Multilayer thermal insulation composite material containing solid waste base and preparation method of multilayer thermal insulation composite material
By using a multi-layer composite material structure and a low-temperature curing process, the problems of low solid waste utilization and insufficient material performance in existing technologies have been solved, realizing the preparation of efficient and low-cost thermal insulation composite materials with excellent thermal insulation, fireproof, waterproof and mechanical properties.
Patent Information
- Application Number
- CN202512058298.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-31
- Publication Date
- 2026-02-06
AI Technical Summary
Existing technologies make it difficult to develop a composite material that can efficiently dispose of solid waste, while also possessing excellent thermal insulation, fire resistance, waterproofing, and mechanical properties, and at a low cost.
The thermal insulation composite material adopts a multi-layer structure, including a protective and decorative layer, a solid waste-based thermal insulation core layer, and an interface reinforcement layer. The protective and decorative layer is composed of polymer emulsion, inorganic filler, and chopped fiber, the thermal insulation core layer is composed of industrial solid waste mixture and expanded perlite, and the interface reinforcement layer is impregnated with polymer emulsion. Combined with a low-temperature curing process, the material is prepared efficiently.
It achieves efficient utilization of industrial solid waste, reduces raw material costs, improves the thermal insulation, fire resistance, water resistance and bonding strength of materials, simplifies construction procedures, and is suitable for large-scale production.
Smart Images

Figure CN121469115A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermal insulation composite materials technology, and in particular to a multilayer thermal insulation composite material containing solid waste base and its preparation method. Background Technology
[0002] With the increasing demands for building energy conservation, the demand for thermal insulation materials is growing. Traditional organic thermal insulation materials (such as polystyrene boards and polyurethane) have problems such as low fire resistance, easy aging, and poor environmental performance; while inorganic thermal insulation materials (such as rock wool and foam glass) have disadvantages such as high cost, high production energy consumption, or high water absorption.
[0003] Meanwhile, the stockpiling of large quantities of industrial solid waste (such as fly ash, slag, and waste glass powder) not only occupies land but also poses a potential threat to the environment. Existing technologies have already attempted to utilize solid waste to prepare thermal insulation materials.
[0004] For example, Chinese patent CN101607815B discloses a method for preparing fly ash sintered bricks, which uses a large amount of fly ash and bentonite to replace clay in brick making. This results in fly ash sintered bricks with good thermal insulation performance, good smoothness, and resistance to peeling and cracking, while also achieving energy saving and environmental protection. However, the above-mentioned materials have poor water resistance and low strength.
[0005] Chinese patent CN118373665A discloses a solid waste foam ceramic insulation material and its preparation method. The method involves mixing coal gangue, shale slag, fly ash, granite waste powder, carbide slag, marble waste powder, steel slag, glass waste powder, and water to obtain a mixture. This mixture is then placed in a mold and extruded to obtain a green body. After drying, the green body is sintered to obtain the solid waste foam ceramic insulation material. This invention achieves efficient comprehensive utilization of eight types of solid waste, including coal gangue, carbide slag, and fly ash, and produces a high-performance foam ceramic insulation material. However, this method involves a high sintering temperature, increasing processing costs, and the prepared material has relatively poor insulation performance.
[0006] Therefore, developing a composite material that can efficiently dispose of solid waste, possess excellent thermal insulation, fire resistance, waterproofing, and mechanical properties, and is also low in cost has become an urgent problem to be solved in this field. Summary of the Invention
[0007] In view of this, the purpose of the present invention is to provide a multilayer thermal insulation composite material containing solid waste base, which takes into account low thermal conductivity (high thermal insulation), sufficient mechanical strength, excellent fire resistance and good water resistance.
