Nickel oxide nanoparticles prepared by low-temperature chemical precipitation and their application in inverted perovskite solar cells
Nickel oxide nanoparticles were prepared by low-temperature chemical precipitation, which solved the problems of dispersion and interface matching of the nickel oxide hole transport layer, improved the efficiency and stability of perovskite solar cells, and achieved efficient charge transport and interface carrier transfer.
Patent Information
- Application Number
- CN202511692769.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-11-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-11-18
AI Technical Summary
In existing inverted perovskite solar cells, the nickel oxide hole transport layer suffers from problems such as poor dispersion, high impurity content, low conductivity, and interfacial energy level mismatch, resulting in insufficient cell stability and efficiency.
Nickel oxide nanoparticles were prepared by low-temperature chemical precipitation. By controlling the particle size and dispersibility, the conductivity and interfacial contact of the nickel oxide film were regulated, and the interface matching was improved by combining the self-assembled molecular layer.
It improves the photoelectric conversion efficiency and long-term stability of perovskite solar cells, enhances the charge transport performance of nickel oxide thin films, improves interfacial contact and carrier transfer, and suppresses nonradiative recombination.
Smart Images

Figure CN121292536B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of perovskite solar cell technology, and relates to nickel oxide nanoparticles prepared by low-temperature chemical precipitation method and their application in inverted perovskite solar cells. Background Technology
[0002] Inverted perovskite solar cells (PSCs) have achieved certified power conversion efficiencies (PCE) exceeding 27% and exhibited excellent long-term stability. Currently, high-efficiency inverted PSCs often employ nickel oxide or self-assembled atom (SAM) molecules as hole transport layers (HTLs). However, the interface between the nickel oxide HTL and the perovskite layer is prone to redox reactions, reducing the long-term stability of the cell. Furthermore, the bonding between SAM and transparent conductive oxide (TCO) substrates (such as indium-doped tin oxide (ITO) and fluorine-doped tin oxide (FTO)) is weak. At high temperatures, this weak interaction causes SAM to easily desorb from the transparent electrode, thereby reducing the device's thermal stability and long-term performance. Studies have shown that the bonding force between SAM and nickel oxide nanoparticles is much stronger than that with the transparent electrode. Therefore, researchers used SAM and nickel oxide to construct a bilayer HTL, overcoming the instability challenges of nickel oxide or SAM-only HTLs, significantly improving the HTL / perovskite buried interface and the long-term stability of the cell. However, the bonding force between SAM and nickel oxide nanoparticles is much stronger than that with the transparent electrode. Therefore, researchers used SAM and nickel oxide to construct a bilayer HTL, overcoming the instability challenges of nickel oxide or SAM-only HTLs, significantly improving the HTL / perovskite buried interface and the long-term stability of the cell. x The formation of a bilayer HTL with SAM still presents several key challenges, hindering the realization of highly efficient and stable inverted perovskite solar cells. Firstly, NiO... x Nanoparticles have drawbacks such as poor dispersibility, high impurity content, and low electrical conductivity and hole mobility, which will reduce the efficiency of NiO. x Hole transport and extraction capabilities of thin films. Secondly, SAM in NiO... x The low coverage, tendency to aggregate, and insufficient adhesion of the thin film not only reduce the charge transport capacity of the SAM layer but also lead to poor perovskite crystallinity and low buried interface quality. Finally, the energy level mismatch between the bilayer HTL and the perovskite layer results in severe nonradiative recombination of charge carriers. Therefore, there is an urgent need to develop simple and effective methods to simultaneously address these intractable problems and further improve the PCE and long-term operational stability of inverted PSCs.
[0003] In the past few years, researchers have proposed a variety of strategies to address NiO. xThe challenges faced by SAM bilayer HTLs include SAM / perovskite interface control, SAM layer doping and modification, and the development of novel SAMs. Introducing modifying molecules into the SAM / perovskite interface can fill areas not covered by SAM, passivate defects on the perovskite substrate surface, promote perovskite crystallization, and lower the interface energy barrier, thereby promoting interfacial charge transfer, suppressing nonradiative recombination, and improving the stability of the buried interface. However, this method struggles to effectively control the underlying NiO layer. x And SAM layer. Furthermore, by developing novel SAMs and modifying commonly used SAMs, it is possible to suppress SAM aggregation, increase coverage, enhance interface defect passivation, improve perovskite crystallization, and reduce interface energy level mismatch, thereby improving the photovoltaic performance and stability of the cell. However, this strategy cannot solve the NiO... x The problems with the layered structure are significant. In short, it's difficult to simultaneously solve all the above problems through SAM doping and SAM / perovskite interface modulation. It should be noted that, considering the layered stacked structure of perovskite solar cells, the lower functional layers significantly affect the growth and quality of subsequent functional layers. Therefore, a bottom-up modulation strategy holds promise for simultaneously addressing all the above problems. In recent years, most research has focused on the modulation of SAM and its interface with perovskite, with a lack of research on nickel oxide layer modulation. For example, nickel oxide nanoparticle doping and post-treatment can improve cell efficiency and stability, but this method may introduce new impurity phases, which are detrimental to the long-term stability of the cell. Therefore, there is an urgent need to address these issues through simple NiO layer modulation. x By controlling the nanoparticle synthesis process, we can simultaneously regulate the multifunctional layers and interfaces from the bottom up, and solve all the problems existing in HTL and buried interface, ultimately achieving long-term stable and efficient inverted PSCs. Summary of the Invention
[0004] In view of this, one objective of the present invention is to provide a method for preparing nickel oxide nanoparticles by low-temperature chemical precipitation; a second objective of the present invention is to provide nickel oxide nanoparticles prepared by the method for preparing nickel oxide nanoparticles by low-temperature chemical precipitation; a third objective of the present invention is to provide an application of nickel oxide nanoparticles in inverted perovskite solar cells; a fourth objective of the present invention is to provide an inverted perovskite solar cell containing nickel oxide nanoparticles; and a fifth objective of the present invention is to provide a method for preparing an inverted perovskite solar cell containing nickel oxide nanoparticles.
[0005] To achieve the above objectives, the present invention provides the following technical solution: 1. A method for preparing nickel oxide nanoparticles by low-temperature chemical precipitation, the method comprising the following steps: (1) Ni(NO3)2·6H2O (nickel nitrate hexahydrate) and NaOH (sodium hydroxide) were dissolved in water to obtain NaOH solution and Ni(NO3)2 solution, respectively, and then placed in an ice-water bath for vigorous stirring; (2) Under the condition that the temperature is not higher than 10℃ and the stirring speed is 800-1200rpm, NaOH solution is added dropwise to Ni(NO3)2 solution until pH=10-10.2, and the reaction is continued for 30-60min to obtain Ni(OH)2 suspension; (3) After stirring the Ni(OH)2 (nickel hydroxide) suspension, solid-liquid separation was performed, and the precipitate was obtained by washing with deionized water; (4) The precipitate is placed in a freeze dryer for drying. After freezing, it is placed in a vacuum chamber for vacuum drying to obtain Ni(OH)2 powder. The Ni(OH)2 powder is placed in a muffle furnace and annealed under air conditions to obtain NiO. x (Nickel oxide) nanoparticles.
[0006] Preferably, in step (1), the concentration of NaOH in the NaOH solution is 0.04-0.1 g / mL, and the concentration of Ni(NO3)2 solution is 0.05-0.1 g / mL; In step (2), the dripping rate is 20-40 drops / min; In step (4), the freeze drying specifically refers to freeze drying at -100℃ for 3 hours, and the annealing condition is 270℃ for 2 hours.
[0007] 2. Nickel oxide nanoparticles prepared according to the above preparation method.
[0008] 3. Application of the above-mentioned nickel oxide nanoparticles in inverted perovskite solar cells.
[0009] 4. An inverted perovskite solar cell containing nickel oxide nanoparticles, wherein the inverted perovskite solar cell comprises, from bottom to top, a transparent conductive glass, a hole transport layer, a self-assembled molecular layer, a perovskite light-absorbing layer, an electron transport layer, a hole blocking layer, and a back electrode; The hole transport layer is made of the aforementioned nickel oxide nanoparticles.
