Alloy steel chain with high wear resistance and corrosion resistance and preparation method thereof
Through systematic composition design, heat treatment process, and surface composite strengthening treatment, the shortcomings of chain steel in terms of wear resistance and corrosion resistance have been solved, achieving synergistic optimization of high strength and high toughness, and improving the fatigue life and corrosion resistance of the chain.
Patent Information
- Application Number
- CN202511963388.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-24
- Publication Date
- 2026-03-24
AI Technical Summary
Existing high-strength chain steels have shortcomings in optimizing the composition ratio of the matrix material, controlling the morphology of inclusions, surface composite strengthening, and matching manufacturing process parameters, making it difficult to simultaneously meet the service requirements under harsh working conditions in terms of wear resistance and corrosion resistance.
Through systematic composition design and proportion constraints, inclusion modification treatment, heat treatment microstructure regulation and surface composite strengthening treatment, the synergistic optimization of high strength and toughness of the matrix and high wear and corrosion resistance of the surface is achieved. By using specific element proportions and heat treatment processes, a multiphase microstructure and a multi-layer surface-strengthened structure are formed.
It significantly improves the fatigue life and corrosion resistance of the chain, achieving a good match between high strength and high toughness, and extending the service life of the chain.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of steelmaking technology, specifically relating to a highly wear-resistant and corrosion-resistant alloy steel chain and its preparation method. Background Technology
[0002] Industrial chains, as key load-bearing components in mechanical transmission and material handling systems, are widely used in mining, port loading and unloading, marine engineering, and chemical production. With the development of modern industry towards heavy-duty, continuous, and extreme operating conditions, increasingly stringent requirements are being placed on the performance of industrial chains. Particularly in typical applications such as mining scraper conveyors, marine mooring systems, and chemical material handling, chains not only need to withstand high-frequency alternating and impact loads, but also face the challenges of abrasive wear, corrosive media erosion, and accelerated failure due to the combined effects of these factors. Statistics show that unplanned downtime caused by chain failure accounts for a significant proportion of equipment malfunctions in mines and ports, resulting in substantial economic losses and safety hazards.
[0003] Traditional circular link chains typically use medium-carbon alloy structural steel, such as 23MnNiMoCr54 and 25MnV, as the base material. These materials undergo quenching and tempering to achieve a tempered sorbitic structure, balancing strength and toughness. However, this design suffers from several shortcomings: First, the silicon-aluminum ratio lacks systematic optimization, failing to fully leverage their synergistic effects in deoxidation, grain refinement, and solid solution strengthening. Second, the addition of microalloying elements is often arbitrary, failing to establish a quantitative ratio matching the carbon content, making precise control of carbide precipitation difficult. Third, insufficient attention is paid to the nitrogen-boron ratio design, affecting the grain boundary segregation strengthening effect of boron and the morphological distribution of nitrides. These issues limit further improvements in the strength and toughness of the base material.
[0004] In terms of inclusion control, the morphology, size, and distribution of oxide and sulfide inclusions in steel have a significant impact on the fatigue performance and corrosion resistance of chains. Al₂O₃ inclusions formed by traditional smelting processes are angular, while sulfide inclusions are elongated and distributed along the rolling direction. These inclusions are prone to becoming the initiation point for fatigue cracks under alternating stress and constitute active sites for electrochemical corrosion in corrosive environments. Although calcium treatment and rare earth treatment technologies have been applied in the iron and steel metallurgy field, the systematic control scheme for inclusions in high-strength chain steel still needs improvement.
[0005] In terms of surface strengthening, existing technologies mainly employ single nitriding or single coating processes. While gas nitriding or ion nitriding can form a high-hardness nitride layer on the steel surface, the porous structure and microcracks of the nitrided layer provide penetration channels for corrosive media, resulting in limited improvement in corrosion resistance. Electroplating, such as zinc plating and chromium plating, offers some corrosion protection, but the bonding strength between the coating and the substrate is insufficient, making it prone to peeling failure under conditions of wear and tear from the chain links. Furthermore, a single surface treatment process cannot simultaneously meet the dual requirements of wear resistance and corrosion resistance.
[0006] In chain manufacturing, flash butt welding is a core process in the production of round link chains, and the quality of the weld joint directly determines the overall performance of the chain. Current processes lack systematic optimization of preheating, flash parameters, and upsetting parameters, leading to coarse-grain embrittlement in the weld heat-affected zone. Subsequent heat treatment processes mostly employ the traditional quenching and tempering route, and there is still a lack of mature process solutions for achieving high strength while retaining an appropriate amount of retained austenite to improve toughness.
