Negative electrode active material and preparation method thereof, sodium ion battery and electric device

By coating a porous hard carbon material with a hard carbon layer to form a closed-pore structure, the problem of low coulombic efficiency of porous carbon anode materials is solved, thus improving the performance and stability of sodium-ion batteries.

CN121460518APending Publication Date: 2026-02-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411056627.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2026-02-03

AI Technical Summary

Technical Problem

When porous carbon is used as the anode material for sodium-ion batteries, the open pores come into contact with the electrolyte, resulting in low initial coulombic efficiency and reversible capacity.

Method used

By coating the surface of porous hard carbon material with a hard carbon coating layer, the open pores are transformed into a closed pore structure, forming a hard carbon material, including a porous hard carbon core and a hard carbon coating layer. The specific surface area is controlled at 1 m²/g to 10 m²/g, the pore volume is 0.005 cm³/g to 0.023 cm³/g, and the pore size is 1.9 nm to 2.5 nm. The hard carbon material is formed by mixing liquid phenolic resin with porous carbon and performing multi-stage heat preservation treatment.

Benefits of technology

It improves the initial coulombic efficiency and battery capacity of sodium-ion batteries, enhances the storage capacity of sodium ions and the cycle stability of the battery, and reduces electrolyte decomposition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121460518A_ABST
    Figure CN121460518A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, and discloses a negative electrode active material and a preparation method thereof, a sodium ion battery and an electric device. The negative electrode active material comprises a hard carbon material; the hard carbon material comprises a porous hard carbon core and a hard carbon coating layer; the hard carbon coating layer is coated on the surface of the porous hard carbon core; the holes of the hard carbon material comprise closed holes; the specific surface area of the hard carbon material is 1-10m < 2 > / g. According to the application, the hard carbon coating layer is coated on the surface of the porous hard carbon material, open pores of the porous hard carbon are transformed into a closed pore structure, and the closed pore structure is beneficial to sodium ion storage and also enables an electrolyte not to enter and be decomposed easily. The specific surface area of the hard carbon material is within the range of 1-10m < 2 > / g, and the hard carbon material is suitable for the sodium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of batteries, in particular to a negative electrode active material, a preparation method thereof, a sodium ion battery and an electric device. BACKGROUND

[0002] Porous carbon belongs to amorphous carbon, which contains a large number of micropores and mesopores inside, and the specific surface area can reach 500-2000m 2 / g. If it is directly used as a negative electrode material of a sodium ion battery, a large number of open pores will cause a large amount of electrolyte to be decomposed in the discharge process, resulting in extremely low first coulomb efficiency and reversible capacity.

[0003] Therefore, if porous carbon is applied in the negative electrode of a sodium ion battery, it needs to be modified, and the open pores need to be transformed into a closed pore structure that is conducive to sodium ion storage and is not easy to cause a large amount of electrolyte to enter and decompose. SUMMARY

[0004] In view of the above problems, the embodiments of the present application provide a negative electrode active material, a preparation method thereof, a sodium ion battery and an electric device, aiming to solve the problem of low first coulomb efficiency caused by the contact between the open pores of porous carbon and the electrolyte decomposition.

[0005] In a first aspect, the embodiments of the present application provide a negative electrode active material, which comprises a hard carbon material; the hard carbon material comprises a porous hard carbon inner core and a hard carbon coating layer; the hard carbon coating layer is coated on the surface of the porous hard carbon inner core; the pores of the porous hard carbon inner core comprise closed pores; and the specific surface area of the hard carbon material is 1m 2 / g-10m 2 / g.

[0006] The embodiments of the present application transform the open pores of the porous hard carbon material into a closed pore structure by coating a hard carbon coating layer on the surface of the porous hard carbon material, which is conducive to sodium ion storage and also makes the electrolyte not easy to enter and decompose. The specific surface area of the hard carbon material of the embodiments of the present application is in the range of 1m 2 / g-10m 2 / g, which is suitable for a sodium ion battery.

[0007] In some embodiments, the pore volume of the hard carbon material is 0.005cm 3 / g-0.023cm 3 / g. When the pore volume is in the above range, more active sites can be provided for sodium ions, and the electron conduction path is shortened.

[0008] In some embodiments, the average pore size in the hard carbon material is 1.9 nm to 2.5 nm. When the pore size of the hard carbon material is within the above range, it is beneficial to improve the battery capacity and cycle life.

[0009] In some embodiments, the hard carbon material is tested using X-ray diffraction to determine the interplanar spacing d of the hard carbon material. 002 The distance between crystal planes is 0.374 nm to 0.385 nm. 002 Within the aforementioned range, sodium ion diffusion is favorable, resulting in higher energy storage density and higher cycle stability.

[0010] In some embodiments, the Dv50 particle size of the hard carbon material is 5 μm to 10 μm. A Dv50 particle size within this range is beneficial for improving the volumetric energy density of the material.

[0011] Secondly, embodiments of this application provide a method for preparing a negative electrode active material, comprising the following steps: mixing phenolic resin with porous carbon and drying it to obtain a mixture; the phenolic resin includes a liquid thermosetting resin; subjecting the mixture to a pre-heat preservation treatment followed by a carbonization treatment to obtain a hard carbon material; wherein the phenolic resin forms a hard carbon coating layer through carbonization treatment; the porous carbon forms a porous hard carbon core through carbonization treatment; the pre-heat preservation treatment includes multi-stage heat preservation treatment at 100℃~200℃.

[0012] This application uses liquid thermosetting phenolic resin. Compared to solid phenolic resin powder, liquid thermosetting phenolic resin has a lower degree of crosslinking and can be directly cured and crosslinked by heating, offering controllable crosslinking and ease of operation. Furthermore, multi-stage heat preservation treatment at 100℃~200℃ reduces side reactions, ensuring a more complete curing reaction and allowing for full crosslinking and growth on the porous carbon surface.

[0013] In some embodiments, the number-average molecular weight of the phenolic resin is 100 g / mol to 1000 g / mol.

[0014] In some embodiments, the phenolic resin has a linear molecular structure.

[0015] In some embodiments, the multi-stage heat preservation treatment includes: heating at a rate of 1°C / min to 5°C / min to 100°C to 150°C and holding for 1 hour to 3 hours, then heating by 10°C to 30°C and holding for 1 hour to 3 hours until the temperature reaches 190°C to 200°C and is held for 1 hour to 3 hours. By employing the above-mentioned multi-stage heat preservation treatment and controlling the heating rate, the curing reaction at each stage can be made more complete.