[0008] To achieve the above objectives, the present invention provides the following technical solution:
[0009] A multi-layer thermal insulation composite material containing solid waste base, comprising, from top to bottom, a protective decorative layer, a solid waste base thermal insulation core layer, and an interface reinforcement layer;
[0010] The protective decorative layer comprises the following raw materials in parts by weight: 80-100 parts polymer emulsion, 40-50 parts inorganic filler, 0-5 parts pigment, 1-5 parts chopped fiber, 0.5-2 parts thickener, and 1-2 parts defoamer.
[0011] The solid waste-based insulation core layer comprises the following raw materials in parts by weight: 50-80 parts of industrial solid waste mixture, 5-10 parts of expanded perlite, 5-15 parts of alkaline activator, 0.5-3 parts of foaming agent, 0.1-1 parts of foam stabilizer, 1-5 parts of toughening fiber, and 15-30 parts of water.
[0012] The interface reinforcement layer is a porous nonwoven fabric or mesh fabric impregnated with polymer emulsion.
[0013] Preferably, the thickness of the protective decorative layer is 0.5-2mm, mainly serving as weather resistance, waterproofing, and decoration; the thickness of the solid waste-based thermal insulation core layer is 200-300mm; and the thickness of the interface reinforcement layer is 0.2-2mm, used to enhance the bonding strength between the composite material and the building wall.
[0014] Preferably, the polymer emulsion is any one of acrylic emulsion, polyacrylate emulsion, polyurethane emulsion, and styrene-acrylic emulsion.
[0015] Preferably, the inorganic filler is at least one of quartz powder, fumed silica, and calcium carbonate.
[0016] Preferably, the length of the chopped fiber is 6-12 mm, and the chopped fiber is polypropylene chopped fiber or chopped glass fiber treated with a silane coupling agent.
[0017] Preferably, the thickener is hydroxypropyl methylcellulose; and the defoamer is an organosilicon defoamer.
[0018] Preferably, the industrial solid waste mixture is composed of fly ash, blast furnace slag, and waste glass powder mixed in a mass ratio of 40-60:20-40:10-30. The preparation method of the industrial solid waste mixture involves ball milling the industrial solid waste to reduce its particle size to below 30 μm, followed by soaking in a 1.5-3 g / L Na₂SO₄ solution for 10-24 hours.
[0019] Ball milling not only reduces particle size but also destroys the inert layer on the surface, increases surface energy and defect sites, and significantly improves chemical reactivity. Then, soaking in Na2SO4 solution dissolves surface-active ions, further enhancing chemical reactivity.
[0020] Preferably, the alkaline activator is a composite solution of water glass and sodium hydroxide, with a modulus of 1.0-1.8.
[0021] Preferably, the foaming agent is a mixture of hydrogen peroxide, aluminum powder, and ferrosilicon powder in a mass ratio of 5:0.1-0.5:0.1-0.5; and the foam stabilizer is sodium dodecyl sulfate.
[0022] Preferably, the toughening fiber is any one of polypropylene fiber, polyacrylonitrile fiber, or wood fiber; the length of the toughening fiber is 8-15 mm.
