A polyamide composition, its preparation and use
By using a combination of polyamide resin with a crystallinity of ≥45%, aramid fiber, polyurethane, and polysiloxane, the problems of wear and noise in high-torque transmission components of nylon modified materials have been solved, resulting in a polyamide composition with high torque, low wear, and low noise, suitable for transmission components such as gears.
Patent Information
- Application Number
- CN202610547069.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-23
- Publication Date
- 2026-06-16
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials technology, and in particular to a polyamide composition, its preparation method, and its application. Background Technology
[0002] Nylon is a thermoplastic with excellent strength, toughness, and self-lubricating properties, and is currently widely used in industries such as electronics, home appliances, textiles, automobiles, and military. Conventional nylon modification schemes typically involve adding carbon fiber (e.g., patent CN207906394U), glass fiber (e.g., CN117024952A), and wear-resistant additives such as ultra-high molecular weight polyethylene (e.g., patent CN115819966B) to reduce material wear. While inorganic fibers can effectively reduce wear, their incompatibility with resins leads to rough surfaces and high noise levels during operation. Organic ultra-high molecular weight polyethylene can effectively reduce wear and noise, but its addition affects the rigidity of the matrix material, resulting in low torque and limiting its application in fields requiring high torque, such as humanoid robots and industrial intelligence, which require high-torque transmission components.
[0003] Aramid fibers are characterized by high strength, high toughness, and high abrasion resistance. Their textile materials are used in fields such as large ship ropes and aircraft arresting cables, but are rarely used in modified plastics. This is because they are difficult to disperse in thermoplastic resins, which can easily cause stress concentration and internal defects. Therefore, although adding a certain proportion of aramid fibers can reduce material wear, it will also reduce the material's mechanical properties and make processing difficult.
[0004] Therefore, there is an urgent need in the field for a polyamide composition that simultaneously achieves high torque, low wear, and low noise to meet the requirements of transmission components. Summary of the Invention
[0005] The purpose of this invention is to provide a polyamide composition that simultaneously achieves high torque, low wear, and low noise, as well as its preparation method and application.
[0006] This invention is achieved through the following technical solution:
[0007] A polyamide composition, by weight, comprises the following components:
[0008] 74-91 parts of polyamide resin;
[0009] 6-15 parts of fiber filler;
[0010] 3-7 parts polyurethane;
[0011] 0.5-3 parts of polysiloxane;
[0012] The fiber filler is aramid fiber;
[0013] The polyamide resin has a crystallinity >45%.
[0014] The test method for the crystallinity of polyamide resin is as follows: wide-angle X-ray diffraction (XRD) is used in accordance with JIS K 0131:1996 "General Rules for X-ray Diffraction Analysis"; the sample is taken from an injection-molded rod with a diameter of 5 mm and a length of 30 mm, made into a flat thin sheet and pretreated by vacuum drying; Cu target Kα rays are used to scan at a speed of 2° / min in the range of 2θ of 5° to 40°, and the integral area Ac of the crystalline peak and the integral area Aa of the amorphous peak are obtained by peak fitting. The crystallinity is calculated according to the formula Xc=Ac / (Ac+Aa)×100%; each group of parallel tests is performed at least 3 times, and the average value is taken as the test result. The report should include sample information, test conditions, diffraction pattern and crystallinity value.
[0015] In the polyamide composition of the present invention, the content of polyamide resin can be any value or a range between 74 parts, 75 parts, 76 parts, 77 parts, 78 parts, 79 parts, 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, 89 parts, 90 parts, and 91 parts; the content of aramid fiber can be any value or a range between 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, and 15 parts; the content of polyurethane can be any value or a range between 3 parts, 4 parts, 5 parts, 6 parts, and 7 parts; and the content of silicone can be any value or a range between 0.5 parts, 1 part, 1.5 parts, 2 parts, 2.5 parts, and 3 parts. The crystallinity of polyamide resin can be any value or a range between two values, such as 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, for example, 50-70%.
