A method for preparing high-purity quartz sand by ultraviolet light complexation

By treating quartz sand with ultraviolet light complexation, combined with complexing leaching agents and mild chemical conditions, the problem of poor impurity removal in existing technologies has been solved, achieving efficient preparation of high-purity quartz sand, reducing energy consumption and waste liquid treatment difficulty, and making it suitable for high-end applications such as semiconductors and photovoltaics.

CN122212153BActive Publication Date: 2026-11-10SHANDONG KELUTE NEW MATERIAL TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610443363.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-04-07
Publication Date
2026-11-10
Estimated Expiration
2046-04-07

AI Technical Summary

Technical Problem

Existing technologies are unable to effectively remove impurities such as titanium from quartz sand, resulting in high-purity quartz sand that cannot meet the requirements of high-end applications. Furthermore, existing processes are energy-intensive and difficult to treat waste liquid.

Method used

The ultraviolet complexation method involves adding a complexing leaching agent to quartz particles, stirring them under ultraviolet light, and then performing leaching under mild chemical conditions and gas introduction. The particles are then separated, washed, and finally dried to obtain high-purity quartz sand.

Benefits of technology

It effectively removes impurities such as Ti, Fe, Al, Na, and K from quartz sand, meeting the needs of high-end fields. The process conditions are mild, reducing energy consumption and the difficulty of waste liquid treatment, and it has advantages for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122212153B_ABST
    Figure CN122212153B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing high-purity quartz sand using ultraviolet (UV) light complexation, belonging to the field of high-purity quartz materials. The method includes the following steps: crushing and sieving quartz raw materials to obtain quartz particles; performing preliminary purification on the quartz particles; placing the preliminarily purified quartz particles in a reactor, adding a complexing leaching agent to the reactor, irradiating the mixture with UV light, and stirring the mixture; separating the mixture after UV complexation leaching to obtain post-leaching quartz particles; washing the post-leaching quartz particles with deionized water; and dehydrating and drying the washed quartz particles to obtain high-purity quartz sand. This invention utilizes the synergistic effect of UV light and a complexing agent to extract quartz particles, effectively removing impurities from quartz and meeting the application requirements of high-end fields such as semiconductors and photovoltaics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-purity quartz materials, and in particular to a method for preparing high-purity quartz sand by ultraviolet light complexation. Background Technology

[0002] High-purity silica sand is a fundamental material for strategic emerging industries such as semiconductors, photovoltaics, optical fiber communication, and high-end optics. With the continuous evolution of integrated circuit manufacturing processes and the rapid development of the photovoltaic industry, the requirements for the purity of silica sand are increasing day by day.

[0003] Currently, the preparation of high-purity quartz sand mainly relies on quartz raw material purification routes. Its core processes include physical beneficiation methods such as magnetic separation, flotation, and gravity separation, as well as chemical treatment methods such as calcination, acid leaching, and chlorination roasting. However, existing technologies are still not ideal in removing certain impurities, especially titanium impurities, which have become a key bottleneck restricting the improvement of high-purity quartz sand purity. Conventional magnetic separation-flotation processes have limited impurity removal rates, and the slow dissolution kinetics of titanium during acid leaching result in titanium content in the final product often ranging from 0.5 to 5 ppm, which is insufficient to meet the demands of high-end applications.

[0004] In recent years, researchers have attempted to improve the removal rate of titanium by employing enhanced methods such as pressurized acid leaching and high-temperature chlorination. For example, they have optimized processes such as sorting, leaching, and calcination to remove impurity elements; and used segmented vacuum heat treatment technology to remove impurities and hydroxyl groups. However, these methods are energy-intensive and their removal effect on lattice titanium remains unsatisfactory. Summary of the Invention

[0005] This invention provides a method for preparing high-purity quartz sand by ultraviolet light complexation, which overcomes the shortcomings of existing technologies such as poor impurity removal and poor process stability, and ensures the purity of quartz sand.

[0006] The method for preparing high-purity quartz sand by ultraviolet light complexation includes the following steps:

[0007] Step S1: Crush and sieve the quartz raw material to obtain quartz particles;

[0008] Step S2: Perform preliminary purification on the quartz particles;

[0009] Step S3: Place the pre-purified quartz particles in a reactor, add a complexing leaching agent to the reactor, irradiate the mixture in the reactor with ultraviolet light, and stir the mixture.

[0010] Step S4: Separate the mixed system after ultraviolet light complexation leaching to obtain post-leaching treated quartz particles;

[0011] Step S5: Wash the post-immersion treated quartz particles with deionized water.