[0016] In some embodiments, the multi-stage insulation treatment includes the following five stages: the first stage temperature is 100℃~110℃; the second stage temperature is 110℃~130℃; the third stage temperature is 140℃~160℃; the fourth stage temperature is 170℃~190℃; and the fifth stage temperature is 190℃~200℃. Using the above five-stage insulation treatment allows for a more complete reaction at each stage, thereby generating a network with higher cross-linking properties. This network maintains its structure without deformation during high-temperature carbonization, resulting in a higher residual carbon rate and a denser, more complete carbonized coating layer.

[0017] In some embodiments, the carbonization treatment includes holding at 1100℃ to 1300℃ for 1 hour to 3 hours. Controlling the carbonization temperature within the above range can improve the carbonization effect of the phenolic resin.

[0018] In some embodiments, the mass ratio of the phenolic resin to the porous carbon is from 3:4 to 2:1. Controlling the mass ratio of the phenolic resin to the porous carbon within the above range can improve both the initial efficiency and the specific capacity.

[0019] Thirdly, embodiments of this application provide a sodium-ion battery, including a negative electrode sheet. The negative electrode sheet includes a negative current collector and a negative active material layer disposed on at least one surface of the negative current collector. The negative active material layer includes the negative active material described in the first aspect, or a negative active material obtained by the preparation method of the negative active material described in the second aspect. By employing the above-mentioned negative active material, the initial coulombic efficiency of the sodium-ion battery is improved.

[0020] Fourthly, embodiments of this application provide an electrical device including the aforementioned sodium-ion battery. By employing the aforementioned sodium-ion battery, the operational stability of the electrical device is improved.

[0021] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0022] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the alternative embodiments below. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0023] Figure 1 This is a cross-sectional structural diagram of the electrode sheet in some embodiments of this application;

[0024] Figure 2This is a schematic diagram of the structure of the electrode assembly in some embodiments of this application;

[0025] Figure 3 This is a schematic diagram of the vehicle structure according to some embodiments of this application;

[0026] Figure 4 Transmission electron microscope (TEM) images of the negative electrode active materials of some embodiments of this application;

[0027] Figure 5 Transmission electron microscope (TEM) images of the negative electrode active materials of some embodiments of this application;

[0028] Figure 6 X-ray diffraction patterns of the negative electrode active materials of some embodiments of this application;

[0029] The reference numerals in the detailed embodiments are as follows:

[0030] 10-Electrode; 1-Current collector; 2-Active material layer;

[0031] 20 - Electrode assembly; 101 - Negative electrode; 102 - Positive electrode; 201 - Negative electrode tab; 202 - Positive electrode tab; 203 - Separator;

[0032] 40-battery;

[0033] 50 - Electrical appliance; 501 - Controller; 502 - Motor. Detailed Implementation

[0034] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.

[0036] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0037] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0038] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.

[0039] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).

[0040] In the description of the embodiments of this application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application.

[0041] In the description of the embodiments of this application, unless otherwise expressly specified and limited, the technical terms such as "installation," "connection," "joining," and "fixing" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. For those skilled in the art, the specific meaning of the above terms in the embodiments of this application can be understood according to the specific circumstances.

[0042] In the industry, a closed-cell structure is usually obtained by mixing macromolecular biomass, polymer resin or sugar with activated carbon materials and carbonizing them at high temperature, thereby preventing the large-scale entry and consumption of electrolyte.

[0043] However, during the high-temperature carbonization process, carbohydrates and large-molecule biomass produce a large amount of volatile gases, such as CO, H2, and CO2. This causes them to lose a significant amount of mass and undergo volume deformation compared to their precursors. Consequently, the coating layer covering the activated carbon surface shrinks or expands during carbonization, forming a non-dense coating layer. This prevents complete coverage of the open pores of the activated carbon, leaving a large amount of electrolyte still in contact with and decomposing the electrolyte, resulting in an unsatisfactory initial coulombic efficiency.

[0044] Based on this, embodiments of this application provide a negative electrode active material, including a hard carbon material; the hard carbon material includes a porous hard carbon core and a hard carbon coating layer; the hard carbon coating layer coats the surface of the porous hard carbon core; the pores of the porous hard carbon core include closed pores; the specific surface area of ​​the hard carbon material is 1 m². 2 / g~10m 2 / g.

[0045] This application embodiment transforms the open pores of porous hard carbon material into a closed-pore structure by coating the surface of the material with a hard carbon coating layer. The closed-pore structure facilitates sodium ion storage while also preventing electrolyte ingress and decomposition. The specific surface area of ​​the hard carbon material in this application embodiment is 1 m². 2 / g~10m 2 Within the range of / g, it is suitable for sodium-ion batteries. Specific surface area of ​​a material refers to the surface area per unit mass of an object. Surface area is divided into outer surface area and inner surface area. Ideally, non-porous materials only have an outer surface area, typically with a small specific surface area, while porous or multi-porous materials have a larger inner surface area, thus resulting in a higher specific surface area. Generally, the smaller the particles and the more pores a material has, the larger its specific surface area will be. A larger specific surface area for the negative electrode active material means it can provide more sodium ion migration channels and shorten the sodium ion transport path, thereby improving the battery's kinetic performance. However, if the specific surface area is too large, it also means an increased contact area with the electrolyte, which can exacerbate electrolyte decomposition during the first cycle, leading to a decrease in initial efficiency. Therefore, hard carbon materials with the above-mentioned specific surface area can both improve battery kinetic performance and reduce electrolyte decomposition.

[0046] In some embodiments, the pore volume of the hard carbon material is 0.005 cm³. 3 / g~0.023cm 3 / g. The pore volume of hard carbon materials refers to the total pore volume per unit mass of material, which can be measured by nitrogen adsorption. This method involves condensing liquid nitrogen at low temperatures, allowing the pores of the material to fill with adsorbed nitrogen, and then measuring the amount of nitrogen adsorbed within the pores, thus reflecting the pore size and distribution. The closed-pore structure in hard carbon materials provides storage space for sodium ions. When the pore volume is within the aforementioned range, it provides a more suitable number of active sites for sodium ions, shortens the electron conduction path, and increases the overall capacity.