[0023] Another object of the present invention is to provide a method for preparing a multilayer thermal insulation composite material containing a solid waste base, comprising the following steps:
[0024] (1) Lay an interface reinforcement layer in the mold;
[0025] (2) Preparation of thermal insulation core layer slurry: Mix the industrial solid waste mixture, foam stabilizer and toughening fiber evenly according to the formula; then add alkaline activator and water, and stir at 600-700 rpm for 1-3 minutes to form a uniform slurry; finally add foaming agent, and stir at 300-400 rpm for 30-60 seconds to obtain thermal insulation core layer slurry;
[0026] (3) Casting: The thermal insulation core layer slurry is cast into the mold with the interface reinforcement layer laid;
[0027] (4) Foaming and curing: Foaming and curing at 40-70℃ for 4-12 hours, then demolding and curing for 7-28 days to obtain the composite of thermal insulation core material and interface reinforcement layer;
[0028] (5) Preparation of protective decorative layer: Mix and stir the raw materials of the protective decorative layer to form a paste, and apply it evenly to the composite material in step (4) by scraping or rolling. Dry and cure at room temperature for 48-72 hours to obtain the multi-layer thermal insulation composite material.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] This invention prepares a multi-layer thermal insulation composite material containing solid waste, comprising a protective and decorative layer, a solid waste-based thermal insulation core layer, and an interface reinforcement layer. The main component of the solid waste-based thermal insulation core layer is a mixture of industrial solid wastes, with a high proportion of solid waste in the raw materials, achieving high-value-added resource utilization of bulk industrial solid waste and significantly reducing raw material costs. The multi-layer composite structure exhibits superior performance. The thermal insulation core layer, through the synergistic effect of various solid wastes, forms a high-strength, water-resistant geopolymer gel under alkaline activation, with a uniform closed-cell structure formed internally through chemical foaming, resulting in low thermal conductivity. The interface reinforcement layer effectively solves the problem of poor adhesion between inorganic insulation boards and walls, improving the system's safety and impact resistance. The protective and decorative layer provides excellent weather resistance, water resistance, and decorative properties, achieving integrated thermal insulation and decoration, and simplifying construction procedures. The raw materials of this invention are all inorganic or flame-retardant materials, improving fire resistance. The process of this invention is simple, requiring no high-temperature sintering, employing low-temperature curing, resulting in low energy consumption, a continuous process flow, and easy large-scale production. Attached Figure Description
[0031] Figure 1 This is a structural diagram of the multilayer thermal insulation composite material containing solid waste base prepared according to the present invention;
[0032] Figure 1 1 is the protective and decorative layer, 2 is the solid waste-based thermal insulation core layer, and 3 is the interface reinforcement layer. Detailed Implementation
[0033] This invention provides a multi-layer thermal insulation composite material containing a solid waste base, comprising, from top to bottom, a protective decorative layer, a solid waste-based thermal insulation core layer, and an interface reinforcement layer; the structure of the multi-layer thermal insulation composite material is as follows: Figure 1 .
[0034] The protective decorative layer comprises the following raw materials in parts by weight: 80-100 parts polymer emulsion, 40-50 parts inorganic filler, 0-5 parts pigment, 1-5 parts chopped fiber, 0.5-2 parts thickener, and 1-2 parts defoamer.
[0035] The solid waste-based insulation core layer comprises the following raw materials in parts by weight: 50-80 parts of industrial solid waste mixture, 5-10 parts of expanded perlite, 5-15 parts of alkaline activator, 0.5-3 parts of foaming agent, 0.1-1 parts of foam stabilizer, 1-5 parts of toughening fiber, and 15-30 parts of water.
[0036] The interface reinforcement layer is a porous nonwoven fabric or mesh fabric impregnated with polymer emulsion.
[0037] The protective decorative layer of the present invention has a thickness of 0.5-2mm and mainly serves as a weather-resistant, waterproof and decorative layer; the solid waste-based thermal insulation core layer has a thickness of 200-300mm; and the interface reinforcement layer has a thickness of 0.2-2mm, which is used to enhance the bonding strength between the composite material and the building wall.
[0038] In the protective decorative layer, the polymer emulsion is any one of acrylic emulsion, polyacrylate emulsion, polyurethane emulsion, and styrene-acrylic emulsion; the inorganic filler is at least one of quartz powder, fumed silica, and calcium carbonate; the length of the chopped fiber is 6-12 mm, specifically chopped polypropylene fiber or chopped glass fiber treated with a silane coupling agent; the thickener is hydroxypropyl methylcellulose; and the defoamer is an organosilicon defoamer.
[0039] In the solid waste-based insulation core layer, the industrial solid waste mixture is composed of fly ash, blast furnace slag and waste glass powder mixed in a mass ratio of 40-60:20-40:10-30;
[0040] The alkaline activator is a composite solution of water glass and sodium hydroxide with a modulus of 1.0-1.8; the foaming agent is a mixture of hydrogen peroxide, aluminum powder and ferrosilicon powder in a mass ratio of 5:0.1-0.5:0.1-0.5; the foam stabilizer is sodium dodecyl sulfate; the toughening fiber is any one of polypropylene fiber, polyacrylonitrile fiber or wood fiber, and the length of the toughening fiber is 8-15 mm.
