High-softness butyl sealant capable of not sticking hands and not softening wire harnesses and preparation method of high-softness butyl sealant

By adjusting the ratio of butyl rubber and polyisobutylene, and combining inorganic fillers, flame retardants, polyester plasticizers, and rubber filler oil, a highly flexible, non-sticky, and non-softening butyl sealant for wire harnesses was prepared. This solved the problems of laborious operation, stickiness, and wire harness softening, and improved safety and insulation performance.

CN121699536APending Publication Date: 2026-03-20KUNSHAN INAUTEK AUTOMOTIVE COMPONENTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610036294.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-13
Publication Date
2026-03-20

AI Technical Summary

Technical Problem

Existing automotive wiring harness sealants have several drawbacks during use, including being difficult to apply, sticky to the hands, softening the wiring harness leading to decreased insulation performance, and posing safety hazards.

Method used

By using a suitable ratio of butyl rubber and polyisobutylene, combined with inorganic fillers, flame retardants, polyester plasticizers and rubber filler oil, a highly flexible, non-sticky and non-softening butyl sealant for wire harnesses is prepared. The sealant's flexibility, flame retardancy and non-stickiness are ensured through appropriate formulation design.

Benefits of technology

It achieves effortless operation, is non-sticky, and does not soften the wire harness, ensuring the safety and insulation performance of the sealant and meeting regulatory flame retardant requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of sealants, and discloses a high-softness butyl sealant without sticking hands and softening wire harnesses and a preparation method of the high-softness butyl sealant. The butyl sealant is prepared from the following raw materials: 5-15 parts of butyl rubber; 3 to 15 parts of polyisobutene; 3-8 parts of petroleum resin; 30-60 parts of an inorganic filler; 15 to 30 parts of a flame retardant; 0.5 to 1.5 parts of a coloring agent; 5-15 parts of a polyester plasticizer; and 5-15 parts of rubber filling oil. The butyl rubber and the polyisobutene are mixed for use, and the hardness of the sealant is suitable for manual operation through a proper proportion; compared with the common plasticizer, the polyester plasticizer has the advantages that the polypropylene glycol adipate is large in molecular weight, low in volatility and low in mobility, cannot migrate to the wire harness from the sealant, and cannot soften the wire harness; the polyester plasticizer and the rubber filling oil are mixed for use, and the sealant has the effect of not sticking hands but sticking lines through a proper proportion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sealant technology, specifically to a highly flexible, non-sticky, non-softening butyl sealant for wire harnesses and its preparation method. Background Technology

[0002] Automotive wiring harnesses are the main network of a car's electrical system, composed of multi-core copper wires, connector terminals, and insulating protective layers, bundled together to form an integrated system connecting the circuits. Their core functions include transmitting electrical drive components (such as motors and lights) and transmitting sensor signals to the control unit, much like the car's "nervous system." To ensure the long-term and stable operation of this "nervous system," the wiring harness's sealing and waterproofing are crucial.

[0003] Currently, automotive wiring harness sealants commonly use sheets with a cone penetration of around 60 (1 / 10 mm) and blocks with a cone penetration of around 100 (1 / 10 mm). Sheets are harder than blocks, requiring operators to pull them apart and wrap them around the wiring harness. Prolonged use can lead to operator fatigue and complaints, but sheets do not soften the wiring harness. Blocks are softer and also require operators to pull them apart and wrap them around the harness. Because they are softer, operators don't need to exert much effort. Therefore, without considering cost, operators tend to prefer blocks. However, because blocks need to achieve high flexibility (the higher the cone penetration, the softer the product, and the easier it is for the operator to use), the formulation generally requires more plasticizers and softeners. Normally, the more plasticizer added, the easier it is for the wiring harness to be impregnated by the plasticizer in the sealant, leading to softening of the wiring harness sheath, affecting insulation performance, and creating safety hazards. Summary of the Invention

[0004] To address the aforementioned technical problems, the present invention aims to provide a highly flexible, non-sticky, and non-softening butyl sealant and its preparation method. The high flexibility of this butyl sealant makes it easier for operators to use; its non-stickiness eliminates concerns about the sealant being difficult to clean after application, thus improving efficiency; its non-softening properties fundamentally protect the wire harness and eliminate safety hazards; and its flame retardancy meets regulatory requirements.

