A method for preparing large-size forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloys
Through three vacuum self-consumable melting processes and multi-stage forging, high-strength, high-toughness, and high-impact-resistant duplex titanium alloy forgings were prepared, solving the problem of insufficient performance of titanium alloy forgings in the existing technology, and making them suitable for marine engineering equipment.
Patent Information
- Application Number
- CN202611007097.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-07-08
AI Technical Summary
Existing titanium alloy forging processes cannot simultaneously meet the extreme requirements of high strength, high toughness, and high impact resistance, especially in the production of large-size forgings, where deformation efficiency is low and the material's impact performance is insufficient.
Dual-phase titanium alloy ingots were prepared by three-stage vacuum arc remelting. The process involved high-temperature β-zone forging, cross-phase upsetting and drawing forging, and quasi-β-forging, including multiple upsetting and alternating temperature control, to form a basket structure, ensuring the high strength and toughness of the alloy.
We have developed duplex titanium alloy forgings with high strength, high toughness and high impact resistance, which meet the performance requirements of marine equipment and improve production efficiency and material adaptability.
Smart Images

Figure CN122500116B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of titanium alloys, and more specifically, to a method for preparing large-sized forgings of high-strength, high-toughness, and high-impact-resistant duplex titanium alloys. Background Technology
[0002] Titanium and titanium alloys have received widespread attention in the fields of shipbuilding, marine engineering equipment and marine engineering equipment mining due to their high strength, good plasticity and toughness, corrosion resistance and excellent fatigue performance. Related equipment has a large demand for titanium alloy forgings, plates, pipes and other parts, and at the same time, it has put forward higher requirements for the comprehensive properties of titanium alloys, such as mechanical strength, plasticity, toughness, impact resistance and formability.
[0003] Currently, the main titanium alloys used in marine engineering include Ti62A, TA31, and TC4.
[0004] (1) TA31 titanium alloy (or Ti80) is a high-strength, high-toughness, weldable marine structural titanium alloy with a nominal composition of Ti-6Al-3Nb-2Zr-1Mo and a yield strength Rp. 0.2 With a tensile strength of ≥740MPa, tensile strength Rm≥875MPa, elongation A≥12%, and impact energy KV2≥47J, it is widely used in key components of deep-sea equipment and ships.
[0005] (2) Ti62A titanium alloy is a high-strength and high-toughness damage-tolerant α+β alloy. Its nominal chemical composition is Ti-6Al-3Mo-2Zr-2Sn-1V-1Cr, and its yield strength Rp is 0.2 With a strength of ≥950MPa, elongation A≥9%, and impact energy KV2≥20J, this material was developed specifically to meet the stringent requirements of a 10,000-meter manned deep-sea submersible for its core pressure-bearing materials.
[0006] (3) TC4 titanium alloy is a high-strength, high-toughness, weldable marine structural titanium alloy with a nominal composition of Ti-6Al-4V and a yield strength Rp. 0.2 With an impact strength of ≥795MPa, elongation A≥10%, and impact energy KV2≥24J, it is the most classic α+β type titanium alloy, accounting for 50% of the total titanium alloy usage. It has strong versatility and is suitable for multiple fields such as aviation, medical, chemical, and marine industries.
[0007] Furthermore, based on classic titanium alloys such as Ti6246 (nominal chemical composition: Ti-6Al-2Sn-4Zr-6Mo) and Ti62222 (nominal chemical composition: Ti-6Al-2Mo-2Cr-2Zr-2Sn-1Nb-1Fe), new alloy systems have been derived through composition optimization: Ti5321 (nominal chemical composition: Ti-5Al-3Mo-3V-2Cr-2Zr-1Nb-1Fe) and Ti90 (nominal chemical composition: Ti-5.5Al-4Zr-1Sn-1Nb-0.3Mo). These titanium alloys belong to the Ti-Al-Sn-Zr-Mo-Si-X alloy series, and through reasonable composition design, they achieve excellent comprehensive mechanical properties. However, existing grades of titanium alloys all have performance limitations and cannot simultaneously meet the extreme requirements of high strength, high toughness, and impact resistance.
[0008] As is well known, besides chemical composition, the microstructure of titanium alloys has a significant impact on their mechanical properties. The processing technology of titanium alloys (such as deformation temperature and heat treatment regime) directly determines their final microstructure, and thus their mechanical properties. Typical microstructures of duplex titanium alloys include equiaxed, basketweave, biphase, and Widmanstätten structures, and their mechanical property characteristics are as follows:
[0009] (1) Equiaxed structure, characterized by a large number of equiaxed primary α phases (about 20-50%) uniformly distributed in fine β transformation structure; alloys with this structure need to be forged or rolled in the α+β two-phase region (40-50℃ below the β phase transformation point) and then recrystallized and annealed. Alloys with this structure often have high strength, high plasticity and excellent fatigue resistance, but relatively low fracture toughness and creep resistance.
[0010] (2) Basket mesh structure, the microstructure is characterized by the elongation of the original β grains, the precipitation of fine α lamellae interwoven into a basket mesh inside the grains, and the discontinuous α phase at the grain boundaries; titanium alloys with this structure need to be forged in the β single-phase region (above the β phase transformation point) (β forging), or near-β forging, and combined with specific heat treatment; this type of alloy has excellent fracture toughness, creep resistance and damage tolerance, so its comprehensive mechanical properties are excellent; however, its room temperature plasticity and low cycle fatigue performance are relatively poor.
[0011] (3) Two-phase microstructure: The microstructure is characterized by a certain proportion of equiaxed primary α phase (approximately 15-30%) and fine acicular α or α+β transformation microstructure. Titanium alloys with this microstructure combine forging processes in the α+β two-phase region and the β single-phase region. For example, β-phase forging followed by α+β-phase processing, or near-β forging followed by solution aging treatment. These alloys possess excellent comprehensive mechanical properties, achieving an optimal balance between strength, plasticity, and fracture toughness, and are considered the ideal microstructure for most high-temperature titanium alloys.
[0012] (4) Widmanstätten structure: The microstructure is characterized by coarse, primitive β grains with continuous α-phase films at the grain boundaries and coarse, straight, and parallel α-lamellae within the grains, forming a classic Widmanstätten structure. Alloys with this structure need to be heated in the β single-phase region and then slowly cooled; or cooled and then aged in the β single-phase region. These alloys have the highest fracture toughness and creep resistance, but the worst room temperature plasticity, impact toughness, and low-cycle fatigue performance.
[0013] Hot working is one of the most common deformation methods for titanium alloys. Forging and rolling, for example, allow for the control of plastic deformation by applying temperature and pressure, thereby obtaining the corresponding microstructure, dimensional morphology, and mechanical properties. The α→β phase transformation temperature T in titanium alloys... β This is an important basis for selecting the heating temperature in hot working. β The microstructures obtained by the above heat treatments are all Widmanstätten structures, which have high strength but poor ductility and toughness. β The microstructure obtained by the following hot working is a biaxial or equiaxed microstructure, exhibiting a good balance of strength and toughness. Therefore, the vast majority of titanium alloys are used in an equiaxed or biaxial microstructure. However, in T... β The deformation resistance during the following hot working is significantly higher than that of T. β The above deformations cause T to β The following hot working processes have poor deformation efficiency, limited deformation per cycle, and are prone to cracking. Therefore, many titanium alloy products are manufactured at relatively high temperatures in industrial processes to ensure formability, but this inevitably results in a loss of some product properties.
[0014] Currently, there are many processes for forging deformation in the β phase region. For example, Chinese Patent Publication No. CN109482796A provides a β forging and heat treatment method for TC4 titanium alloy disc forgings. It uses a 400KJ machine hammer forging, heats the forging temperature to 30℃~40℃ above the phase transformation point, and performs β phase region forging with a deformation of up to 40%. After forging, it is first air-cooled for 5 to 6 minutes, and then water-cooled to obtain a uniform and fine forged basket structure. The post-forging heat treatment involves solution treatment at a temperature of 30~40℃ below the phase transformation point, water cooling, and then aging heat treatment at 620~630℃ to obtain a stable and fine basket structure with high strength and a certain degree of plasticity. Chinese Patent Publication No. CN105441845A discloses a forging process for abnormal microstructure of TC18 titanium alloy raw materials, which includes the following steps: a) performing β forging on the billet with a phase transformation point above 1-2 heats, the forging temperature being 15-30℃ above the phase transformation point, and the deformation being controlled between 20-40%; b) performing forging on the billet with a phase transformation point below 2-2 heats, the forging temperature being 20-40℃ below the phase transformation point, and the deformation being controlled between 15-30%; c) performing β forging on the billet with a phase transformation point above 1 heats, the forging temperature being 10-20℃ above the phase transformation point, and the deformation being controlled between 15-25%. This process can effectively avoid the formation of fine-grained bright band microstructure defects and can meet the requirements for mass production of TC18 titanium alloy free forgings. Chinese Patent Publication No. CN105063527A discloses a method for preparing TA5-A alloy disc forging billets. This method involves upsetting and drawing above the phase transformation point during intermediate billet forging to break up the coarse as-cast structure, and then upsetting and drawing below the phase transformation point to further refine and homogenize the structure. The finished forging billet is forged using β forging, ensuring sufficient deformation to obtain a small amount of equiaxed α+ coarse lamellar α structure, thus obtaining a high-performance TA5-A alloy disc that meets technical requirements. While all these techniques employ β forging, these processes are not suitable for large deformation or continuous deformation processes. Furthermore, while these processes aim to obtain alloys with high strength and high fracture toughness, they do not offer advantages in impact performance; that is, they cannot simultaneously meet the extreme requirements of high strength, high toughness, and impact resistance.