[0012] Step S6: Dehydrate and dry the washed quartz particles to obtain high-purity quartz sand.

[0013] According to the aforementioned method for preparing high-purity quartz sand by ultraviolet light complexation, the preliminary purification in step S2 includes one or more of the following: desliming, scrubbing, ball milling, gravity separation, and magnetic separation.

[0014] Furthermore, the initial purification method for S2 is magnetic separation with a magnetic field strength of 1.5~2.5T.

[0015] According to the aforementioned method for preparing high-purity quartz sand by ultraviolet light complexation, the complexing leaching agent in step S3 is a mixed solution including a complexing agent and an oxidizing agent.

[0016] The complexing agent is selected from one or more of oxalic acid, citric acid, EDTA, and DTPA, and the amount added is 7% to 20% of the mass of the quartz sand.

[0017] The oxidant is selected from one or more of hydrogen peroxide, sodium persulfate, and peracetic acid, and the amount added is 1% to 3.5% of the mass of the quartz sand.

[0018] The pH of the mixed solution should be controlled between 2 and 4.

[0019] According to the aforementioned method for preparing high-purity quartz sand by ultraviolet light complexation, in step S3, the leaching temperature is 60~95℃, the leaching time is 2~8 hours, the ultraviolet light wavelength is 254~365nm, and the light intensity is 500~3000μW / cm².

[0020] According to the aforementioned method for preparing high-purity quartz sand by ultraviolet light complexation, during the leaching process in step S3, air or oxygen is introduced into the reactor at a flow rate of 0.1~1.0 L / min.

[0021] According to the aforementioned method for preparing high-purity quartz sand by ultraviolet light complexation, the solid-liquid separation in step S4 is achieved through one or more combinations of centrifugal separation or natural sedimentation filtration.

[0022] According to the aforementioned method for preparing high-purity quartz sand by ultraviolet light complexation, the step between S4 and S5 further includes:

[0023] Step S7, Ultrasonic treatment: Place the quartz particles that have undergone the immersion treatment in step S4 into a 0.01~0.05mol / L hydrofluoric acid solution and clean them for 10~30 minutes under the action of ultrasonic waves at 40~80kHz.

[0024] According to the aforementioned method for preparing high-purity quartz sand by ultraviolet light complexation, step S6 involves centrifugal dehydration, which is performed using a high-speed rotary drum centrifuge.

[0025] Alternatively, high-temperature dehydration can be used, drying at 100~150℃.

[0026] Furthermore, the reactor includes:

[0027] A reaction vessel containing quartz particles and a complexing leaching agent in its inner cavity;

[0028] The ultraviolet lamp is partially inserted into the inner cavity of the reaction vessel and partially connected to the control device outside the reaction vessel.

[0029] The stirring paddle is partially inserted into the inner cavity of the reaction vessel and partially connected to a rotation source outside the reaction vessel.

[0030] A heating jacket is fitted over the outer wall of the reaction vessel;

[0031] The feed pipe has one end located outside the reaction vessel and the other end inserted into the inner cavity of the reaction vessel;

[0032] The exhaust port is located at the top of the reaction vessel;

[0033] The discharge port is located at the bottom of the reaction vessel; and

[0034] A vent pipe, one end of which is connected to an air or oxygen source, and the other end is inserted from the top of the reaction vessel and extends to the bottom of the inner cavity of the reaction vessel.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) This invention uses the synergistic effect of ultraviolet light and complexing agent to extract quartz particles, effectively removing impurity elements such as Ti, Fe, Al, Na, and K from quartz, thus meeting the needs of high-end fields such as semiconductors and photovoltaics.

[0037] (2) The process conditions of this invention are mild, with a leaching temperature of 60~95℃ and normal pressure operation. It does not require special equipment such as high pressure kettles and high temperature roasting furnaces, resulting in low investment costs and low operating energy consumption. Compared with high temperature chlorination process, this invention has greater advantages for industrial application.

[0038] (3) The present invention uses weak acid conditions during extraction, which makes waste liquid treatment easier and produces no highly corrosive wastewater; the complexing agent can be partially recycled and reused, reducing reagent consumption and environmental pollution, which is different from the problems of difficult waste liquid treatment and serious pollution in some existing processes. Attached Figure Description

[0039] Figure 1 A flowchart of a method for preparing high-purity quartz sand by ultraviolet light complexation;

[0040] Figure 2 This is a schematic diagram of the reactor structure.