[0007] In summary, existing technologies have room for improvement in areas such as matrix material composition optimization, inclusion morphology control, surface composite strengthening treatment, and manufacturing process parameter matching. There is an urgent need to develop a high wear-resistant and corrosion-resistant alloy steel chain and its preparation method that can systematically solve the above problems. Summary of the Invention
[0008] To address the shortcomings of existing high-strength chain steel technologies in areas such as matrix material composition optimization, inclusion morphology control, surface wear-resistant and corrosion-resistant composite strengthening, and matching of manufacturing process parameters, this invention aims to provide a high-wear-resistant and corrosion-resistant alloy steel chain and its preparation method. This alloy steel chain achieves synergistic optimization of high strength and toughness of the matrix and high wear-resistant and corrosion-resistant surface properties through systematic composition design and proportion constraints, inclusion modification treatment, heat treatment microstructure control, and surface composite strengthening treatment, meeting the service requirements under harsh working conditions such as mining, ports, and marine engineering.
[0009] To achieve the above objectives, the present invention adopts the following technical solution: The high wear-resistant and corrosion-resistant alloy steel chain provided by this invention comprises the following components by weight percentage: C 0.20-0.26%, Si 0.45-0.70%, Al 0.35-0.65%, Mn 0.70-1.10%, Cr 1.50-2.20%, Mo 0.40-0.65%, Ni 0.60-1.20%, Cu 0.20-0.50%, B 0.0010-0.0025%, N 0.003-0.008%, at least one microalloying element selected from V 0.08-0.15% and Nb 0.025-0.050%, and at least one inclusion-controlling element selected from Ca 0.0015-0.0040% and rare earth RE 0.015-0.035%; the balance being Fe and unavoidable impurities. Of the impurities, P ≤ 0.010%, S ≤ 0.006%, and O ≤ 0.0015%.
[0010] In the above composition design, C is the main strengthening element, controlled within the low to medium carbon range to balance strength and weldability; Si and Al jointly undertake deoxidation and solid solution strengthening functions; Mn, Cr, Mo, and Ni synergistically improve hardenability and tempering stability, among which Cr can also improve corrosion resistance and nitriding layer performance, Mo can suppress temper brittleness, and Ni can improve low-temperature toughness; Cu can improve corrosion resistance in atmospheric and seawater environments; trace amounts of B significantly improve hardenability through grain boundary segregation; N forms nitrides and carbonitrides with Al, V, Nb, etc., playing a role in grain refinement and precipitation strengthening, while protecting the effectiveness of B.
[0011] The microalloying elements V and Nb are the key elements for precipitation strengthening in this invention. V precipitates in the form of nanoscale VC during tempering, producing a significant secondary hardening effect; Nb mainly exists in the form of NbC in austenite, inhibiting grain growth by pinning grain boundaries; the combined addition of V and Nb can achieve both grain refinement strengthening and precipitation strengthening.
[0012] Ca and RE are key elements for inclusion morphology control in this invention. Ca can transform Al2O3 into low-melting-point calcium aluminate and MnS into (Ca,Mn)S complex sulfides; RE has a strong affinity for oxygen and sulfur, and can generate spherical rare earth oxysulfides and rare earth sulfides. After modification treatment, the inclusions are spherical or near-spherical, and the stress concentration effect is significantly reduced.
[0013] One of the core innovations of this invention lies in establishing the following proportioning constraint system: (a) Silicon-aluminum ratio constraints: The total mass of Si and Al is 0.85-1.25%, and the Al / Si mass ratio is 0.6-1.2. The total amount of silicon and aluminum determines the deoxidation effect and the degree of solid solution strengthening, while the Al / Si ratio affects the type of oxide inclusions and the performance of the nitriding layer. When the Al / Si ratio is too low, the deoxidation product is mainly SiO2, which is not easily modified by Ca or RE; when the ratio is too high, coarse Al2O3 clusters are easily formed. The ratio range of this invention can obtain easily modifiable calcium aluminate inclusions, while ensuring that the nitriding layer has a good Al-N strengthening effect.
[0014] (b) Nitrogen-Boron Ratio Constraints: The atomic ratio of N to B, N / B, is 1.5-3.0. Nitrogen and boron compete with each other in steel. An appropriate amount of nitrogen can form BN with boron to protect some boron from oxidation, while leaving enough solid-solid boron to agglomerate at the grain boundaries. When the N / B atomic ratio is below 1.5, the protective effect of nitrogen on boron is insufficient, and boron easily combines with oxygen and fails; when it is above 3.0, excessive nitrogen forms too much BN with boron, weakening the grain boundary strengthening effect of boron.