[0015] Furthermore, Chinese Patent Publication No. CN 121874537 A discloses a method for preparing large-size TC4 titanium alloy bars with high impact toughness and A1-level non-destructive testing. This method involves using a multi-stage high-temperature single-phase β-region large deformation forging process on the secondary finished ingot during the billet-making stage. Axial upsetting, lateral upsetting, and diagonal upsetting are used to fully break and refine the as-cast grains. Subsequently, repeated forging at temperatures around the phase transformation point using a "high-low-high-low" cycle achieves grain homogenization and eliminates original grain boundaries through high-temperature dynamic recrystallization. Combined with multi-stage diagonal elongation forging, this effectively reduces deformation dead zones in angular areas. Finally, multi-stage forging in the two-phase region, combined with heat treatment, further optimizes the microstructure and controls the lamellar α-structure to ensure low-temperature impact performance. However, this technology mainly targets TC4 titanium alloy bars, whose microstructure is predominantly equiaxed, and the alloy's impact toughness is approximately 24 J. The material's impact performance is not advantageous; that is, it cannot simultaneously meet the extreme requirements of high strength, high toughness, and impact resistance.
[0016] Therefore, it is necessary to design and provide a process and microstructure control method for high-strength and high-impact titanium alloy forgings to meet the needs of marine equipment for high-strength, high-toughness, and high-impact titanium alloys and large-size forgings. Summary of the Invention
[0017] To address the shortcomings of existing technologies, the present invention aims to provide a method for preparing large-scale forgings of high-strength, high-toughness, and high-impact-resistant duplex titanium alloys. The method involves first obtaining a titanium alloy ingot through electrode pressing and three rounds of vacuum arc remelting, followed by initial forging in the high-temperature β-region, where multiple upsetting and drawing processes thoroughly break down the as-cast grains. Next, cross-phase region upsetting and drawing forging is performed, inducing recrystallization to refine the grains and eliminate the α-phase at grain boundaries through repeated upsetting and drawing. Finally, quasi-β-forging is performed to form a basketweave structure, thereby ensuring the duplex titanium alloy possesses high strength, high toughness, and high impact-resistant mechanical properties. This invention can improve the impact performance of titanium alloy forgings while ensuring their strength and toughness, meeting the performance requirements of large-scale titanium alloy forgings for marine equipment.
[0018] To achieve the above objectives, the present invention adopts the following technical solution:
[0019] This invention provides a method for preparing high-strength, high-toughness, and high-impact-resistant duplex titanium alloy forgings based on quasi-β forging, comprising the following steps:
[0020] P1, Preparation of dual-phase titanium alloy VAR ingots, as detailed below:
[0021] The raw materials were prepared according to the nominal composition of the duplex titanium alloy Ti-5Al-2Mo-2V-1.3Cr-1.3Zr-1Sn-1Fe-0.09O, pressed and welded into electrodes, and then the duplex titanium alloy VAR ingot was obtained through three vacuum consumable melting processes.
[0022] P2, the dual-phase titanium alloy VAR ingot obtained in step P1 is subjected to high-temperature β-zone forging, as follows:
[0023] The dual-phase titanium alloy VAR ingot is heated to 1100-1150℃, held at that temperature, and then subjected to 2-3 axial upsetting and drawing processes to obtain the first forging billet. After that, it is returned to the furnace and heated to 1000-1050℃, held at that temperature, and then subjected to 2-3 axial upsetting and drawing processes, controlling the upsetting and drawing deformation to 50-70%. After shaping, it is air-cooled to room temperature to obtain the second forging billet.
[0024] P3, the second forging billet is subjected to alternating upsetting and drawing forging in the cross-phase region, as detailed below:
[0025] The second forging billet is heated to 930–970°C, held at that temperature, and then subjected to 2–3 axial upsetting and drawing processes. After shaping, the α-phase → β-phase transformation temperature of the forging billet is tested to obtain the third forging billet. The billet is then returned to the furnace and heated to 30–50°C below the β-phase transformation point, held at that temperature, and then subjected to 2–3 axial upsetting and drawing processes. After shaping, the fourth forging billet is obtained. The billet is then returned to the furnace and heated to 30–50°C above the β-phase transformation point, held at that temperature, and then subjected to 2–3 axial upsetting and drawing processes. After shaping, the billet is air-cooled to room temperature to obtain the fifth forging billet. The billet is then returned to the furnace and heated to 30–50°C below the β-phase transformation point, held at that temperature, and then subjected to 2–3 axial upsetting and drawing processes with an upsetting deformation of 50–70%. After shaping, the billet is air-cooled to room temperature to obtain the sixth forging billet.
[0026] P4, the sixth forging billet undergoes quasi-β forging forming and microstructure control, as detailed below:
[0027] The sixth forging billet is heated to 30–50°C below the β phase transformation point, held at that temperature, and then subjected to 2–3 axial upsetting and drawing operations with an upsetting deformation of 50–70%. After shaping, it is air-cooled to room temperature to obtain the seventh forging billet. The billet is then returned to the furnace and heated to 30–50°C below the β phase transformation point, and then upset, widened, drawn, and shaped with an upsetting deformation of 40–60% to obtain the eighth forging billet. The billet is then returned to the furnace and heated to 10–30°C above the β phase transformation point, and then drawn, widened, and shaped with an elongation deformation of 20–30% to form a large-sized forging with a thickness of 200–300 mm, a width of 1460–1560 mm, and a length of 1565–1665 mm. After air-cooling to room temperature, it becomes a large-sized forging of high-strength, high-toughness, and high-impact dual-phase titanium alloy with a basketweave structure.
[0028] In step P1, to ensure the strong and ductile mechanical properties of the titanium alloy material, composition design and experimental exploration were conducted. The nominal composition of the dual-phase titanium alloy of this invention is Ti-5Al-2Mo-2V-1.3Cr-1.3Zr-1Sn-1Fe-0.09O. Considering the strengthening effects of Al, Mo, V, Cr, and Fe, and taking into account the tendency of element segregation and intermetallic compound formation, 5% Al, 2% Mo and V, and 1.3% Cr and 1% Fe were added during alloy design to ensure the mechanical strength of the alloy. In addition, the contents of Mo, Cr, and Fe were controlled during alloy design to control the segregation behavior of alloying elements. At the same time, 1.3% of the neutral element Zr and 1% Sn were added to achieve high ductility, mainly because the alloying of Zr and Sn can improve the lattice c / a parameter of α-Ti, thereby facilitating the activation of non-basal planes during plastic deformation. Slippage achieves plasticization. The aforementioned β-phase forming elements improve the stability of the β-phase, allowing a certain amount of the β-phase to be retained in the microstructure after forging and cooling.
[0029] Preferably, in step P1:
[0030] The raw materials used in the formulation include Grade 1 sponge titanium standard granules, Al beans, AlMo50 master alloy, AlV50 master alloy, AlCr70 master alloy, sponge Zr, TiSn80 master alloy, iron nails and TiO2.
[0031] The composition of the dual-phase titanium alloy VAR ingot, by mass percentage, is as follows: Al: 4.5%~5.5%, Mo: 1.5%~2.5%, V: 1.5%~2.5%, Cr: 1%~2%, Zr: 1%~2%, Sn: 0.5%~1.5%, Fe: 0.5%~1.5%, with the balance being Ti and unavoidable impurity elements; the unavoidable impurity elements are C≤0.02%, O≤0.12%, N≤0.01%, H≤0.002%.