[0041] In the interface reinforcement layer, the polymer emulsion is any one of acrylic emulsion, polyacrylate emulsion, polyurethane emulsion, and styrene-acrylic emulsion; the interface reinforcement layer is prepared by impregnating porous nonwoven fabric or mesh fabric in acrylic emulsion, and then placing it in a mold to cure at room temperature for 24-48 hours.
[0042] The preparation method of the multilayer thermal insulation composite material containing solid waste includes the following steps:
[0043] (1) Lay an interface reinforcement layer in the mold;
[0044] (2) Preparation of thermal insulation core layer slurry: Mix the industrial solid waste mixture, foam stabilizer and toughening fiber evenly according to the formula; then add alkaline activator and water, and stir at 600-700 rpm for 1-3 minutes to form a uniform slurry; finally add foaming agent, and stir at 300-400 rpm for 30-60 seconds to obtain thermal insulation core layer slurry;
[0045] (3) Casting: The thermal insulation core layer slurry is cast into the mold with the interface reinforcement layer laid;
[0046] (4) Foaming and curing: Foaming and curing at 40-70℃ for 4-12 hours, then demolding and curing for 7-28 days to obtain the composite of thermal insulation core material and interface reinforcement layer;
[0047] (5) Preparation of protective decorative layer: Mix and stir the raw materials of the protective decorative layer to form a paste, and apply it evenly to the composite material in step (4) by scraping or rolling. Dry and cure at room temperature for 48-72 hours to obtain the multi-layer thermal insulation composite material.
[0048] In a specific embodiment of the present invention, the preparation method of the multilayer thermal insulation composite material containing solid waste base includes the following steps:
[0049] (1) Impregnate porous nonwoven fabric or mesh fabric in acrylic emulsion, and then place it in a mold and cure at room temperature for 24 hours to obtain an interface reinforcement layer;
[0050] (2) Preparation of thermal insulation core layer slurry: The industrial solid waste mixture, foam stabilizer and toughening fiber are dry mixed evenly according to the formula; then the alkaline activator and water are added, and the mixture is stirred at 650 rpm for 3 minutes to form a uniform slurry; finally the foaming agent is added, and the mixture is stirred at 350 rpm for 60 seconds to obtain the thermal insulation core layer slurry.
[0051] (3) Casting: The thermal insulation core layer slurry is cast into the mold with the interface reinforcement layer laid;
[0052] (4) Foaming and curing: Foaming and curing at 45-50℃ for 12 hours, then demolding and curing for 7-28 days to obtain the composite of thermal insulation core material and interface reinforcement layer;
[0053] (5) Preparation of protective decorative layer: Mix and stir the raw materials of the protective decorative layer to make a paste, and apply it evenly to the composite material in step (4) by scraping. Dry and cure at room temperature for 72 hours to obtain the multi-layer thermal insulation composite material.
[0054] In a specific embodiment of the present invention, the preparation method of the industrial solid waste mixture is as follows: the industrial solid waste is ball-milled to make its particle size less than 30 μm, and then soaked in a 2 g / L Na2SO4 solution for 24 h, with a solid-liquid ratio of 1:10.
[0055] The present invention will be further described below with reference to the embodiments.
[0056] Example 1
[0057] A multi-layer thermal insulation composite material containing a solid waste base comprises, from top to bottom, a protective decorative layer, a solid waste-based thermal insulation core layer, and an interface reinforcement layer; the structure of the multi-layer thermal insulation composite material is as follows: Figure 1 .