[0010] Preferably, the transparent conductive glass is either ITO (indium tin oxide) or FTO (fluorine-doped tin oxide); The material of the self-assembled molecular layer is any one or more of the following: Me-4PACz ([3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphate), 2PACz ([2-(9H-carbazole-9-yl)ethyl]phosphonic acid), 4PABCz ([2-(9H-9'-phenyl-3,3'-di-carbazole-9-yl)butyl]phosphate), tBu-4PACz ([4-(3,6-di-tert-butyl-9H-carbazole-9-yl)butyl]phosphate), DCZ-4P ([2-(3,3'-di-carbazole-9-yl)butyl]bisphosphate), and 2PADCB ([2-(7H-dibenzo-carbazole-7-yl)ethyl]phosphate). The perovskite light-absorbing layer is made of ABX3, where A is CH3NH3. + CH(NH2)2 + Cs + or Rb + Any one or more of the following, where B is Pb 2+ Sn 2+ Or Ge 2+ Any one or more of them, X is Cl - ,Br - or I - Any one or more of the following; The electron transport layer is made of PC. 61 BM ([6,6]-phenyl C 61 Methyl butyrate), C 60 (Fullerene), SnO2, BaSnO3, TiO2 or ZnO; The hole-blocking layer is made of BCP (dimethyl-4,7-diphenyl-1,10-phenanthroline). The material of the back electrode is any one of Ag, Cu or low-temperature carbon electrode.
[0011] Preferably, the hole transport layer has a thickness of 10-30 nm, the self-assembled molecular layer has a thickness of 1-2 nm, the perovskite light-absorbing layer has a thickness of 500-1000 nm, the electron transport layer has a thickness of 30-100 nm, the hole blocking layer has a thickness of 2-5 nm, and the back electrode has a thickness of 80-200 nm.
[0012] 5. The method for fabricating the above-mentioned inverted perovskite solar cell, wherein the fabrication method comprises the following steps: (1) The transparent conductive glass is pretreated with ultraviolet ozone or plasma to obtain a conductive substrate; (2) The above nickel oxide nanoparticles are dispersed in deionized water and then spin-coated onto the conductive substrate treated in step (1). The hole transport layer can be prepared by annealing. (3) Spin-coating the solution of self-assembled molecules onto the hole transport layer described in step (2), and then annealing to obtain the self-assembled molecular layer; (4) Spin-coat the solution of perovskite precursor material onto the self-assembled molecular layer in step (3). During the spin-coating process, add anti-solvent or directly spin-coat the perovskite wet film in a vacuum chamber and evacuate it. Then anneal it to prepare the perovskite layer. (5) Spin-coating the solution of electron transport layer material onto the perovskite layer described in step (4) to prepare an electron transport layer; (6) The hole blocking layer material is applied to the electron transport layer described in step (5) by spin coating or thermal evaporation to obtain the hole blocking layer; (7) Prepare a back electrode on the hole blocking layer described in step (6).
[0013] Preferably, in step (1), the conductive glass is treated with ultraviolet ozone or plasma for 5 to 30 minutes; In step (2), the above nickel oxide nanoparticles are dispersed in deionized water at a mass-volume ratio of 5-30:1, mg:mL, and ultrasonically vibrated for 10-30 min. The dispersion is then filtered using PVDF. The filtered nanoparticle dispersion is spin-coated on conductive glass at a speed of 2000-6000 rpm for 10-60 s and annealed at 100-150℃ for 5-30 min to prepare the hole transport layer. In step (3), the material of the self-assembled molecule is dissolved in an organic solvent at a mass-volume ratio of 0.1 to 1:1, mg:mL. The mixture is filtered with PTFE and spin-coated onto the hole transport layer at a speed of 2000 to 6000 rpm for 10 to 60 s. The mixture is then annealed at 60 to 100°C for 5 to 20 min to obtain the self-assembled molecule layer. The organic solvent is any one or more of ethanol, isopropanol, or methanol. In step (4), a solution of perovskite precursor material with a concentration of 1.0 to 1.8 mol / L is dropped onto the self-assembled molecular layer described in step (3), and the perovskite layer is prepared by anti-solvent method or vacuum flash evaporation method. In step (5), the electron transport layer is prepared by solution method or thermal evaporation method.
[0014] Preferably, the antisolvent method specifically involves spin coating at a speed of 3000–6000 rpm for 20–60 s, adding 80–150 μL of antisolvent dropwise at the 10th–40th s, and annealing at 100–150°C for 10–60 min. The vacuum flash evaporation method specifically involves: spin coating at a speed of 2000-3000 rpm for 5-10 s, then spin coating at a speed of 3000-6000 rpm for 20-60 s, placing the perovskite wet film in a vacuum chamber with a vacuum degree of 5-15 Pa for 5-30 s, and annealing at 100-150℃ for 10-60 min; Specifically, the solution method involves spin-coating a solution of electron transport layer material with a concentration of 10–20 mg / mL onto the perovskite layer described in step (4) at a spin speed of 2000–5000 rpm for 20–60 s. The thermal evaporation method specifically involves depositing the electron transport layer material onto the perovskite layer in step (4) at an evaporation rate of 0.1–0.3 Å / s, with a thickness of 10–50 nm.
[0015] The beneficial effects of this invention are as follows: 1. This invention provides a method for preparing nickel oxide nanoparticles by low-temperature chemical precipitation, wherein the impurity content (such as NO3) is controlled by low-temperature regulation. - CO3 2- (etc.), ion ratio (e.g., Ni) 3+ / Ni 2+ The proportions, particle size, and dispersion of nickel oxide films can be used to regulate their conductivity, hole mobility, and surface active sites, ultimately improving the charge transport performance of nickel oxide films.
[0016] 2. This invention discloses an inverted perovskite solar cell containing nickel oxide nanoparticles. Nickel oxide nanoparticles synthesized by a low-temperature chemical precipitation method are used to prepare the hole transport layer and applied to the inverted perovskite solar cell. Studies have shown that nickel oxide (NiO) prepared by the low-temperature chemical precipitation method… x The nanoparticles increased the coverage of self-assembled molecules on the surface, promoted perovskite crystallization, and improved the interfacial contact between the hole transport layer and the perovskite layer, thereby improving the long-term stability of the buried interface and the device. Furthermore, the NiO prepared by the low-temperature chemical precipitation method... x The energy levels of the hole transport layer constructed by self-assembled molecules are more matched with those of the perovskite layer, promoting interfacial carrier transfer and extraction, and suppressing nonradiative recombination of interfacial carriers. NiO prepared by low-temperature chemical precipitation... x Nanoparticles improve the photoelectric conversion efficiency, long-term operational stability, and damp-heat stability of perovskite solar cells.
[0017] 3. Inverted perovskite solar cells with band gaps of 1.55 eV, 1.68 eV, and 1.78 eV, synthesized using nickel oxide nanoparticles via low-temperature chemical precipitation, achieved power conversion efficiencies (PCEs) of 27.17%, 24.15%, and 20.36%, respectively. A 1.55 eV perovskite module (14 cm⁻¹) based on nickel oxide nanoparticles synthesized via low-temperature chemical precipitation was also achieved. 2 It achieved a PCE of 23.18%.
[0018] 4. The 1.55 eV inverted perovskite solar cell prepared based on nickel oxide nanoparticles synthesized by low-temperature chemical precipitation retained 91.9% of its initial efficiency after continuous operation at the maximum power point for 2100 h, and retained 91.4% of its initial efficiency after aging at 85℃ / 85%RH for 2000 h.