[0032] In step P1, the use of three vacuum self-consumable melting is to achieve uniform and stable melting, improve the uniformity of ingot composition, reduce inclusions and segregation, and ensure dense structure and high purity. It is necessary to strictly control the vacuum degree, leakage rate, steady-state current, steady-state voltage and cooling time. The process involves three stages: First, vacuum arc remelting remelts the sponge titanium and alloying element-pressed electrodes in a vacuum, primarily completing preliminary alloying, removing volatile impurities, and partially removing gases, resulting in a Φ560mm primary unfinished ingot with poor uniformity. Second, the primary unfinished ingot is melted into a Φ660mm secondary unfinished ingot. This process uses the primary ingot as the arc remelting electrode to promote alloying element diffusion, reduce macroscopic segregation, refine the solidification structure, and further reduce the content of gases and non-metallic inclusions, obtaining a more uniform intermediate ingot. Third, the secondary unfinished ingot is melted into a Φ760mm duplex titanium alloy VAR ingot. This process uses the secondary unfinished ingot as the electrode for final remelting, aiming to completely dissolve residual high-melting-point inclusions, minimize microscopic segregation (especially for β-stabilizing elements such as Mo, V, Cr, and Fe), and improve compositional and microstructure uniformity.
[0033] Preferably, in step P1, the three-stage vacuum consumable melting process includes the following steps:
[0034] The first vacuum self-consumption melting was carried out with the vacuum degree controlled at ≤5.0Pa, the leakage rate at ≤1Pa / min, the steady-state current at 13~15kA, and the steady-state voltage at 20~32V. The ingot obtained from the melting was cooled in a water-cooled copper crucible crystallizer for 3~5 hours to obtain a Φ560 primary non-finished ingot.
[0035] The second vacuum self-consumption melting process was carried out with the vacuum degree controlled at ≤3.0Pa, the leakage rate at ≤1Pa / min, the steady-state current at 15~17kA, and the steady-state voltage at 31~33V. The ingot obtained from the melting process was cooled in a water-cooled copper crucible crystallizer for 4~7 hours to obtain a Φ660 secondary non-finished ingot.
[0036] The third vacuum self-consumable melting process was carried out with the vacuum degree controlled at ≤3.0Pa, the leakage rate at ≤1Pa / min, the steady-state current at 17~19kA, and the steady-state voltage at 32~35V. The ingot obtained from the melting process was cooled in a water-cooled copper crucible crystallizer for 5~9 hours to obtain a duplex titanium alloy VAR ingot with a specification of Φ760.
[0037] Preferably, step P2 specifically includes the following processes:
[0038] P21. First, the dual-phase titanium alloy VAR ingot is coated with two layers of glass insulation coating. Then, it is placed in an electric heating furnace at a furnace temperature of 800±10℃ and heated for 6±0.5h. The temperature is confirmed to reach 1100~1150℃ and held for 9~12h. Then, it is axially upsetting and drawing 2~3 times with an upsetting deformation of 50~70% to form a square billet with a side length of 720~750mm and a length of 1350~1400mm. The billet is then shaped to obtain the first forging billet.
[0039] P22, return the hot material of the first forging billet completed in step P21 to the furnace, raise the temperature for 3 to 4 hours, confirm that the temperature reaches 1000 to 1050℃, and hold it for 2 to 5 hours. Then, perform 2 to 3 axial upsetting and drawing operations, with an upsetting deformation of 50 to 70%. After that, perform square billet shaping to form an octagonal forging billet with a cross-sectional side length of 750 to 800 mm and a length of 1480 to 1540 mm. Then, air cool it to room temperature and grind it to remove cracks and defects to obtain the second forging billet.
[0040] Preferably, step P3 specifically includes the following processes:
[0041] P31. The second forging billet is coated with two layers of glass insulation coating, and then placed in an electric heating furnace at a furnace temperature of 800±10℃ for 2-3 hours. The temperature is confirmed to reach 930-970℃ and held for 7-11 hours. Then, it is axially upsetting 2-3 times with an upsetting deformation of 50-70%. Subsequently, it is shaped into a square billet with a side length of 720-750mm and a cuboid shape with a length of 1350-1400mm. The α-phase → β-phase transformation temperature of the forging billet is tested by taking a sample from the hot material to obtain the third forging billet.
[0042] P32, return the hot third forged billet obtained in step P31 to the furnace, and heat it up for 1 to 2 hours until the temperature reaches 30 to 50°C below the β phase transformation point, i.e., T. β -50℃~T β -30℃, this T β The temperature is set to the α→β phase transformation temperature and held for 9–11 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming an octagonal forging blank with a cross-sectional side length of 750–800 mm and a length of 1480–1540 mm. After that, the octagonal square blank is shaped to obtain the fourth forging blank.
[0043] P33, first return the hot material of the fourth forged billet obtained in step P32 to the furnace, and raise the temperature for 2 to 3 hours until it reaches 30 to 50°C above the β phase transformation point, i.e., T. β +30℃~T β +50℃, this T β The temperature is set to the α→β phase transformation temperature and held for 5–8 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming a square billet with a side length of 750–770 mm and a length of 1350–1410 mm. The billet is then shaped to obtain the fifth forging billet.
[0044] P34, return the fifth forged billet hot material obtained in step P33 to the furnace, and raise the temperature for 1 to 2 hours until it reaches 30 to 50°C below the β phase transformation point, i.e., T. β -50℃~T β -30℃, this T β The temperature is set to the α→β phase transformation temperature and held for 9–11 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming an octagonal forging billet with a cross-sectional side length of 750–800 mm and a length of 1480–1540 mm. After that, the octagonal square billet is shaped, then air-cooled to room temperature, and then ground to obtain the sixth forging billet.
[0045] Preferably, step P4 specifically includes the following processes:
[0046] P41, apply two coats of glass insulation coating to the sixth forging billet obtained in step P34, then load the furnace at a temperature of 800±10℃ and heat for 1-2 hours, confirming that the temperature reaches 30-50℃ below the β phase transformation point, i.e., T. β -50℃~T β -30℃, this T β The temperature is set to the α→β phase transformation temperature and held for 6–9 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming a square billet with a side length of 750–770 mm and a length of 1350–1410 mm. The billet is then shaped, air-cooled to room temperature, and ground to obtain the seventh forging billet.
[0047] P42, return the hot material of the seventh forged billet obtained in step P41 to the furnace, and raise the temperature for 1 to 2 hours until it reaches 30 to 50°C below the β phase transformation point, i.e., T. β -50℃~T β -30℃, this T β The temperature is set at the α→β phase transformation temperature and held for 3–5 hours. Then, upsetting, widening, drawing, and shaping are carried out, with an upsetting and drawing deformation of 40–60%, forming a rectangular billet with a thickness of 300–340 mm, a width of 1560–1600 mm, and a length of 1350–1450 mm. The billet is then air-cooled to room temperature and ground to obtain the eighth forging billet.
[0048] P43, apply two coats of glass insulation coating to the eighth forging billet obtained in step P42, load the furnace at a temperature of 800±10℃, and heat for 2-3 hours until the temperature reaches 10-30℃ above the β phase transformation point, i.e., T. β +10℃~T β +30℃, this T β The temperature is set to the α→β phase transformation temperature and held for 2–3 hours. Then, the parts are drawn, widened, and shaped. The drawing deformation is 20–30%, forming large-sized forgings with a thickness of 200–300 mm, a width of 1460–1560 mm, and a length of 1565–1665 mm.
[0049] Preferably, in steps P2 to P4, a high-speed forging machine with a tonnage of ≥60MN (such as a high-speed forging machine with a tonnage of 60MN or 80MN or larger) is used for upsetting and drawing, with an upsetting deformation rate of 20 to 35 mm / s and a drawing deformation rate of 30 to 55 mm / s.
[0050] In steps P3 to P4, the T β The temperature is 910–915℃.
[0051] The forging process and heat treatment of this invention have a significant impact on the microstructure of duplex titanium alloys:
[0052] In steps P2 to P4, high-temperature β-zone forging, cross-phase zone upsetting and drawing forging, and quasi-β forging are sequentially employed to form a basket-like structure, thereby improving the impact performance of the duplex titanium alloy forging while enhancing its strength and toughness. During the high-temperature β-zone forging process, multiple upsetting and drawing operations are performed at 1100–1150℃ and 1000–1050℃ respectively, using high-temperature, large-deformation methods to fully break down the as-cast structure of the large-size duplex titanium alloy VAR ingot. During the cross-phase zone alternating upsetting and drawing forging process, repeated upsetting and drawing forging is performed at 930–970℃ and T... β The following temperatures (T) β -50℃~T β -30℃), T β The above temperatures (T) β +30℃~T β +50℃) and T β The following temperatures (T) β -50℃~T β Upsetting and drawing forging is performed at -30℃, and recrystallization is achieved to refine the grains and eliminate the α phase at grain boundaries through alternating forging across the β phase region; subsequently, during the quasi-β forging forming process, temperatures below the β phase transformation point (T) are used. β -50℃~T β Two forging processes at -30℃ and temperatures above the β phase transformation point (T) β +10℃~T β The alloy undergoes quasi-β forging at +30℃ to form a basket-like microstructure, ensuring that the duplex titanium alloy possesses high strength, high toughness, and high impact resistance.