[0058] The protective decorative layer comprises the following raw materials in parts by weight: 100 parts polymer emulsion, 50 parts inorganic filler, 1 part titanium dioxide pigment, 4 parts chopped fibers, 1.7 parts thickener, and 1.3 parts defoamer;
[0059] The solid waste-based insulation core layer comprises the following raw materials in parts by weight: 80 parts of industrial solid waste mixture, 8 parts of expanded perlite, 15 parts of alkaline activator, 2.4 parts of foaming agent, 0.7 parts of foam stabilizer, 3 parts of toughening fiber, and 30 parts of water.
[0060] The interface reinforcement layer is a porous nonwoven fabric impregnated with a polymer emulsion.
[0061] The protective decorative layer of the present invention has a thickness of 2mm; the solid waste-based thermal insulation core layer has a thickness of 250mm; and the interface reinforcement layer has a thickness of 2mm.
[0062] In the protective decorative layer, the polymer emulsion is a polyacrylate emulsion; the inorganic filler is a mixture of fumed silica and calcium carbonate in a mass ratio of 1:1; the chopped fibers are 6-12 mm long polypropylene chopped fibers; the thickener is hydroxypropyl methylcellulose; and the defoamer is polydimethylsiloxane.
[0063] In the solid waste-based insulation core layer, the industrial solid waste mixture is composed of fly ash, blast furnace slag, and waste glass powder mixed in a mass ratio of 60:30:20; the alkaline activator is a composite solution of water glass and sodium hydroxide with a modulus of 1.2; the foaming agent is a mixture of hydrogen peroxide, aluminum powder, and ferrosilicon powder in a mass ratio of 5:0.2:0.2; the foam stabilizer is sodium dodecyl sulfate; and the toughening fiber is polypropylene fiber with a length of 8-15 mm.
[0064] In the interface enhancement layer, the polymer emulsion is an acrylic emulsion.
[0065] Example 2
[0066] A multi-layer thermal insulation composite material containing a solid waste base comprises, from top to bottom, a protective decorative layer, a solid waste-based thermal insulation core layer, and an interface reinforcement layer; the structure of the multi-layer thermal insulation composite material is as follows: Figure 1 .
[0067] The protective decorative layer comprises the following raw materials in parts by weight: 90 parts polymer emulsion, 40 parts inorganic filler, 3 parts titanium dioxide pigment, 4 parts chopped fibers, 1.9 parts thickener, and 1.4 parts defoamer;
[0068] The solid waste-based insulation core layer comprises the following raw materials in parts by weight: 70 parts of industrial solid waste mixture, 10 parts of expanded perlite, 15 parts of alkaline activator, 2.1 parts of foaming agent, 0.6 parts of foam stabilizer, 4 parts of toughening fiber, and 30 parts of water.
[0069] The interface reinforcement layer is a porous nonwoven fabric impregnated with a polymer emulsion.
[0070] The protective decorative layer of the present invention has a thickness of 2mm; the solid waste-based thermal insulation core layer has a thickness of 250mm; and the interface reinforcement layer has a thickness of 2mm.
[0071] In the protective decorative layer, the polymer emulsion is a polyacrylate emulsion, the inorganic filler is a mixture of quartz powder and fumed silica in a mass ratio of 1:1, the short-cut fibers are polypropylene short-cut fibers with a length of 6-12 mm, the thickener is hydroxypropyl methylcellulose, and the defoamer is polydimethylsiloxane.
[0072] In the solid waste-based insulation core layer, the industrial solid waste mixture is composed of fly ash, blast furnace slag, and waste glass powder mixed in a mass ratio of 50:20:20; the alkaline activator is a composite solution of water glass and sodium hydroxide with a modulus of 1.2; the foaming agent is a mixture of hydrogen peroxide, aluminum powder, and ferrosilicon powder in a mass ratio of 5:0.1:0.2; the foam stabilizer is sodium dodecyl sulfate; and the toughening fiber is wood fiber with a length of 8-15 mm.
[0073] In the interface reinforcement layer, the polymer emulsion is a polyacrylate emulsion.
