Modified spherical lithium iron phosphate with high compaction density as well as preparation method and application of modified spherical lithium iron phosphate

By employing multi-gradient sintering and boron nitride modification processes, a core-shell structure for lithium iron phosphate was constructed, which solved the problems of low compaction density and uneven doping in lithium iron phosphate materials, thereby improving the electrochemical performance and cycle stability of the materials.

CN121426073APending Publication Date: 2026-01-30HUBEI XINGFA CHEM GRP CO LTD

Patent Information

Application Number
CN202511531754.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-24
Publication Date
2026-01-30

AI Technical Summary

Technical Problem

Existing lithium iron phosphate materials have low compaction density, uneven carbon coating affecting material performance, and impurity generation during high-temperature sintering affects purity and cycle stability.

Method used

A multi-gradient sintering process combined with boron nitride synergistic modification was adopted. The core-shell structure was constructed by preparing an iron-based core and building a lithium-phosphorus mixed layer. Modified phenolic resin and boron nitride nanosheets were used for uniform doping to form a continuous carbon layer and lattice doping.

Benefits of technology

A high compaction density (≥2.55 g/cm3) was achieved for lithium iron phosphate, which improved the electrochemical performance and cycle stability of the material, as well as the morphological uniformity and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121426073A_ABST
    Figure CN121426073A_ABST
Patent Text Reader

Abstract

The invention discloses high-compaction-density modified spherical lithium iron phosphate and a preparation method and application thereof.The preparation method comprises the steps that a composite iron source precursor and modified phenolic resin are compounded to form a spherical inner core, and then the spherical inner core is coated with a lithium-phosphorus mixed layer to construct a core-shell structure; the modified spherical lithium iron phosphate with the characteristics of'spherical core-porous shell 'is prepared by introducing boron nitride nanosheets as a structure-directing agent and a doping source and combining a dynamic gradient sintering process, and the modified phenolic resin is obtained by grafting water-soluble phenolic resin and polyethylene glycol, and the solid content of the modified phenolic resin is greater than or equal to 50%. The modified lithium iron phosphate with the compaction density larger than or equal to 2.55 g / cm < 3 > and the capacity retention ratio larger than 92.0% after 1C circulation 2000 times is prepared, and the technical bottlenecks that doping is not uniform, morphology is out of control and the compaction density is low in a traditional process are solved.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The application belongs to the technical field of battery materials, and particularly relates to a modified spherical lithium iron phosphate with high tap density and a preparation method and application thereof. BACKGROUND

[0002] Lithium-ion batteries are a new type of green energy and are widely used in electric vehicles, mobile phones, computers and other fields. Among them, lithium iron phosphate (LiFePO4) is an important positive electrode material. Due to its high safety, low cost, stable structure, long cycle life and other advantages, it has become one of the most potential positive electrode materials in the industry. However, although lithium iron phosphate has many advantages, it still faces some challenges in practical application. First, the tap density of lithium iron phosphate material is relatively low, usually 2.3~2.4g / cm 3 around, which limits its application in power batteries. Second, the traditional preparation method is difficult to simultaneously consider high tap density and good morphology of the material. In addition, the common problems in the prior art also include uneven doping, morphology out of control, and short cycle life at high polarization voltage, etc.

[0003] To solve these problems, researchers have adopted various methods, such as optimizing particle size, surface modification with high-conductivity materials, and ion doping, etc. Among them, carbon coating is a simple and effective method that can improve the conductivity and stability of the material. However, a uniform carbon coating layer usually makes the particle surface smoother or forms a certain steric hindrance, which is not conducive to the close packing of particles, thereby leading to the decrease of tap density and tap density of the material. High tap density is the key to improving the volume energy density of the battery. How to realize high-density compaction while ensuring good conductivity is the key to technological research. The effect of carbon coating is highly dependent on the uniformity, continuity and thickness of the carbon layer, which is affected by factors such as mixing uniformity, pyrolysis temperature and atmosphere control in production, and it is difficult to ensure that the coating quality of each batch and each particle is highly consistent. In addition, during the high-temperature sintering process, the pyrolysis of carbon source not only forms a conductive carbon layer, but also may produce gases (such as H2O, CO, CO2, etc.), which will affect the reducing property of the sintering environment, and may cause Fe 2+ to be oxidized to Fe 3+ , generating magnetic impurities such as Fe2P, which affects the purity and cycle stability of the material. In addition, impurity elements (such as S, N, etc.) in the carbon source may also remain in the material.