[0053] Preferably, in the microstructure of the high-strength, high-toughness, and high-impact-resistant duplex titanium alloy large-size forgings, the β phase content is 3-20%, and the remainder is α phase; the β phase is elongated, with a length of 0.2-10 μm (the average length of the β phase is 2-3 μm, and the average aspect ratio is 3-5:1); the α phase is elongated, with a length of 0.2-90 μm (the average length of the α phase is approximately 6-30 μm, and the average aspect ratio is approximately 4-6:1).
[0054] The high-strength, high-toughness, and high-impact dual-phase titanium alloy large-size forgings have a yield strength ≥879MPa (e.g., 879~892MPa), tensile strength ≥978MPa (e.g., 978~990MPa), elongation ≥13.9% (e.g., 13.9%~14.9%), room temperature impact energy KV2 ≥48.3J (e.g., 48.3~51.1J), and fracture toughness K Q ≥101MPa·m 1 / 2 (e.g., 101~106 MPa·m) 1 / 2 ).
[0055] Preferably, it also includes P5, heat treatment and machining, in which the large-size forging obtained in step P43 is subjected to aging heat treatment, held at 500℃~600℃ for 2~4h, then air-cooled to room temperature, and the black skin on the surface of the large-size forging blank is removed and the surface crack defects are ground off by machine tool processing.
[0056] Preferably, the high-strength, high-toughness, and high-impact dual-phase titanium alloy large-size forgings after heat treatment in step P5 have a yield strength ≥ 862 MPa (e.g., 862~875 MPa), tensile strength ≥ 963 MPa (e.g., 963~973 MPa), elongation ≥ 11.8% (e.g., 11.8%~12.3%), room temperature impact energy KV2 ≥ 47.2 J (e.g., 47.2~48.8 J), and fracture toughness K Q ≥106MPa·m 1 / 2 (e.g., 106~116 MPa·m) 1 / 2 ).
[0057] This invention further regulates the mechanical properties of duplex titanium alloys through heat treatment after forging. Aging heat treatment can reduce the tensile strength, impact toughness and plasticity of forgings, but it will improve the fracture toughness of forgings, i.e. damage tolerance. These changes in mechanical properties are related to the microstructure evolution of the titanium alloy forging, specifically as follows: (1) Aging heat treatment promotes the recovery of the forging structure, that is, it eliminates some of the forging deformation substructure, which easily leads to a decrease in tensile mechanical strength; (2) Aging heat treatment does not change the basket structure morphology formed by quasi-β forging, but it will lead to a certain degree of coarsening of the α+β lamellar structure, which easily leads to a decrease in tensile mechanical strength and impact toughness; (3) Since the β-forming elements enhance the stability of the β phase, 3-20% of the β phase is still retained after forging. Aging heat treatment also easily induces the precipitation of nano-secondary α phase. This phase strengthens the alloy by pinning dislocations. That is, the precipitation of nano-secondary α phase refines the microstructure and hinders the crack propagation path, thereby improving fracture toughness and enhancing the material's ability to resist crack instability propagation, that is, improving damage tolerance performance. Therefore, in actual production, it can be determined whether to carry out a heat treatment process after the forging process of this invention based on the actual needs of the user.
[0058] The present invention has the following beneficial effects:
[0059] 1. This invention involves initial forging in the high-temperature β region (960~1150℃), followed by multiple upsetting and drawing processes to fully break down the as-cast grains; then, cross-phase region upsetting and drawing forging is performed, using T... β The following temperatures (T) β -50℃~T β -30℃ and above (T β +30℃~T β Repeated upsetting and drawing forging at +50℃ refines the grains and eliminates the α phase at grain boundaries through recrystallization; finally, at a temperature below the β phase transformation point (T... β -50℃~T β Two forging processes at -30℃ and above the β phase transformation point (T β +10℃~T β The quasi-β forging process is carried out at +30℃ to form a fine basket structure, thereby ensuring that the duplex titanium alloy has high strength, high toughness and high impact resistance mechanical properties, meeting the strength and high impact resistance requirements of titanium alloy forgings for marine engineering equipment.
[0060] 2. In the final heat of the forming forging process of the quasi-β forging in this invention, T is used. β +10℃~T β Within a temperature range of +30℃, the alloy exhibits low resistance to deformation during processing, making it easier to form. Combined with reasonable control of the deformation amount and rate of each forming process, efficient forging is achieved, resulting in a wider range of industrial production adaptability.
[0061] 3. This invention obtains a duplex titanium alloy forging with basket-like microstructure by controlling the quasi-β forging and aging heat treatment process, which has high strength and excellent toughness and impact performance.
[0062] 4. Compared with existing TC4, TC4ELI and TA31 titanium alloys for marine engineering, the high-strength, high-toughness and high-impact dual-phase titanium alloy with a nominal composition of Ti-5Al-2Mo-2V-1.3Cr-1.3Zr-1Sn-1Fe-0.09O prepared by this invention has the advantages of high strength, high plasticity, high impact resistance and low cost. Moreover, the preparation method is universal, has a short production cycle and high repeatability. Attached Figure Description
[0063] Figure 1 This is a flowchart of the method for preparing high-strength, high-toughness, and high-impact-resistant duplex titanium alloy forgings based on quasi-β forging according to the present invention;
[0064] Figure 2 This is a microstructure diagram of the high-strength, high-toughness, and high-impact-resistant duplex titanium alloy forging prepared in Example 1 of this invention;
[0065] Figure 3 This is a microstructure phase distribution diagram of the high-strength, high-toughness, and high-impact-resistant dual-phase titanium alloy forging prepared in Example 1 of this invention;
[0066] Figure 4 This is a microstructure orientation diagram of the high-strength, high-toughness, and high-impact-resistant duplex titanium alloy forging prepared in Example 1 of this invention;
[0067] Figure 5 This is a microstructure diagram of the high-strength, high-toughness, and high-impact dual-phase titanium alloy forging prepared in Example 2 of this invention. Detailed Implementation
[0068] To better understand the above-mentioned technical solutions of the present invention, the technical solutions of the present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0069] Example 1
[0070] Combination Figure 1 As shown, the preparation method of the high-strength, high-toughness, and high-impact-resistant duplex titanium alloy forging in this embodiment is as follows:
[0071] P1, Preparation of dual-phase titanium alloy VAR ingots, as detailed below:
[0072] Grade 1 sponge titanium standard granules, Al beads, AlMo50 master alloy, AlV50 master alloy, AlCr70 master alloy, sponge Zr, TiSn80 master alloy, iron nails, and TiO2 were prepared according to the nominal composition of duplex titanium alloy: Ti-5Al-2Mo-2V-1.3Cr-1.3Zr-1Sn-1Fe-0.09O. The mixture was pressed into electrode blocks and welded into electrodes. A titanium alloy VAR ingot was obtained through three vacuum arc remelting processes. First, a single VAR melting process was performed (vacuum degree ≤ 5.0 Pa, leakage rate ≤ 1 Pa / min, steady-state current 13~15 kA, steady-state voltage 20~32 V), followed by crystallization in a water-cooled copper crucible. After cooling in a water-cooled copper crucible crystallizer for 3-5 hours, a Φ560 primary unfinished ingot is obtained. This ingot is then subjected to a second VAR melting process (vacuum degree ≤3.0 Pa, leakage rate ≤1 Pa / min, steady-state current 15-17 kA, steady-state voltage 31-33 V). After cooling in a water-cooled copper crucible crystallizer for 4-7 hours, a Φ660 secondary unfinished ingot is obtained. This ingot is then subjected to a third VAR melting process (vacuum degree ≤3.0 Pa, leakage rate ≤1 Pa / min, steady-state current 17-19 kA, steady-state voltage 32-35 V). After cooling in a water-cooled copper crucible crystallizer for 5-9 hours, a Φ760 tertiary finished ingot is obtained. This tertiary finished ingot is used as the dual-phase titanium alloy VAR ingot.
[0073] P2, the dual-phase titanium alloy VAR ingot obtained in step P1 is subjected to high-temperature β-zone forging, as follows:
[0074] P21. First, the dual-phase titanium alloy VAR ingot is coated with two layers of glass insulation coating. Then, it is placed in an electric heating furnace at a furnace temperature of 800℃ for 6 hours. Once the temperature reaches 1100~1120℃, it is held for 10 hours. Next, it is axially upsetting 2 to 3 times with an upsetting deformation of 50 to 70%, forming a square billet with a side length of 720 to 750 mm and a length of 1350 to 1400 mm. Then, the billet is shaped to obtain the first forging billet.