[0015] (c) Vanadium-Carbon Ratio Constraint: When the matrix material contains V, if it does not contain Nb, the mass ratio of V to C is 0.35-0.65; if it also contains Nb, the mass ratio of V to (C-0.129×Nb) is 0.35-0.65, where 0.129 is the ratio of the relative atomic masses of carbon to niobium (i.e., 12.01 / 92.91≈0.129). This constraint is based on the fact that Nb preferentially combines with C to form stable NbC (stoichiometric ratio of 1:1 atomic ratio), and approximately 0.129% of C is consumed for every 1% of Nb. When calculating the V / C ratio, the amount of carbon fixed by Nb needs to be deducted to ensure effective carbon matching of vanadium. When the V / C mass ratio is controlled within the range of 0.35-0.65, it can ensure that an appropriate amount of nano-sized VC is precipitated during tempering to produce a significant secondary hardening effect. When the ratio is below 0.35, the amount of VC precipitated is insufficient, and the secondary hardening effect is not obvious. When the ratio is above 0.65, the excessive V forms coarse carbides or dissolves in the matrix, resulting in a significant decrease in plasticity and toughness.
[0016] Furthermore, the microstructure of the heat-treated matrix material consists of nanoscale MC-type carbides dispersed on a tempered sorbite matrix. These MC-type carbides are VC, NbC, or (V,Nb)C solid solutions with an average particle size of 5-30 nm. The microstructure also contains 3-8% by volume of retained austenite, distributed in a thin film between the original austenite grain boundaries and martensite laths. This thin film of retained austenite can blunt crack tips, hinder crack propagation, and induce martensitic transformation (TRIP effect) through strain, resulting in phase transformation strengthening and significantly improving the fracture toughness of the steel.
[0017] Furthermore, the oxide inclusions in the matrix material are at least one of spherical or near-spherical calcium aluminate and rare earth sulfide, and the equivalent circle diameter of a single oxide inclusion is ≤10μm and the aspect ratio is ≤2.0; the sulfide inclusions are at least one of (Ca,Mn)S composite sulfide and rare earth sulfide that have been modified by calcium and / or rare earth and are distributed in a spindle-shaped or spherical shape.
[0018] Furthermore, the alloy steel chain also includes a composite reinforcing layer formed on the surface of the base material, comprising, from the outside in: a sealing layer (thickness 0.3-1.2 μm), used to seal micropores and microcracks and block the penetration channels of corrosive media; an oxide layer (thickness 0.8-2.5 μm, main phase Fe3O4), serving as a transition layer between the sealing layer and the nitriding layer and providing preliminary corrosion resistance protection; and a nitriding compound layer (thickness 10-20 μm, main phase ε-Fe). 2-3 The hardness of N and / or γ'-Fe4N can reach HV 650-1000, which plays a major role in wear resistance; the nitrided diffusion layer (depth 0.25-0.45mm) is composed of ferrite with dissolved nitrogen and dispersed alloy nitrides, which play a role in hardness gradient transition and supporting the compound layer.
[0019] The present invention also provides a method for preparing the above-mentioned alloy steel chain, comprising the following steps: S1. Smelting: Smelting molten steel and refining it. During the refining stage, Ca and / or rare earth elements (RE) are added to modify inclusions, and the steel billet is then cast. Smelting can be carried out using an electric arc furnace or converter for primary smelting, followed by LF refining and VD or RH vacuum degassing. Calcium is added via wire feeding in the form of calcium-iron alloy or silicon-calcium alloy, and rare earth elements are added in the form of mixed rare earth alloy or rare earth ferrosilicon.
[0020] S2. Forming and Welding: The steel billet is rolled or forged into a bar, and the bar is bent into a chain link and flash butt welded. Further, the end faces of the chain links can be preheated before flash butt welding at a temperature of 150-250℃ to reduce the cooling rate of the heat-affected zone and avoid hardened structures and cold cracks. The preferred process parameters for flash butt welding are: flash speed 0.8-1.5 mm / s, flash allowance 8-15 mm, upsetting speed 30-60 mm / s, and upsetting allowance 4-8 mm.
[0021] S3. Austenitizing treatment: Heat the welded chain links to 900-930℃ and hold for 1.5-2.5 min / mm based on the nominal diameter of the chain links to ensure that carbon and alloying elements are fully dissolved into the austenite.
[0022] S4. Quenching and Isothermal Transformation Treatment: After austenitizing, the chain links are cooled to 200-280℃ in a quenching medium and then transferred to an isothermal furnace at 480-540℃ for isothermal transformation treatment for 0.5-2 hours, followed by air cooling to room temperature. This step employs a combined heat treatment process of "quenching + isothermal transformation": rapid cooling to 200-280℃ in the quenching medium causes some austenite to transform into martensite while retaining some untransformed austenite; then, isothermal treatment is performed in an isothermal furnace, causing partial bainitic transformation of the untransformed austenite, while carbon atoms diffuse into the retained austenite, making it carbon-rich and stable, ultimately remaining in the microstructure as a thin film. Further, the quenching medium is a polyalkylene glycol water-soluble quenching liquid or rapid quenching oil, with the temperature controlled at 40-70℃.