[0016] In one embodiment, the polyamide resin accounts for 60-90 wt%, the aramid fiber accounts for 4.5-16 wt%, the polyurethane accounts for 2.3-8 wt%, and the silicone accounts for 0.35-3.5 wt%, based on the total weight percentage of the polyamide composition.
[0017] Preferably, the polyamide resin has a crystallinity > 60%.
[0018] In some embodiments, the viscosity range of the polyamide resin may be 1.8-2.6 (test standard ISO 3072007), the melting point range may be 220-330°C, and the test standard is ISO 11357-1:2023.
[0019] The polyamide resin is selected from aliphatic polyamide or semi-aromatic polyamide, and preferably, the polyamide resin is selected from at least one of PA66, PA46, PA10T, PA6T / 66, and PA12T.
[0020] The crystallinity range of PA66 is 45-55%, the crystallinity range of PA46 is 50-70%, the crystallinity range of PA10T is 45-55%, the crystallinity range of PA6T / 66 is 45-55%, and the crystallinity range of PA12T is 45-55% or more.
[0021] The aramid fibers include one or more of poly(p-phenylene terephthalamide) fibers and poly(m-phenylene isophthalamide) fibers.
[0022] The average length of the aramid fiber can range from 1 to 15 mm, and preferably, the average length of the aramid fiber is 3 to 6 mm.
[0023] The average length of aramid fibers can be any value or a range between 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, and 15 mm. The average length is determined by taking 2 mg of particles, placing them in a transparent petri dish, adding an appropriate amount of trifluoroacetic acid to fully dissolve the particles, and then, under a two-dimensional microscope, counting the lengths of the aramid fibers within the particles. The arithmetic mean of these lengths is recorded as the length of the modified aramid fibers.
[0024] The diameter range of aramid fibers can be 8-15 micrometers. The test method is as follows: take 2mg of particles, put the particles into a transparent petri dish, add an appropriate amount of trifluoroacetic acid, dissolve the particles completely, and then count the diameter of the aramid fibers in the particles under a two-dimensional microscope. The arithmetic mean of the diameters is recorded as the diameter of the aramid fibers in the modified material.
[0025] In some embodiments, the weight-average molecular weight of polyurethane can range from 20,000 to 80,000. The test method is gel permeation chromatography: the determination is carried out in accordance with ISO 16014-1 and ISO 16014-3; a calibration curve is established using tetrahydrofuran (THF) or N,N-dimethylformamide (DMF) containing a small amount of buffer as the mobile phase and polystyrene (PS) standard is used; the test is conducted at room temperature, and the weight-average molecular weight Mw, number-average molecular weight Mn, and molecular weight distribution index PDI are calculated from the chromatogram; the sample needs to be dissolved and filtered before the test, and the test is performed in parallel at least twice, and the average value is taken as the result.
[0026] Polysiloxane is added in the form of polysiloxane powder or polysiloxane masterbatch. When added in the form of polysiloxane masterbatch, the carrier is selected from at least one of PA66, PA6, PBT, and PP. The polysiloxane accounts for 30-80% of the mass of the masterbatch. 0-20 parts of additives can be added according to actual needs, such as 0.001-20 parts of additives, which are selected from flame retardants, antioxidants, lubricants, mold release agents, dyes, etc.
[0027] Alternatively, 0-5 parts of filler can be added. The filler is a non-fibrous filler, such as graphite or molybdenum disulfide.
[0028] The method for preparing the polyamide composition of the present invention includes the following steps: mixing the components evenly according to the formula, and extruding and granulating the mixture through a twin-screw extruder to obtain the polyamide composition.
[0029] The stability range of the screw barrel is ±30℃ from the melting point of the polyamide resin.
[0030] The present invention also relates to an article prepared using the polyamide composition of the present invention.
[0031] Preferably, the transmission component prepared using the polyamide composition of the present invention may be a gear.
[0032] The present invention has the following beneficial effects:
[0033] First, by selecting polyamide resin with a crystallinity of more than 45%, the wear resistance of the material can be significantly improved. This is because if the crystal content is too low, there will be more amorphous regions and the molecular chains will be relatively loose. The gears made from this material are very easy to detach from the system during operation, which leads to increased wear.