[0041] Explanation of reference numerals in the attached figures:

[0042] 1. Reaction vessel; 2. Ultraviolet lamp; 3. Stirring paddle; 4. Rotary source; 5. Heating jacket; 6. Feed pipe; 7. Exhaust port; 8. Discharge port; 9. Vent pipe. Detailed Implementation

[0043] To make the technical problem to be solved, the technical solution and advantages of the present invention clearer, the following description will be provided in conjunction with the accompanying drawings. Figure 1 and Figure 2 The technical solution of the present invention will be clearly and completely described in conjunction with specific embodiments.

[0044] Figure 1 The flowchart illustrates a method for preparing high-purity quartz sand using ultraviolet (UV) photocomplexation. The method includes the following steps:

[0045] Step S1: Crush and sieve the quartz raw material to obtain quartz particles. The specific particle size of the quartz particles is 50~300μm.

[0046] Step S2: The quartz particles obtained in step S1 are subjected to preliminary purification. Preliminary purification includes one or more of the following: desliming, scrubbing, ball milling, gravity separation, and magnetic separation. When using magnetic separation, the magnetic field strength is 1.5~2.5T to remove strongly magnetic minerals.

[0047] Step S3: Place the pre-purified quartz particles in a reactor, add a complexing leaching agent, irradiate the mixture with ultraviolet light, and stir the mixture. The leaching temperature is 60-95℃, the leaching time is 2-8 hours, the ultraviolet wavelength is 254-365nm, and the light intensity is 500-3000μW / cm². The complexing leaching agent is a mixed solution including a complexing agent and an oxidizing agent. The complexing agent is selected from one or more of oxalic acid, citric acid, EDTA, and DTPA, and the amount added is 7%-20% of the quartz sand mass. The oxidizing agent is selected from one or more of hydrogen peroxide, sodium persulfate, and peracetic acid, and the amount added is 1%-3.5% of the quartz sand mass. The pH of the mixed solution is controlled at 2-4.

[0048] Step S4: Separate the mixture system after UV complexation leaching in step S3 to obtain post-leaching treated quartz particles. Solid-liquid separation is achieved through one or more combinations of centrifugal separation or natural sedimentation filtration. This rapidly achieves complete separation of the quartz sand solid phase and the complexation leachate liquid phase. The separated complexation leachate, after filtration and concentration adjustment with added reagents, can be recycled for the next batch of leaching, reducing reagent consumption.

[0049] Step S5: Wash the post-immersion treated quartz particles with deionized water. Wash the quartz particles with deionized water until neutral (conductivity less than 2 μS / cm).

[0050] Step S6: Dehydrate and dry the quartz particles cleaned in step S5 to obtain high-purity quartz sand. Centrifugal dehydration is performed using a high-speed rotary drum centrifuge; or, high-temperature dehydration is performed by drying at 100~150℃.

[0051] Optionally, in step S3, during the leaching process, air or oxygen is introduced into the reactor at a flow rate of 0.1~1.0 L / min to enhance the oxidation effect.

[0052] Optionally, the following may be included between step S4 and step S5:

[0053] Step S7, Ultrasonic Treatment: Place the quartz particles treated in Step S4 into a 0.01~0.05mol / L hydrofluoric acid solution and clean them for 10~30 minutes under ultrasonic waves at 40~80kHz. Ultrasonic treatment removes the complex products and reaction residues adsorbed on the surface of the quartz particles, preventing secondary adsorption of impurities and further improving product purity.

[0054] The present invention provides specific embodiments and comparative examples as follows, and all chemical reagents used are commercially available.

[0055] Example 1:

[0056] Step S1: Take quartz raw material, and crush it in a jaw crusher for coarse crushing, a double roll crusher for medium crushing, and a vibrating screen to obtain quartz particles with a particle size of 100~200μm. The inner lining of the crushing equipment is made of high-purity corundum material to avoid iron contamination.

[0057] Step S2: The sieved quartz particles are passed through a periodic high gradient magnetic separator with a magnetic field strength of 2.0T, a magnetic separation medium of steel wool, and a flow rate of 0.5 cm / s. The magnetic separation is performed twice to remove magnetic minerals such as ilmenite and magnetite.