[0023] S5. High-temperature tempering treatment: Tempering temperature 530-580℃, tempering time 1-3h, promotes the precipitation of microalloying elements such as V and Nb in the form of nano-sized MC-type carbides, and produces a secondary hardening effect.
[0024] Furthermore, a microtexturing process can be included between S5 and S6: a pulsed laser is used to fabricate an array of microtextured pits in the wear area where the chain links contact each other, with an equivalent diameter of 50-120 μm, a depth of 12-35 μm, a center-to-center distance between adjacent pits of 150-400 μm, and an area ratio of 10-18%. The microtextured pits can serve as a space for collecting wear debris to prevent three-body wear, and under lubrication conditions, they can also serve as a micro oil pool to store lubricant.
[0025] S6. Plasma nitriding treatment: The nitriding atmosphere is a mixture of N2 and H2, with an N2:H2 volume ratio of 1:3 to 1:1. The nitriding temperature is 460-500℃, and the nitriding time is 5-8 hours. Furthermore, the furnace pressure is 200-600 Pa, the glow discharge voltage is 500-750 V, and the duty cycle is 30-60%.
[0026] S7. Post-oxidation treatment: carried out in an oxidizing atmosphere containing water vapor, at an oxidation temperature of 480-510℃ and an oxidation time of 20-40 min, to form a dense Fe3O4 oxide film on the surface of the nitrided layer.
[0027] S8. Sealing treatment: One of the following methods shall be adopted: (a) Dip into the hydrolysate of γ-aminopropyltriethoxysilane or γ-glycidoxypropyltrimethoxysilane and cure at 100-130℃ for 15-30 min; (b) Dip into the conversion solution containing hexafluorozirconic acid for 2-5 min, wash with water and dry at 80-100℃; (c) Dip into the sol-gel precursor of tetraethyl orthosilicate and epoxy resin and cure at 120-150℃ for 20-40 min.
[0028] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention establishes a triple ratio constraint system of Al / Si ratio, N / B atomic ratio, and V / C mass ratio, achieving synergistic optimization of various properties such as deoxidation effect, inclusion morphology, grain refinement, hardenability, and precipitation strengthening, so that the matrix material maintains high strength while having good plasticity and toughness. At the same time, through calcium and / or rare earth modification treatment, harmful angular Al2O3 and elongated MnS are transformed into spherical or near-spherical composite inclusions, significantly reducing stress concentration effect and improving the fatigue life and corrosion resistance of steel.
[0029] (2) The present invention adopts a composite heat treatment process of "quenching + isothermal transformation + high temperature tempering" to obtain a multiphase structure of "tempered sorbite + nano-sized MC-type carbide + thin film-like retained austenite". The nano-sized MC-type carbide can provide a significant precipitation strengthening effect, and the thin film-like retained austenite can provide additional plasticity and toughness reserves through the TRIP effect, which is conducive to achieving a good match between high strength and high toughness.
[0030] (3) The four-layer composite reinforcement structure of “sealing layer + oxide layer + nitriding compound layer + nitriding diffusion layer” designed in this invention has a clear function and works together. The nitriding layer can provide high hardness and wear resistance, and the oxide layer and sealing layer work together to block corrosion channels, which is beneficial to improve the wear resistance and corrosion resistance of the chain at the same time. The optional micro-texture treatment can further improve the tribological properties, which is beneficial to extend the service life of the chain. Detailed Implementation
[0031] The present invention will be further described below with reference to specific embodiments, but these embodiments are not intended to limit the invention to these specific implementations. Those skilled in the art should recognize that the present invention covers all possible alternatives, improvements, and equivalents included within the scope of the claims. Example 1
[0032] This embodiment provides a highly wear-resistant and corrosion-resistant alloy steel chain, the chemical composition (weight percentage) of its base material is shown in Table 1.
[0033] The preparation method of this embodiment includes the following steps: S1. Smelting: Primary smelting is performed in an electric arc furnace, followed by LF refining and VD vacuum degassing. At the end of LF refining, a silicon-calcium alloy is added via wire feeding to modify inclusions; the calcium addition is controlled at 0.0028% Ca. The resulting steel billet is then cast.
[0034] S2. Forming and Welding: The steel billet is rolled into φ26mm bars, and the bars are bent into chain links. The end faces of the chain links are preheated to 200℃ before flash butt welding. Flash butt welding process parameters: flash speed 1.2mm / s, flash allowance 12mm, upsetting speed 45mm / s, upsetting allowance 6mm.
[0035] S3. Austenitizing treatment: Heat the welded chain links to 915℃ and hold for 52 minutes (calculated at 2.0 min / mm).
[0036] S4. Quenching and Isothermal Transformation Treatment: After the austenitized chain segments are cooled to 240°C in a polyalkylene glycol water-soluble quenching liquid (temperature 55°C), they are taken out and immediately transferred to an isothermal furnace at 510°C for isothermal transformation treatment for 1 hour, and then air-cooled to room temperature.