[0074] Comparative Example 1
[0075] A multi-layer thermal insulation composite material containing solid waste base is different from Example 1 in that Comparative Example 1 does not have a protective decorative layer.
[0076] Comparative Example 2
[0077] A multilayer thermal insulation composite material containing solid waste base is different from Example 1 in that Comparative Example 2 does not have an interface reinforcement layer.
[0078] Comparative Example 3
[0079] A multilayer thermal insulation composite material containing solid waste base differs from Example 1 in that the solid waste base thermal insulation core layer of Comparative Example 3 does not contain toughening fibers.
[0080] Comparative Example 4
[0081] A multi-layer thermal insulation composite material containing solid waste base differs from Example 1 in that expanded perlite is not added to the solid waste base thermal insulation core layer of Comparative Example 4.
[0082] Comparative Example 5
[0083] A multi-layer thermal insulation composite material containing solid waste base differs from Example 1 in that waste glass powder is not added to the industrial solid waste mixture of the solid waste base thermal insulation core layer in Comparative Example 5.
[0084] Comparative Example 6
[0085] A multilayer thermal insulation composite material containing solid waste base, which differs from Example 1 in that the amount of polymer emulsion added in the protective decorative layer of Comparative Example 6 is 50 parts.
[0086] Comparative Example 7
[0087] A multilayer thermal insulation composite material containing solid waste base, which differs from Example 1 in that the foaming agent in Comparative Example 7 is hydrogen peroxide.
[0088] Comparative Example 8
[0089] A multilayer thermal insulation composite material containing solid waste base differs from Example 1 in that the industrial solid waste mixture in Comparative Example 8 is not treated with Na2SO4 solution soaking.
[0090] Thermal conductivity and strength tests were conducted on the multilayer thermal insulation composite materials in Examples 1-2 and Comparative Examples 1-6, and the porosity was calculated. The results are shown in Table 1.
[0091] Table 1
[0092] Thermal conductivity (W / (m·K)) Compressive strength (MPa) Porosity (%) Example 1 0.315 13.4 72 Example 2 0.347 12.1 68 Comparative Example 1 0.329 10.3 64 Comparative Example 2 0.342 11.2 67 Comparative Example 3 0.336 8.7 65 Comparative Example 4 0.612 10.6 53 Comparative Example 5 0.376 7.3 66 Comparative Example 6 0.376 10.1 67 Comparative Example 7 0.459 11.3 47 Comparative Example 8 0.575 11.7 62
[0093] High-pressure water seepage tests were conducted on the multilayer thermal insulation composite materials in Examples 1-2 and Comparative Examples 1-6. Water was sprayed from top to bottom onto the different composite materials using a water gun at the same water pressure. After spraying for 1 hour, the spraying area of the waterproof thermal insulation material board was cut open to measure the water seepage depth. The results are shown in Table 2.
[0094] Table 2
[0095] Seepage depth (mm) Example 1 1.7 Example 2 1.9 Comparative Example 1 4.7 Comparative Example 2 2.0 Comparative Example 3 1.6 Comparative Example 4 1.8 Comparative Example 5 1.7 Comparative Example 6 3.4 Comparative Example 7 1.4 Comparative Example 8 2.8
[0096] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A multilayer thermal insulation composite material containing a solid waste base, characterized in that, From top to bottom, it includes a protective decorative layer, a solid waste-based thermal insulation core layer, and an interface reinforcement layer; The protective decorative layer comprises the following raw materials in parts by weight: 80-100 parts polymer emulsion, 40-50 parts inorganic filler, 0-5 parts pigment, 1-5 parts chopped fiber, 0.5-2 parts thickener, and 1-2 parts defoamer. The solid waste-based insulation core layer comprises the following raw materials in parts by weight: 50-80 parts of industrial solid waste mixture, 5-10 parts of expanded perlite, 5-15 parts of alkaline activator, 0.5-3 parts of foaming agent, 0.1-1 parts of foam stabilizer, 1-5 parts of toughening fiber, and 15-30 parts of water. The interface reinforcement layer is a porous nonwoven fabric or mesh fabric impregnated with polymer emulsion.