[0058] Step S3: Take 500g of magnetically separated quartz particles and place them in a reactor. Add 1000mL of complexing leaching agent to the reactor, irradiate the mixture with ultraviolet light, and stir the mixture. The ultraviolet wavelength is 254nm, the light intensity of the ultraviolet lamp is 1500μW / cm², and the stirring speed is 300 rpm. The complexing leaching agent composition is: oxalic acid added at 12% of the quartz sand mass, citric acid added at 8% of the quartz sand mass, and hydrogen peroxide added at 2% of the quartz sand mass. Adjust the pH to 3.5 with dilute hydrochloric acid. Control the leaching temperature at 80℃ and leach at this constant temperature for 4 hours.

[0059] Step S4: After the ultraviolet light complexation leaching in step S3 is completed, the mixture system is separated by natural sedimentation filtration to obtain post-leaching treated quartz particles.

[0060] Step S5: Wash the post-immersion treated quartz particles with deionized water. Wash the quartz particles with deionized water until neutral (conductivity less than 2 μS / cm).

[0061] Step S6: Dry the quartz particles washed with deionized water in an oven at 120°C for 4 hours to obtain high-purity quartz sand.

[0062] The reactor used in step S3 is as follows: Figure 2 As shown, the reactor includes a reaction vessel 1, an ultraviolet lamp 2, a stirring paddle 3, a heating jacket 5, a feed pipe 6, an exhaust port 7, a discharge port 8, and a vent pipe 9.

[0063] The inner cavity of reaction vessel 1 contains quartz particles and a complexing leaching agent. It is made of high-transmittance ultraviolet-light quartz glass, cylindrical in shape, 30cm high, 20cm inner diameter, and 1cm wall thickness. A portion of the ultraviolet lamp 2 is inserted into the inner cavity of reaction vessel 1, while the other portion is connected to an external control device. The bottom of the ultraviolet lamp 2 is 5cm from the bottom of the reactor to ensure uniform illumination of the entire reaction system. A protective sleeve is fitted around the ultraviolet lamp 2 to protect it from direct contact with the complexing leaching agent and prevent corrosion. A stirring paddle 3 is installed outside the protective sleeve of the ultraviolet lamp. Made of polytetrafluoroethylene (PTFE), it is highly corrosion-resistant and prevents the introduction of impurities. The blades of the stirring paddle 3 are 3-5cm from the bottom of the inner cavity of reaction vessel 1, and the stirring speed is adjustable from 100 to 500 rpm. A portion of the stirring paddle 3 is inserted into the inner cavity of reaction vessel 1, while the other portion is connected to a rotation source 4 external to reaction vessel 1. The rotation source 4 can be any device capable of outputting rotation, such as a motor, engine, hydraulic motor, or a combination of one of these with a reducer. A heating jacket 5 is fitted onto the outer wall of the reaction vessel 1. The heating jacket 5 is a water bath heating jacket, with adjustable heating temperature from 60 to 95℃ and a constant temperature accuracy of ±2℃. It is used to maintain a stable temperature during the leaching process and ensure smooth reaction. One end of the feed pipe 6 is located outside the reaction vessel 1, and the other end is inserted into the inner cavity of the reaction vessel 1. It is used to add quartz particles and complexing leaching agent into the inner cavity of the reaction vessel 1. The exhaust port 7 is located at the top of the reaction vessel 1 to discharge gases generated during the reaction and excess gases introduced. The discharge port is located at the bottom of the reaction vessel 1 to discharge the leached material. One end of the vent pipe 9 is connected to an air or oxygen source, and the other end is inserted from the top of the reaction vessel 1 and extends to the bottom of the inner cavity of the reaction vessel 1. The vent pipe 9 is made of polytetrafluoroethylene, has a diameter of 1cm, and its outlet is 2cm from the bottom. Air or oxygen is introduced into the bottom of the inner cavity of the reaction vessel 1 through the vent pipe 9.

[0064] Example 2:

[0065] The difference from Example 1 is that in step S3, air is introduced into the reactor during the leaching process at a rate of 0.3 L / min; otherwise, it is completely consistent with Example 1.

[0066] Example 3:

[0067] The difference from Example 1 is that in step S3, oxygen is introduced into the reactor during the leaching process at a rate of 0.3 L / min; otherwise, it is completely consistent with Example 1.

[0068] Example 4:

[0069] The difference from Example 1 is that: between step S4 and step S5, the following is also included:

[0070] Step S7, Ultrasonic Treatment: Place the quartz particles that have undergone the immersion treatment in step S4 into a 0.02 mol / L hydrofluoric acid solution and clean them for 15 minutes under the action of 60 kHz ultrasound.

[0071] Example 5:

[0072] The difference from Example 1 is that in step S3, air is introduced into the reactor during the leaching process at a rate of 0.3 L / min; otherwise, it is completely consistent with Example 1.