[0047] In some embodiments, the average pore size of the hard carbon material is 1.9 nm to 2.5 nm. The pores in the negative electrode material provide a conduction path for sodium ions, and the pore size affects the diffusion rate of sodium ions. Smaller pore sizes may restrict the rapid diffusion of sodium ions, thereby hindering charge transfer during charging and discharging, and thus reducing battery capacity. Controlling the pore size of the hard carbon material within the above-mentioned range provides channels for the rapid passage of sodium ions, which is beneficial for improving battery capacity.

[0048] In some embodiments, X-ray diffraction is used to test hard carbon materials, and the interplanar spacing d of the hard carbon materials is... 002 The wavelength ranges from 0.374 nm to 0.385 nm. 002 d represents the interplanar spacing of the (002) peak in the X-ray diffraction pattern of carbon materials. 002 The size of the interplanar spacing determines the width of the channels for sodium ion insertion and extraction in hard carbon materials. A suitable interplanar spacing facilitates the rapid insertion and extraction of sodium ions, thereby improving the material's sodium storage capacity. (Interplanar spacing d) 002 Within the aforementioned range, sodium ion diffusion is favorable, resulting in higher energy storage density and higher cycle stability.

[0049] In some embodiments, the Dv50 particle size of the hard carbon material is 5 μm to 10 μm. Dv50 represents the particle size value corresponding to 50% of the cumulative amount in the material's particle size distribution curve. As an example, the Dv50 particle size can be typical but not limiting values ​​such as 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, and 10 μm. The particle size of the anode material affects the tap density, compaction density, and specific surface area of ​​the material. A Dv50 particle size within the above range is beneficial for improving the volumetric energy density of the material.

[0050] Secondly, embodiments of this application provide a method for preparing a negative electrode active material, comprising the following steps: mixing phenolic resin with porous carbon and drying it to obtain a mixture; the phenolic resin is a liquid thermosetting resin; subjecting the mixture to pre-heat preservation treatment and then carbonization treatment to obtain a hard carbon material; wherein, the phenolic resin forms a hard carbon coating layer through carbonization treatment; the porous carbon forms a porous hard carbon core through carbonization treatment; the pre-heat preservation treatment includes multi-stage heat preservation treatment at 100℃~200℃.

[0051] In this embodiment, phenolic resin is used as the carbon coating precursor. Phenolic resin is a biomass macromolecular material, and its highly cross-linked network allows for further disordered stacking of carbon molecules, resulting in a high residual carbon rate and high sodium storage capacity. The residual carbon rate here refers to the percentage of the weight of the residue remaining after an organic material decomposes at a certain high temperature compared to the original weight. During high-temperature carbonization, phenolic resin undergoes thermal decomposition, generating gaseous and solid residues. A high residual carbon rate indicates that after the phenolic resin decomposes at high temperature, the weight of the residue is a high percentage of the original weight, meaning that most of the phenolic resin did not thermally decompose under high-temperature carbonization conditions and still maintains its original structure. This residual material can form a coating layer on the porous carbon surface. Therefore, if its high cross-linking density is applied to the coating field, the arrangement of the coating layer network can be controlled at the molecular level. Smaller cross-linked networks can effectively prevent electrolyte leakage, thereby achieving dense coating. In this embodiment, a liquid thermosetting phenolic resin is selected. Liquid means having fluidity, which means it can better coat porous carbon. Thermosetting resins are materials that can undergo chemical reactions and cross-linking to cure into high molecular weight polymers under heating conditions. Liquid thermosetting phenolic resins are generally low molecular weight liquids before curing; they undergo chemical reactions and cross-linking during heating. Compared to solid phenolic resin powder, liquid thermosetting phenolic resins do not reach their maximum degree of cross-linking and can be directly cured and cross-linked by heating, offering controllable cross-linking levels and ease of operation. Multi-stage heat treatment further enhances the curing reaction, allowing for thorough cross-linking and growth on porous carbon surfaces.

[0052] In this embodiment, before carbonization, phenolic resin and porous carbon are uniformly mixed using a liquid phase, allowing phenolic resin molecules to uniformly cover the surface of the porous carbon. After a pre-heating treatment, the phenolic resin can slowly and fully cure on the surface of the porous carbon, gradually extending into a three-dimensional network, thereby better covering the surface of the porous carbon and exhibiting a strong "in-situ coating" behavior. Therefore, its cross-linked network can effectively cover the open pores of the porous carbon. Then, carbonization is used to form a porous hard carbon core, and the phenolic resin coating layer is carbonized to form a hard carbon coating layer. The open pores of the porous carbon are transformed into a closed-pore structure through hard carbon coating.

[0053] The curing and crosslinking reaction of phenolic resin mainly involves condensation and dehydration reactions between the phenolic hydroxyl groups, aldehyde groups, and hydrogen functional groups on the benzene ring in the molecular units, forming methylene bonds and ether bonds, thereby achieving the connection between molecular units. During this process, as the condensation reaction occurs, the molecular weight of the molecular units increases, forming a three-dimensional polymer network from linear oligomers. These condensation reactions typically occur gradually between 100℃ and 200℃, and the degree of saturation of the reaction determines the degree of crosslinking. The decomposition temperature of phenolic resin is around 200℃. Therefore, using multi-stage heat preservation treatment when heating to 100℃–200℃ can reduce the generation of side reactions, resulting in better crosslinking between molecules rather than excessive self-decomposition.

[0054] This application employs a multi-stage heat preservation process to ensure that the reaction at each stage is fully realized, preventing excessively rapid heating and reaction kinetics. This prevents the decomposition of many cross-linked bonds before complete heating, and avoids numerous side reactions detrimental to highly cross-linked networks. Consequently, a large amount of molecular components evaporates, resulting in insufficient reserves of key cross-linked chemical bonds and weak cross-linking. A network with sufficiently high cross-linking exhibits stronger thermosetting properties, maintains less structural deformation during high-temperature carbonization, and thus retains higher levels of carbon residue, resulting in a denser and more complete carbonized coating layer.

[0055] After coating porous carbon using the preparation method of this application embodiment, compared with the non-multi-stage heat preservation and curing strategy, the carbon residue rate of the method of this application embodiment is higher under the same amount of phenolic resin used. Furthermore, it has better coating properties than powdered thermoplastic and thermosetting phenolic resins, reducing the open-cell performance of the porous carbon. This improves the initial efficiency of the coating material, i.e., the hard carbon material, and reduces electrolyte consumption during charging and discharging.

