vanadium pentoxide to prepare key materials for vanadium batteries.

2. The method for preparing the key material for vanadium batteries according to claim 1, characterized in that, In step S1, the ammonium salt is at least one of ammonium sulfate, ammonium chloride, and ammonium nitrate. The amount of ammonium salt added is (0.22~0.41):1 based on the mass ratio of ammonium ions to V in the alkaline vanadium-containing leachate. The acid is at least one of sulfuric acid, hydrochloric acid, and nitric acid. The reaction time is 30~90 min.

3. The method for preparing key materials for vanadium batteries according to claim 2, characterized in that, In step S1, the amount of ammonium salt added is (0.27~0.33):1 based on the mass ratio of ammonium ions to V in the alkaline vanadium-containing leachate, the pH is 5~5.5, the temperature is 20~40℃, and the reaction time is 60min.

4. The method for preparing the key material for vanadium batteries according to claim 1, characterized in that, In step S2, the solution containing ammonium ions is at least one of ammonium sulfate solution, ammonium chloride solution, and ammonium nitrate solution, the concentration of ammonium ions in the solution containing ammonium ions is 6~48 g / L, the amount of sodium decavanadate solid added is 1:(5~8) based on the solid-liquid ratio of sodium decavanadate solid to the solution containing ammonium ions, and the reaction time is 60~120 min.

5. The method for preparing the key material for vanadium batteries according to claim 4, characterized in that, In step S2, the concentration of ammonium ions in the solution containing ammonium ions is 36~48 g / L, the amount of sodium decavanadate solid added is 1:6 based on the solid-liquid ratio of sodium decavanadate solid to the solution containing ammonium ions, the temperature is 100℃, and the reaction time is 90 min.

6. The method for preparing the key material for vanadium batteries according to claim 1, characterized in that, In step S3, the calcination temperature is 500~600℃, the calcination time is 1~3h, and the back dissolution and recrystallization are carried out in the following manner: first, the high-purity ammonium vanadate, water, and alkali are mixed, and the pH of the solution is controlled to be 9-10, and back dissolution is carried out. The alkali is at least one of sodium hydroxide and potassium hydroxide. After the solid is completely dissolved, ammonium salt is added and recrystallization is carried out. The ammonium salt is at least one of ammonium sulfate, ammonium chloride, and ammonium nitrate. The amount of ammonium salt added is (0.54~1.09)∶1 based on the mass ratio of ammonium ion to V in the back solution, and the recrystallization time is 60~90min.

7. The method for preparing the key material for vanadium batteries according to claim 1, characterized in that, Step S4 includes: placing the mixture of high-purity vanadium pentoxide and sulfuric acid solution into the negative electrode storage tank of the electrolysis device, adjusting the total vanadium concentration to 1.5~1.7 mol / L, adding sulfuric acid solution with the same acidity as the negative electrode to the positive electrode storage tank, and applying the solution at a current density of 100~500 mA / cm². 2 Under constant current electrolysis conditions, vanadium battery electrolyte is prepared by vanadium-ion battery electrolyte.

8. A key material for vanadium batteries, characterized in that, It is prepared using the preparation method of any one of the key materials for vanadium batteries according to claims 1-7.