[0019] 5. This invention employs a low-temperature chemical precipitation method to prepare nickel oxide nanoparticles. This method is simple, reproducible, and widely applicable, and is of great significance in promoting the industrialization of perovskite solar cells. Other advantages, objectives, and features of this invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination, or may be learned from the practice of this invention. The objectives and other advantages of this invention can be realized and obtained through the following description. Attached Figure Description
[0020] To make the objectives, technical solutions, and advantages of the present invention clearer, the preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings, wherein: Figure 1 In the middle, 'a' represents the RT-NiO prepared in Comparative Example 1. x TEM image of b, and LT-NiO prepared in Example 1. x TEM image of the image, c is the particle size distribution statistics of nickel oxide nanoparticles prepared in Comparative Example 1 and Example 1; Figure 2 In the text, A and C represent nickel oxide nanoparticles (RT-NiO) prepared in Comparative Example 1, respectively. x Theoretical calculation diagram of Ni vacancy formation energy in bulk and on the surface, where B and D are the nickel oxide nanoparticles (LT-NiO) prepared in Example 1. x Theoretical calculation diagram of Ni vacancy formation energy in bulk phase and surface; Figure 3 A and B are RT-NiO in Comparative Example 1. x And Example 1 LT-NiO x Comparison of particle size and Zeta potential of the precursor solution before aging; C and D are RT-NiO in Comparative Example 1.x And Example 1 LT-NiO x Comparison of particle size and zeta potential after 40 days of aging of the precursor solution; Figure 4 A and B are RT-NiO in Comparative Example 1. x Thin film and LT-NiO in Example 1 x SEM images of the thin film before aging, C and D are RT-NiO in Comparative Example 1. x Thin film and LT-NiO in Example 1 x SEM image of the film after 40 days of aging; Figure 5 For comparison, RT-NiO in Example 1 x Thin film and LT-NiO in Example 1 x The electrical conductivity of the thin film (A) and hole migration map (B); Figure 6 In the middle, A and B are respectively RT-NiO in Comparative Example 1 x Thin film and LT-NiO in Example 1 x XPS plot of Ni 2p orbitals in the thin film; Figure 7 In the diagrams, A and B are the FTIR and Raman spectra of RT-Ni(OH)2 in Comparative Example 1 and LT-Ni(OH)2 in Example 1, respectively. Figure 8 For comparison, RT-NiO in Example 1 x And LT-NiO in Example 1 x FTIR plot; Figure 9 In the middle, A and B are respectively RT-NiO in Comparative Example 1 x And LT-NiO in Example 1 x XPS plot of N 1s orbital; Figure 10 In the diagram, A, B, and C represent the self-assembled molecules in theoretical NiO, RT-NiO in Comparative Example 1, and RT-NiO, respectively. x And LT-NiO in Example 1 x Theoretical calculation diagram of adsorption energy on the thin film surface; Figure 11 In the diagram, A, B, and C represent the self-assembled molecules in theoretical NiO, RT-NiO in Comparative Example 1, and RT-NiO, respectively. x And LT-NiO in Example 1 x Theoretical calculation diagram of the film surface coverage; Figure 12 In Comparative Example 2, A and B represent RT-NiO. x / SAM film and LT-NiO in Example 2x / P 2p of SAM thin film 3 / 2 XPS graph; Figure 13 In Comparative Example 2, A and B represent RT-NiO. x / SAM film and LT-NiO in Example 2 x Conductive atomic force microscopy (C-AFM) image of a SAM thin film; Figure 14 In the middle, A and B are respectively the ITO / RT-NiO in Comparative Example 2. x / SAM / perovskite and ITO / LT-NiO in Example 2 x SEM image of the perovskite bottom surface in the perovskite sample; Figure 15 In the middle, A and B are respectively the ITO / RT-NiO in Comparative Example 2. x / SAM / perovskite and ITO / LT-NiO in Example 2 x Ultrafast reflectance spectra of / SAM / perovskite samples; Figure 16 In Comparative Example 2, A and B represent RT-NiO deposited in the sample. x SEM images of the surface and cross-section of the perovskite film on the SAM substrate before and after aging, with C and D representing the LT-NiO film in Example 2, respectively. x SEM images of the surface and cross-section of the perovskite film on the SAM substrate before and after aging; Figure 17 In Comparative Example 2, A and B represent RT-NiO... x / SAM and LT-NiO in Example 2 x PL mapping image of the bottom surface of the perovskite film prepared on the SAM substrate after aging. C and D are respectively the RT-NiO in Comparative Example 1. x / SAM and LT-NiO in Example 2 x PL mapping image of the bottom surface of the perovskite film prepared on the SAM substrate after aging; Figure 18 Based on RT-NiO in Comparative Example 1 x The perovskite solar cell with a bandgap of 1.55 eV (Comparative Example 2) and the LT-NiO in Example 1 x Current density-voltage curve of the fabricated 1.55 eV bandgap perovskite solar cell (Example 2); Figure 19 MPPT images of the 1.55 eV bandgap perovskite solar cell devices prepared in Example 2 and Example 2 are provided for comparison. Figure 20 Stability graphs of 1.55 eV bandgap perovskite solar cell devices prepared in Example 2 and Example 2 at 85°C / 85%RH; Figure 21 Based on LT-NiO in Example 2 x The prepared perovskite module with a band gap of 1.55 eV (14 cm⁻¹) 2 The current density-voltage curve of ) Figure 22 The RT-NiO used in Comparative Example 3 is respectively... x And in Example 3, LT-NiO x Current density-voltage curves of a 1.68 eV bandgap perovskite solar cell on a substrate during forward and reverse scanning. Figure 23 For comparison, in Example 4, RT-NiO was used. x And in Example 4, LT-NiO x Current density-voltage curves of a 1.78 eV bandgap perovskite solar cell on a substrate during forward and reverse scanning. Figure 24 For comparison, in Example 4, RT-NiO was used. x And in Example 4, LT-NiO x MPPT plot of current for a perovskite solar cell with a bandgap of 1.78 eV on a substrate. Detailed Implementation
[0021] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments are only schematic representations of the basic concept of the present invention. Unless otherwise specified, the following embodiments and features can be combined with each other.
[0022] Comparative Example 1 Nickel oxide nanoparticles were prepared by a room-temperature chemical precipitation method, as detailed below: (1) Add 9.0g Ni(NO3)2·6H2O (nickel nitrate hexahydrate) to a beaker containing 180mL of water and stir to dissolve at room temperature to obtain Ni(NO3)2 solution. Add 3.0g NaOH (sodium hydroxide) to a beaker containing 75mL of water and stir to dissolve at room temperature to obtain NaOH solution. Place the Ni(NO3)2 solution and NaOH solution in an ice-water bath and stir vigorously. (2) Under the conditions of room temperature and stirring at 1000 rpm, add NaOH solution to Ni(NO3)2 solution at a rate of 20 drops / min until pH=10, and continue the reaction for 30 min to obtain Ni(OH)2 suspension; (3) The above Ni(OH)2 (nickel hydroxide) suspension was stirred at 800 rpm for 5 min and centrifuged to separate solid and liquid. It was washed with deionized water and the precipitate was obtained by repeated centrifugation and washing. (4) The above precipitate was placed in a freeze dryer and dried at -100℃ for 3 hours. After freezing, it was placed in a vacuum chamber at 5 Pa and dried for 15 hours to obtain Ni(OH)2 powder. The Ni(OH)2 powder was placed in a muffle furnace and annealed at 270℃ for 2 hours under air conditions to obtain nickel oxide nanoparticles (RT-NiO) prepared by room temperature chemical precipitation method. x ).