[0075] P22, the hot material of the first forging billet obtained in step P21 is returned to the furnace, the heating time is 3 hours, the temperature is confirmed to reach 1030-1050℃, and it is held for 3 hours. Then, axial upsetting is performed 2-3 times, with upsetting deformation of 50-70%. Then, the billet is shaped to obtain an octagonal forging billet with a cross-sectional side length of 750-800mm and a length of 1480-1540mm. Then, it is air-cooled to room temperature and ground to remove cracks and defects to obtain the second forging billet.
[0076] P3, the second forging billet is subjected to cross-phase region upsetting forging, as detailed below:
[0077] P31, the second forged billet obtained in step P22 is brushed with two coats of glass insulation coating, then placed in an electric heating furnace at a furnace temperature of 800±10℃ for 3 hours, confirming that the temperature reaches 950℃~960℃, and held at that temperature for 9 hours. Next, it undergoes 2-3 axial upsetting operations, with an upsetting deformation of 50-70%. Subsequently, it is shaped into a square billet with a side length of 720-750mm and a cuboid shape with a length of 1350-1400mm. The edges are then sampled by beveling on a saw, and the α-phase → β-phase transformation temperature (referred to as T) of the billet is tested. β The temperature was 910℃, and the third forging billet was obtained;
[0078] P32, return the hot material from the third forged billet obtained in step P31 to the furnace, and raise the temperature for 2 hours to confirm that the temperature reaches 870℃~880℃, which is 30℃~40℃ below the β phase transformation point (T). β -40℃ to T β -30℃, T β =910℃), this T β The temperature is set to the α→β phase transformation temperature and held for 9–11 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming an octagonal forging blank with a cross-sectional side length of 750–800 mm and a length of 1480–1540 mm. After that, the octagonal square blank is shaped to obtain the fourth forging blank.
[0079] P33, return the fourth forged billet hot material obtained in step P32 to the furnace, and raise the temperature for 2 to 3 hours until it reaches 940℃ to 950℃, which is 30℃ to 40℃ above the β phase transformation point (T). β +30℃ to T β +40℃, T β =910℃), this T β The temperature is set to the α→β phase transformation temperature and held for 5–8 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming a square billet with a side length of 750–770 mm and a length of 1350–1410 mm. The billet is then shaped to obtain the fifth forging billet.
[0080] P34, return the fifth forged billet hot material obtained in step P33 to the furnace, and raise the temperature for 1 to 2 hours until it reaches 870℃ to 880℃, which is 30℃ to 40℃ below the β phase transformation point (T). β -40℃ to T β -30℃, T β =910℃), this T βThe temperature is set to the α→β phase transformation temperature and held for 9–11 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming an octagonal forging blank with a cross-sectional side length of 750–800 mm and a length of 1480–1540 mm. After that, the octagonal square blank is shaped, then air-cooled to room temperature, and then ground to obtain the sixth forging blank.
[0081] P4, the sixth forging billet is subjected to quasi-β forging forming and microstructure control;
[0082] P41, apply two coats of glass insulation coating to the sixth forging billet obtained in step P34, then load it into the furnace at 800℃ and heat it for 1 hour, confirming that the temperature reaches 870~880℃, that is, 30~40℃ below the β phase transformation point (T). β -40℃~T β -30℃, T β =910℃), this T β The temperature is set to the α→β phase transformation temperature and held for 6–9 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming a square billet with a cross-sectional side length of 750–770 mm and a cuboid shape with a length of 1350–1410 mm. The billet is then shaped to obtain the seventh forging billet.
[0083] P42, return the hot material of the seventh forged billet obtained in step P41 to the furnace, and raise the temperature for 1 hour to confirm that the temperature reaches 870-880℃, that is, 30-40℃ below the β phase transformation point (T). β -40℃~T β -30℃, T β =910℃), this T β The temperature is set at the α→β phase transformation temperature and held for 3–5 hours. Then, upsetting, widening, drawing, and shaping are carried out. The upsetting and drawing deformation is 40–60%, forming a square billet with a thickness of 300–340 mm, a width of 1560–1600 mm, and a length of 1350–1450 mm. The billet is then air-cooled to room temperature and ground to obtain the eighth forging billet.
[0084] P43, apply two coats of glass insulation coating to the eighth forging billet obtained in step P42, load the furnace at 800℃ and heat for 1 hour, confirming that the temperature reaches 920-930℃, which is 10-20℃ above the β phase transformation point (T). β +10℃~T β +20℃), this T βThe temperature is set to the α→β phase transformation temperature and held for 2–3 hours. Then, the material is drawn, widened, and shaped. The drawing deformation is 20–30%, forming a forging with a thickness of 200–300 mm, a width of 1460–1560 mm, and a length of 1565–1665 mm. This is a large-size forging of high-strength, high-toughness, and high-impact dual-phase titanium alloy with a basket-like structure.
[0085] Figure 2 , Figure 3 , Figure 4 These are EBSD characterization microstructure images of the same region in the high-strength, high-toughness, and high-impact-resistant duplex titanium alloy forging of Example 1 of the present invention. Figure 2 This is a contrast diagram of the area, which shows obvious net basket organization features; Figure 3 By analyzing the phase distribution map of this region, the contents of β phase and α phase can be calculated. Figure 4 This is an orientation diagram of the region, showing the crystallographic orientation of the laths (red, blue, etc. represent different orientations). As can be seen from the diagram, the microstructure of this high-strength, high-toughness, and high-impact dual-phase titanium alloy forging is a fine and uniform basket-like structure. The β phase content in the microstructure is 10-15%, with the remainder being the α phase. The β phase is elongated, with an average length of 2.3 μm and an average aspect ratio of 3.7, and the length range of the β phase is 0.2-7.8 μm. The α phase is also elongated, with an average length of 6.5 μm and an average aspect ratio of 4.3, and the length range of the α phase is 0.2-17 μm.
[0086] The high-strength, high-toughness, and high-impact-resistant duplex titanium alloy forgings prepared in this embodiment were subjected to performance testing. Tensile mechanical properties were tested according to GB / T 228.1-2021, impact toughness according to GB / T 229-2020, and plane strain fracture toughness according to GB / T 21143-2025. The test results are shown in Table 1. The yield strength of the high-strength, high-toughness, and high-impact-resistant duplex titanium alloy forgings in this embodiment is 892 MPa, tensile strength is 989 MPa, elongation is 14.9%, room temperature impact energy KV is 251.1 J, and fracture toughness K... Q 106 MPa·m 1 / 2 .
[0087] Example 2
[0088] This embodiment uses the method of embodiment 1, the difference being that step P5, heat treatment and machining, is included after step P43, as follows:
[0089] The forgings obtained in step P43 were subjected to aging heat treatment, held at 560℃ for 4 hours, then air-cooled to room temperature, and the black skin on the surface of the large-size forging blank was removed and the surface cracks were polished by machine tool processing.
[0090] Figure 5The figures show the microstructure and phase distribution of the high-strength, high-toughness, and high-impact dual-phase titanium alloy forging of this embodiment. As can be seen from the figures, the microstructure of the high-strength, high-toughness, and high-impact dual-phase titanium alloy forging is a fine and uniform basket-like structure. The β phase content in the microstructure is 5-10%, and the remainder is α phase. The β phase is elongated with an average length of 2.3 μm and an average aspect ratio of 3.4. The length range of the β phase is 0.8-6.9 μm. The α phase is elongated with an average length of 30.3 μm and an average aspect ratio of 5.0. The length range of the α phase is 0.8-88.4 μm.
[0091] The high-strength, high-toughness, and high-impact dual-phase titanium alloy forgings prepared in this embodiment were tested using the testing method of Example 1. The test results are shown in Table 1. After aging heat treatment, the high-strength, high-toughness, and high-impact dual-phase titanium alloy forgings of this embodiment have a yield strength of 875 MPa, a tensile strength of 973 MPa, an elongation of 12.3%, a room temperature impact energy KV2 of 48.8 J, and a fracture toughness K Q 116 MPa·m 1 / 2 .