[0037] S5. High-temperature tempering treatment: tempering temperature 555℃, tempering time 2h.
[0038] S6. Plasma nitriding treatment: The nitriding atmosphere is a mixture of N2 and H2, with a N2:H2 volume ratio of 1:2. The nitriding temperature is 480℃, the nitriding time is 6.5h, the furnace pressure is 400Pa, the glow discharge voltage is 620V, and the duty cycle is 45%.
[0039] S7. Post-oxidation treatment: carried out in an oxidizing atmosphere containing water vapor, at an oxidation temperature of 495℃ and an oxidation time of 30min.
[0040] S8. Sealing treatment: Dip in γ-aminopropyltriethoxysilane hydrolysate and cure at 115℃ for 22 min.
[0041] TEM characterization showed that the MC-type carbides in Example 1 had an average particle size of about 15 nm and were diffusely distributed on the tempered sorbite matrix. Example 2
[0042] The difference between this embodiment and Embodiment 1 is that the matrix material does not contain Nb, but only contains 0.12% V, with a V / C mass ratio of 0.52. The remaining components and process parameters are the same as in Embodiment 1. Example 3
[0043] The difference between this embodiment and Embodiment 1 is that the matrix material contains no V, only 0.038% Nb. Because it contains no V, the proportioning constraint (c) is not applicable. The remaining components and process parameters are the same as in Embodiment 1. Example 4
[0044] This embodiment provides a highly wear-resistant and corrosion-resistant alloy steel chain. The chemical composition of its matrix material is close to the lower limit of each element's range, as shown in Table 1. The mass ratio of V / (C-0.129×Nb) is 0.41, the total amount of Si+Al is 0.86%, the Al / Si ratio is 0.78, and the N / B atomic ratio is 1.6.
[0045] The process parameters in the preparation method are as follows: austenitizing temperature 900℃, holding time calculated at 1.5 min / mm; after quenching, cooling to 280℃ and removing, isothermal temperature 480℃, isothermal time 0.5 h; tempering temperature 530℃, tempering time 1 h; nitriding temperature 460℃, nitriding time 5 h; post-oxidation temperature 480℃, oxidation time 20 min. Sealing treatment is performed using method (b), immersing in a conversion solution containing hexafluorozirconic acid for 3 min, followed by washing with water and drying at 90℃. Example 5
[0046] This embodiment provides a highly wear-resistant and corrosion-resistant alloy steel chain. The chemical composition of its matrix material is close to the upper limit of each element range, as shown in Table 1. The mass ratio of V / (C-0.129×Nb) is 0.59, the total amount of Si+Al is 1.23%, the Al / Si ratio is 0.81, and the N / B atomic ratio is 2.8.
[0047] The process parameters in the preparation method are as follows: austenitizing temperature 930℃, holding time calculated at 2.5 min / mm; after quenching, cooling to 200℃ and removing, isothermal temperature 540℃, isothermal time 2h; tempering temperature 580℃, tempering time 3h; nitriding temperature 500℃, nitriding time 8h; post-oxidation temperature 510℃, oxidation time 40min. The sealing treatment uses method (c), impregnating with a sol-gel precursor blend of tetraethyl orthosilicate and epoxy resin, curing at 135℃ for 30min. Example 6
[0048] The difference between this embodiment and Embodiment 1 is that rare earth element (RE) is used instead of Ca in the inclusion modification treatment, and a mixed rare earth alloy is added at the end of LF refining, with the amount of rare earth added controlled at 0.025% RE. The remaining components and process parameters are the same as in Embodiment 1. Example 7
[0049] The difference between this embodiment and Embodiment 1 is that a microtexturing process is added between S5 and S6. A pulsed laser (wavelength 1064nm, pulse width 100ns, frequency 20kHz) is used to process an array of microtextured pits in the wear area where the chain links contact each other. The equivalent diameter of the pits is 85μm, the depth is 22μm, the center-to-center distance between adjacent pits is 200μm, and the area ratio is 14%. The remaining components and process parameters are the same as in Embodiment 1. Comparative Example 1
[0050] The difference between this comparative example and Example 2 is that the V content is 0.15%, the C content is 0.20%, and the V / C mass ratio is approximately 0.75, which exceeds the 0.35-0.65 range defined in this invention. The remaining components and process parameters are the same as in Example 2. Comparative Example 2
[0051] The difference between this comparative example and Example 1 is that the N content is 0.008%, the B content is 0.0010%, and the N / B atomic ratio is approximately 6.2, which exceeds the 1.5-3.0 range defined in this invention. The remaining components and process parameters are the same as in Example 1. Comparative Example 3
[0052] The difference between this comparative example and Example 1 is that the Si content is 0.70%, the Al content is 0.65%, and the total Si+Al content is 1.35%, which exceeds the 0.85-1.25% range defined in this invention; the Al / Si ratio is 0.93, which is within the range defined in this invention. The remaining components and process parameters are the same as in Example 1. Comparative Example 4