[0023] Comparative Example 2 A 1.55 eV bandgap perovskite solar cell was fabricated, wherein the hole transport layer material of the perovskite solar cell was the nickel oxide nanoparticles (RT-NiO) prepared in Comparative Example 1. x The specific method is as follows: (1) ITO transparent conductive glass was used as a conductive substrate. It was ultrasonically cleaned for 20 min by glass cleaner, deionized water, acetone and anhydrous ethanol in sequence. After being dried with nitrogen, it was pretreated with ultraviolet ozone for 15 min and cooled to obtain the pretreated conductive substrate for use. (2) 10 mg of nickel oxide nanoparticles (RT-NiO) prepared in Comparative Example 1 were used. x The RT-NiO was dispersed in 1 mL of deionized water and sonicated for 10 min. Then, it was filtered using PVDF to obtain RT-NiO. x Nanoparticle dispersion. Then, 50 μL of NiO was taken. x The nanoparticles were dispersed at 5000 rpm and spin-coated onto the conductive substrate from step (1) for 30 s. Then, RT-NiO was prepared by annealing at 150 °C for 10 min. x Hole transport layer; (3) Dissolve 0.3 mg of Me-4PACz molecules in 1 mL of anhydrous ethanol and shake for 30 min. Then, filter using PTFE to obtain the Me-4PACz solution. Subsequently, take 55 μL of the Me-4PACz solution and rotate at 5000 rpm in the RT-NiO2 reactor from step (2). x A self-assembled molecular layer was obtained by spin-coating the hole transport layer for 30 s and then annealing it at 100 °C for 10 min. (4) Dissolve 20.78 mg cesium iodide (CsI), 247.68 mg formamidine iodide (FAI), 12.72 mg methylamine iodide (MAI), 15.00 mg methylamine chloride (MACl), and 796.55 mg lead iodide (PbI2, 10% excess) in 1 ml of a mixed solvent of N,N-dimethylformamide (DMF) and N,N-dimethyl sulfoxide (DMSO) at a volume ratio of 4:1 to form 1.73 M CsI. 0.05 MA 0.05 FA 0.9 PbI3 perovskite precursor solution was used. Then, 65 μL of the perovskite precursor solution was spin-coated onto the self-assembled molecular layer in step (3) at a speed of 2000 rpm for 10 s in the first step, and then spin-coated at a speed of 4000 rpm for 10 s in the second step. Then, the perovskite wet film was placed in a vacuum chamber and evacuated at 5 Pa for 11 s. Next, it was annealed at 150 °C for 1 min, then annealed at 100 °C for 10 min, and cooled to room temperature to obtain the perovskite layer. (5) Take 10 mg PC 61 BM was dissolved in 1 mL of chlorobenzene and shaken for 1 h. Then, PC was obtained by filtration using PTFE. 61 BM solution. Then, take 30 μL of PC. 61 BM solution was spin-coated onto the perovskite layer in step (4) for 40 s at a rotation speed of 2500 rpm to obtain PC. 61 BM thin film; (6) Take 500 mg C 60 The powder was placed in a vacuum evaporation crucible and evaporated at a rate of 0.1 Å / s. 60 Deposition of PC in step (5) 61 A 21 nm thick C film was fabricated on a BM thin film. 60 film; (7) Place 500 mg of BCP powder in a vacuum evaporation crucible and deposit BCP at an evaporation rate of 0.1 Å / s on the C in step (6). 60 A 6 nm thick BCP film was fabricated on the film. (8) Place 1g of Ag particles in a vacuum evaporation tungsten boat and deposit Ag on the BCP film of step (7) at an evaporation rate of 0.5 Å / s to obtain an Ag back electrode with a thickness of 100 nm.
[0024] Comparative Example 3 A 1.68 eV bandgap perovskite solar cell was fabricated, wherein the hole transport layer material of the perovskite solar cell was the nickel oxide nanoparticles (RT-NiO) prepared in Comparative Example 1. x The specific method is as follows: (1) ITO transparent conductive glass was used as a conductive substrate. It was ultrasonically cleaned for 20 min by glass cleaner, deionized water, acetone and anhydrous ethanol in sequence. After being dried with nitrogen, it was pretreated with ultraviolet ozone for 15 min and cooled to obtain the pretreated conductive substrate for use. (2) 20 mg of nickel oxide nanoparticles (RT-NiO) prepared in Comparative Example 1 were used. x The RT-NiO was dispersed in 1 mL of deionized water and sonicated for 10 min. Then, it was filtered using PVDF to obtain RT-NiO. x Nanoparticle dispersion, then take 50 μL NiO x The nanoparticles were dispersed at 5000 rpm and spin-coated onto the conductive substrate from step (1) for 30 s. Then, RT-NiO was prepared by annealing at 150 °C for 15 min. x Hole transport layer; (3) Dissolve 0.3 mg of MeO-2PACz molecules in 1 mL of anhydrous ethanol and shake for 30 min. Then, filter using PTFE to obtain the MeO-2PACz solution. Subsequently, take 55 μL of the MeO-2PACz solution and rotate at 5000 rpm for RT-NiO in step (2). x Spin-coating was performed on the hole transport layer for 30 s. Next, the self-assembled molecular layer was obtained by annealing at 100 °C for 10 min. (4) Dissolve 18.20 mg cesium iodide (CsI), 192.60 mg formamidine iodide (FAI), 536.00 mg lead iodide (PbI2, 10% excess), 131.00 mg lead bromide (PbBr2), and 23.50 mg methylammonium bromide (MABr) in 1 mL of a 4:1 mixture of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) to prepare 1.4 M CsI. 0.05 MA 0.15 FA 0.8 PbI 2.28 Br 0.72The perovskite precursor solution was prepared, and then 55 μL of perovskite precursor solution was taken and spin-coated on the self-assembled molecular layer in step (3) at a speed of 1000 rpm for 10 s in the first step, and then spin-coated at a speed of 5000 rpm for 40 s in the second step. 200 μL of antisolvent chlorobenzene (CB) was added dropwise at the 20th s. Subsequently, the perovskite wet film was annealed at 100 ℃ for 15 min and cooled to obtain the perovskite layer.
[0025] (5) Take 23 mg PC 61 BM was dissolved in 1 mL of chlorobenzene and shaken for 1 h. Then, PC was obtained by filtration using PTFE. 61 BM solution. Then, take 30 μL of PC. 61 BM solution was spin-coated onto the perovskite layer in step (4) for 40 s at a rotation speed of 2500 rpm to obtain PC. 61 BM thin film; (6) Take 500 mg C 60 The powder was placed in a vacuum evaporation crucible and evaporated at a rate of 0.1 Å / s. 60 Deposition of PC in step (5) 61 A 15 nm thick C film was fabricated on a BM thin film. 60 film; (7) Place 500 mg of BCP powder in a vacuum evaporation crucible and deposit BCP at an evaporation rate of 0.1 Å / s on the C in step (6). 60 A 5 nm thick BCP film was fabricated on the film. (8) Place 1g of Ag particles in a vacuum evaporation tungsten boat and deposit Ag on the BCP film of step (7) at an evaporation rate of 0.5 Å / s to obtain an Ag back electrode with a thickness of 100 nm.
[0026] Comparative Example 4 A 1.78 eV bandgap perovskite solar cell was fabricated, wherein the hole transport layer material of the perovskite solar cell was the nickel oxide nanoparticles (RT-NiO) prepared in Comparative Example 1. x The specific method is as follows: (1) ITO transparent conductive glass was used as a conductive substrate. It was ultrasonically cleaned for 20 min by glass cleaner, deionized water, acetone and anhydrous ethanol in sequence. After being dried with nitrogen, it was pretreated with ultraviolet ozone for 15 min and cooled to obtain the pretreated conductive substrate for use. (2) 15 mg of nickel oxide nanoparticles (RT-NiO) prepared in Comparative Example 1 were used. x The RT-NiO was dispersed in 1 mL of deionized water and sonicated for 10 min. Then, it was filtered using PVDF to obtain RT-NiO. xNanoparticle dispersion. Then, 50 μL of NiO was taken. x The nanoparticles were dispersed at 2500 rpm and spin-coated onto the conductive substrate from step (1) for 30 s. Then, RT-NiO was prepared by annealing at 150 °C for 20 min. x Hole transport layer; (3) Dissolve 0.5 mg of Me-4PACz molecules in 1 mL of anhydrous ethanol and shake for 30 min. Then, filter using PTFE to obtain the Me-4PACz solution. Subsequently, take 55 μL of the Me-4PACz solution and rotate at 4000 rpm in the RT-NiO2 reactor from step (2). x A self-assembled molecular layer was obtained by spin-coating the hole transport layer for 40 s and then annealing it at 100 °C for 10 min. (4) Dissolve 62.35 mg cesium iodide (CsI), 165.07 mg ammonium iodide (MAI), 221.30 mg lead iodide (PbI2), and 264.25 mg lead bromide (PbBr2) in 1 mL of a mixed solvent of N,N-dimethylformamide (DMF) and N,N-dimethyl sulfoxide (DMSO) in a volume ratio of 4:1 to form 1.2 M Cs 0.2 FA 0.8 PbI 1.8 Br 1.2 Perovskite precursor solution, then take 50 μL of perovskite precursor solution, spin coat it on the self-assembled molecular layer in step (3) at a speed of 500 rpm for 5 s in the first step, then spin coat it at a speed of 4000 rpm for 40 s in the second step, add 700 μL of antisolvent diethyl ether at 35 s, then anneal the perovskite wet film at 100℃ for 15 min, and obtain the perovskite layer after cooling; (5) Take 21 mg PC 61 BM was dissolved in 1 mL of chlorobenzene and shaken for 1 h. Then, PC was obtained by filtration using PTFE. 61 BM solution. Then, take 30 μL of PC. 61 BM solution was spin-coated onto the perovskite layer in step (4) for 40 s at a rotation speed of 2500 rpm to obtain PC. 61 BM thin film; (6) Take 500 mg C 60 The powder was placed in a vacuum evaporation crucible and evaporated at a rate of 0.1 Å / s. 60 Deposition of PC in step (5) 61 A 15 nm thick C film was fabricated on a BM thin film. 60 film; (7) Place 500 mg of BCP powder in a vacuum evaporation crucible and deposit BCP at an evaporation rate of 0.1 Å / s on the C in step (6). 60 A 5 nm thick BCP film was fabricated on the film. (8) Place 1g of Ag particles in a vacuum evaporation tungsten boat and deposit Ag on the BCP film of step (7) at an evaporation rate of 0.5 Å / s to obtain an Ag back electrode with a thickness of 100 nm.