[0005] To achieve the above objectives, the present invention provides the following technical solution: A highly flexible, non-sticky, and non-softening butyl sealant for wire harnesses, comprising the following components by weight: 5-15 parts of butyl rubber; 3-15 parts of polyisobutylene; 3-8 parts of petroleum resin; 30-60 parts of inorganic filler; 15-30 parts flame retardant; Colorant: 0.5–1.5 parts; 5-15 parts of polyester plasticizer; 5-15 parts of rubber filler oil.

[0006] Preferably, the raw materials for preparing the butyl sealant, by weight, comprise the following components: 10 parts butyl rubber; 8 parts of polyisobutylene; 5 parts petroleum resin; 30 parts of inorganic filler; 30 parts flame retardant; 1 part colorant; 10 parts polyester plasticizer; 6 parts rubber filler oil.

[0007] Preferably, the butyl rubber is a common non-halogenated butyl rubber.

[0008] Preferably, the polyisobutylene is one or a combination of several of the following: 1300 molecular weight polyisobutylene, 2400 molecular weight polyisobutylene, and 50000 molecular weight polyisobutylene.

[0009] Preferably, the petroleum resin is one or a combination of petroleum resin and hydrogenated petroleum resin.

[0010] Preferably, the inorganic filler is one or a combination of several of talc, silica, mica powder and light calcium carbonate.

[0011] Preferably, the flame retardant is a combination of one or more of red phosphorus, aluminum hydroxide and nitrogen-containing flame retardants.

[0012] Preferably, the colorant is carbon black.

[0013] Preferably, the polyester plasticizer is polypropylene adipate.

[0014] Preferably, the rubber filler oil is white oil.

[0015] The present invention also provides a method for preparing the above-mentioned butyl sealant, comprising the following steps: (1) Prepare raw materials containing butyl rubber, polyisobutylene, tackifying resin, inorganic filler, flame retardant, colorant, polyester plasticizer and rubber filler oil according to the formula; (2) First, stir the butyl rubber and polyisobutylene in step (1) in a kneader for 20-40 minutes. Then, add the colorant, 40% polyester plasticizer and 50% inorganic filler and stir in the kneader for 20-30 minutes until there are no particles. Then, add the flame retardant, 40% polyester plasticizer and the remaining inorganic filler and stir for 15-25 minutes until there are no particles. Then, add the petroleum resin for 15-25 minutes. Then, add the remaining 20% ​​polyester plasticizer and rubber filler oil and stir evenly. Then, while stirring, vacuum the whole thing for 10-20 minutes. The vacuum pressure is ≥0.08MPa. Finally, the rubber compound is obtained. Among them, since the polyester plasticizer has a large molecular weight and high viscosity, in order to fully disperse it, the polyester plasticizer needs to be added in a distributed manner. (3) After storing the adhesive material in step (2) at 40°C for 1 day, it is extruded at 80°C, cut into small sections according to customer requirements, wrapped with release film, and then packed into boxes to obtain a highly soft, non-sticky, and non-softening butyl sealant for wire harnesses.

[0016] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention uses a mixture of butyl rubber and polyisobutylene, and through a suitable ratio, the hardness of the sealant is suitable for workers to operate. 2. This invention uses a mixture of inorganic fillers and flame retardants. By using an appropriate ratio, the sealant has good flame retardancy while reducing costs. 3. Unlike plasticizers in conventional rubber formulations, this invention uses polyester plasticizers. Compared with ordinary plasticizers, polypropylene adipate has a large molecular weight, low volatility, and low migration. It will not migrate from the sealant to the wire harness, does not soften the wire harness, and ensures safety for long-term use.