[0034] Secondly, by selecting aramid fiber as the fiber filler, the wear resistance of the material is improved, while ensuring a low noise level and a high torque level when the transmission components are running.
[0035] Meanwhile, by using polyurethane as a compatibilizer, this invention can significantly improve the dispersion performance of aramid fibers in resin.
[0036] Furthermore, adding polysiloxane as a surface lubricant can significantly reduce noise and wear. Detailed Implementation
[0037] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.
[0038] The experimental materials used in this invention are sourced from the following sources:
[0039] PA66: Measured crystallinity is 50%, PA66 EPR27, Pingdingshan Shenma Engineering Plastics Co., Ltd., melting point 263℃;
[0040] PA46: Measured crystallinity is 70%, Stanyl PA46 TW341-N, Royal DSM Group, melting point 295℃;
[0041] PA10T: Measured crystallinity is 50%, Vicnyl 700 NC003, Zhuhai Wantong Special Engineering Plastics Co., Ltd., melting point 318℃;
[0042] PA6T / 66: Measured crystallinity is 50%, Vicnyl 400 NC003, Zhuhai Wantong Special Engineering Plastics Co., Ltd., melting point 310℃;
[0043] PA12T: Measured crystallinity is 50%, Vicnyl 2900 NC003, Zhuhai Wantong Special Engineering Plastics Co., Ltd., melting point 295℃;
[0044] PA6T / 6I / 66 copolymer: measured crystallinity 40%, Vicnyl 5300 NC003, Zhuhai Wantong Special Engineering Plastics Co., Ltd., melting point 313℃;
[0045] PA610: Measured crystallinity is 18%, PA610 Type I, Shandong Guangyin New Material Co., Ltd., China, melting point 225℃;
[0046] PA6T / 6I copolymer: measured crystallinity 36%, Vicnyl 500 NC003, Zhuhai Wantong Special Engineering Plastics Co., Ltd., melting point 325℃;
[0047] PA10T / 10I copolymer: measured crystallinity 29%, Vicnyl 600 NC003, Zhuhai Wantong Special Engineering Plastics Co., Ltd., melting point 290℃;
[0048] PA6 crystallinity: 35%, PA6 HY2800, Haiyang Technology Co., Ltd., melting point 225℃.
[0049] TPAE: PEBAX® 4533 SP 01, Manufacturer: arkema, Melting point: 147℃;
[0050] Aramid fiber A: AR246C, average fiber length 6mm, Guangzhou Longwan Trading Co., Ltd.;
[0051] Aramid fiber B: Kevlar® 1F106, with an average fiber length of 3mm, DuPont;
[0052] Long glass fiber masterbatch: PA66-LG50 HSNC001, with a glass fiber weight content of 50% and an average length of 6 mm for the long fibers, Kingfa Science & Technology Co., Ltd.
[0053] Carbon fiber: HexTow® AS4C 6mm Chopped, Hexcel, with an average fiber length of 6 mm;
[0054] Basalt fiber: Basalt Chopped Strand 6mm, Technobasalt, with an average fiber length of 6 mm;
[0055] Polyurethane A: Purchased from Covestro, Texin® 985AU;
[0056] Polyurethane B: Purchased from Lanxess, Witcobond W-240, the raw material was obtained after drying and dispersion;
[0057] Polyurethane C: Purchased from BASF, model Trixene WB 149, the raw material was obtained after drying and dispersion.
[0058] Silicone Masterbatch A: Carrier is PA6, silicone content is 50 wt%, MB50-011, Dow Corning;
[0059] Silicone Masterbatch B: Carrier is PA6, silicone content is 71 wt%, KJ-A01, Kaijie;
[0060] Other surface lubricants: LLDPE LL6101, ExxonMobil;
[0061] Antioxidant: RIANOX 1098.
[0062] Preparation method of polyamide compositions in examples and comparative examples: The components were mixed uniformly according to the specified ratio, and then extruded and granulated using a twin-screw extruder to obtain the polyamide composition. The stability range of the screw barrel was ±30°C from the melting point of the polyamide resin.