[0027] Example 1
[0028] Nickel oxide nanoparticles (LT-NiO) were prepared by a low-temperature chemical precipitation method. x The specific preparation method is as follows: (1) Add 9.0g Ni(NO3)2·6H2O (nickel nitrate hexahydrate) to a beaker containing 180mL of water, stir and dissolve in an ice-water bath for 30min to obtain Ni(NO3)2 solution, add 3.0g NaOH (sodium hydroxide) to a beaker containing 75mL of water, stir and dissolve in an ice-water bath for 30min to obtain NaOH solution; (2) Under the conditions of 0℃ and stirring at 1000rpm, NaOH solution is added dropwise to Ni(NO3)2 solution at a rate of 20 drops / min until pH=10, and the reaction is continued for 30min to obtain Ni(OH)2 suspension; (3) The above Ni(OH)2 (nickel hydroxide) suspension was stirred at 800 rpm for 5 min and centrifuged to separate solid and liquid. It was washed with deionized water and the precipitate was obtained by repeated centrifugation and washing. (4) The above precipitate was placed in a freeze dryer and dried at -100℃ for 3 hours. After freezing, it was placed in a vacuum chamber at 5 Pa and dried for 15 hours to obtain Ni(OH)2 powder. The Ni(OH)2 powder was placed in a muffle furnace and annealed at 270℃ for 2 hours under air conditions to obtain nickel oxide nanoparticles (LT-NiO) prepared by low-temperature chemical precipitation method. x ).
[0029] Figure 1 In the middle, 'a' represents the RT-NiO prepared in Comparative Example 1. x TEM image of b, and LT-NiO prepared in Example 1. x TEM images, c shows the particle size distribution statistics of nickel oxide nanoparticles prepared in Comparative Example 1 and Example 1. Figure 1 As can be seen from this, LT-NiO x With RT-NiO x In comparison, nickel oxide nanoparticles (LT-NiO) prepared by low-temperature chemical precipitation method... xThe smaller and more uniform particle size indicates that the grain growth of nickel oxide nanoparticles can be controlled by low-temperature chemical precipitation, thereby obtaining finer and more uniform nanoparticles.
[0030] Figure 2 In the text, A and C represent nickel oxide nanoparticles (RT-NiO) prepared in Comparative Example 1, respectively. x Theoretical calculation diagram of Ni vacancy formation energy in bulk and on the surface, where B and D are the nickel oxide nanoparticles (LT-NiO) prepared in Example 1. x Theoretical calculations of Ni vacancy formation energies in the bulk and surface phases. (From...) Figure 2 As can be seen, the formation energy of Ni vacancies on the nickel oxide surface is much smaller than that in the bulk phase, making it easier for Ni vacancies to form on the nickel oxide surface. Since nickel oxide nanoparticles prepared by low-temperature chemical precipitation have a larger specific surface area, they thus have more Ni vacancies on their surface.
[0031] Figure 3 A and B are RT-NiO in Comparative Example 1. x And Example 1 LT-NiO x Comparison of particle size and Zeta potential of the precursor solution before aging; C and D are RT-NiO in Comparative Example 1. x And Example 1 LT-NiO x Comparison of particle size and zeta potential after 40 days of aging of the precursor solution. Figure 3 As can be seen from the data, LT-NiO before and after aging... x The high zeta potential and smaller, more uniform particle size indicate that LT-NiO x Nanoparticles exhibit a higher surface electrostatic distribution, inhibiting their aggregation in solution and improving the stability of the nickel oxide precursor solution. In contrast, RT-NiO... x After aging, the dispersion exhibited obvious precipitation and stratification, and its Zeta potential decreased sharply, indicating that RT-NiO... x Nanoparticles are prone to aggregation and are unstable.
[0032] Figure 4 A and B are RT-NiO in Comparative Example 1. x Thin film and LT-NiO in Example 1 x SEM images of the thin film before aging, C and D are RT-NiO in Comparative Example 1. x Thin film and LT-NiO in Example 1 x SEM image of the film after 40 days of aging. Figure 4 As can be seen from this, RT-NiO x After aging, the thin film developed obvious pores, while LT-NiOx The film remained almost unchanged and still exhibited excellent compactness. This indicates that LT-NiO x Nanoparticles are not prone to aggregation and have excellent humidity stability.
[0033] Figure 5 For comparison, RT-NiO in Example 1 x Thin film and LT-NiO in Example 1 x The electrical conductivity (A) and hole migration map of the thin film (B). From Figure 5 As can be seen from this, compared with RT-NiO x Compared to thin films, LT-NiO x The thin film exhibits higher electrical conductivity and hole mobility, indicating that LT-NiO x Thin films have better electrical properties, which is beneficial for hole transport and collection.
[0034] Figure 6 In the middle, A and B are respectively RT-NiO in Comparative Example 1 x Thin film and LT-NiO in Example 1 x XPS plot of the Ni 2p orbitals in the thin film. From Figure 6 As can be seen from this, RT-NiO x Ni in thin films 3+ / Ni 2+ The proportion is lower than LT-NiO x Ni in thin films 3+ / Ni 2+ The ratio. This is due to LT-NiO. x With RT-NiO x Compared to those with higher specific surface area, LT-NiO has more Ni vacancies on its surface, thus improving its performance. x Chinese Ni 3+ The content of.
[0035] Figure 7 In Figure A and B, the FTIR and Raman spectra of RT-Ni(OH)2 in Comparative Example 1 and LT-Ni(OH)2 in Example 1, respectively. From... Figure 7 As can be seen, compared with RT-Ni(OH)2, LT-Ni(OH)2 contains less NO3-. - With CO3 2- The vibrational peak intensity of impurity ions was significantly weakened. This indicates that low-temperature chemical precipitation can suppress side reactions, thereby inhibiting NO3-. - With CO3 2- Formation of impurity ions.
[0036] Figure 8 For comparison, RT-NiO in Example 1 xAnd LT-NiO in Example 1 x FTIR plot. From Figure 8 As can be seen from the above, after the heating reaction, RT-NiO x There is still a relatively strong NO3 in China. - With CO3 2- The vibration peak, while LT-NiO x The vibrational peaks of impurity ions in LT-NiO are significantly weakened. This indicates that... x It contains fewer impurities.
[0037] Figure 9 In the middle, A and B are respectively RT-NiO in Comparative Example 1 x And LT-NiO in Example 1 x XPS plot of the N 1s orbit. From Figure 9 As can be seen from this, compared with LT-NiO x Compared to RT-NiO x It has higher NO3 - The content of impurity ions indicates that the low-temperature chemical precipitation method can suppress the formation of impurity ions.
[0038] Figure 10 In the diagram, A, B, and C represent the self-assembled molecules in theoretical NiO, RT-NiO in Comparative Example 1, and RT-NiO, respectively. x And LT-NiO in Example 1 x A theoretically calculated graph of the adsorption energy on the thin film surface. From... Figure 10 As can be seen from this, compared with RT-NiO x In comparison, SAM molecules and LT-NiO x They have higher adsorption energies. This is due to LT-NiO x More Ni exists on the surface 3+ This provides more binding sites for SAM molecules, thereby improving the binding of SAM with LT-NiO. x Adsorption energy.