[0017] 4. This invention uses a mixture of polyester plasticizer and rubber filler oil. By using an appropriate ratio, the sealant is not sticky to the touch but has the effect of sticking to the wire. Detailed Implementation

[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0019] Unless otherwise specified below, all raw materials used in this application are commercially available materials.

[0020] Table 1 lists the raw material grades and manufacturer information: Example 1: A method for preparing a highly flexible, non-sticky, and non-softening butyl sealant for wire harnesses, comprising the following steps: (1) Prepare raw materials according to the proportion; by weight, the raw materials for preparing the butyl sealant include the following components: 10 parts butyl rubber; 8 parts polyisobutylene; 5 parts petroleum resin; 30 parts inorganic filler; 30 parts flame retardant; 1 part colorant; 10 parts polyester plasticizer; and 6 parts rubber filler oil.

[0021] (2) First, stir the butyl rubber and polyisobutylene in the kneader for 20-40 minutes. Then, add the colorant, 40% polyester plasticizer and 50% inorganic filler and stir in the kneader for 20-30 minutes until there are no particles. Then, add the flame retardant, 40% polyester plasticizer and the remaining inorganic filler and stir for 15-25 minutes until there are no particles. Then, add the petroleum resin for 15-25 minutes. Then, add the remaining 20% ​​polyester plasticizer and rubber filler oil and stir evenly. Then, while stirring, vacuum the whole thing for 10-20 minutes. The vacuum pressure is ≥0.08MPa. Finally, the rubber compound is obtained. (3) After storing the adhesive material in step (2) at 40°C for 1 day, it is extruded at 80°C, cut into small sections according to customer requirements, wrapped with release film, and then packed into boxes to obtain a highly soft, non-sticky, and non-softening butyl sealant for wire harnesses.

[0022] The butyl rubber mentioned above is ordinary non-halogenated butyl rubber, specifically Yanshan Petrochemical 1751; the polyisobutylene is 1300 molecular weight polyisobutylene, specifically Dalin PB1300; the petroleum resin is petroleum resin, specifically Henghe C5 petroleum resin HHC-1100; the inorganic filler is talc powder, specifically Guangdong Chaoyue Powder Talc Powder B-666; the flame retardant is red phosphorus, specifically Henan Kewei Flame Retardant New Material 2500 mesh; the colorant is pigment carbon black, specifically Shanghai Baiyan N330 carbon black; the polyester plasticizer is polypropylene adipate, specifically Nanjing Shouqianshou Chemical Polyester Plasticizer PPA-1500; and the rubber filler oil is white oil, specifically Hangzhou Fuda 70# white oil.

[0023] Examples 2-4: The preparation method of a highly flexible, non-sticky, and non-softening butyl sealant for wire harnesses differs from Example 1 only in that the amounts of each component are different, as detailed in the table below.

[0024] Table 2 shows the comparison of the dosage of each component in Examples 1-4: Comparative Examples 1-5: A method for preparing a highly flexible, non-sticky, and non-softening butyl sealant for wire harnesses differs from Example 1 only in the amount of each component. Compared to Example 1, Comparative Example 1 contains no flame retardant; Comparative Example 2 contains no rubber filler oil; Comparative Example 3 contains no polyester plasticizer; Comparative Example 4 contains no polyester plasticizer and replaces it with DOTP; and Comparative Example 5 adjusts the ratio of polyester plasticizer and rubber filler oil.

[0025] Table 3 shows the comparison of the dosage of each component in Comparative Examples 1-5: The performance of the butyl sealant prepared in the above embodiments and comparative examples was tested, and the test results are shown in the table below.