[0073] The interval between steps S4 and S5 also includes:

[0074] Step S7, Ultrasonic Treatment: Place the quartz particles that have undergone the immersion treatment in step S4 into a 0.02 mol / L hydrofluoric acid solution and clean them for 15 minutes under the action of 60 kHz ultrasound.

[0075] Example 5 is a combination of Example 1, Example 2 and Example 4.

[0076] Example 6:

[0077] The difference from Example 1 is that in step S3, the complexing leaching agent is: EDTA added at 10% of the mass of the quartz sand, sodium persulfate added at 1.5% of the mass of the quartz sand, and dilute hydrochloric acid is used to adjust the pH of the mixed solution to 3.5. The ultraviolet light wavelength is 365 nm, the light intensity is 500 μW / cm², the leaching temperature is 60℃, and the leaching is carried out at a constant temperature for 8 hours; air is also introduced at a flow rate of 0.3 L / min.

[0078] Example 7:

[0079] The difference from Example 1 is that in step S3, the complexing leaching agent is: DTPA is added at 7.5% of the mass of quartz sand, peracetic acid is added at 1% of the mass of quartz sand, and dilute hydrochloric acid is used to adjust the pH of the mixed solution to 4.0; the ultraviolet light wavelength is 312nm, the light intensity is 2000μW / cm², the leaching temperature is 85℃, and the leaching is carried out at a constant temperature for 3 hours; and air is introduced at a rate of 0.5L / min.

[0080] Example 8:

[0081] The difference from Example 1 is that in step S3, the complexing leaching agent is: oxalic acid is added at 15% of the mass of quartz sand, hydrogen peroxide is added at 3.2% of the mass of quartz sand, and dilute hydrochloric acid is used to adjust the pH of the mixed solution to 2.5; the ultraviolet light wavelength is 254nm, the light intensity is 3000μW / cm², the leaching temperature is 95℃, and the leaching is carried out at a constant temperature for 2 hours; and oxygen is introduced at a flow rate of 0.8L / min.

[0082] Comparative Example 1:

[0083] The difference from Example 1 is that: between steps S2 and S4, only conventional acid leaching is performed without ultraviolet light or complexing agents, using only 0.5 mol / L hydrochloric acid, with a leaching temperature of 80°C and a leaching time of 4 hours. The remaining steps are the same as in Example 1.

[0084] Comparative Example 2:

[0085] The difference from Example 1 is that the step between S2 and S4 is a complexation leaching reaction, without ultraviolet light irradiation, the complexation leaching agent is the same as in Example 1, and the remaining steps and conditions are the same as in Example 1.

[0086] The product samples from Examples 1 to 8, Comparative Examples 1 and 2 were tested for impurity elements according to the method in JY / T0567-2020. The test results are shown in Table 1.

[0087] Table 1

[0088]

[0089] By comparing the impurity element detection data of the examples and comparative examples, the ultraviolet light complexation leaching process provided by the present invention has a superior purification effect compared with the traditional process. As shown in the detection data in Table 1, the contents of the main impurity elements (Ti, Fe, Al, Na, K) in the products of the examples are significantly lower than those of the comparative examples. In particular, the removal effect of key impurities such as iron and titanium is significantly better than the prior art, especially Example 8, which has the best overall performance.

[0090] Comparing the data from Examples 1, 2, and 3, it can be found that aeration treatment improves the removal effect of impurity elements. The effect of introducing oxygen is better than that of introducing air. Introducing oxidizing gas during the leaching process can promote the decomposition of peroxides and enhance the oxidative leaching efficiency of impurity elements, which is an important means to improve the process effect.

[0091] In Examples 4 and 5, an ultrasonic treatment step was added after leaching. Data shows that the content of each impurity element in Example 4 was slightly lower than that in Example 1, indicating that ultrasonic treatment can further remove residual impurities.

[0092] Compared with Comparative Example 1, Examples 1 to 8 achieved a significant improvement in purity by introducing various methods such as ultraviolet light, complexing agents, and peroxides.

[0093] Compared with Comparative Example 2, it was found that ultraviolet light is not only a supplementary condition, but also a key technology that can promote leaching efficiency and impurity removal effect through photochemical reaction.

[0094] In summary, this invention organically combines multiple technical elements such as ultraviolet irradiation, complexation leaching, temperature control, and aeration treatment to form a systematic high-purity quartz sand preparation process, which has significant practical implications for promoting the development of the quartz new materials industry. Unlike simple technical aggregation, these technical elements have a synergistic effect, making the overall effect superior to the simple summation of individual elements.

