Casing, individual cells and battery pack
By controlling the product of gloss, phase change conversion rate, and sidewall height of the titanium alloy battery casing, the problems of cracking and fracture during the forming process of the titanium alloy casing were solved, achieving a balance between high ductility and strength of the battery casing, and improving the forming stability and structural rigidity of the battery.
Patent Information
- Application Number
- CN202611142206.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-07-30
AI Technical Summary
Titanium alloy battery casings are prone to cracking or breaking during molding, affecting the molding stability and strength of the battery.
By adjusting the product A×X×H of the shell's gloss A, phase transformation conversion rate X, and sidewall height H within the range of 3.5≤A×X×H≤1911, the forming process of the titanium alloy is optimized, residual stress is reduced, and the ductility and strength of the shell are balanced.
This improves the molding stability and structural rigidity of the casing, reduces the risk of fracture during the stretching process, and ensures the high ductility and strength of the battery.
Smart Images

Figure CN122677600B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of new energy technology, specifically to a casing, a single battery cell, and a battery pack. Background Technology
[0002] To meet the demand for lightweight batteries, the battery casing can be made of titanium alloy, which can reduce the overall weight of the battery, increase energy density, and titanium alloy has excellent corrosion resistance and high strength, which can effectively extend the battery's service life.
[0003] In the battery casing manufacturing process, it is usually made from a single piece of metal sheet through a stretching process, and the sidewalls and bottom wall are integrally formed. However, when titanium alloy is used for stretching, due to the high yield strength and low plastic deformation capacity of titanium alloy, cracks are prone to occur in the sidewalls of the casing, or cracks are prone to occur at the corners of the sidewalls and bottom wall, and even breakage may occur. Summary of the Invention
[0004] In view of this, this application provides a casing, a single battery cell, and a battery pack to solve the problem that titanium alloy casings are prone to cracking or even breakage during molding.
[0005] In a first aspect, this application provides a housing, comprising: The end wall and side wall are integrally formed, with the side wall extending from one end of the end wall in a direction perpendicular to the plane of the end wall; the side wall and the end wall together form a receiving cavity; The titanium content in the shell is ≥99.0%; the gloss of the shell is A GU; and the phase transformation conversion rate of the shell is X AHX. The height of the sidewall is H mm along the direction perpendicular to the plane containing the end wall; It satisfies: 3.5≤A×X×H≤1911.
[0006] Beneficial Effects: This application improves the shell's ductility while maintaining its strength and molding stability by adjusting the range of A×X×H, ensuring sufficient structural stiffness and resistance to deformation even with high ductility. Specifically, when the values of A×X×H exceed the upper limit, the proportion of glossiness A, the proportion of phase transformation conversion rate X, or the proportion of sidewall height H becomes too high. An excessively high proportion of glossiness A intensifies the phase transformation of titanium, making it more prone to α-phase to β-phase transformation, leading to reduced shell strength. An excessively high proportion of phase transformation conversion rate X results in excessive coarsening of β-phase grains, further reducing shell strength. Furthermore, an excessively high proportion of stretching height leads to increased deformation of the end walls and / or sidewalls, also affecting the shell's structural strength and increasing the risk of shell breakage during battery vibration. When A×X×H is below the lower limit, the proportion of glossiness A is too small, the proportion of phase transformation conversion rate X is too small, or the proportion of sidewall height H is too low. The proportion of glossiness A is too small, resulting in insufficient release of residual stress. The proportion of phase transformation conversion rate X is too small, which means that the proportion of α phase is relatively high. This makes the shell have high strength but poor plasticity and insufficient material ductility. The shell is more difficult to form, and cracks are easy to occur between the end wall and the sidewall during stretching, which affects the molding yield.
[0007] Secondly, this application also provides a single-cell battery, comprising: Battery cell; And as described above, the battery cell is housed within the housing cavity of the housing.
[0008] Since a single battery cell includes a casing and has the same effect as the casing, it will not be elaborated further here.
[0009] Thirdly, this application also provides a battery pack, comprising: The housing; and multiple individual batteries as described above housed within the housing.
[0010] Since the battery pack includes individual cells and has the same effect as individual cells, it will not be elaborated further here. Attached Figure Description
[0011] To more clearly illustrate the technical solutions in the specific embodiments of this application or the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0012] Figure 1 This is an exploded view showing that the shell of this application is cylindrical; Figure 2 This is a front view of the end wall of the cylindrical shell in this application; Figure 3 for Figure 2 Schematic diagram of section AA; Figure 4 for Figure 3 Enlarged view of point B in the middle; Figure 5 for Figure 3 Enlarged view of point C in the middle; Figure 6 This is a three-dimensional schematic diagram showing that the shell of this application is prismatic. Figure 7 This is a schematic diagram of the battery device of this application; Figure 8 This is an exploded view of the battery pack in this application.
[0013] Explanation of reference numerals in the attached figures: 1. End wall; 11. First groove; 12. First protrusion; 2. Side wall; 21. Second groove; 22. Second protrusion; 3. Receiving cavity; 4. Opening; 5. Cover plate; 900, Vehicle; 800, Battery unit; 810, Battery pack; 811, Housing; 812, Cover; 813, Battery group; 700, Controller. Detailed Implementation
[0014] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0015] In the description of this application, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0016] In the description of this application, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.
[0017] Furthermore, the technical features involved in the different embodiments of this application described below can be combined with each other as long as they do not conflict with each other.
[0018] In the molding process, the battery casing is usually made from a single piece of metal sheet through a stretching process, and the side walls and bottom walls are integrally formed. However, during stretching, cracks are prone to occur in the side walls of the casing, or at the corners of the side walls and bottom walls, and even breakage may occur.