[0056] In some embodiments, porous carbon may include activated carbon, ordered mesoporous carbon, nanoporous carbon, etc. Porous carbon is a carbon material with high permeability and controllable pore size, exhibiting high specific capacity and cycle stability. In some embodiments, porous carbon is selected from activated carbon. Activated carbon has good electrical conductivity and abundant pores and pore walls, providing more reaction sites for sodium-ion batteries.

[0057] In some embodiments, the porous carbon selected has a specific surface area of ​​500 m². 2 / g~1000m 2 / g, as an example, the specific surface area can be 500m². 2 / g、550m 2 / g、600m 2 / g、650m 2 / g、700m 2 / g、750m 2 / g、800m 2 / g、850m 2 / g、900m 2 / g、950m 2 / g, 1000m 2 Typical but not limiting values ​​such as / g. Porous carbon with the above-mentioned specific surface area is selected, exhibiting more suitable electrochemical activity for sodium-ion batteries.

[0058] In some embodiments, the porous carbon selected is predominantly micropores. Porous carbon pores can be categorized into micropores, mesopores, and macropores based on size. Micropores have a diameter less than 2 nm, mesopores range from 2 nm to 50 nm, and macropores have a diameter greater than 50 nm. Selecting porous carbon with predominantly micropores is more beneficial for the sodium storage performance of hard carbon anode materials.

[0059] In some embodiments, the selected porous carbon has a Dv50 particle size of 5 μm to 10 μm.

[0060] In some embodiments, the number-average molecular weight of the phenolic resin is 100 g / mol to 1000 g / mol. As examples, typical but non-limiting values ​​for the number-average molecular weight include 100 g / mol, 200 g / mol, 300 g / mol, 400 g / mol, 500 g / mol, 600 g / mol, 700 g / mol, 800 g / mol, 900 g / mol, and 1000 g / mol. Phenolic resins with a number-average molecular weight between 100 g / mol and 1000 g / mol belong to first-order resins, whose molecular units are mainly linear small-molecule polymers. These resins can undergo a series of curing reactions by heating, specifically within a heating range of 100°C to 200°C, ultimately forming an insoluble and infusible three-dimensional cross-linked network framework. This framework, acting as a coating layer, does not deform during heating above 200°C, better preventing the shrinkage of the originally covering surface coating layer due to volume deformation during carbonization, thus exposing porous carbon pores.

[0061] In some embodiments, the phenolic resin has a linear molecular structure. Phenolic resins with a linear molecular structure have a more regular structure, better performance, and lower molecular weight, and can undergo in-situ crosslinking and curing reactions by heating between 100°C and 200°C.

[0062] In some embodiments, the phenolic resin may be selected from a liquid viscous thermosetting resin obtained by reacting phenol with formaldehyde under alkaline medium and formaldehyde excess conditions. By customizing or synthesizing liquid thermosetting phenolic resins with smaller molecular weights, their in-situ crosslinking properties can be stronger and their controllability can be enhanced.

[0063] In some embodiments, the method for preparing a mixture by mixing and drying phenolic resin and porous carbon can be achieved by dissolving the phenolic resin in a solvent using a liquid-phase method to form a phenolic resin solution. Examples of solvents include ethanol, acetone, and glycerol polyols. The porous carbon is then dispersed in the phenolic resin solution, stirred until homogeneous, and dried to obtain a porous carbon-phenolic resin mixture. Drying can be performed using methods commonly used in the art, such as natural air drying, oven drying, or heat drying, which will not be elaborated upon here.

[0064] In some embodiments, the step of pre-insulating and then carbonizing a porous carbon-phenolic resin mixture to obtain a hard carbon material specifically includes the following: placing the porous carbon-phenolic resin mixture in a reactor and heating it to a high temperature, causing the phenolic resin to partially or completely pyrolyze into carbonaceous material. Examples of reactors include tubular furnaces. During the carbonization process, as the temperature rises, the phenolic resin is decomposed into low-molecular-weight compounds. This reaction generates a large amount of gas and volatile substances. By introducing an inert gas, oxygen and impurities in the air can be isolated, protecting the coating layer from oxidation and contamination. Examples of inert gases include nitrogen, argon, and helium.

[0065] In some embodiments, the multi-stage heat preservation process in the pre-heat preservation step, where the temperature is raised to 100℃~200℃, includes the following steps: raising the temperature at 1℃ / min~5℃ / min to 100℃~150℃ and holding for 1h~3h, then raising the temperature by 10℃~30℃ and holding for 1h~3h, until the temperature reaches 190℃~200℃ and is held for 1h~3h. This refers to a multi-stage heat preservation strategy based on the curing principle of liquid thermosetting phenolic resin, considering its curing reaction at different temperature stages. By setting multiple heat preservation stages at 100℃~200℃, each lasting 1h~3h, the resin is fully cured. As an example, the temperature can be maintained at 100℃, 150℃, 180℃, and 200℃ for 1 to 3 hours each; or at 100℃, 120℃, 150℃, 180℃, and 200℃ for 1 to 3 hours each; or at 120℃, 140℃, 160℃, 180℃, and 200℃ for 1 to 3 hours each; or at 150℃, 180℃, and 200℃ for 1 to 3 hours each. Simultaneously, the heating rate should be controlled to be a slow increase of 1℃ / min to 5℃ / min. As an example, typical but non-limiting values ​​for the heating rate include 1℃ / min, 2℃ / min, 3℃ / min, 4℃ / min, and 5℃ / min. By employing the aforementioned multi-stage heat preservation treatment and controlling the heating rate, the curing reaction at each stage can be made more complete, preventing excessively rapid heating that could lead to overly vigorous reactions or a rapid reaction rate that would cause the reaction to proceed too quickly to the next stage, thus hindering the formation of a uniform, high-density cross-linked network. Furthermore, this slow heating and multi-stage heat preservation strategy, under conditions of more complete reaction, prevents the generation of a large number of side reactions, reducing the formation of free low-polymer compounds and preventing them from escaping as volatiles during carbonization. This further improves the carbon residue rate, which means less skeleton deformation and less shrinkage of the coating layer during carbonization.

[0066] In one specific embodiment, the multi-stage heat preservation process is as follows: the temperature is increased to 150°C at a heating rate of 2°C / min and held for 2 hours; then the temperature is increased to 180°C at a heating rate of 2°C / min and held for 2 hours; then the temperature is increased to 200°C at a heating rate of 2°C / min and held for 2 hours; then the temperature is increased to the carbonization temperature at a heating rate of 5°C / min and held for 2 hours.