9. A preparation system for a key material in vanadium batteries, characterized in that, A method for preparing vanadium battery key materials according to any one of claims 1-7, wherein the preparation system comprises: The ammonium salt vanadium precipitation subsystem includes: a vanadium precipitation reaction tank for carrying out a weakly acidic ammonium salt vanadium precipitation reaction; an ammonium salt storage tank for adding ammonium salt to the vanadium precipitation reaction tank; an acid storage tank for adding acid to the vanadium precipitation reaction tank; a pH meter for detecting the pH of the slurry in the vanadium precipitation reaction tank; a vanadium precipitation temperature control device for controlling the temperature of the slurry in the vanadium precipitation reaction tank; and a vanadium precipitation solid-liquid separation device fluidly connected to the vanadium precipitation reaction tank for solid-liquid separation of the products after the vanadium precipitation reaction. A solid-phase crystallization sodium ammonium substitution subsystem includes: a crystallization reaction tank for receiving solid sodium decavanadate obtained after solid-liquid separation from the vanadium precipitation solid-liquid separation device and performing a solid-phase crystallization sodium ammonium substitution reaction on it; an ammonium solution storage tank for preparing a solution containing ammonium ions and adding the solution containing ammonium ions to the crystallization reaction tank; a pH meter for detecting the pH of the slurry in the crystallization reaction tank; a crystallization temperature control device for controlling the temperature of the slurry in the crystallization reaction tank; and a crystallization solid-liquid separation device fluidly connected to the crystallization reaction tank for solid-liquid separation of the product after the substitution reaction. A vanadium pentoxide preparation subsystem includes: a first drying device for receiving and drying high-purity ammonium vanadate obtained after solid-liquid separation from the crystallization solid-liquid separation device; a first calcination device for receiving and calcining the dried high-purity ammonium vanadate from the first drying device; and a first vanadium pentoxide storage silo for receiving high-purity vanadium pentoxide produced after calcination from the first calcination device; and / or includes: a recrystallization reaction tank for receiving and recrystallizing high-purity ammonium vanadate obtained after solid-liquid separation from the crystallization solid-liquid separation device; an alkali storage silo for adding alkali to the recrystallization reaction tank; a pH meter for detecting the pH of the slurry in the recrystallization reaction tank; and a alkali storage silo for adding alkali to the recrystallization reaction tank. The system includes an ammonium salt storage silo for ammonium salt, a recrystallization solid-liquid separation device fluidly connected to the recrystallization reaction tank for solid-liquid separation of the product after recrystallization reaction, a second drying device for receiving and drying the high-purity ammonium metavanadate product obtained after solid-liquid separation from the recrystallization solid-liquid separation device, a second calcination device for receiving and calcining the dried high-purity ammonium metavanadate product from the second drying device, and a second vanadium pentoxide storage silo for receiving the high-purity vanadium pentoxide produced after calcination from the second calcination device. The recrystallization solid-liquid separation device is fluidly connected to the ammonium solution storage tank in the solid-phase crystallization ammonium sodium replacement subsystem to supply it with the filtrate and washing water produced after solid-liquid separation. A vanadium battery key material preparation subsystem receives high-purity vanadium pentoxide from a first vanadium pentoxide storage silo or a second vanadium pentoxide storage silo and uses the high-purity vanadium pentoxide to prepare key materials for vanadium batteries. A pure water supply subsystem, connected to the ammonium salt vanadium precipitation subsystem, the solid-phase crystallization ammonium sodium substitution subsystem, and the vanadium pentoxide preparation subsystem, is used to supply pure water to the vanadium precipitation solid-liquid separation device of the ammonium salt vanadium precipitation subsystem, the crystallization reaction tank and the crystallization solid-liquid separation device of the solid-phase crystallization ammonium sodium substitution subsystem, and the recrystallization reaction tank and the recrystallization solid-liquid separation device of the vanadium pentoxide preparation subsystem.

10. The preparation system for key vanadium battery materials according to claim 9, characterized in that, It also includes one or more of the following: The vanadium slag leaching subsystem is used to leach vanadium slag to obtain an alkaline vanadium-containing crude leachate. The solid-phase crystallization sodium ammonium sodium replacement subsystem is connected to the vanadium slag leaching subsystem and is used to supply the filtrate and washing water generated after solid-liquid separation to it for leaching vanadium slag. A raw material pretreatment subsystem is used to pretreat the crude alkaline vanadium-containing leachate and supply the pretreated alkaline vanadium-containing leachate to the ammonium salt vanadium precipitation subsystem. The raw material pretreatment subsystem includes: a storage tank for storing the crude alkaline vanadium-containing leachate; a filter device for filtering the crude alkaline vanadium-containing leachate to remove suspended solids; and a buffer tank for storing the filtered alkaline vanadium-containing leachate. The buffer tank is fluidly connected to the vanadium precipitation reaction tank of the ammonium salt vanadium precipitation subsystem to supply the alkaline vanadium-containing leachate to it. A steam injection subsystem, which is connected to the ammonium salt vanadium precipitation subsystem and the solid-phase crystallization ammonium sodium replacement subsystem, is used to inject steam into the vanadium precipitation reactor of the ammonium salt vanadium precipitation subsystem and the crystallization reactor of the solid-phase crystallization ammonium sodium replacement subsystem to control the reaction temperature; A wastewater treatment subsystem, which is connected to the vanadium precipitation solid-liquid separation device of the ammonium salt vanadium precipitation subsystem, is used to receive and treat the filtrate and washing water generated after solid-liquid separation. The vanadium battery key material preparation subsystem includes an electrolysis device with a positive electrode storage tank and a negative electrode storage tank. The negative electrode storage tank is used to store a mixture of high-purity vanadium pentoxide and sulfuric acid solution received from a first vanadium pentoxide storage silo or a second vanadium pentoxide storage silo. The positive electrode storage tank is used to store a sulfuric acid solution with the same acidity as the negative electrode storage tank. The electrolysis device prepares vanadium electrolyte through electrolysis.

Citation Information

Patent Citations

  • Process for preparing high-purity vanadium pentoxide by adopting ammonium metavanadate as raw material

    CN102603000A

  • Method for preparing high purity vanadium pentoxide through using ammonium metavanadate

    CN102730757A

  • Method for preparing high-purity vanadium from heteropolyacid impurity in amine extraction mode

    CN103540745A

  • A purification method for deep silicon removal from ammonium metavanadate

    CN106044853B

  • Method for preparing high-purity vanadium pentoxide by using vanadium-contained material

    CN106676289A

Cited By

  • Vanadium battery electrolyte and preparation method and preparation system thereof

    CN121317873A