[0004] Chinese patent CN120607234A discloses a low-cost, high-density lithium iron phosphate cathode material production method. The method involves adding iron phosphate and a lithium source to a carboxylated carbon nanotube dispersion, stirring, filtering, drying, compacting, and transferring the mixture into a rotary kiln for low-temperature sintering to obtain an inorganic carbon-doped iron phosphate precursor. This precursor is then stirred evenly with a lithium source in a polyvinyl alcohol solution, compacted, and molded to obtain an organic carbon-coated lithium iron phosphate mixture. Finally, this mixture is divided into saggers and fed into a roller furnace for high-temperature sintering and cooling to obtain a low-cost, high-density lithium iron phosphate cathode material. This method improves upon the shortcomings of conventional lithium iron phosphate materials, such as poor morphological consistency and suboptimal electrochemical performance, caused by the limited number of layers and lateral expansion arrangements.

[0005] Chinese patent CN116553507A discloses a high-density lithium iron phosphate material and its precursor densification process. The process involves melting a lithium iron phosphate precursor material to form spherical single crystals, then heating and sintering them. Superheated steam is then introduced, and a carbon-containing gas is introduced while maintaining the temperature, forming a thin carbon coating on the surface. After cooling, the high-density lithium iron phosphate material is obtained. This invention, through vapor-phase deposition of a carbon layer, effectively improves the conductivity, rate capability, and other properties of lithium iron phosphate, enhancing its conductivity and chemical stability.

[0006] However, existing carbon coating methods still have some limitations, such as uneven carbon coating or defects, which affect the overall performance of the material. Therefore, it is of great significance to develop a novel preparation method that can simultaneously improve the compaction density of lithium iron phosphate, improve its morphology, and achieve uniform doping. Summary of the Invention

[0007] To address the aforementioned technical problems, this invention provides a modified spherical lithium iron phosphate with high compaction density, its preparation method, and its application. A multi-gradient sintering process, combined with a boron nitride synergistic modification process, significantly improves the compaction density and electrochemical performance of lithium iron phosphate.

[0008] To achieve the above objectives, the present invention provides a method for preparing modified spherical lithium iron phosphate with high solid density, comprising the following steps: (1) Preparation of iron-based core: The composite iron source and surfactant are mixed, ball-milled, and then modified phenolic resin is added. After ultrasonic treatment, the mixture is dried and sintered to obtain the iron-based core. (2) Preparation of lithium-phosphorus mixed layer: Lithium source, phosphorus source and cellulose nanocrystals are added to water and mixed to obtain lithium-phosphorus mixed layer slurry; (3) Assembly and modification: Lithium-phosphorus mixed layer slurry and boron nitride nanosheets are added to the iron-based core, and the mixture is stirred and dried to obtain the coating material; (4) Sintering: The coating material is sintered in gradient, cooled, discharged and crushed to obtain modified spherical lithium iron phosphate with high compaction density.

[0009] Preferably, the mass ratio of the composite iron source to the surfactant and the modified phenolic resin in step (1) is 1: (0.5-2): (0.08-0.15).

[0010] Further preferably, the composite iron source is a mixture of ferrous sulfate and ferrous oxalate in a molar ratio of 1: (0.2-0.5); the surfactant is a quaternary ammonium salt surfactant; and the modified phenolic resin is prepared by grafting a water-soluble phenolic resin with polyethylene glycol.

[0011] More preferably, the solid content of the modified phenolic resin is ≥50%, and the carbon residue rate is >40%.

[0012] More preferably, the quaternary ammonium salt surfactant is any one of dodecyltrimethylammonium chloride, dodecyl dimethyl benzyl ammonium chloride, and hexadecyl trimethyl ammonium chloride; and the mass ratio of the water-soluble phenolic resin to polyethylene glycol is 10: (1-3).

[0013] Further, the molecular weight of the polyethylene glycol is 400-2000 Da.