[0067] In some embodiments, the multi-stage heat preservation treatment includes the following five stages: the first stage temperature is 100℃~110℃; the second stage temperature is 110℃~130℃; the third stage temperature is 140℃~160℃; the fourth stage temperature is 170℃~190℃; and the fifth stage temperature is 190℃~200℃. Using the above five-stage heat preservation treatment allows for a more complete reaction at each stage, preventing the decomposition of many cross-linked bonds before complete heating due to excessively rapid heating and reaction kinetics. This also avoids side reactions that are detrimental to the formation of highly cross-linked networks, leading to the volatilization of molecular components, insufficient retention of key cross-linked chemical bonds, and weak cross-linking. A network with sufficiently high cross-linking properties exhibits stronger thermosetting properties, maintains its structural integrity during high-temperature carbonization, and thus has higher residual carbon, resulting in a denser and more complete carbonized coating layer.

[0068] In some embodiments, a hard carbon material is prepared by pre-heating a porous carbon-phenolic resin mixture followed by carbonization. This carbonization process includes holding at 1000°C to 1300°C for 1 to 3 hours. Specifically, this refers to a multi-stage heat treatment at 100°C to 200°C, followed by further heating to 1000°C to 1300°C and holding for 1 to 3 hours to carbonize the phenolic resin. It is generally believed that phenolic resin begins to carbonize above 300°C; however, in the embodiments of this application, carbonization of the phenolic resin is more effective between 1000°C and 1300°C.

[0069] In some embodiments, during the preparation of hard carbon materials, the mass ratio of phenolic resin to porous carbon is 1:2 to 2:1. Examples of such ratios include 1:2, 1.5:2, 1:1, 2:1.5, and 2:1. If the mass ratio of phenolic resin to porous carbon is too small, it means the carbon coating percentage is too low, potentially resulting in a thin coating layer or insufficient coating to cover the pores of the porous carbon. Therefore, even with good curing, the specific capacity and initial efficiency of the coated material cannot be maximized. Conversely, if the mass ratio is too high, it means the carbon coating percentage is too high. During carbonization, the volatile components occupy too much of the available pore volume of the activated carbon, resulting in unsatisfactory sodium storage capacity and initial efficiency. Controlling the mass ratio of phenolic resin to porous carbon within the above range allows for better performance in both initial efficiency and specific capacity.

[0070] Thirdly, embodiments of this application provide a sodium-ion battery, including a negative electrode sheet. The negative electrode sheet includes a negative current collector and a negative active material layer disposed on at least one side surface of the negative current collector. The negative active material layer includes the aforementioned negative active material. By employing the aforementioned negative active material, the initial coulombic efficiency of the sodium-ion battery is improved.

[0071] The components of a sodium-ion battery are described in detail below.

[0072] Please refer to Figure 1 , Figure 1 This is a schematic diagram of the structure of the electrode 10 in some embodiments of this application. The electrode 10 includes a current collector 1 and an active material layer 2, the active material layer 2 being disposed on at least one side of the current collector 1.

[0073] Current collector 1 refers to the component used to collect current. Depending on the application, current collector 1 can be either a negative electrode current collector or a positive electrode current collector. When current collector 1 is a negative electrode current collector, the corresponding active material layer 2 coated on the negative electrode current collector is a negative electrode active material layer, and the resulting electrode 10 is a negative electrode electrode. When current collector 1 is a positive electrode current collector, the corresponding active material layer 2 coated on the positive electrode current collector is a positive electrode active material layer, and the resulting electrode 10 is a positive electrode electrode. Taking a sodium-ion battery as an example, optionally, the negative electrode current collector is copper foil, and the positive electrode current collector is aluminum foil. Furthermore, current collector 1 can have various shapes, such as strips or squares, and is not limited here.

[0074] The active material layer 2 includes active materials, conductive agents, and binders. Active materials refer to materials that participate in electrochemical oxidation / reduction reactions. Optionally, the active material is a powder. When active material layer 2 is a negative electrode material layer, the active material is a negative electrode active material. When active material layer 2 is a positive electrode material layer, the active material is a positive electrode active material. Taking a sodium-ion battery as an example, the negative electrode material can be artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, sodium metal negative electrodes, etc.; the positive electrode material can be, but is not limited to, transition metal oxides, polyanionic compounds, Prussian blue analogs, etc. The conductive agent refers to the material that collects microcurrents between active materials and between the active material and current collector 1. The conductive agent can be, but is not limited to, conductive graphite, carbon nanotubes, acetylene black, etc. The binder is the material that binds the active materials together to enhance the electronic contact between the active material and the conductive agent, and between the active material and current collector 1. The binder may be, but is not limited to, styrene-butadiene rubber (SBR), acrylonitrile, acrylate, polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), etc.

[0075] The current collector 1 has a first surface and a second surface opposite to each other along the thickness direction of the current collector 1. At least one side of the current collector 1 includes the first surface and / or the second surface of the current collector 1. It is understood that the active material layer 2 may be disposed on the first surface, or on the second surface, or the active material layer 2 may be disposed on both the first surface and the second surface.

[0076] Please refer to Figure 2 , Figure 2This is a schematic diagram of the structure of the electrode assembly 20 in some embodiments of this application. The electrode assembly 20 is the component in the battery where the electrochemical reaction occurs. The electrode assembly 20 is mainly formed by winding or stacking an electrode structure that integrates a negative electrode 101 and a positive electrode 102. A separator 203 is usually provided between adjacent negative electrode 101 and positive electrode 102. The negative current collector is connected to a negative electrode tab 201, and the positive current collector is connected to a positive electrode tab 202.

[0077] [Negative electrode plate]

[0078] The negative electrode 101 includes a negative electrode current collector and a negative electrode material layer, the negative electrode material layer being coated on the surface of the negative electrode current collector. Taking a sodium-ion battery as an example, the material of the negative electrode current collector can be copper. The negative electrode can include a sodium metal negative electrode, a carbon material negative electrode, and other non-carbon material negative electrodes.

[0079] In some embodiments, the negative electrode active material may further include at least one of artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, and tin-based materials.

[0080] In some embodiments, the negative electrode active material may also include a binder. Examples of binders include styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, carboxymethyl chitosan, etc.

[0081] In some embodiments, the negative electrode active material further includes a conductive agent. Examples of conductive agents include superconducting carbon, acetylene black, carbon black, Ketjen black, carbon nanotubes, graphene, etc.