[0063] Test methods:
[0064] (1) Peak torque and operating noise test: Refer to the test method of GB / T 3480.1-2019; the specific test method is as follows: use a composite material injection mold for gear, the mold parameters are: number of teeth: 31, base circle diameter: 62mm, tooth width: 12mm, tooth root height: 1mm, tooth tip height: 1.25mm; install the injection molded gear and the fixed metal gear on the test machine, preload about 5% of the limit torque, gradually load until the gear fails, and record the maximum torque at failure, which is the peak torque of the material. During the process, refer to the test method of IEC 60704-1:2021; record the dB value of the maximum noise during the whole process, which is marked as the operating noise. The specific method for testing operating noise is as follows: A composite material injection mold for gears is used, with the following parameters: number of teeth: 31, base circle diameter: 62mm, tooth width: 12mm, tooth root height: 1mm, tooth tip height: 1.25mm. The injection-molded gear and the fixed metal gear are then mounted on the testing machine, with a preload of approximately 5% of the limit torque. The running time is 30 minutes, and the maximum noise level in dB during the entire process is recorded, which is then marked as the operating noise.
[0065] (2) Wear test: Refer to method B in JIS K 7218:1986, use a bar with a diameter of 5mm and a length of 30mm, select a load of 100N, and a friction time of 4 hours. After the test, calculate the wear amount of the material to obtain the wear value.
[0066] Table 1: Component content and test results of polyamide compositions in Examples 1-7
[0067] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 PA66 82.5 PA10T 82.5 PA6T / 66 82.5 PA12T 82.5 PA46 82.5 75 90 Aramid fiber A 10 10 10 10 10 15 6 Polyurethane A 5 5 5 5 5 3 7 Silicone Masterbatch A 2 2 2 2 2 0.5 3 antioxidants 0.5 0.5 0.5 0.5 0.5 0 0.5 Peak torque NM 11.2 13.2 12.5 11.9 13.1 14.5 10.6 Maximum noise dB 32 40 36 32 30 39 30 <![CDATA[Wear value 10 -3 mm 3 > 68 58 63 65 54 42 76
[0068] The content of silicone masterbatch in the embodiments and comparative tables of this invention represents the actual weight parts of polysiloxane.
[0069] As can be seen from Examples 1-5, the polyamide with a crystallinity >60% in Example 5 has low noise, low wear, and a peak torque exceeding 13 N.M.
[0070] Table 1: Component content and test results of polyamide compositions in Examples 8-11
[0071] Example 8 Example 9 Example 10 Example 11 PA46 82.5 82.5 82.5 82.5 Aramid fiber A 10 10 10 Aramid fiber B 10 Polyurethane A 5 5 Polyurethane B 5 Polyurethane C 5 Silicone Masterbatch A 2 2 2 Silicone Masterbatch B 2 antioxidants 0.5 0.5 0.5 0.5 Peak torque NM 13.5 12.4 13.8 13.3 Maximum noise dB 29 32 30 31 <![CDATA[Wear value 10 -3 mm 3 > 55 58 55 74
[0072] As can be seen from the marketed examples, the polyamide composition of the present invention has a peak torque ≥10 NM, a maximum noise level ≤42 dB, and an abrasion value ≤85 × 10 Nm. -3 mm 3 .
[0073] Table 3: Component content and test results of polyamide compositions in Comparative Examples 1-3
[0074] Comparative Example 1 Comparative Example 2 Comparative Example 3 PA46 82.5 82.5 82.5 Fiberglass 10 carbon fiber 10 Basalt fiber 10 Polyurethane A 5 5 5 Silicone Masterbatch A 2 2 2 antioxidants 0.5 0.5 0.5 Peak torque NM 8.1 10.7 9.0 Maximum noise dB 36 75 67 <![CDATA[Wear value 10 -3 mm 3 > 320 51 207
[0075] Note: Glass fiber is added through long glass fiber masterbatch; the table shows the actual glass fiber content.