[0092] Example 3
[0093] Combination Figure 1 As shown, the preparation method of the high-strength, high-toughness, and high-impact-resistant duplex titanium alloy forging in this embodiment is as follows:
[0094] P1, Preparation of dual-phase titanium alloy VAR ingots, as detailed below:
[0095] Grade 1 sponge titanium standard granules, Al beads, AlMo50 master alloy, AlV50 master alloy, AlCr70 master alloy, sponge Zr, TiSn80 master alloy, iron nails, and TiO2 were prepared according to the nominal composition of duplex titanium alloy: Ti-5Al-2Mo-2V-1.3Cr-1.3Zr-1Sn-1Fe-0.09O. The mixture was pressed into electrode blocks and welded into electrodes. A titanium alloy VAR ingot was obtained through three vacuum arc remelting processes. First, a single VAR melting process was performed (vacuum degree ≤ 5.0 Pa, leakage rate ≤ 1 Pa / min, steady-state current 13~15 kA, steady-state voltage 20~32 V), followed by crystallization in a water-cooled copper crucible. After cooling in a water-cooled copper crucible crystallizer for 3-5 hours, a Φ560 primary unfinished ingot is obtained. This ingot is then subjected to a second VAR melting process (vacuum degree ≤3.0 Pa, leakage rate ≤1 Pa / min, steady-state current 15-17 kA, steady-state voltage 31-33 V). After cooling in a water-cooled copper crucible crystallizer for 4-7 hours, a Φ660 secondary unfinished ingot is obtained. This ingot is then subjected to a third VAR melting process (vacuum degree ≤3.0 Pa, leakage rate ≤1 Pa / min, steady-state current 17-19 kA, steady-state voltage 32-35 V). After cooling in a water-cooled copper crucible crystallizer for 5-9 hours, a Φ760 tertiary finished ingot is obtained. This tertiary finished ingot is used as the dual-phase titanium alloy VAR ingot.
[0096] P2, the dual-phase titanium alloy VAR ingot obtained in step P1 is subjected to high-temperature β-zone forging, as follows:
[0097] P21. First, the dual-phase titanium alloy VAR ingot is coated with two layers of glass insulation coating. Then, it is placed in an electric heating furnace at a furnace temperature of 800℃ for 6 hours. Once the temperature reaches 1120~1150℃, it is held for 10 hours. Next, it is axially upsetting 2~3 times with an upsetting deformation of 50~60%, forming a square billet with a side length of 720~750mm and a length of 1350~1400mm. Then, the billet is shaped to obtain the first forging billet.
[0098] P22, the hot material of the first forging billet obtained in step P21 is returned to the furnace, the heating time is 3 hours, the temperature is confirmed to reach 1000~1130℃, and it is held for 3 hours. Then, axial upsetting is performed 2 to 3 times, with upsetting deformation of 50~60%. Then, the billet is shaped to obtain an octagonal forging billet with a cross-sectional side length of 750~800mm and a length of 1480~1540mm. Then, it is air-cooled to room temperature and ground to remove cracks and defects to obtain the second forging billet.
[0099] P3, the second forging billet is subjected to cross-phase region upsetting forging, as detailed below:
[0100] P31, the second forged billet obtained in step P22 is brushed with two coats of glass insulation coating, then placed in an electric heating furnace at a furnace temperature of 800±10℃ for 3 hours, confirming that the temperature reaches 930~950℃, and held at that temperature for 9 hours. Next, it undergoes 2~3 axial upsetting operations, with an upsetting deformation of 50~60%. Subsequently, it is shaped into a square billet with a side length of 720~750mm and a length of 1350~1400mm. The edges are then sampled by beveling on a saw, and the α-phase → β-phase transformation temperature (referred to as T) of the billet is tested. β The temperature was 910℃, and the third forging billet was obtained;
[0101] P32, return the hot material of the third forged billet obtained in step P31 to the furnace, and raise the temperature for 2 hours to confirm that the temperature reaches 860℃~870℃, that is, 40℃~50℃ below the β phase transformation point (T). β -50℃ to T β -40℃, T β =910℃), this T β The temperature is set to the α→β phase transformation temperature and held for 9–11 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–60%, forming an octagonal forging blank with a cross-sectional side length of 750–800 mm and a length of 1480–1540 mm. After that, the octagonal square blank is shaped to obtain the fourth forging blank.
[0102] P33, return the fourth forged billet hot material obtained in step P32 to the furnace, and raise the temperature for 2 to 3 hours until it reaches 950 to 960°C, which is 40 to 50°C above the β phase transformation point (T). β +40℃ to T β +50℃, T β =910℃), this T β The temperature is set to the α→β phase transformation temperature and held for 5–8 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–60%, forming a square billet with a cross-sectional side length of 750–770 mm and a cuboid shape with a length of 1350–1410 mm. After that, the billet is shaped to obtain the fifth forging billet.
[0103] P34, return the fifth forged billet hot material obtained in step P33 to the furnace, and raise the temperature for 1 to 2 hours until it reaches 860℃ to 870℃, which is 40℃ to 50℃ below the β phase transformation point (T). β -50℃ to T β -40℃, T β =910℃), this T βThe temperature is set to the α→β phase transformation temperature and held for 9–11 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–60%, forming an octagonal forging blank with a cross-sectional side length of 750–800 mm and a length of 1480–1540 mm. After that, the octagonal square blank is shaped, then air-cooled to room temperature, and then ground to obtain the sixth forging blank.
[0104] P4, the sixth forging billet is subjected to quasi-β forging forming and microstructure control;
[0105] P41, apply two coats of glass insulation coating to the sixth forging billet obtained in step P34, then load it into the furnace at 800℃ and heat it for 1 hour, confirming that the temperature reaches 860~870℃, which is 40~50℃ below the β phase transformation point (T). β -50℃~T β -40℃, T β =910℃), this T β The temperature is set to the α→β phase transformation temperature and held for 6–9 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–60%, forming a square billet with a cross-sectional side length of 750–770 mm and a cuboid shape with a length of 1350–1410 mm. The billet is then shaped to obtain the seventh forging billet.
[0106] P42, return the hot material of the seventh forged billet obtained in step P41 to the furnace, and raise the temperature for 1 hour to confirm that the temperature reaches 860~870℃, that is, 40~50℃ below the β phase transformation point (T). β -50℃~T β -40℃, T β =910℃), this T β The temperature is set at the α→β phase transformation temperature and held for 3–5 hours. Then, upsetting, widening, drawing, and shaping are carried out. The upsetting and drawing deformation is 50–60%, forming a square billet with a thickness of 300–340 mm, a width of 1560–1600 mm, and a length of 1350–1450 mm. The billet is then air-cooled to room temperature and ground to obtain the eighth forging billet.
[0107] P43, apply two coats of glass insulation coating to the eighth forging billet obtained in step P42, load the furnace at 800℃ and heat for 1 hour, confirming that the temperature reaches 930~940℃, which is 20~30℃ above the β phase transformation point (T). β +20℃~T β +30℃), this T βThe temperature is set to the α→β phase transformation temperature and held for 2–3 hours. Then, the material is drawn, widened, and shaped. The drawing deformation is 50–60%, forming a forging with a thickness of 200–300 mm, a width of 1460–1560 mm, and a length of 1565–1665 mm. This is a large-size forging of high-strength, high-toughness, and high-impact dual-phase titanium alloy with a basket-like structure.
[0108] The microstructure of the high-strength, high-toughness, and high-impact dual-phase titanium alloy forging prepared in this embodiment is a fine and uniform basket-like morphology. The β phase content in the microstructure is 10~15%, and the remainder is α phase. The β phase is elongated, with an average length of 2.8 μm and an average aspect ratio of 4.1:1. The length range of the β phase is 0.8~9.7 μm. The α phase is elongated, with an average length of 9.3 μm and an average aspect ratio of 5.2. The length range of the α phase is 0.8~30 μm.
[0109] The high-strength, high-toughness, and high-impact dual-phase titanium alloy forgings prepared in this embodiment were tested using the testing method of Example 1. The test results are shown in Table 1. After aging heat treatment, the high-strength, high-toughness, and high-impact dual-phase titanium alloy forgings of this embodiment have a yield strength of 879 MPa, a tensile strength of 978 MPa, an elongation of 13.9%, a room temperature impact energy KV2 of 48.3 J, and a fracture toughness K Q 101 MPa·m 1 / 2 .
[0110] Example 4
[0111] This embodiment uses the method of embodiment 3, the difference being that: after step P43, step P5 is also included, which involves heat treatment and machining, as detailed below:
[0112] The forgings obtained in step P43 were subjected to aging heat treatment, held at 560℃ for 4 hours, then air-cooled to room temperature, and the black skin on the surface of the large-size forging blank was removed and the surface cracks were polished by machine tool processing.
[0113] The microstructure of this high-strength, high-toughness, and high-impact dual-phase titanium alloy forging is a fine and uniform basket-like structure. The microstructure includes 5-10% β phase and the remainder is α phase; both β and α phases are elongated.
[0114] The high-strength, high-toughness, and high-impact dual-phase titanium alloy forgings prepared in this embodiment were subjected to performance testing using the testing method of Example 1. The test results are shown in Table 1. After aging heat treatment, the high-strength, high-toughness, and high-impact dual-phase titanium alloy forgings of this embodiment have a yield strength of 862 MPa, a tensile strength of 963 MPa, an elongation of 11.8%, a room temperature impact energy KV2 of 47.2 J, and a fracture toughness K Q 106 MPa·m 1 / 2 .