[0082] In some embodiments, the negative electrode sheet of a sodium-ion battery can be prepared by dispersing the above-mentioned components for preparing the negative electrode sheet, such as negative electrode active material, conductive agent, binder and any other components, in a solvent to form a negative electrode slurry, coating the negative electrode slurry onto a negative electrode current collector, and obtaining the negative electrode sheet after drying, cold pressing and other processes.

[0083]

Positive Electrode

[0084] The positive electrode 102 includes a positive current collector and a positive active material layer, with the positive active material layer coated on the surface of the positive current collector. Taking a sodium-ion battery as an example, the material of the positive current collector can be aluminum, and the positive material layer includes the positive electrode material, which can be sodium vanadium phosphate, sodium iron pyrophosphate, etc.

[0085] In some embodiments, the positive electrode sheet of a sodium-ion battery can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as positive active material, conductive agent, binder and any other components, in a solvent to form a positive electrode slurry, coating the positive electrode slurry onto a positive current collector, and obtaining the positive electrode sheet after drying, cold pressing and other processes.

[0086]

Isolation Film

[0087] The separator 203 is a porous plastic film that allows sodium ions in the electrolyte to pass through freely, but isolates the negative electrode 101 and the positive electrode 102, preventing electrons inside the battery from passing through freely. The separator 203 can be made of materials such as PP (polypropylene) or PE (polyethylene).

[0088] Fourthly, embodiments of this application provide an electrical device including the aforementioned sodium-ion battery.

[0089] The sodium-ion batteries disclosed in some embodiments of this application can be used, but are not limited to, in electrical devices such as vehicles, ships, or aircraft. A power system comprising such an electrical device can be used, incorporating batteries disclosed in this application.

[0090] Electrical devices can include, but are not limited to, vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys, and power tools. Vehicles can include, but are not limited to, gasoline-powered cars, natural gas-powered cars, or new energy vehicles. New energy vehicles can include, but are not limited to, pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles. Spacecraft include airplanes, rockets, space shuttles, and spacecraft. Electric toys include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys. Power tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers.

[0091] For ease of explanation, the following embodiments will be described using a vehicle 50 as an example of an electrical device according to an embodiment of this application.

[0092] Please refer to Figure 3 , Figure 3This is a schematic diagram of the structure of a vehicle 50 provided in some embodiments of this application. A battery 40 is disposed inside the vehicle 50, and the battery 40 may be located at the bottom, front, or rear of the vehicle 50. The battery 40 can be used to power the vehicle 50; for example, the battery 40 can serve as the operating power source for the vehicle 50. The vehicle 50 may also include a controller 501 and a motor 502. The controller 501 is used to control the battery 40 to supply power to the motor 502, for example, to meet the power needs of the vehicle 50 during starting, navigation, and driving.

[0093] In some embodiments of this application, the battery 40 can not only serve as the operating power source for the vehicle 50, but also as the driving power source for the vehicle 50, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 50.

[0094] In some embodiments of this application, battery 40 may include one or more battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple battery cells connected in series, parallel, or mixed configurations via a busbar.

[0095] A single battery cell can be a rechargeable battery. A rechargeable battery is a battery cell that can be recharged after it has been discharged, allowing the active materials to be activated and the cell to continue to be used.

[0096] The battery cells can be lithium-ion batteries, sodium-ion batteries, sodium-lithium-ion batteries, lithium metal batteries, sodium metal batteries, lithium-sulfur batteries, magnesium-ion batteries, nickel-metal hydride batteries, nickel-cadmium batteries, lead-acid batteries, etc.

[0097] The following description is based on specific embodiments.

[0098] The embodiments and comparative examples of this application employ four different pre-heat preservation and then carbonization processes, as detailed below:

[0099] Method 1: Increase the temperature to 1200℃ at a rate of 5℃ / min and hold for 2 hours.

[0100] Method 2: Increase the temperature to 200℃ at 2℃ / min, hold for 2 hours, then increase the temperature to 1200℃ at 5℃ / min, and hold for 2 hours.

[0101] The third method: Increase the temperature to 150℃ at 2℃ / min and hold for 2 hours; then increase the temperature to 180℃ at 2℃ / min and hold for 2 hours; then increase the temperature to 200℃ at 2℃ / min and hold for 2 hours; finally increase the temperature to 1200℃ at 5℃ / min and hold for 2 hours.

[0102] Method 4: Increase the temperature to 100℃ at 2℃ / min and hold for 2 hours; then increase the temperature to 120℃ at 2℃ / min and hold for 2 hours; increase the temperature to 150℃ at 2℃ / min and hold for 2 hours; then increase the temperature to 180℃ at 2℃ / min and hold for 2 hours; then increase the temperature to 200℃ at 2℃ / min and hold for 2 hours; finally, increase the temperature to 1200℃ at 5℃ / min and hold for 2 hours.

[0103] Example 1:

[0104] (1) Preparation of hard carbon materials

[0105] Porous carbon: Selected with a specific surface area of ​​900 m² 2 / g of activated carbon, with pores mainly composed of micropores, was broken down to a Dv50 of 7±0.5μm.

[0106] Phenolic resin: Liquid thermosetting phenolic resin was selected and purchased from Maclean's Reagents.

[0107] Phenolic resin and activated carbon were added to an ethanol solution at a mass ratio of 1:1 and stirred until homogeneous for 3 hours. The mixture was then dried to obtain a final product. The mixture was placed in a tube furnace, and nitrogen gas was introduced for a third heating and carbonization process: the temperature was increased to 150℃ at 2℃ / min and held for 2 hours; then increased to 180℃ at 2℃ / min and held for 2 hours; then increased to 200℃ at 2℃ / min and held for 2 hours; finally, the temperature was increased to 1200℃ at 5℃ / min and held for 2 hours. After carbonization, a product with a specific surface area of ​​9 m² was obtained. 2 / g of hard carbon material.

[0108] (2) Assembly of button cells

[0109] The prepared hard carbon material was mixed with styrene-butadiene rubber (SBR) as a binder, sodium carboxymethyl cellulose (CMC-Na) as a thickener, and carbon black as a conductive agent in a mass ratio of 96.2:1.8:1.2:0.8 in an appropriate amount of deionized water to form a uniform negative electrode slurry. The negative electrode slurry was uniformly coated onto the surface of the copper foil current collector and dried in an oven for later use. Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain an organic solvent. NaPF6 was then dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L. A CR2430 coin cell was then assembled in an argon-protected glove box using a sodium metal sheet as the counter electrode and a polyethylene (PE) film as the separator.