[0014] Preferably, the particle size of the material after ball milling in step (1) is D50=1-3 μm.

[0015] Preferably, the drying is performed by pressurized spray drying, and the low-temperature sintering is performed by calcining at 400-500°C for 2-3h in an inert atmosphere.

[0016] Preferably, the amount of the phosphorus source and the lithium source in step (2) is in a molar ratio of P:Li=1: (1.02-1.05); and the amount of the cellulose nanocrystal added is 0.15-0.3wt% of the lithium-phosphorus mixture.

[0017] Further preferably, the phosphorus source is one or more of lithium dihydrogen phosphate, monoammonium phosphate, and phosphoric acid; and the lithium source is one or more of lithium acetate, lithium carbonate, lithium dihydrogen phosphate, and lithium hydroxide.

[0018] Further preferably, the cellulose nanocrystal has an aspect ratio of 20:1 and is purchased from Sigma Reagent.

[0019] Preferably, the molar ratio of the iron-based inner core to the lithium-phosphorus mixed layer slurry in step (3) is Fe: P=1: (0.98-1.02); and the amount of the boron nitride nanosheet is 1-3% of the mass of the iron-based inner core.

[0020] Further preferably, the boron nitride nanosheet has an average particle size of 1.0 μm and a purity of ≥99.9%, and is purchased from Hefei Zhonghang Nanometer.

[0021] Preferably, the drying in step (3) is spray drying with an outlet temperature of 80-100℃.

[0022] Preferably, the gradient sintering in step (4) is five-stage gradient sintering in an inert atmosphere.

[0023] Further preferably, the five-stage gradient sintering is: stage I, heating to 300-400℃ at 5℃ / min and holding for 2h; stage II, heating to 400-550℃ at 3℃ / min and holding for 3h; stage III, heating to 550-700℃ at 5℃ / min and holding for 2-10h; stage IV, heating to 700-750℃ at 10℃ / min and holding for 2-8h; and stage V, slow cooling to below 100℃.

[0024] Further preferably, the inert atmosphere is nitrogen with a flow rate of 100-200mL / min.

[0025] The application also provides a high-density modified spherical lithium iron phosphate prepared by the above preparation method, which has a core-shell structure and a tap density of ≥2.55g / cm 3 .

[0026] The application also provides the use of the product prepared by the above preparation method in a lithium ion battery cathode material.

[0027] The application has the following advantages: 1. The iron source is used as a precursor to form a spherical iron-based core with a modified phenolic resin, and a lithium-phosphorus mixed layer is coated to construct a core-shell structure, and a multi-gradient sintering process is used to achieve high tap density of the material, with a tap density of 2.55g / cm 3 The capacity retention rate can reach 92% after 2000 1C / 1C cycles, thus improving the application performance of the material in power batteries.

[0028] 2. The water-soluble phenolic resin is grafted with polyethylene glycol to obtain a modified phenolic resin, which improves the water solubility and mechanical properties of the phenolic resin, effectively solving the morphology control problem in the preparation process of traditional phenolic resin, and finally obtaining a modified lithium iron phosphate with a regular spherical structure. At the same time, the modified phenolic resin sintering forms a continuous carbon layer (thickness <5nm), and the PEG grafting enhances the flexibility of the carbon layer, avoiding the rupture of spray drying.

[0029] 3. Boron nitride nanosheets are introduced as a two-dimensional structure directing agent and a doping source, and boron nitride is decomposed into B2O3 and active N at high temperature, realizing lattice doping and surface modification at the same time. B / N co-doping improves the lithium ion diffusion coefficient to 10 -13 cm 2The / s level achieves uniform element doping, effectively overcoming the shortcomings of uneven doping in traditional processes and improving the electrochemical performance and consistency of the material. Attached Figure Description

[0030] Figure 1 This is a schematic diagram of the preparation method of the present invention.

[0031] Figure 2 This is a SEM image of the spherical lithium iron phosphate prepared in Example 1.

[0032] Figure 3 This is a SEM image of the spherical lithium iron phosphate prepared in Example 3. Detailed Implementation

[0033] The technical solution of the present invention will be further explained and described below with reference to the accompanying drawings and specific embodiments. It is worth noting that the following embodiments are only preferred embodiments of the present invention and should not be construed as limiting the present invention. The scope of protection of the present invention should be determined by the contents of the claims. Modifications and substitutions made by those skilled in the art to the technical solution of the present invention without creative effort all fall within the scope of protection of the present invention.