[0053] The difference between this comparative example and Example 1 is that steps S6, S7, and S8 are omitted, i.e., plasma nitriding, post-oxidation, and sealing treatment are not performed. The remaining components and process parameters are the same as in Example 1. Comparative Example 5
[0054] The difference between this comparative example and Example 1 is that no Ca or rare earth element RE is added during the smelting process to modify inclusions. All other components and process parameters are the same as in Example 1. Comparative Example 6
[0055] The difference between this comparative example and Example 1 is that step S4 uses a conventional quenching process, where the austenitized chain links are directly cooled to room temperature in the quenching liquid without isothermal transformation treatment. The remaining components and process parameters are the same as in Example 1. Comparative Example 7
[0056] This comparative example uses the composition system of the commonly used grade 23MnNiMoCr54 in existing technology: C 0.21-0.25%, Si 0.15-0.30%, Mn 1.20-1.40%, Cr 0.40-0.60%, Ni 0.40-0.60%, Mo 0.40-0.50%, with the balance being Fe. Conventional quenching and tempering processes (quenching + high-temperature tempering) are employed, without surface composite strengthening treatment. Comparative Example 8
[0057] The difference between this comparative example and Example 1 is that the Si content is 0.45%, the Al content is 0.65%, and the total Si+Al content is 1.10% (within the range of 0.85-1.25%), but the Al / Si ratio is 1.44, which exceeds the 0.6-1.2 range specified in this invention. The remaining components and process parameters are the same as in Example 1. Performance testing
[0058] The sample preparation and sampling methods for the embodiments and comparative examples of this invention are described below: (1) Mechanical property test specimens (tensile, impact) and matrix hardness test specimens: taken from the chain link body after S5 high temperature tempering treatment (avoiding the weld area), and processed into standard test specimens according to the corresponding standards. (2) Residual austenite content and nano carbide characterization sample: The sample was taken from the chain segment body after high temperature tempering of S5. The XRD sample was tested after removing the surface decarburized layer by mechanical grinding. The TEM sample was prepared by double spray electrolytic thinning method. (3) Nitriding layer performance (surface hardness, layer depth), corrosion resistance (salt spray test), and wear resistance test samples: taken from the surface of the finished chain links after S8 sealing treatment. For Comparative Examples 4 and 7, which did not undergo S6-S8 surface treatment, their corrosion resistance and wear resistance test samples were taken from the surface of the chain links after the corresponding processes were completed.
[0059] The testing methods used in the embodiments and comparative examples of this invention are as follows: (1) Mechanical property test: tensile strength, yield strength and elongation after fracture were tested according to GB / T 228.1-2021 "Metallic materials tensile test - Part 1: test method at room temperature"; room temperature impact energy was tested according to GB / T 229-2020 "Metallic materials Charpy pendulum impact test method" and the specimen was a standard V-notch specimen of 10mm×10mm×55mm.
[0060] (2) Hardness test: The hardness of the matrix was tested according to GB / T 230.1-2018 "Metallic materials Rockwell hardness test Part 1: Test method"; the surface hardness and hardness gradient of the nitrided layer were tested according to GB / T 4340.1-2024 "Metallic materials Vickers hardness test Part 1: Test method", with a load of 0.98N (HV0.1).
[0061] (3) Nitriding layer depth test: The test shall be carried out in accordance with GB / T 11354-2005 "Determination of nitriding layer depth and metallographic structure inspection of steel parts" and the effective nitriding layer depth shall be determined by the hardness gradient method (up to the matrix hardness +50HV).
[0062] (4) Residual austenite content test: The test shall be conducted in accordance with the X-ray diffraction method for quantitative determination of residual austenite in steel.
[0063] (5) Inclusion rating: Rating shall be carried out in accordance with GB / T 10561-2023 "Standard rating chart microscopic test method for determination of non-metallic inclusion content in steel".
[0064] (6) Corrosion resistance test: The neutral salt spray test shall be conducted in accordance with GB / T 10125-2021 “Artificial Atmosphere Corrosion Test Salt Spray Test”, and the time when red rust appears shall be recorded.
[0065] (7) Wear resistance test: The test ring-block sliding wear test was conducted according to GB / T 12444-2006 "Test Methods for Wear of Metallic Materials - Test Ring-Block Sliding Wear Test". Test conditions: The test ring material was GCr15 steel (hardness 60HRC), the test block was taken from the surface of the chain link (after S8 treatment), the load was 100N, the test ring speed was 200r / min, the test time was 2h, and the wear amount was determined by the mass loss method. The test was conducted under unlubricated (dry friction) conditions.