[0076] As can be seen from Comparative Examples 1-3, glass fiber, carbon fiber, and basalt fiber cannot replace aramid fiber and cannot simultaneously achieve the effects of high torque, low wear, and low noise.
[0077] Table 4: Component content and test results of polyamide compositions in Comparative Examples 4-8
[0078] Comparative Example 4 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 PA6T / 6I / 66 copolymer 82.5 PA610 82.5 PA6T / 6I copolymer 82.5 PA10T / 10I copolymer 82.5 PA6 82.5 Aramid fiber A 10 10 10 10 10 Polyurethane A 5 5 5 5 5 Silicone Masterbatch A 2 2 2 2 2 antioxidants 0.5 0.5 0.5 0.5 0.5 Peak torque NM 11.4 11.4 10.4 11.8 11.2 Maximum noise dB 39 37 45 40 38 <![CDATA[Wear value 10 -3 mm 3 > 108 693 167 119 576
[0079] As can be seen from Comparative Examples 4-8, polyamide resins with a crystallinity of less than 50% cannot simultaneously achieve the technical effects of high torque, low noise, and low wear.
[0080] Table 5: Component content and test results of polyamide compositions in Comparative Examples 9-11
[0081] Comparative Example 9 Comparative Example 10 Comparative Example 11 PA46 82.2 82.5 82.5 TPAE 5 Aramid fiber A 10 10 10 Polyurethane A 5 0 Silicone Masterbatch A 2 7 Other surface lubricants 2 antioxidants 0.5 0.5 0.5 Peak torque NM 10.6 11.8 7.1 Maximum noise dB 35 41 43 <![CDATA[Wear value 10 -3 mm 3 > 984 118 501
[0082] As can be seen from Comparative Example 9, TPAE cannot replace polyurethane to achieve the technical effects of the present invention, especially due to its poor wear resistance.
[0083] As can be seen from Comparative Example 10, other surface lubricants in the field cannot simultaneously achieve the technical effects of high torque, low noise, and low wear.
[0084] As can be seen from Comparative Example 11, the performance of all technologies is poor when polyurethane is not present.
Claims
1. A polyamide composition, characterized in that, By weight, it includes the following components: 74-91 parts of polyamide resin; 6-15 parts of fiber filler; 3-7 parts polyurethane; 0.5-3 parts of polysiloxane; The fiber filler is aramid fiber; The polyamide resin has a crystallinity >45%.
2. The polyamide composition according to claim 1, characterized in that, The polyamide resin has a crystallinity >60%.
3. The polyamide composition according to claim 1, characterized in that, The polyamide resin is selected from aliphatic polyamide or semi-aromatic polyamide, and preferably, the polyamide resin is selected from at least one of PA66, PA46, PA10T, PA6T / 66, and PA12T.
4. The polyamide composition according to claim 1, characterized in that, The average length of the aramid fiber is 1-15 mm.
5. The polyamide composition according to claim 1, characterized in that, The polysiloxane is added in the form of polysiloxane powder or polysiloxane masterbatch. When added in the form of polysiloxane masterbatch, the carrier resin is selected from at least one of PA66, PA6, PBT, and PP.
6. The polyamide composition according to claim 1, characterized in that, Based on parts by weight, it also includes 0-20 parts of additives, said additives being selected from at least one of flame retardants, antioxidants, lubricants, release agents, and dyes; and / or includes 0-5 parts of fillers, said fillers being selected from one or more of graphite and molybdenum disulfide.
7. A method for preparing the polyamide composition according to any one of claims 1-6, characterized in that, The process includes the following steps: mixing the components evenly according to the formula, and granulating the mixture by extrusion through a twin-screw extruder to obtain a polyamide composition.
8. An article prepared using the polyamide composition according to any one of claims 1-6.
9. A transmission component prepared using the polyamide composition according to any one of claims 1-6, wherein the transmission component is a gear.
Citation Information
Patent Citations
Composite material for bearing retainer and preparation method of composite material
CN117024952A
Novel combined material gear
CN207906394U