[0110] Example 2

[0111] The difference between this embodiment and Embodiment 1 is that the hard carbon material is prepared using the fourth heating carbonization procedure: heating to 100°C at 2°C / min and holding for 2 hours; then heating to 120°C at 2°C / min and holding for 2 hours; then heating to 150°C at 2°C / min and holding for 2 hours; then heating to 180°C at 2°C / min and holding for 2 hours; then heating to 200°C at 2°C / min and holding for 2 hours; finally heating to 1200°C at 5°C / min and holding for 2 hours. After carbonization, a specific surface area of ​​6 m² is obtained. 2 / g of hard carbon material.

[0112] Example 3

[0113] The difference between this embodiment and Embodiment 1 is that the mass ratio of phenolic resin to activated carbon in the preparation of the hard carbon material is 2:1. After carbonization using the third heating carbonization procedure, a specific surface area of ​​9 m² is obtained. 2 / g of hard carbon material.

[0114] Example 4

[0115] The difference between this embodiment and Embodiment 1 is that in the preparation of the hard carbon material, the mass ratio of phenolic resin to activated carbon is 2:1, and the carbonization process is carried out using the fourth heating carbonization procedure. After carbonization, a specific surface area of ​​5 m² is obtained. 2 / g of hard carbon material.

[0116] Example 5

[0117] The difference between this embodiment and Embodiment 1 is that: in the preparation of the hard carbon material, the mass ratio of phenolic resin to activated carbon is 3:4, and the carbonization process is carried out using the third heating carbonization procedure.

[0118] Example 6

[0119] The difference between this embodiment and Embodiment 1 is that: in the preparation of the hard carbon material, the mass ratio of phenolic resin to activated carbon is 3:4, and the carbonization process is carried out using the fourth heating carbonization procedure.

[0120] Comparative Example 1

[0121] The difference between this comparative example and Example 1 is that the hard carbon material was prepared using the first heating carbonization procedure: heating to 1200°C at a rate of 5°C / min and holding at that temperature for 2 hours. After carbonization, a specific surface area of ​​37 m² was obtained. 2 / g of hard carbon material.

[0122] Comparative Example 2

[0123] The difference between this comparative example and Example 1 is that the hard carbon material was prepared using a second heating carbonization procedure: heating to 200°C at 2°C / min and holding for 2 hours, then heating to 1200°C at 5°C / min and holding for 2 hours. After carbonization, a specific surface area of ​​13 m² was obtained. 2 / g of hard carbon material.

[0124] Comparative Example 3

[0125] The difference between this comparative example and Example 1 is that the mass ratio of phenolic resin to activated carbon in the preparation of the hard carbon material is 2:1, and the carbonization process is carried out using the first heating carbonization procedure. After carbonization, a specific surface area of ​​21 m² is obtained. 2 / g of hard carbon material.

[0126] Comparative Example 4

[0127] The difference between this comparative example and Example 1 is that the mass ratio of phenolic resin to activated carbon in the preparation of the hard carbon material is 2:1, and the second heating carbonization procedure is used for carbonization. After carbonization, a specific surface area of ​​15 m² is obtained. 2 / g of hard carbon material.

[0128] Comparative Example 5

[0129] The difference between this comparative example and Example 1 is that the mass ratio of phenolic resin to activated carbon in the preparation of the hard carbon material is 1:2, and the carbonization process is carried out using the third heating carbonization procedure. After carbonization, a specific surface area of ​​55 m² is obtained. 2 / g of hard carbon material.

[0130] Comparative Example 6

[0131] The difference between this comparative example and Example 1 is that the mass ratio of phenolic resin to activated carbon in the preparation of the hard carbon material is 1:2, and the carbonization process is carried out using the sixth heating carbonization procedure. After carbonization, a specific surface area of ​​47 m² is obtained. 2 / g of hard carbon material.

[0132] Performance testing

[0133] To verify the progressiveness of the embodiments of this application, the performance of the hard carbon materials and sodium-ion batteries prepared in Examples 1 to 6 and Comparative Examples 1 to 6 were tested using the following characterization methods:

[0134] (1) Determination of the degree of curing and crosslinking of phenolic resin

[0135] Weigh 10g of thermosetting phenolic resin and heat it to 1200℃ using the four heating carbonization programs mentioned above. Then weigh the product mass and divide 10g from this mass to obtain the residual carbon rate of the phenolic resin. The degree of cross-linking and curing is judged by the size of the residual carbon rate.

[0136] (2) Analysis and testing of specific surface area, pore volume and pore size distribution

[0137] Nitrogen adsorption-desorption was used to characterize the specific surface area of ​​the coated material. The coating effect was verified by the change in specific surface area before and after coating. The pore volume and pore size distribution of the hard carbon material were determined by nitrogen adsorption.

[0138] Specific test method: Refer to GB / T 19587-2017, use the nitrogen adsorption specific surface area analysis test method, and calculate it using the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis and pore volume can be determined by the ASAP 3020 surface area and pore size analyzer of Micromeritics, USA.

[0139] The size and distribution of the apertures can be observed using a transmission electron microscope.

[0140] (4) Measurement of interplanar spacing d002

[0141] The interplanar spacing d002 was measured using an X-ray diffractometer (XRD).

[0142] (5) Laser particle size analysis test

[0143] The volumetric particle size distribution (Dv50) of hard carbon materials is a well-known concept in the art, representing the particle size corresponding to a cumulative volumetric distribution percentage of 50%. It can be determined using instruments and methods known in the art. For example, it can be conveniently determined using a laser particle size analyzer, referring to GB / T 19077-2016, Particle Size Distribution Laser Diffraction Method. The testing instrument can be the Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd., UK.

[0144] (6) Battery (materials or electrodes) performance testing

[0145] At 25°C, the coin cells prepared in each example and comparative example were first discharged to 0V at a constant current density of 10mA / g, and the first discharge capacity of the coin cells was recorded; then, they were charged to 2.0V at a constant current density of 10mA / g, and the first charge capacity of the coin cells was recorded.

[0146] The reversible specific capacity (mAh / g) of hard carbon material = the first charge capacity of a coin cell / the mass of the carbon material.