[0034] In the following examples, the free phenol content of the water-soluble phenolic resin was <0.1%, and the pH value was 9-12; the cellulose nanocrystals were purchased from Sigma Reagent, with an aspect ratio of 20:1; and the boron nitride nanosheets were purchased from Hefei Zhonghang Nano, with an average particle size of 1.0 μm and a purity of ≥99.9%.

[0035] Example 1 (1) Take ferrous sulfate (FeSO4·7H2O) and ferrous oxalate (FeC2O4·2H2O) at a molar ratio of 1:0.35 to use as a composite iron source; add hexadecyltrimethylammonium chloride containing 1.5wt% to the composite iron source, add pure water to keep the solid content at 48%, and ball mill to D50=2.0μm to obtain ball milled material; (2) Water-soluble phenolic resin and polyethylene glycol (PEG-600) were mixed at a mass ratio of 10:2 and grafted at 80°C. After reacting for 0.5 h, modified phenolic resin was obtained, wherein the solid content of the modified phenolic resin was 52% and the carbon residue rate was 42%. (3) The ball-milled material was mixed with 0.1wt% modified phenolic resin, ultrasonically treated for 30 min, and then spray-dried under pressure (inlet temperature 180℃, outlet temperature 85℃). The dried material was then placed in a nitrogen atmosphere and calcined at 450℃ for 2.5 h to obtain a spherical iron-based core. (4) Lithium dihydrogen phosphate (LiH2PO4) and lithium hydroxide (LiOH) were dissolved in deionized water according to the molar ratio of P:Li = 1:1.03, so that the solid content was kept at 48%, 0.25wt% cellulose nanocrystals were added, and stirring was performed to obtain a lithium-phosphorus mixed layer slurry; (5) The spherical iron-based core was mixed with the lithium-phosphorus mixed layer slurry according to the molar ratio of Fe:P = 1:1.00, 1.5wt% boron nitride nanosheets were added, and after stirring, spray drying (outlet temperature 90℃) was performed to obtain a coating material; (6) The coating material was placed in a tube furnace, nitrogen was introduced, and the flow rate of nitrogen was 150mL / min, and five-stage gradient sintering was performed: Ⅰ 5℃ / min→350℃, 2h; Ⅱ 3℃ / min→500℃, 3h; Ⅲ 5℃ / min→650℃, 4h; Ⅳ 10℃ / min→720℃, 6h; Ⅴ Slow cooling to room temperature; The product was crushed through a 100 mesh sieve to obtain a high compaction density of modified spherical lithium iron phosphate.

[0036] Example 2 Method, step by example 1, the molar ratio of ferrous sulfate (FeSO4·7H2O) and ferrous oxalate (FeC2O4·2H2O) in step (1) is changed to 1:0.2; The amount of boron nitride nanosheets in step (5) is changed to 1.0wt%; The sintering condition of stage IV in step (6) is changed to 700℃ for 8h, and a high compaction density of modified spherical lithium iron phosphate is prepared.

[0037] Example 3 Method, step by example 1, the molar ratio of ferrous sulfate (FeSO4·7H2O) and ferrous oxalate (FeC2O4·2H2O) in step (1) is changed to 1:0.5; The polyethylene glycol (PEG-600) in step (2) is changed to polyethylene glycol (PEG-400); The sintering condition of stage IV in step (6) is changed to 750℃ for 6h, and a high compaction density of modified spherical lithium iron phosphate is prepared.

[0038] Example 4 Method, step by example 1, 1.5wt% hexadecyl trimethyl ammonium chloride in step (1) is replaced by 0.5wt% dodecyl dimethyl benzyl ammonium chloride; The mass ratio of water-soluble phenolic resin to polyethylene glycol in step (2) is changed to 10:1, wherein the polyethylene glycol is PEG1200; Step (4) is changed to ammonium phosphate and lithium acetate in a molar ratio of P:Li=1:1.02, and the amount of cellulose nanocrystals is changed to 0.15wt%; Step (5) is changed to mixing the spherical iron-based inner core and the lithium-phosphorus mixed layer slurry in a molar ratio of Fe:P=1:0.98, and the amount of boron nitride nanosheet is changed to 1wt%; The modified spherical lithium iron phosphate with high compaction density is prepared.