[0026] Table 4 shows the performance test results of the sealants prepared in Examples 1-4 and Comparative Examples 1-5: Test method description: 1. Cone penetration: Tested according to GB / T 269-2023 standard, test temperature 23±2℃, total weight of cone and rod 150g, drop time 5s; 2. Is it sticky to the touch? At room temperature, hold about 30-40g of the block of adhesive in your hand, hold it for 2-3 seconds, and then open it to check if there is any sticky residue. 3. Attaching the thread: Press the product to a thickness of 1.5-2.0mm, and cut into 20mm pieces. Prepare 10 x 30cm long 1.5mm² PVC wires, each 80mm long. Mark both ends of one wire clearly. Then, press the middle sections of all 10 wires together at a 20mm angle. On an 80mm film, spaced 5-7mm apart, roll up the film from one end to bundle the wire harness. Wrap it with release film, hold it tightly for 2-3 seconds, and then release it. Let it sit at room temperature for 20 minutes. Then clamp one end of the marked wire onto the clamp of the tensile testing machine, and clamp the other 9 wires onto the lower clamp of the tensile testing machine. Start the tensile testing machine at a pulling speed of 100mm / min. Record the maximum force during the test and observe whether there is any residual adhesive on the pulled wire. 4. Combustion performance: Tested in accordance with GB 8410-2006; 5. Whether the wire has been softened: Prepare a sample according to the wire adhesion test method, then place the wrapped sample with release paper and put it in an oven at 70℃ for 7 days. After cooling to room temperature, peel off the wire at the wrapped part and compare the feel with the original wire to check whether the wire has been softened. 6. High temperature resistance: Press the finished rubber block into a 1.5-2.0mm thick sheet, and cut 25mm pieces. With a size of 100 mm, prepare the sample according to the requirements of JC / T 942-2022. Then place the whole sample in an oven at 125 °C for 24 h, and then take it out to observe whether there is any flow and deformation of the sample; 7. Low-temperature resistance: Press the finished rubber block into a film with a thickness of 1.5-2.0 mm, and cut it into 25 With a size of 100 mm, prepare the sample according to the requirements of JC / T 942-2022, and then place it in a low-temperature box at -40 °C for 24 h. Then take it out to observe whether there is any cracking and deformation on the surface and whether there are still sticking lines.

[0027] It can be seen from the above data that compared with Example 1, in Example 2, the ratio of butyl rubber and polyisobutylene was changed, but the softness and hardness of the rubber compound, whether it is sticky to the hand, and the high-temperature resistance performance have all changed significantly, and all are adverse changes. The rubber compound is very soft and sticky, and there is flow and deformation at high temperature; compared with Example 1, in Example 3, the ratio of butyl rubber and polyisobutylene and the ratio of inorganic filler and flame retardant were changed, the flame retardancy was significantly deteriorated, and the rubber compound also became significantly harder; compared with Example 1, in Example 4, the ratio of polyester plasticizer and rubber filling oil was changed, and all performances were close to those of Example 1, but the rubber compound was slightly sticky to the hand.

[0028] Compared with Example 1, in Comparative Example 1, the flame retardant was directly omitted and all replaced with inorganic filler, and the flame retardancy of the rubber compound did not meet GB 8410; compared with Example 1, in Comparative Example 2, the rubber filling oil was omitted and all replaced with polyester plasticizer, but the rubber compound showed a non-sticking line phenomenon; compared with Example 1, in Comparative Example 3, the polyester plasticizer was omitted and all replaced with rubber filling oil, and all indicators were qualified, but it was very sticky to the hand; compared with Example 1, in Comparative Example 4, the polyester plasticizer was omitted and all replaced with DOTP, and all indicators were qualified, but the wire was softened; compared with Example 1, in Comparative Example 5, the ratio of plasticizer and rubber filling oil was adjusted, and all indicators were qualified, but the rubber compound was sticky to the hand.

[0029] It can be seen from the formulations and test data of the examples and comparative examples that: the combined use of butyl rubber and polyisobutylene can affect the penetrometer (softness and hardness) of the rubber compound and the stickiness to the hand; the use of flame retardant can significantly improve the flame retardant performance of the rubber compound, but for cost considerations, the proportion of flame retardant needs to be tried with different ratios to achieve the best balance between flame retardant performance and cost; the replacement of DOTP with polyester plasticizer has little effect on the rubber compound (penetrometer), but DOTP will soften the wire, and there will be risks for the long-term use of the wire; the combined use of polyester plasticizer and rubber filling oil can affect the stickiness of the rubber compound to the hand and the sticking line performance, and they cannot be used alone.