[0095] Finally, it should be noted that the above-described embodiments are merely specific implementations of the present invention, used to illustrate the technical solutions of the present invention, and not to limit them. The scope of protection of the present invention is not limited thereto. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that any person skilled in the art can still modify or easily conceive of changes to the technical solutions described in the foregoing embodiments within the scope of the technology disclosed in the present invention, or make equivalent substitutions for some of the technical features; and these modifications, changes, or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be covered within the scope of protection of the present invention.

Claims

1. A method for preparing high-purity quartz sand by ultraviolet light complexation, characterized in that, Includes the following steps: Step S1: Crush and sieve the quartz raw material to obtain quartz particles; Step S2: Perform preliminary purification on the quartz particles; Step S3: Place the pre-purified quartz particles in a reactor, add a complexing leaching agent to the reactor, irradiate the mixture in the reactor with ultraviolet light, and stir the mixture. The complexing leaching agent is a mixed solution including a complexing agent and an oxidizing agent. The complexing agent is selected from one or more of oxalic acid, citric acid, EDTA, and DTPA, and the amount added is 7% to 20% of the mass of quartz sand. The oxidizing agent is selected from one or more of hydrogen peroxide, sodium persulfate, and peracetic acid, and the amount added is 1% to 3.5% of the mass of quartz sand. The pH of the mixed solution is controlled at 2 to 4. The leaching temperature is 60 to 95°C, the leaching time is 2 to 8 hours, the ultraviolet light wavelength is 254 to 365 nm, and the light intensity is 500 to 3000 μW / cm². During the leaching process, air or oxygen is introduced into the reactor at a flow rate of 0.1 to 1.0 L / min. Step S4: Separate the mixed system after ultraviolet light complexation leaching to obtain post-leaching treated quartz particles; Step S5: Wash the post-immersion treated quartz particles with deionized water. Step S6: Dehydrate and dry the washed quartz particles to obtain high-purity quartz sand.

2. The method for preparing high-purity quartz sand by ultraviolet light complexation according to claim 1, characterized in that, The preliminary purification in step S2 includes one or more of the following: desliming, scrubbing, ball milling, gravity separation, and magnetic separation.

3. The method for preparing high-purity quartz sand by ultraviolet light complexation according to claim 2, characterized in that, The initial purification method for S2 is magnetic separation with a magnetic field strength of 1.5~2.5T.

4. The method for preparing high-purity quartz sand by ultraviolet light complexation according to claim 1, characterized in that, The solid-liquid separation in step S4 is achieved through one or more of the following methods: centrifugal separation or natural sedimentation filtration.

5. The method for preparing high-purity quartz sand by ultraviolet light complexation according to claim 1, characterized in that, The interval between steps S4 and S5 also includes: Step S7, Ultrasonic treatment: Place the quartz particles that have undergone the immersion treatment in step S4 into a 0.01~0.05mol / L hydrofluoric acid solution and clean them for 10~30 minutes under the action of ultrasonic waves at 40~80kHz.

6. The method for preparing high-purity quartz sand by ultraviolet light complexation according to claim 1, characterized in that, Step S6 involves centrifugal dehydration, which is performed using a high-speed rotary drum centrifuge. Alternatively, high-temperature dehydration can be used, drying at 100~150℃.

7. The method for preparing high-purity quartz sand by ultraviolet light complexation according to any one of claims 1 to 6, characterized in that, The reactor includes: The reaction vessel (1) contains quartz particles and complexing leaching agent in its inner cavity; The ultraviolet lamp (2) is partially inserted into the inner cavity of the reaction vessel (1) and partially connected to the control device outside the reaction vessel (1); The stirring paddle (3) is partially inserted into the inner cavity of the reaction vessel (1) and partially connected to the rotation source (4) outside the reaction vessel (1); Heating jacket (5) is fitted onto the outer wall of reaction vessel (1); The feed pipe (6) has one end located outside the reaction vessel (1) and the other end inserted into the inner cavity of the reaction vessel (1); An exhaust port (7) is located at the top of the reaction vessel (1); The discharge port (8) is located at the bottom of the reaction vessel (1); and A vent pipe (9) is connected at one end to an air or oxygen source, and at the other end is inserted from the top of the reaction vessel (1) and extends to the bottom of the inner cavity of the reaction vessel (1).

Citation Information

Patent Citations

  • Quartz sand pickling purification process

    CN112744821A