[0039] Example 5 According to the method and steps of Example 1, 1.5wt% of cetyltrimethylammonium chloride in step (1) is replaced by 2.0wt% of cetyltrimethylammonium chloride; The mass ratio of water-soluble phenolic resin to polyethylene glycol in step (2) is changed to 10:3, wherein the polyethylene glycol is PEG2000; Step (4) is changed to phosphoric acid and lithium dihydrogen phosphate in a molar ratio of P:Li=1:1.05, and the amount of cellulose nanocrystals is changed to 0.30wt%; Step (5) is changed to mixing the spherical iron-based inner core and the lithium-phosphorus mixed layer slurry in a molar ratio of Fe:P=1:1.02, and the amount of boron nitride nanosheet is changed to 3wt%; The modified spherical lithium iron phosphate with high compaction density is prepared.

[0040] Comparative Example 1 According to the method and steps of Example 1, no boron nitride nanosheet is used in step (5), and the spherical lithium iron phosphate is prepared.

[0041] Comparative Example 2 According to the method and steps of Example 1, only the amount of boron nitride nanosheet in step (5) is changed to 3.5wt%, and the lithium iron phosphate is prepared.

[0042] Comparative Example 3 According to the method and steps of Example 1, only the modified phenolic resin in step (2) is replaced by water-soluble phenolic resin, and the lithium iron phosphate is prepared.

[0043] Comparative Example 4 According to the method and steps of Example 1, only the amount of modified phenolic resin in step (2) is changed to 0.25wt%, and the lithium iron phosphate is prepared.

[0044] Comparative Example 5 According to the method and steps of Example 1, only the gradient sintering in step (6) is changed to single-stage sintering: 5℃ / min to 700℃, and the lithium iron phosphate is prepared.

[0045] Comparative Example 6 The method, steps are the same as example 1, only in step (4) without using cellulose nanocrystals, lithium iron phosphate is prepared.

[0046] Comparative example 7 (1) Add an aqueous solution containing 1.5wt% hexadecyl trimethyl ammonium chloride to ferrous sulfate (FeSO4·7H2O), add pure water to keep the solid content at 48%, ball mill to D50=2.0μm, then add water-soluble phenolic resin, ultrasonic treatment for 30min, then pressure spray drying (inlet temperature is 180℃, outlet temperature is 85℃), then the dried material is placed in a nitrogen atmosphere, calcined at 450℃ for 2.5h, to obtain a spherical iron-based core; (2) Dissolve lithium dihydrogen phosphate (LiH2PO4) and lithium hydroxide (LiOH) in deionized water according to the molar ratio P:Li=1:1.03 to keep the solid content at 48%, stir to obtain lithium-phosphorus mixed layer slurry; (3) Mix the spherical iron-based core with the lithium-phosphorus mixed layer slurry according to the molar ratio Fe:P=1:1.00, add 1.5wt% boron nitride nanosheet, stir and then spray dry (inlet temperature is 170℃, outlet temperature is 90℃), to obtain a coated material; (4) Place the coated material in a tube furnace, pass nitrogen gas with a flow rate of 150mL / min, heat to 720℃ at a rate of 10℃ / min and keep for 2h, to prepare lithium iron phosphate.

[0047] Example 6 Take the lithium iron phosphate prepared in the above examples and comparative examples, use a compaction density tester to detect the compaction density under 3T@30s, then take the lithium iron phosphate positive electrode material, PVDF, Super-p prepared in the examples and comparative examples according to the ratio of 90:5:5, calculate the N-methyl pyrrolidone with a solid content of 30%, then homogenize, then coat, dry and punch to obtain a circular electrode sheet, finally assemble the circular electrode sheet, a separator and a lithium sheet into a button cell for testing in a glove box; the button cell is tested for charge and discharge in the voltage range of 2.0-4.3 V, and the results are shown in Table 1: Table 1 Performance indicators of lithium iron phosphate

[0048] The results are shown in Table 1: through the design of core-shell structure (iron-based core + lithium-phosphorus coating layer), boron nitride modification and gradient sintering process, the compaction density of the modified lithium iron phosphate prepared in examples 1-5 is ≥2.55 g / cm 3 , and the cycle performance is significantly better.