[0039] Figure 11 In the diagram, A, B, and C represent the self-assembled molecules in theoretical NiO, RT-NiO in Comparative Example 1, and RT-NiO, respectively. x And LT-NiO in Example 1 x A theoretical calculation diagram of the film surface coverage. From Figure 11 It can be seen that, compared with RT-NiO x In comparison, self-assembled molecules in LT-NiO x The film surface has a higher coverage.
[0040] Example 2
[0041] Fabrication of a 1.55 eV bandgap perovskite solar cell module (14 cm⁻¹)2 The hole transport layer material of this perovskite solar cell is the nickel oxide nanoparticles (LT-NiO) prepared in Example 1. x The preparation steps are as follows: (1) Six sub-cell regions of 0.5 cm × 4 cm, namely P1 lines, with a width of 30 μm were etched on a 5 cm × 5 cm ITO glass using a femtosecond laser. Then, the glass was ultrasonically cleaned for 20 min in sequence with glass cleaner, deionized water, acetone and anhydrous ethanol, dried with nitrogen and pretreated with ultraviolet ozone for 15 min, and cooled to obtain a pretreated conductive substrate for use. (2) 500 mg of LT-NiO prepared by low-temperature precipitation in Example 1 x Nanoparticles were dispersed in 50 mL of deionized water and sonicated for 10 min. Then, LT-NiO was obtained by PVDF filtration. x Nanoparticle dispersion. Then, 500 μL of NiO was taken. x The nanoparticle dispersion was spin-coated onto the conductive substrate from step (1) at 5000 rpm for 30 s. Next, LT-NiO was prepared by annealing at 150 °C for 10 min. x Hole transport layer; (3) Dissolve 5 mg Me-4PACz in 10 mL of anhydrous ethanol, shake for 10 min, and then filter using PTFE to obtain the Me-4PACz solution. Subsequently, add it to a slot coater and coat it onto the LT-NiO from step (2) at a coating speed of 10 mm / s. x A self-assembled molecular layer was prepared on the layer; (4) Dissolve 200.78 mg cesium iodide (CsI), 2470.68 mg formamidine iodide (FAI), 120.72 mg methylamine iodide (MAI), 150.00 mg methylamine chloride (MACl), and 7960.55 mg lead iodide (PbI2, 10% excess) in 10 ml of a mixed solvent of N,N-dimethylformamide (DMF) and N,N-dimethyl sulfoxide (DMSO) at a volume ratio of 4:1 to form 1.73 M CsI. 0.05 MA 0.05 FA 0.9 PbI3 perovskite precursor solution. Subsequently, the precursor solution was added to a slot coater and coated at a speed of 10 mm / s to form the self-assembled molecular layer in step (3). Then, the perovskite wet film was placed in a vacuum chamber and evacuated at 5 Pa for 11 s. Next, it was annealed at 150 °C for 1 min, then annealed at 100 °C for 10 min, and cooled to room temperature to obtain the perovskite layer; (5) Add 1g C60 The powder was placed in a vacuum evaporation crucible and evaporated at a rate of 0.1 Å / s. 60 A 15 nm thick C film was deposited on the perovskite film in step (4). 60 film; (6) Place 700 mg of BCP powder in a vacuum evaporation crucible and deposit the BCP at an evaporation rate of 0.1 Å / s on the C in step (5). 60 A 5 nm thick BCP film was fabricated on the film. (7) Place 3g of Ag particles in a vacuum evaporation tungsten boat and deposit Ag on the BCP film of step (6) at an evaporation rate of 0.5 Å / s to obtain an Ag back electrode with a thickness of 100 nm.
[0042] Figure 12 In Comparative Example 2, A and B represent RT-NiO. x / SAM film and LT-NiO in Example 2 x / P 2p of SAM thin film 3 / 2 XPS graph. From Figure 12 As can be seen from this, compared with RT-NiO x Compared to thin films, SAM in LT-NiO x The thin film surface has a higher adsorption capacity and stronger binding ability.
[0043] Figure 13 In Comparative Example 2, A and B represent RT-NiO. x / SAM film and LT-NiO in Example 2 x Conductive atomic force microscopy (C-AFM) image of a SAM thin film. From Figure 13 As can be seen from this, compared with RT-NiO x In comparison, SAM molecules in LT-NiO x The surface exhibits a more uniform current distribution, indicating that SAM molecules in LT-NiO x The thin film surface has a more uniform distribution.
[0044] Figure 14 In the middle, A and B are respectively the ITO / RT-NiO in Comparative Example 2. x / SAM / perovskite and ITO / LT-NiO in Example 2 x SEM image of the perovskite substrate in a perovskite sample. Figure 14 It can be seen that the deposited LT-NiO x The perovskite substrate has virtually no pores and exhibits excellent density. In contrast, RT-NiO... xThe bottom surface of the perovskite thin film prepared on the substrate has a large number of holes, indicating poor compactness.
[0045] Figure 15 In the middle, A and B are respectively the ITO / RT-NiO in Comparative Example 2. x / SAM / perovskite and ITO / LT-NiO in Example 2 x Ultrafast reflectance spectra of / SAM / perovskite samples. Figure 15 As can be seen from this, LT-NiO x The extraction rate of holes from perovskite films by the thin film is much higher than that of RT-NiO. x film.
[0046] Figure 16 In Comparative Example 2, A and B represent RT-NiO deposited in the sample. x SEM images of the surface and cross-section of the perovskite film on the SAM substrate before and after aging, with C and D representing the LT-NiO film in Example 2, respectively. x SEM images of the surface and cross-section of the perovskite film on a SAM substrate before and after aging. Figure 16 It can be seen that, compared with RT-NiO x In comparison, deposited on LT-NiO x The perovskite film has better bottom surface stability.
[0047] Figure 17 In Comparative Example 2, A and B represent RT-NiO... x / SAM and LT-NiO in Example 2 x PL mapping image of the bottom surface of the perovskite film prepared on the SAM substrate after aging. C and D are respectively the RT-NiO in Comparative Example 2. x / SAM and LT-NiO in Example 2 x PL mapping image of the bottom surface of the perovskite film prepared on the SAM substrate after aging. Figure 17 It can be seen that after aging, RT-NiO x The fluorescence emission intensity of perovskite films on LT-NiO3 substrates is significantly reduced, while that on LT-NiO3 substrates is significantly reduced. x The PL strength of the perovskite film on the substrate only decreased slightly. This indicates that LT-NiO x Nanoparticles can improve the stability of the buried interface of the battery.
[0048] Figure 18 Based on RT-NiO in Comparative Example 1 x The fabricated perovskite solar cell with a bandgap of 1.55 eV (Comparative Example 2) and the LT-NiO based in Example 1 xCurrent density-voltage curves of the fabricated 1.55 eV bandgap perovskite solar cell (Example 2). From... Figure 18 As can be seen from this, compared with RT-NiO x Compared to LT-NiO x The battery achieves a higher PCE. Based on LT-NiO x The perovskite solar cell achieved a PCE of 27.17%, with a short-circuit current density ( J SC The value was 26.43 mA / cm. 2 Open circuit voltage ( V OC The voltage is 1.193 V and the fill factor (FF) is 86.17%, which significantly improves the device performance compared to the substrate.
[0049] Figure 19 MPPT plots of the 1.55 eV bandgap perovskite solar cell devices prepared in Example 2 and Example 2 are shown. Figure 19 As can be seen from this, LT-NiO x The perovskite solar cell device based on [substrate name] maintained 91.9% of its initial PCE after 2100 hours of continuous operation at maximum power output. In contrast, [substrate name] based on [substrate name]... x The perovskite solar cell device based on this substrate retained only 79.44% of its initial PCE after 1100 h.