[0030] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A highly flexible, non-sticky, and non-softening butyl sealant for wire harnesses, characterized in that: The raw materials for preparing this butyl sealant, by weight, include the following components: 5-15 parts of butyl rubber; 3-15 parts of polyisobutylene; 3-8 parts of petroleum resin; 30-60 parts of inorganic filler; 15-30 parts flame retardant; Colorant: 0.5–1.5 parts; 5-15 parts of polyester plasticizer; 5-15 parts of rubber filler oil.

2. The butyl sealant for a highly flexible, non-sticky, and non-softening wire harness according to claim 1, characterized in that: The raw materials for preparing this butyl sealant, by weight, include the following components: 10 parts butyl rubber; 8 parts of polyisobutylene; 5 parts petroleum resin; 30 parts of inorganic filler; 30 parts flame retardant; 1 part colorant; 10 parts polyester plasticizer; 6 parts rubber filler oil.

3. The butyl sealant for a highly flexible, non-sticky, and non-softening wire harness according to claim 1, characterized in that: The butyl rubber is a common non-halogenated butyl rubber; the polyisobutylene is one or a combination of several of the following: 1300 molecular weight polyisobutylene, 2400 molecular weight polyisobutylene, and 50000 molecular weight polyisobutylene.

4. The butyl sealant for a highly flexible, non-sticky, and non-softening wire harness according to claim 1, characterized in that: The petroleum resin is one or a combination of several of petroleum resins and hydrogenated petroleum resins.

5. The butyl sealant for a highly flexible, non-sticky, and non-softening wire harness according to claim 1, characterized in that: The inorganic filler is one or a combination of several of the following: talc, silica, mica powder, and light calcium carbonate.

6. The butyl sealant for a highly flexible, non-sticky, and non-softening wire harness according to claim 1, characterized in that: The flame retardant is one or a combination of several of the following: red phosphorus, aluminum hydroxide, and nitrogen-containing flame retardants.

7. The butyl sealant for a highly flexible, non-sticky, and non-softening wire harness according to claim 1, characterized in that: The colorant is pigment carbon black.

8. The butyl sealant for a highly flexible, non-sticky, and non-softening wire harness according to claim 1, characterized in that: The polyester plasticizer is polypropylene adipate.

9. The butyl sealant for a highly flexible, non-sticky, and non-softening wire harness according to claim 1, characterized in that: The rubber filler oil is white oil.

10. A method for preparing the butyl sealant according to any one of claims 1-9, characterized in that: Includes the following steps: (1) Prepare raw materials containing butyl rubber, polyisobutylene, tackifying resin, inorganic filler, flame retardant, colorant, polyester plasticizer and rubber filler oil according to the formula; (2) First, stir the butyl rubber and polyisobutylene in the kneader for 20-40 minutes. Then, add the colorant, 40% polyester plasticizer and 50% inorganic filler and stir in the kneader for 20-30 minutes until there are no particles. Then, add the flame retardant, 40% polyester plasticizer and the remaining inorganic filler and stir for 15-25 minutes until there are no particles. Then, add the petroleum resin for 15-25 minutes. Then, add the remaining 20% ​​polyester plasticizer and rubber filler oil and stir evenly. Then, while stirring, vacuum the whole thing for 10-20 minutes. The vacuum pressure is ≥0.08MPa. Finally, the rubber compound is obtained. (3) After storing the adhesive material in step (2) at 40°C for 1 day, it is extruded at 80°C, cut into small sections according to customer requirements, wrapped with release film, and then packed into boxes to obtain a highly soft, non-sticky, and non-softening butyl sealant for wire harnesses.