Claims

1. A method of producing a modified spherical lithium iron phosphate with a high compaction density, characterized by: It comprises the following steps: (1) Iron-based core preparation: after mixing, ball milling the composite iron source and surfactant, adding modified phenolic resin, drying and sintering after ultrasonic treatment, the iron-based core is obtained; (2) Lithium-phosphorus mixed layer preparation: adding lithium source, phosphorus source and cellulose nanocrystals in water, mixing to obtain lithium-phosphorus mixed layer slurry; (3) Assembly and modification: adding lithium-phosphorus mixed layer slurry and boron nitride nanosheet to the iron-based core, stirring and drying to obtain a coated material; (4) Sintering: gradient sintering, cooling, discharging, and crushing the coated material to obtain high-density modified spherical lithium iron phosphate.

2. The process for the preparation of modified spherical lithium iron phosphate with high compacted density according to claim 1, characterized in that: The mass ratio of the composite iron source to the surfactant and the modified phenolic resin in step (1) is 1: (0.5-2): (0.03-0.15).

3. The method for preparing high-density modified spherical lithium iron phosphate according to claim 1, characterized in that: The composite iron source is a mixture of ferrous sulfate and ferrous oxalate in a molar ratio of 1: (0.2-0.5); the surfactant is a quaternary ammonium salt surfactant; and the modified phenolic resin is prepared by grafting polyethylene glycol modification to water-soluble phenolic resin.

4. The method for preparing high-density modified spherical lithium iron phosphate according to claim 3, characterized in that: The quaternary ammonium salt surfactant is any one of dodecyltrimethylammonium chloride, dodecyl dimethyl benzyl ammonium chloride, and hexadecyl trimethyl ammonium chloride; and the mass ratio of the water-soluble phenolic resin to polyethylene glycol is 10: (1-3).

5. The method for preparing high-density modified spherical lithium iron phosphate according to claim 1, characterized in that: The amount of the phosphorus source and lithium source in step (2) is in a molar ratio of P: Li = 1: (1.02-1.05); and the amount of cellulose nanocrystals added is 0.15-0.3wt% of the lithium-phosphorus mixture.

6. The method for preparing high-density modified spherical lithium iron phosphate according to claim 5, characterized in that: The phosphorus source is one or more of lithium dihydrogen phosphate, monoammonium phosphate, and phosphoric acid; and the lithium source is one or more of lithium acetate, lithium carbonate, lithium dihydrogen phosphate, and lithium hydroxide.

7. The method for preparing high-density modified spherical lithium iron phosphate according to claim 1, characterized in that: The molar ratio of the iron-based core to the lithium-phosphorus mixed layer slurry in step (3) is Fe: P = 1: (0.98-1.02); and the amount of boron nitride nanosheet is 1-3% of the mass of the iron-based core.

8. The process for preparing a high tap density modified spherical lithium iron phosphate of claim 1, characterized in that: The gradient sintering in step (4) is five-stage gradient sintering in an inert atmosphere; and the five-stage gradient sintering is stage I: heating to 300-400℃ at 5℃ / min and holding for 2h; stage II: heating to 400-550℃ at 3℃ / min and holding for 3h; stage III: heating to 550-700℃ at 5℃ / min and holding for 2-10h; stage IV: heating to 700-750℃ at 10℃ / min and holding for 2-8h; and stage V: slow cooling to below 100℃.

9. A high-density modified spherical lithium iron phosphate prepared by the method of any one of claims 1-8.

10. The application of the product prepared by the method of any one of claims 1-8 in a lithium ion battery positive electrode material.

Citation Information

Patent Citations

  • High-compaction lithium iron phosphate material and precursor densification treatment process thereof

    CN116553507A

  • Production method of low-cost and high-compaction lithium iron phosphate positive electrode material

    CN120607234A

Cited By

  • High-compaction lithium iron phosphate as well as preparation method and application thereof

    CN121872347A