[0050] Figure 20 To compare the stability of the 1.55 eV bandgap perovskite solar cell devices prepared in Example 2 and Example 2 at 85°C / 85%RH. From Figure 20 It can be seen from this that after 2000 h at 85℃ / 85% LT-NiO x The perovskite-based solar cell device still maintains an initial PCE of 91.4%. In contrast, the RT-NiO substrate... x The perovskite solar cell device based on this substrate had an initial PCE of only 84.8% after 2000 h.
[0051] Figure 21 Based on LT-NiO in Example 2 x The prepared perovskite module with a band gap of 1.55 eV (14 cm⁻¹) 2 The current density-voltage curve of ( ). From Figure 21 As can be seen from this, based on LT-NiO x 1.55 eV bandgap perovskite solar cell module (14 cm) 2 ) achieved a PCE of 23.18%, of which J SC4.55 mA / cm 2 , V OC It is 6.57 V, and the FF is 77.8%.
[0052] Example 3
[0053] Fabrication of a 1.68 eV bandgap perovskite solar cell module (14 cm⁻¹) 2 The hole transport layer material of this perovskite solar cell is the nickel oxide nanoparticles (LT-NiO) prepared in Example 1. x The difference between this preparation and Comparative Example 3 is that the nickel oxide nanoparticles (RT-NiO) prepared by room temperature chemical precipitation in Comparative Example 1 are used instead of the nickel oxide nanoparticles (RT-NiO) prepared by room temperature chemical precipitation. x Replace ) with nickel oxide nanoparticles (RT-NiO) prepared by low-temperature chemical precipitation in Example 1. x The remaining preparation steps are the same as in Comparative Example 3.
[0054] Figure 22 The RT-NiO used in Comparative Example 3 is respectively... x And in Example 3, LT-NiO x Current density-voltage curves for a 1.68 eV bandgap perovskite solar cell on a substrate during forward and reverse scans. From... Figure 22 As can be seen from this, LT-NiO x A perovskite solar cell with a 1.68 eV bandgap based on a substrate achieved a PCE of 24.15%, where the short-circuit current ( J sc The value was 22.09 mA / cm². 2 Open circuit voltage ( V oc The voltage is 1.285 V, the fill factor (FF) is 85.06%, and it is similar to RT-NiO. x Compared to devices based on this substrate, its device performance is significantly improved.
[0055] Example 4
[0056] Fabrication of a 1.78 eV bandgap perovskite solar cell module (14 cm⁻¹) 2 The hole transport layer material of this perovskite solar cell is the nickel oxide nanoparticles (LT-NiO) prepared in Example 1. x The difference between this preparation and Comparative Example 4 is that the nickel oxide nanoparticles (RT-NiO) prepared by room temperature chemical precipitation in Comparative Example 1 are used instead of the nickel oxide nanoparticles (RT-NiO) prepared by room temperature chemical precipitation in Comparative Example 1. x Replace ) with nickel oxide nanoparticles (RT-NiO) prepared by low-temperature chemical precipitation in Example 1.x The remaining preparation steps are the same as in Comparative Example 4.
[0057] Figure 23 For comparison, in Example 4, RT-NiO was used. x And in Example 4, LT-NiO x Current density-voltage curves for a 1.78 eV bandgap perovskite solar cell on a substrate during forward and reverse scans. From... Figure 23 As can be seen from this, LT-NiO x A perovskite solar cell with a 1.78 eV bandgap based on a substrate achieved a PCE of 20.36%, of which J sc 18.83 mA / cm 2 , V oc The voltage is 1.261 V, and the FF is 85.85%, compared with RT-NiO. x Compared to devices based on this substrate, its device performance is significantly improved.
[0058] Figure 24 For comparison, in Example 4, RT-NiO was used. x And in Example 4, LT-NiO x MPPT plot of current for a perovskite solar cell with a 1.78 eV bandgap substrate. From Figure 24 As can be seen from this, LT-NiO x The perovskite solar cell device based on [substrate name] maintained 92.75% of its initial PCE after 500 hours of continuous operation at maximum power output. In contrast, [substrate name] based on [substrate name]... x The perovskite solar cell device based on the substrate only retains 80% of the initial PCE after 250 h.
[0059] Example 5
[0060] Nickel oxide nanoparticles (LT-NiO) were prepared by a low-temperature chemical precipitation method. x The specific preparation method is as follows: (1) Add 18.0g Ni(NO3)2·6H2O (nickel nitrate hexahydrate) to a beaker containing 180mL of water, stir and dissolve in an ice-water bath for 30min to obtain Ni(NO3)2 solution, add 7.5.0g NaOH (sodium hydroxide) to a beaker containing 75mL of water, stir and dissolve in an ice-water bath for 30min to obtain NaOH solution; (2) Under the conditions of 10℃ and stirring at 800rpm, NaOH solution is added dropwise to Ni(NO3)2 solution at a rate of 20 drops / min until pH=10.2, and the reaction is continued for 30min to obtain Ni(OH)2 suspension; (3) The above Ni(OH)2 (nickel hydroxide) suspension was stirred at 800 rpm for 5 min and centrifuged to separate solid and liquid. It was washed with deionized water and the precipitate was obtained by repeated centrifugation and washing. (4) The above precipitate was placed in a freeze dryer and dried at -100℃ for 3 hours. After freezing, it was placed in a vacuum chamber at 5 Pa and dried for 15 hours to obtain Ni(OH)2 powder. The Ni(OH)2 powder was placed in a muffle furnace and annealed at 270℃ for 2 hours under air conditions to obtain nickel oxide nanoparticles (LT-NiO) prepared by low-temperature chemical precipitation method. x ).
[0061] Similarly, testing revealed that the nickel oxide nanoparticles (LT-NiO) prepared by the low-temperature chemical precipitation method in Example 5... x (and the nickel oxide nanoparticles (LT-NiO) prepared by the low-temperature chemical precipitation method in Example 1) x Its function is basically the same in inverted perovskite solar cells.
[0062] In addition, the transparent conductive glass of the above-mentioned inverted perovskite solar cell can be replaced with FTO (fluorine-doped tin oxide) instead of ITO (indium tin oxide) in the above embodiments; the material of the self-assembled molecular layer can be replaced with any one or more of 2PACz ([2-(9H-carbazole-9-yl)ethyl]phosphonic acid), 4PABCz ([2-(9H-9'-phenyl-3,3'-di-carbazole-9-yl)butyl]phosphoric acid), tBu-4PACz ([4-(3,6-di-tert-butyl-9H-carbazole-9-yl)butyl]phosphoric acid), DCZ-4P ([2-(3,3'-di-carbazole-9-yl)butyl]bisphosphoric acid), and 2PADCB ([2-(7H-dibenzo-carbazole-7-yl)ethyl]phosphoric acid) instead of Me-4PACz ([3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid); and A in the perovskite light-absorbing layer material can be replaced with CH3NH3. + CH(NH2)2 + Cs + or Rb + B can be replaced by any one or more of the following: B can be replaced by Pb. 2+ Sn 2+ Or Ge 2+ X can be replaced by any one or more of the following, and X can be replaced by Cl. - ,Br - or I -Any one or more of the above can be substituted; the material of the electron transport layer can be PC. 61 BM ([6,6]-phenyl C 61 Methyl butyrate), SnO2, BaSnO3, TiO2 or ZnO, or any one or more of these can replace C. 60 (Fullerene); The back electrode material can be either Cu or low-temperature carbon electrode to replace Ag, and nickel oxide nanoparticles (LT-NiO) are prepared by the low-temperature chemical precipitation method of this invention. x As a hole transport layer material, its performance is basically the same as that of Examples 2 to 4 above.