[0115] Comparative Example 1
[0116] This embodiment uses the method of Embodiment 1, the difference being that the specific steps of step P43 are as follows:
[0117] The eighth forging billet obtained in step P42 is coated with two layers of glass insulation coating, and then heated in a furnace at a temperature of 800℃ for 1 hour to reach a temperature of 870-880℃, which is 30-40℃ below the β phase transformation point (T). β -40℃~T β -30℃, T β =910℃), this T β The temperature is set to the α→β phase transformation temperature and held for 2–3 hours. Then, the material is drawn, widened, and shaped. The drawing deformation is 20–30%, forming a forging with a thickness of 200–300 mm, a width of 1460–1560 mm, and a length of 1565–1665 mm. This is a large-size dual-phase titanium alloy forging. Its microstructure is mainly composed of equiaxed α structure, while the β transformation structure forms lamellar α structure.
[0118] The duplex titanium alloy forgings prepared in this comparative example were tested for performance using the testing method of Example 1. The test results are shown in Table 1. After aging heat treatment, the high-strength, high-toughness, and high-impact duplex titanium alloy forgings of this example have a yield strength of 836 MPa, a tensile strength of 935 MPa, an elongation of 17.6%, a room temperature impact energy KV2 of 46.5 J, and a fracture toughness K Q 85 MPa·m 1 / 2 .
[0119] Table 1 Mechanical properties of duplex titanium alloy forgings
[0120]
[0121] As shown in Table 1, compared with Comparative Example 1, the microstructure of the high-strength, high-toughness, and high-impact dual-phase titanium alloy forgings prepared in the embodiments of the present invention is a basketweave structure. Its yield strength is 862~892 MPa, tensile strength is 963~989 MPa, elongation is 11.8~14.9%, room temperature impact energy KV2 is 47.2~51.1 J, and fracture toughness K... Q 101~116 MPa·m 1 / 2 Therefore, it can be seen that the duplex titanium alloy forgings prepared by the method of the present invention can not only ensure the strength and toughness of the duplex titanium alloy forgings, but also have high impact performance and fracture toughness, which has important engineering application value.
[0122] As can be seen from Examples 1 and 2, and Examples 3 and 4, aging heat treatment causes a decrease in the tensile mechanical strength, impact toughness, and plasticity of forgings, but it improves fracture toughness, i.e., damage tolerance. The reason is that: (1) the plastic deformation of forging activates dislocation slip, and dynamic recrystallization is difficult to eliminate a large number of deformation substructures. Therefore, after cooling, the microstructure of large-size forgings contains deformation substructures. With high residual stress, the deformation substructures in the basket structure produce a deformation strengthening effect (or dislocation strengthening). In addition, aging heat treatment can promote recovery and eliminate the deformation substructures formed in the early forging to a certain extent. Therefore, the recovery during the aging heat treatment process can reduce the alloy strength, but can improve the impact toughness, fracture toughness and plasticity of the alloy; (2) the aging heat treatment will not change the basket structure formed by the quasi-β forging, but will lead to a certain degree of coarsening of the α+β lamellar structure, which can easily lead to a decrease in tensile mechanical strength and impact toughness; (3) at the same time, since the β forming elements enhance the stability of the β phase, 3-20% of the β phase is still retained after forging. The aging heat treatment can also easily induce the precipitation of nano-secondary α phase. This phase strengthens the alloy by pinning dislocations. That is, the precipitation of nano-secondary α phase refines the microstructure and hinders the crack propagation path, thereby improving the fracture toughness and enhancing the material's ability to resist crack instability propagation, that is, improving the damage tolerance performance. Therefore, the aging heat treatment can effectively improve the fracture toughness of the dual-phase titanium alloy forgings and reduce the yield strength, tensile strength, elongation and room temperature impact energy of the dual-phase titanium alloy forgings to a certain extent. Therefore, in actual production, it can be determined whether to carry out a heat treatment process after the forging process of the present invention in combination with the actual needs of the user.
[0123] Combining Example 1 and Comparative Example 1, it can be seen that when the final forging process in Comparative Example 1 did not utilize a temperature range 10–30°C above the β phase transformation point, a titanium alloy forging with a basket-like structure could not be obtained. This is because the forming temperature was only 870–880°C, which is 30–40°C below the β phase transformation point (i.e., T...). β -40℃~T β -30℃, T β =910℃), resulting in its microstructure being mainly composed of isometric α-structure, while β-transformation tissue forms lamellar α-structure. s The microstructure of this type of structure, although having a higher elongation than that of the present invention, has lower yield strength, tensile strength, room temperature impact energy, and fracture toughness than the duplex titanium alloy forging with a basket-like structure of the present invention. It is difficult to simultaneously meet the extreme requirements of high strength, high toughness, and impact resistance.
[0124] Those skilled in the art should recognize that the above embodiments are merely illustrative of the present invention and are not intended to limit the present invention. Any variations or modifications to the above embodiments that are within the spirit and essence of the present invention will fall within the scope of the claims of the present invention.
Claims
1. A method for preparing large-sized forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloy, characterized in that: Includes the following steps: P1, Preparation of dual-phase titanium alloy VAR ingots, as detailed below: The raw materials were prepared according to the nominal composition of the duplex titanium alloy Ti-5Al-2Mo-2V-1.3Cr-1.3Zr-1Sn-1Fe-0.09O, pressed and welded into electrodes, and then the duplex titanium alloy VAR ingot was obtained through three vacuum consumable melting processes. P2, the dual-phase titanium alloy VAR ingot obtained in step P1 is subjected to high-temperature β-zone forging, as follows: The dual-phase titanium alloy VAR ingot is heated to 1100-1150℃, held at that temperature, and then subjected to 2-3 axial upsetting and drawing processes to obtain the first forging billet. After that, it is returned to the furnace and heated to 1000-1050℃, held at that temperature, and then subjected to 2-3 axial upsetting and drawing processes, controlling the upsetting and drawing deformation to 50-70%. After shaping, it is air-cooled to room temperature to obtain the second forging billet. P3, the second forging billet is subjected to alternating upsetting and drawing forging in the cross-phase region, as detailed below: The second forging billet is heated to 930–970°C, held at that temperature, and then subjected to 2–3 axial upsetting and drawing processes. After shaping, the α-phase → β-phase transformation temperature of the forging billet is tested to obtain the third forging billet. The billet is then returned to the furnace and heated to 30–50°C below the β-phase transformation point, held at that temperature, and then subjected to 2–3 axial upsetting and drawing processes. After shaping, the fourth forging billet is obtained. The billet is then returned to the furnace and heated to 30–50°C above the β-phase transformation point, held at that temperature, and then subjected to 2–3 axial upsetting and drawing processes. After shaping, the billet is air-cooled to room temperature to obtain the fifth forging billet. The billet is then returned to the furnace and heated to 30–50°C below the β-phase transformation point, held at that temperature, and then subjected to 2–3 axial upsetting and drawing processes with an upsetting deformation of 50–70%. After shaping, the billet is air-cooled to room temperature to obtain the sixth forging billet. P4, the sixth forging billet undergoes quasi-β forging forming and microstructure control, as detailed below: The sixth forging billet is heated to 30–50°C below the β phase transformation point, held at that temperature, and then subjected to 2–3 axial upsetting and drawing operations with an upsetting deformation of 50–70%. After shaping, it is air-cooled to room temperature to obtain the seventh forging billet. The billet is then returned to the furnace and heated to 30–50°C below the β phase transformation point, and then upset, widened, drawn, and shaped with an upsetting deformation of 40–60% to obtain the eighth forging billet. The billet is then returned to the furnace and heated to 10–30°C above the β phase transformation point, and then drawn, widened, and shaped with an elongation deformation of 20–30% to form a large-sized forging with a thickness of 200–300 mm, a width of 1460–1560 mm, and a length of 1565–1665 mm. After air-cooling to room temperature, it becomes a large-sized forging of high-strength, high-toughness, and high-impact dual-phase titanium alloy with a basketweave structure.
2. The method for preparing large-size forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloy according to claim 1, characterized in that: In step P1: The raw materials used in the formulation include Grade 1 sponge titanium standard granules, Al beans, AlMo50 master alloy, AlV50 master alloy, AlCr70 master alloy, sponge Zr, TiSn80 master alloy, iron nails and TiO2. In step P1, the composition of the dual-phase titanium alloy VAR ingot is as follows by mass percentage: Al: 4.5%~5.5%, V: 1.5%~2.5%, Mo: 1.5%~2.5%, Cr: 1%~2%, Zr: 1%~2%, Sn: 0.5%~1.5%, Fe: 0.5%~1.5%, with the balance being Ti and unavoidable impurity elements; The unavoidable impurity elements are C≤0.02%, O≤0.12%, N≤0.01%, and H≤0.002%.