[0066] The chemical composition (weight percentage) of the matrix materials for each embodiment and comparative example is shown in Table 1.
[0067] Table 1. Chemical composition (wt%) of each example and comparative example: .
[0068] Note: "-" in the table indicates that the element was not added; in each embodiment and comparative example, P≤0.008%, S≤0.005%, O≤0.0012%, and the balance is Fe.
[0069] The proportioning parameters for each embodiment and comparative example are shown in Table 2.
[0070] Table 2. Proportioning parameters for each embodiment and comparative example: .
[0071] Performance test results The performance test results of each embodiment and comparative example are shown in Tables 3 and 4.
[0072] Table 3 Mechanical properties and hardness tests of each embodiment and comparative example: .
[0073] Table 4. Surface properties and corrosion and wear resistance of each embodiment and comparative example: .
[0074] Note: Comparative Examples 4 and 7 were not surface treated, therefore no data related to the nitriding layer is available.
[0075] Results Analysis As can be seen from the test results in Tables 3 and 4, the present invention has significant comprehensive performance advantages compared with the prior art. Comparative Example 7, using the traditional grade 23MnNiMoCr54 and conventional quenching and tempering process, showed tensile strength, impact energy, and time to red rust appearance in the salt spray test of 1085 MPa, 52 J, and 36 h, respectively. In contrast, Example 1 showed corresponding values of 1280 MPa, 72 J, and 528 h, representing improvements of 18%, 38%, and approximately 15 times, respectively. This difference stems from the proportioning constraint system established in this invention: the V / C ratio of Comparative Example 1 exceeded the limit, resulting in an impact energy reduction to 42 J; the N / B atomic ratio of Comparative Example 2 exceeded the limit, reducing the yield strength to 1020 MPa; and the total Si+Al content of Comparative Example 3 and the Al / Si ratio of Comparative Example 8 both exceeded the limit, leading to a deterioration in inclusion rating to Class B, grade 1.5. These results indicate that the various constraints in the proportioning constraint system are independent yet synergistic, indispensable for ensuring the matching of matrix strength and toughness and controlling inclusion morphology.
[0076] Regarding the selection of microalloying elements and processes, Example 1 used a composite addition of V and Nb, which exhibited superior strength and toughness compared to Example 2 (1255 MPa / 68 J) and Example 3 (1215 MPa / 75 J) with V added alone, balancing the secondary hardening effect of V with the grain boundary pinning effect of Nb. Process verification showed that Comparative Example 6, using conventional quenching omitting isothermal transformation treatment, had a residual austenite content of only 1.5 vol%, and its impact energy decreased to 45 J; Comparative Example 5, without Ca / RE modification treatment, suffered a deterioration in inclusion rating to Class B coarse series 2.0, and its impact energy decreased to 55 J. Therefore, isothermal transformation and inclusion modification treatment play a crucial role in obtaining ideal multiphase microstructure and inclusion morphology.
[0077] Regarding surface strengthening, Comparative Example 4, without composite strengthening treatment, showed red rust in just 48 hours and wear of 85.5 mg in the salt spray test, while Example 1 showed wear of 528 hours and 12.5 mg, respectively. Corrosion resistance and wear resistance were improved by approximately 10 times and 6 times, respectively, fully demonstrating the effectiveness of the four-layer composite structure of "sealing layer + oxide layer + nitriding compound layer + nitriding diffusion layer". Example 7, based on this, added microtextured treatment, further reducing wear to 8.5 mg, a 32% reduction compared to Example 1. This indicates that microtextured pits can effectively improve tribological properties and further extend the chain's service life.
[0078] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A highly wear-resistant and corrosion-resistant alloy steel chain, characterized in that, The base material of the alloy steel chain comprises the following components by weight percentage: C 0.20-0.26%, Si 0.45-0.70%, Al 0.35-0.65%, Mn 0.70-1.10%, Cr 1.50-2.20%, Mo 0.40-0.65%, Ni 0.60-1.20%, Cu 0.20-0.50%, B 0.0010-0.0025%, N 0.003-0.008%, at least one microalloying element selected from V 0.08-0.15% and Nb 0.025-0.050%, and at least one inclusion-controlling element selected from Ca 0.0015-0.0040% and rare earth RE 0.015-0.035%; the balance being Fe and impurities; Of the impurities, P ≤ 0.010%, S ≤ 0.006%, and O ≤ 0.0015%; The matrix material satisfies the following proportioning constraints: (a) The total mass of Si and Al is 0.85-1.25%, and the mass ratio of Al / Si is 0.6-1.2; (b) The atomic ratio of N to B, N / B, is 1.5-3.0; (c) When the matrix material contains V: if it does not contain Nb, the mass ratio of V to C is 0.35-0.65; if it contains Nb, the mass ratio of V to (C-0.129×Nb) is 0.35-0.
65.