[0063] In summary, this invention proposes a low-temperature chemical precipitation method for preparing nickel oxide nanoparticles for use as the hole transport layer in inverted perovskite solar cells. Compared with nickel oxide nanoparticles prepared by room-temperature chemical precipitation, the NiO prepared by the low-temperature chemical precipitation method... x Nanoparticles exhibit lower impurity content, higher electrical conductivity, and higher hole mobility. Furthermore, NiO prepared by a low-temperature chemical precipitation method... x Nanoparticles increase the coverage of self-assembled molecules on the surface, promote perovskite crystallization, and improve the interfacial contact between the hole transport layer and the perovskite layer, thereby enhancing the long-term stability of the buried interface and the device. Furthermore, NiO prepared by low-temperature chemical precipitation... x The hole transport layer constructed by self-assembled molecules better matches the energy levels of the perovskite layer, promoting interfacial carrier transfer and extraction, and suppressing nonradiative recombination of interfacial carriers. Inverted perovskite solar cells with band gaps of 1.55 eV, 1.68 eV, and 1.78 eV, synthesized using nickel oxide nanoparticles via low-temperature chemical precipitation, achieved power conversion efficiencies (PCEs) of 27.17%, 24.15%, and 20.36%, respectively. A 1.55 eV perovskite module (14 cm⁻¹) based on nickel oxide nanoparticles synthesized via low-temperature chemical precipitation was also successfully fabricated. 2 The PCE was 23.18%. The 1.55 eV inverted perovskite solar cell retained 91.9% of its initial efficiency after 2100 hours of continuous operation at maximum power point, and retained 91.4% of its initial efficiency after aging at 85℃ / 85%RH for 2000 hours. This method is simple, reproducible, and widely applicable, and is of great significance in promoting the industrialization of perovskite solar cells. Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the present invention, and all such modifications and substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for the low temperature chemical precipitation of nickel oxide nanoparticles, characterized in that, The preparation method includes the following steps: (1) Dissolve Ni(NO3)2·6H2O and NaOH in water to obtain NaOH solution and Ni(NO3)2 solution respectively, and place them in an ice-water bath for vigorous stirring; (2) Under the condition that the temperature is not higher than 10℃ and the stirring speed is 800-1200rpm, NaOH solution is added dropwise to Ni(NO3)2 solution until pH=10-10.2, and the reaction is continued for 30-60min to obtain Ni(OH)2 suspension; (3) After stirring the Ni(OH)2 suspension, solid-liquid separation was performed, and the precipitate was obtained by washing with deionized water; (4) The precipitate is placed in a freeze dryer for drying. After freezing, it is placed in a vacuum chamber for vacuum drying to obtain Ni(OH)2 powder. The Ni(OH)2 powder is placed in a muffle furnace and annealed under air conditions to obtain nickel oxide nanoparticles. In step (1), the concentration of NaOH in the NaOH solution is 0.04-0.1 g / mL, and the concentration of Ni(NO3)2 solution is 0.05-0.1 g / mL; In step (2), the dripping rate is 20-40 drops / min; In step (4), the freeze drying specifically refers to freeze drying at -100℃ for 3 hours, and the annealing condition is 270℃ for 2 hours.
2. Nickel oxide nanoparticles prepared by the preparation method according to claim 1.
3. The application of the nickel oxide nanoparticles according to claim 2 in inverted perovskite solar cells.
4. An inverted perovskite solar cell containing nickel oxide nanoparticles, characterized in that, The inverted perovskite solar cell comprises, from bottom to top, a transparent conductive glass, a hole transport layer, a self-assembled molecular layer, a perovskite light-absorbing layer, an electron transport layer, a hole blocking layer, and a back electrode. The material of the hole transport layer is the nickel oxide nanoparticles as described in claim 2. 5.The inverted perovskite solar cell according to claim 4, characterized in that, The transparent conductive glass is either ITO or FTO. The material of the self-assembled molecular layer is any one or more of ([3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid, [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(9H-9'-phenyl-3,3'-di-carbazole-9-yl)butyl]phosphoric acid, [4-(3,6-di-tert-butyl-9H-carbazole-9-yl)butyl]phosphoric acid, [2-(3,3'-di-carbazole-9-yl)butyl]bisphosphoric acid, and [2-(7H-dibenzo-carbazole-7-yl)ethyl]phosphoric acid; The material of the perovskite light-absorbing layer is ABX3, wherein A is any one or more of CH3NH3 + , CH(NH2)2 + , Cs + , or Rb + , B is any one or more of Pb 2+ , Sn 2+ , or Ge 2+ , and X is any one or more of Cl - , Br - , or I - . The material of the electron transport layer is [6,6]-phenyl C 61 Any one or more of methyl butyrate, fullerene, Sn02, BaSn03, Ti02, or ZnO; The hole-blocking layer is made of dimethyl-4,7-diphenyl-1,10-phenanthroline. The material of the back electrode is any one of Ag, Cu or low-temperature carbon electrode. 6.The inverted perovskite solar cell of claim 4, wherein, The hole transport layer has a thickness of 10-30 nm, the self-assembled molecular layer has a thickness of 1-2 nm, the perovskite light-absorbing layer has a thickness of 500-1000 nm, the electron transport layer has a thickness of 30-100 nm, the hole blocking layer has a thickness of 2-5 nm, and the back electrode has a thickness of 80-200 nm.
7. The method for preparing the inverted perovskite solar cell according to any one of claims 4 to 6, characterized in that, The preparation method includes the following steps: (1) The transparent conductive glass is pretreated with ultraviolet ozone or plasma to obtain a conductive substrate; (2) The nickel oxide nanoparticles described in claim 2 are dispersed in deionized water, and then spin-coated onto the conductive substrate treated in step (1). The hole transport layer can be prepared by annealing. (3) Spin-coating the solution of self-assembled molecules onto the hole transport layer described in step (2), and then annealing to obtain the self-assembled molecular layer; (4) Spin-coat the solution of perovskite precursor material onto the self-assembled molecular layer in step (3). During the spin-coating process, add anti-solvent or directly spin-coat the perovskite wet film in a vacuum chamber and evacuate it. Then anneal it to prepare the perovskite layer. (5) Spin-coat the solution of electron transport layer material onto the perovskite layer described in step (4) to prepare an electron transport layer; (6) The hole blocking layer material is applied to the electron transport layer described in step (5) by spin coating or thermal evaporation to obtain the hole blocking layer; (7) Prepare a back electrode on the hole blocking layer described in step (6).
8. The method for fabricating an inverted perovskite solar cell according to claim 7, characterized in that, In step (1), the conductive glass is treated with ultraviolet ozone or plasma for 5 to 30 minutes; In step (2), the nickel oxide nanoparticles described in claim 2 are dispersed in deionized water at a mass-volume ratio of 5-30:1, mg:mL, and ultrasonically vibrated for 10-30 min. The dispersion is then filtered using PVDF. The filtered nanoparticle dispersion is spin-coated on conductive glass at a speed of 2000-6000 rpm for 10-60 s and annealed at 100-150℃ for 5-30 min to prepare the hole transport layer. In step (3), the material of the self-assembled molecule is dissolved in an organic solvent at a mass-volume ratio of 0.1 to 1:1, mg:mL. The mixture is filtered with PTFE and spin-coated onto the hole transport layer at a speed of 2000 to 6000 rpm for 10 to 60 s. The mixture is then annealed at 60 to 100°C for 5 to 20 min to obtain the self-assembled molecule layer. The organic solvent is any one or more of ethanol, isopropanol, or methanol. In step (4), a solution of perovskite precursor material with a concentration of 1.0 to 1.8 mol / L is dropped onto the self-assembled molecular layer described in step (3), and the perovskite layer is prepared by anti-solvent method or vacuum flash evaporation method. In step (5), the electron transport layer is prepared by solution method or thermal evaporation method.
9. The preparation method according to claim 8, characterized in that, The antisolvent method specifically involves spin coating at 3000–6000 rpm for 20–60 s, adding 80–150 μL of antisolvent dropwise at 10–40 s, and annealing at 100–150 °C for 10–60 min. The vacuum flash evaporation method specifically involves: spin coating at a speed of 2000-3000 rpm for 5-10 s, then spin coating at a speed of 3000-6000 rpm for 20-60 s, placing the perovskite wet film in a vacuum chamber with a vacuum degree of 5-15 Pa for 5-30 s, and annealing at 100-150℃ for 10-60 min; Specifically, the solution method involves spin-coating a solution of electron transport layer material with a concentration of 10–20 mg / mL onto the perovskite layer described in step (4) at a spin speed of 2000–5000 rpm for 20–60 s. The thermal evaporation method specifically involves depositing the electron transport layer material onto the perovskite layer in step (4) at an evaporation rate of 0.1–0.3 Å / s, with a thickness of 10–50 nm.
Citation Information
Patent Citations
Perovskite solar cell and preparation method thereof