3. The method for preparing large-size forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloy according to claim 1, characterized in that: In step P1, the three-stage vacuum consumable melting process includes the following steps: The first vacuum self-consumption melting was carried out with the vacuum degree controlled at ≤5.0Pa, the leakage rate at ≤1Pa / min, the steady-state current at 13~15kA, and the steady-state voltage at 20~32V. The ingot obtained from the melting was cooled in a water-cooled copper crucible crystallizer for 3~5 hours to obtain a Φ560 primary non-finished ingot. The second vacuum self-consumption melting process was carried out with the vacuum degree controlled at ≤3.0Pa, the leakage rate at ≤1Pa / min, the steady-state current at 15~17kA, and the steady-state voltage at 31~33V. The ingot obtained from the melting process was cooled in a water-cooled copper crucible crystallizer for 4~7 hours to obtain a Φ660 secondary non-finished ingot. The third vacuum self-consumable melting process was carried out with the vacuum degree controlled at ≤3.0Pa, the leakage rate at ≤1Pa / min, the steady-state current at 17~19kA, and the steady-state voltage at 32~35V. The ingot obtained from the melting process was cooled in a water-cooled copper crucible crystallizer for 5~9 hours to obtain a duplex titanium alloy VAR ingot with a specification of Φ760.
4. The method for preparing large-size forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloy according to claim 1, characterized in that: Step P2 specifically includes the following procedures: P21. First, the dual-phase titanium alloy VAR ingot is coated with two layers of glass insulation coating. Then, it is placed in an electric heating furnace at a furnace temperature of 800±10℃ and heated for 6±0.5h. The temperature is confirmed to reach 1100~1150℃ and held for 9~12h. Then, it is axially upsetting and drawing 2~3 times with an upsetting deformation of 50~70% to form a square billet with a side length of 720~750mm and a length of 1350~1400mm. The billet is then shaped to obtain the first forging billet. P22, return the hot material of the first forging billet completed in step P21 to the furnace, raise the temperature for 3 to 4 hours, confirm that the temperature reaches 1000 to 1050℃, and hold it for 2 to 5 hours. Then, perform 2 to 3 axial upsetting and drawing operations, with an upsetting deformation of 50 to 70%. After that, perform square billet shaping to form an octagonal forging billet with a cross-sectional side length of 750 to 800 mm and a length of 1480 to 1540 mm. Then, air cool it to room temperature and grind it to remove cracks and defects to obtain the second forging billet.
5. The method for preparing large-scale forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloy according to claim 4, characterized in that: Step P3 specifically includes the following procedures: P31. The second forging billet is coated with two layers of glass insulation coating, and then placed in an electric heating furnace at a furnace temperature of 800±10℃ for 2-3 hours. The temperature is confirmed to reach 930-970℃ and held for 7-11 hours. Then, it is axially upsetting 2-3 times with an upsetting deformation of 50-70%. Subsequently, it is shaped into a square billet with a side length of 720-750mm and a cuboid shape with a length of 1350-1400mm. The α-phase → β-phase transformation temperature of the forging billet is tested by taking a sample from the hot material to obtain the third forging billet. P32, the third forging billet obtained in step P31 is heated and the heating time is 1-2 hours, the temperature is confirmed to reach 30-50°C below the β phase transition point, i.e. T β -50°C to T β -30°C, the T β is the α→β phase transition temperature, and the temperature is maintained for 9-11 hours, then 2-3 times of axial upsetting and drawing are carried out, the upsetting and drawing deformation is 50-70%, an octagonal forging billet with a cross section side length of 750-800 mm and a length of 1480-1540 mm is formed, then octagonal square billet shaping is carried out, and a fourth forging billet is obtained; P33, first return the hot material of the fourth forged billet obtained in step P32 to the furnace, and raise the temperature for 2 to 3 hours until it reaches 30 to 50°C above the β phase transformation point, i.e., T. β +30℃~T β +50℃, this T β The temperature is set to the α→β phase transformation temperature and held for 5–8 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming a square billet with a side length of 750–770 mm and a length of 1350–1410 mm. The billet is then shaped to obtain the fifth forging billet. P34, return the fifth forged billet hot material obtained in step P33 to the furnace, and raise the temperature for 1 to 2 hours until it reaches 30 to 50°C below the β phase transformation point, i.e., T. β -50℃~T β -30℃, this T β The temperature is set to the α→β phase transformation temperature and held for 9–11 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming an octagonal forging billet with a cross-sectional side length of 750–800 mm and a length of 1480–1540 mm. After that, the octagonal square billet is shaped, then air-cooled to room temperature, and then ground to obtain the sixth forging billet.
6. The method for preparing large-size forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloy according to claim 5, characterized in that: Step P4 specifically includes the following procedures: P41, apply two coats of glass insulation coating to the sixth forging billet obtained in step P34, then load the furnace at a temperature of 800±10℃ and heat for 1-2 hours, confirming that the temperature reaches 30-50℃ below the β phase transformation point, i.e., T. β -50℃~T β -30℃, this T β The temperature is set to the α→β phase transformation temperature and held for 6–9 hours. Then, axial upsetting is performed 2–3 times with an upsetting deformation of 50–70%, forming a square billet with a side length of 750–770 mm and a length of 1350–1410 mm. The billet is then shaped, air-cooled to room temperature, and ground to obtain the seventh forging billet. P42, return the hot material of the seventh forged billet obtained in step P41 to the furnace, and raise the temperature for 1 to 2 hours until it reaches 30 to 50°C below the β phase transformation point, i.e., T. β -50℃~T β -30℃, this T β The temperature is set at the α→β phase transformation temperature and held for 3–5 hours. Then, upsetting, widening, drawing, and shaping are carried out, with an upsetting and drawing deformation of 40–60%, forming a rectangular billet with a thickness of 300–340 mm, a width of 1560–1600 mm, and a length of 1350–1450 mm. The billet is then air-cooled to room temperature and ground to obtain the eighth forging billet. P43, apply two coats of glass insulation coating to the eighth forging billet obtained in step P42, load the furnace at a temperature of 800±10℃, and heat for 2-3 hours until the temperature reaches 10-30℃ above the β phase transformation point, i.e., T. β +10℃~T β +30℃, this T β The temperature is set to the α→β phase transformation temperature and held for 2–3 hours. Then, the parts are drawn, widened, and shaped, with a drawing deformation of 20–30%, forming large-sized forgings with a thickness of 200–300 mm, a width of 1460–1560 mm, and a length of 1565–1665 mm. The forgings are then air-cooled to room temperature.
7. The method for preparing large-size forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloy as described in claim 6, characterized in that, In steps P2 to P4, a high-speed forging machine with a tonnage of ≥60MN is used for upsetting and drawing. The upsetting deformation rate is 20-35mm / s, and the drawing deformation rate is 30-55mm / s. In steps P3 to P4, the T β The temperature is 910–915℃.
8. The method for preparing large-size forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloy according to claim 1, characterized in that: In the microstructure of the large-sized high-strength, high-toughness, and high-impact dual-phase titanium alloy forgings, the β phase content is 3-20%, and the remainder is α phase; the β phase is elongated with a length of 0.2-10 μm; the α phase is elongated with a length of 0.2-90 μm. The high-strength, high-toughness, and high-impact-resistant duplex titanium alloy large-size forgings have a yield strength ≥879MPa, tensile strength ≥978MPa, elongation ≥13.9%, room temperature impact energy KV2 ≥48.3J, and fracture toughness K Q ≥101MPa·m 1 / 2 .
9. The method for preparing large-size forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloy according to claim 1, characterized in that: It also includes P5, heat treatment and machining. The large-size forgings obtained in step P4 are subjected to aging heat treatment, held at 500℃~600℃ for 2~4h, then air-cooled to room temperature, and the black skin on the surface of the large-size forging billet is removed and the surface cracks are ground off by machine tool processing.
10. The method for preparing large-size forgings of high-strength, high-toughness, and high-impact dual-phase titanium alloy according to claim 9, characterized in that: The high-strength, high-toughness, and high-impact dual-phase titanium alloy large-size forgings after heat treatment in step P5 have a yield strength ≥862MPa, tensile strength ≥963MPa, elongation ≥11.8%, room temperature impact energy KV2 ≥47.2J, and fracture toughness K Q ≥106MPa·m 1 / 2 .
Citation Information
Patent Citations
Preparation method of alpha titanium alloy forging stock
CN105063527A
Forging technology for abnormal structure of TC18 titanium alloy raw material
CN105441845A
Beta forging and heat treating method of TC4 titanium alloy disc forge piece
CN109482796A
Preparation method of A1-grade nondestructive inspection high-impact-toughness TC4 titanium alloy large-specification bar
CN121874537A
Process method for efficiently preparing high-strength and high-impact-resistance titanium alloy forge piece through beta forging
CN116921596A