2. The alloy steel chain according to claim 1, characterized in that, The microstructure of the matrix material after heat treatment is a tempered sorbite matrix with dispersed nano-sized MC-type carbides, which are VC, NbC or (V,Nb)C solid solutions with an average particle size of 5-30 nm. The microstructure also contains 3-8% retained austenite by volume, which is distributed in a thin film between the original austenite grain boundaries and martensite laths.
3. The alloy steel chain according to claim 1, characterized in that, The oxide inclusions in the matrix material are at least one of spherical or near-spherical calcium aluminate and rare earth sulfide, with the equivalent circle diameter of a single oxide inclusion ≤10μm and the aspect ratio ≤2.0; the sulfide inclusions are at least one of (Ca,Mn)S composite sulfide and rare earth sulfide that have been modified by calcium and / or rare earth and are distributed in a spindle-shaped or spherical shape.
4. The alloy steel chain according to claim 1, characterized in that, The alloy steel chain further includes a composite reinforcing layer formed on the surface of the base material, which, from the outside to the inside, comprises: a sealing layer with a thickness of 0.3-1.2 μm; an oxide layer with a thickness of 0.8-2.5 μm and Fe3O4 as the main phase; and a nitriding compound layer with a thickness of 10-20 μm and ε-Fe as the main phase. 2-3 At least one of N and γ'-Fe4N; a nitriding diffusion layer with a depth of 0.25-0.45 mm.
5. A method for preparing a high wear-resistant and corrosion-resistant alloy steel chain as described in any one of claims 1-4, characterized in that, Includes the following steps: S1. Smelting: Smelting molten steel and refining it. During the refining stage, Ca and / or rare earth RE are added to modify inclusions and then cast to obtain steel billets. S2. Forming and Welding: The steel billet is rolled or forged into a bar, the bar is bent into a chain link and flash butt welded. S3. Austenitizing treatment: Heat the welded chain links to the austenitizing temperature of 900-930℃, and hold for 1.5-2.5 min / mm based on the nominal diameter of the chain links; S4. Quenching and isothermal transformation treatment: After the austenitized chain links are cooled to 200-280℃ in the quenching medium, they are taken out and immediately transferred to an isothermal furnace at 480-540℃ for isothermal transformation treatment for 0.5-2 hours, and then air-cooled to room temperature. S5. High-temperature tempering treatment: The links treated with S4 are subjected to high-temperature tempering at a temperature of 530-580℃ for 1-3 hours. S6. Plasma nitriding treatment: The tempered chain links are subjected to plasma nitriding treatment. The nitriding atmosphere is a mixture of N2 and H2, and the N2:H2 volume ratio is 1:3 to 1:
1. The nitriding temperature is 460-500℃ and the nitriding time is 5-8h. S7. Post-oxidation treatment: The nitrided chain segments are subjected to post-oxidation treatment in an oxidizing atmosphere containing water vapor. The oxidation temperature is 480-510℃ and the oxidation time is 20-40min. S8. Sealing treatment: The oxidized chain segments are sealed to obtain the high wear-resistant and corrosion-resistant alloy steel chain.
6. The preparation method according to claim 5, characterized in that, The quenching medium in S4 is a polyalkylene glycol water-soluble quenching liquid or a rapid quenching oil, and the temperature of the quenching medium is controlled at 40-70℃.
7. The preparation method according to claim 5, characterized in that, The process parameters for plasma nitriding treatment in S6 also include: furnace pressure of 200-600 Pa, glow discharge voltage of 500-750 V, and duty cycle of 30-60%.
8. The preparation method according to claim 5, characterized in that, The sealing process in S8 adopts one of the following methods: (a) Dip in the hydrolysate of γ-aminopropyltriethoxysilane or γ-glycidoxypropyltrimethoxysilane, with a curing temperature of 100-130℃ and a curing time of 15-30 min; (b) Immerse in a conversion solution containing hexafluorozirconic acid for 2-5 minutes, wash with water, and dry at 80-100℃; (c) Dip in a sol-gel precursor of tetraethyl orthosilicate and epoxy resin and cure at 120-150℃ for 20-40 min.
9. The preparation method according to claim 5, characterized in that, Between S5 and S6, a microtexturing process is also included: a pulsed laser is used to process an array of microtextured pits in the wear area where the chain links of the chain contact each other. The equivalent diameter of the microtextured pits is 50-120μm, the depth is 12-35μm, the center-to-center distance between adjacent pits is 150-400μm, and the area ratio of the microtextured pits in the contact area is 10-18%.
10. The preparation method according to claim 5, characterized in that, In step S2, the end face of the chain link is preheated before flash butt welding at a temperature of 150-250℃. The process parameters for flash butt welding include: flash speed of 0.8-1.5 mm / s, flash allowance of 8-15 mm, upsetting speed of 30-60 mm / s, and upsetting allowance of 4-8 mm.