[0147] The initial coulombic efficiency (%) of hard carbon materials = the first charge capacity of the coin cell / the first discharge capacity of the coin cell × 100%.

[0148] Table 1

[0149]

[0150] Table 2

[0151]

[0152] Table 3

[0153]

[0154] Figure 4 and Figure 5 The following are transmission electron microscope (TEM) images of the negative electrode active material of some embodiments of this application. As shown in the figure, the material has a typical disordered turbine-like framework morphology, which is a characteristic morphology of hard carbon. Figure 6 The X-ray diffraction pattern of the negative electrode active material in some embodiments of the application shows a broad peak shape, indicating that the material has a disordered hard carbon structure.

[0155] Table 1 shows the residual carbon rate of the liquid thermosetting phenolic resin of this application under four different pre-insulation treatment followed by carbonization treatment procedures. As can be seen from Table 1, by adopting a multi-stage insulation process, the residual carbon rate of the phenolic resin after carbonization is improved. Moreover, as the number of temperature stages increases during the insulation process, the residual carbon rate is higher, indicating a better degree of crosslinking.

[0156] Table 2 shows the performance data of the materials in Examples 1 to 6 of this application, and Table 3 shows the performance data of the materials in Comparative Examples 1 to 6 of this application. As can be seen from Tables 2 and 3, the performance of Examples 1 and 2 is superior to that of Comparative Examples 1 and 2, and the performance of Examples 3 and 4 is superior to that of Comparative Examples 3 and 4. This indicates that regardless of the coating mass ratio, the reversible specific capacity and first-efficiency value of the hard carbon material under a more complete and extensive carbonization process are better than those under a process with fewer insulation stages. The data confirms that increasing the curing and crosslinking degree of phenolic resin can effectively increase the coating degree of phenolic resin-coated activated carbon, thereby enhancing its sodium storage capacity as a sodium-ion battery anode material.

[0157] Regarding the coating ratio, if the coating ratio is too small, such as in Comparative Examples 5 and 6, where the mass ratio of phenolic resin to activated carbon is 1:2, the coating layer may be too thin or insufficient to cover the open pores of the activated carbon. Therefore, even if a good degree of curing is achieved, the specific capacity and initial efficiency of the coating material cannot reach a high level. However, if the coating ratio is too high, the content of phenolic resin will be too high. During the carbonization process, the volatile components will occupy too much of the available pore volume of the activated carbon, resulting in an unsatisfactory sodium storage capacity and initial efficiency, even though the surface area data shows that it can completely cover most of the open pores of the activated carbon. Under a good phenolic resin coating ratio, such as 3:4 to 2:1, the carbonized coated carbon can cover the open pores of the activated carbon well with minimal damage to the pore volume, and both the initial efficiency and specific capacity can be well achieved.

[0158] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and not to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. These modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application, and they should all be covered within the scope of the claims and specification of this application. In particular, as long as there is no structural conflict, the various technical features mentioned in the embodiments can be combined in any way. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A negative electrode active material, characterized in that, The negative electrode active material includes hard carbon material; the hard carbon material includes a porous hard carbon core and a hard carbon coating layer; the hard carbon coating layer coats the surface of the porous hard carbon core; the pores of the porous hard carbon core include closed pores; the specific surface area of ​​the hard carbon material is 1 m². 2 / g~10m 2 / g.

2. The negative electrode active material according to claim 1, characterized in that, The pore volume of the hard carbon material is 0.005 cm³. 3 / g~0.023cm 3 / g.

3. The negative electrode active material according to claim 1 or 2, characterized in that, The average pore size in the hard carbon material is 1.9 nm to 2.5 nm.

4. The negative electrode active material according to any one of claims 1 to 3, characterized in that, The hard carbon material was tested using X-ray diffraction, and the interplanar spacing d of the hard carbon material was determined. 002 The wavelength ranges from 0.374nm to 0.385nm.

5. The negative electrode active material according to any one of claims 1 to 4, characterized in that, The Dv50 particle size of the hard carbon material is 5μm to 10μm.

6. A method for preparing a negative electrode active material, characterized in that, Includes the following steps: A mixture is obtained by mixing and drying phenolic resin with porous carbon; the phenolic resin includes liquid thermosetting resin. The mixture is subjected to pre-insulation treatment and then carbonization treatment to obtain hard carbon material; wherein, the phenolic resin forms a hard carbon coating layer through carbonization treatment; the porous carbon forms a porous hard carbon core through carbonization treatment; the pre-insulation treatment includes multi-stage insulation treatment at 100℃~200℃.

7. The method for preparing the negative electrode active material according to claim 6, characterized in that, The number-average molecular weight of the phenolic resin is 100 g / mol to 1000 g / mol; and / or, The phenolic resin has a linear molecular structure.

8. The method for preparing the negative electrode active material according to claim 6 or 7, characterized in that, The multi-stage heat preservation process includes: increasing the temperature at 1℃ / min to 5℃ / min to 100℃ to 150℃ and holding for 1h to 3h, then increasing the temperature by 10℃ to 30℃ and holding for 1h to 3h, until the temperature reaches 190℃ to 200℃ and is held for 1h to 3h.

9. The method for preparing the negative electrode active material according to any one of claims 6 to 8, characterized in that, The multi-stage insulation treatment includes the following five stages: the first stage temperature is 100℃~110℃; the second stage temperature is 110℃~130℃; the third stage temperature is 140℃~160℃; the fourth stage temperature is 170℃~190℃; and the fifth stage temperature is 190℃~200℃.

10. The method for preparing the negative electrode active material according to any one of claims 6 to 9, characterized in that, The carbonization process includes holding at 1100℃~1300℃ for 1h~3h.

11. The method for preparing the negative electrode active material according to any one of claims 6 to 10, characterized in that, The mass ratio of the phenolic resin to the porous carbon is 3:4 to 2:

1.

12. A sodium-ion battery, characterized in that, The negative electrode includes a negative electrode sheet, the negative electrode sheet comprising a negative electrode current collector and a negative electrode active material layer disposed on at least one side surface of the negative electrode current collector, the negative electrode active material layer comprising the negative electrode active material as described in any one of claims 1 to 5, or the negative electrode active material obtained by the preparation method of the negative electrode active material as described in any one of claims 6 to 11.

13. An electrical appliance, characterized in that, Including the sodium-ion battery of claim 12.

Citation Information

Cited By

  • Composite hard carbon negative electrode material, preparation method thereof and sodium ion battery

    CN121726397A