2. The multilayer thermal insulation composite material containing solid waste base according to claim 1, characterized in that, The protective decorative layer has a thickness of 0.5-2mm and mainly serves as a weather-resistant, waterproof, and decorative layer; the solid waste-based thermal insulation core layer has a thickness of 200-300mm; and the interface reinforcement layer has a thickness of 0.2-2mm, used to enhance the bonding strength between the composite material and the building wall.
3. The multilayer thermal insulation composite material containing solid waste base according to claim 1, characterized in that, The polymer emulsion is any one of acrylic emulsion, polyacrylate emulsion, polyurethane emulsion, and styrene-acrylic emulsion.
4. The multilayer thermal insulation composite material containing solid waste base according to claim 1, characterized in that, The inorganic filler is at least one of quartz powder, fumed silica, and calcium carbonate.
5. The multilayer thermal insulation composite material containing a solid waste base according to claim 1, characterized in that, The length of the chopped fiber is 6-12 mm, and the chopped fiber is polypropylene chopped fiber or chopped glass fiber treated with a silane coupling agent; the thickener is hydroxypropyl methylcellulose; and the defoamer is an organosilicon defoamer.
6. The multilayer thermal insulation composite material containing solid waste base according to claim 1, characterized in that, The industrial solid waste mixture is composed of fly ash, blast furnace slag and waste glass powder mixed in a mass ratio of 40-60:20-40:10-30.
7. The multilayer thermal insulation composite material containing a solid waste base according to claim 1, characterized in that, The method for preparing the industrial solid waste mixture is as follows: ball milling the industrial solid waste to make its particle size less than 30μm, and then soaking it in a 1.5-3g / L Na2SO4 solution for 10-24h.
8. The multilayer thermal insulation composite material containing a solid waste base according to claim 1, characterized in that, The alkaline activator is a composite solution of water glass and sodium hydroxide with a modulus of 1.0-1.8; the foaming agent is a mixture of hydrogen peroxide, aluminum powder and ferrosilicon powder in a mass ratio of 5:0.1-0.5:0.1-0.5; and the foam stabilizer is sodium dodecyl sulfate.
9. The multilayer thermal insulation composite material containing a solid waste base according to claim 1, characterized in that, The toughening fiber is any one of polypropylene fiber, polyacrylonitrile fiber, or wood fiber; the length of the toughening fiber is 8-15 mm.
10. The method for preparing the multilayer thermal insulation composite material containing solid waste as described in claim 1, characterized in that, Includes the following steps: (1) Lay an interface reinforcement layer in the mold; (2) Preparation of thermal insulation core layer slurry: Mix the industrial solid waste mixture, foam stabilizer and toughening fiber evenly according to the formula; then add alkaline activator and water, and stir at 600-700 rpm for 1-3 minutes to form a uniform slurry; finally add foaming agent, and stir at 300-400 rpm for 30-60 seconds to obtain thermal insulation core layer slurry; (3) Casting: The thermal insulation core layer slurry is cast into the mold with the interface reinforcement layer laid; (4) Foaming and curing: Foaming and curing at 40-70℃ for 4-12 hours, then demolding and curing for 7-28 days to obtain the composite of thermal insulation core material and interface reinforcement layer; (5) Preparation of protective decorative layer: Mix and stir the raw materials of the protective decorative layer to form a paste, and apply it evenly to the composite material in step (4) by scraping or rolling. Dry and cure at room temperature for 48-72 hours to obtain the multi-layer thermal insulation composite material.
Citation Information
Patent Citations
Fly ash sintered brick and manufacture method thereof
CN101607815B
All-solid waste foamed ceramic thermal insulation material and preparation method thereof
CN118373665A