[0019] Research has found that the main cause of cracks or fractures in the sidewalls of the battery casing is the high residual stress after stretching, which prevents the casing from being stretched to a greater height, thus limiting the size of the battery. To address this issue, this application proposes adjusting the gloss of the battery casing to reduce internal residual stress and facilitate casing stretching and forming.
[0020] The following is combined Figures 1 to 8 This describes an embodiment of the present application.
[0021] According to embodiments of this application, in one aspect, a housing is provided, comprising: The end wall 1 and the side wall 2 are integrally formed. The side wall 2 extends from one end of the end wall 1 in a direction perpendicular to the plane of the end wall 1. The side wall 2 and the end wall 1 enclose a receiving cavity 3. An opening 4 is formed at the end of the side wall 2 away from the end wall 1. The titanium content in the shell is ≥99.0%; the gloss of the shell is A GU; and the phase transformation conversion rate of the shell is X AHX. Along the direction perpendicular to the plane containing end wall 1, the height of side wall 2 is H mm; It satisfies: 3.5≤A×X×H≤1911.
[0022] A housing is a component used to provide a space to house electrode assemblies and other parts and isolate them from the outside environment. A housing typically includes a body with an opening at at least one end and a receiving cavity. The opening of the housing can be closed by a cover plate to seal and isolate the internal environment of the battery cell from the external environment.
[0023] Combination Figure 1 , Figure 6As shown, the shell can be cylindrical, elliptical cylindrical, prismatic, etc., wherein the prismatic shape can include square prismatic, rectangular prismatic, hexagonal prismatic or other polygonal cross-section prismatic.
[0024] In this embodiment, the housing includes an integrally formed end wall 1 and a side wall 2, which can be formed from a single piece of metal sheet through a stretching process. The side wall 2 extends along the edge of the end wall 1, and the extension direction of the side wall 2 is perpendicular to the plane of the end wall 1, so that the end wall 1 and the side wall 2 together enclose a receiving cavity 3 for accommodating the battery cell. The opening 4 is disposed opposite to the end wall 1, which facilitates the insertion of the battery cell into the receiving cavity 3 through the opening 4.
[0025] This application can reduce the residual stress of the shell by adjusting the gloss of the shell, thereby facilitating the stretching and forming of the shell; however, if the gloss A is too high, the titanium element will undergo a phase transformation from α phase to β phase, and the phase transformation conversion rate X will increase accordingly, resulting in a decrease in shell strength. The higher the phase transformation conversion rate X, the coarser the β phase grains, and the worse the shell strength. At this time, it is necessary to appropriately reduce the sidewall height H to ensure the forming stability of the shell.
[0026] It should be noted that the phase transformation conversion rate refers to the proportion of the new phase (or the parent phase that participated in the transformation) that has already undergone the phase transformation process; the phase transformation conversion rate quantitatively describes the degree of phase transformation.
[0027] The α phase (Alpha phase) is an allotrope of titanium that exists at lower temperatures and has a hexagonal close-packed (HCP) crystal structure. The hexagonal close-packed crystal structure gives the α phase high strength, good heat resistance and good creep resistance, but it has fewer slip systems and relatively weak plastic deformation ability (i.e., it is brittle).
[0028] The β phase is an allotrope of titanium that exists at higher temperatures and has a body-centered cubic (BCC) crystal structure. The BCC structure has more slip systems, therefore the β phase possesses excellent plasticity, toughness, and cold-forming ability, but its strength and heat resistance are inferior to the α phase.
[0029] Shell structural components typically require high yield strength and tensile strength. Because the crystal structure of the β phase inherently limits its strength compared to the α phase, improper annealing or heat treatment processes (e.g., excessively rapid cooling or excessively high annealing temperature) can lead to an excess of β phase in the microstructure or the formation of coarse β grains, significantly reducing the overall yield strength and tensile strength of the material. Furthermore, excessive β phase can also reduce the material's creep resistance and high-temperature resistance, making it prone to plastic deformation when subjected to the structural loads required by the shell, thus failing to meet the high-strength design requirements.
[0030] Although the alpha phase provides high strength, its close-packed hexagonal structure exhibits poor plastic deformation capacity at room temperature. If the proportion of the alpha phase in the material is too large (for example, the formation of a large number of primary alpha phases or coarse lamellar alpha phases), the material's plasticity and fracture toughness will decrease sharply. This structure is difficult to absorb energy through plastic deformation under impact loads or stress concentration, making it highly susceptible to brittle fracture.
[0031] Therefore, in α+β type titanium alloys, a good balance between strength and toughness is achieved through the proper combination of these two phases.
[0032] This application modifies the residual stress distribution of the shell by adjusting its gloss level (A), thereby indirectly influencing the phase transformation during heat treatment to balance the shell's formability and mechanical strength. Specifically, controlling the gloss level (A) within a suitable range effectively suppresses excessive transformation from the α phase to the β phase, maintaining the phase transformation rate (X) within a reasonable threshold. This ensures that the final microstructure retains a sufficient amount of the α phase to provide necessary strength, while simultaneously retaining an appropriate amount of the β phase to maintain necessary plastic deformation capacity.
[0033] When the gloss level A of the shell is too low, the residual stress is not fully eliminated, the material has insufficient ductility, and cracks or even tears are likely to appear on the sidewall 2 during the stretching process. When the gloss level A of the shell is too high, the phase transformation of titanium element is intensified, the α phase is transformed into the β phase, and the β phase grains are coarsened, which makes the shell more ductile and easier to form, but will lead to a decrease in shell strength.
[0034] The following explains how the gloss of the casing affects its residual stress and toughness: Titanium metal has extremely high "high-temperature activity"; when the annealing temperature is too high, the titanium surface reacts violently with oxygen in the air, forming a thick oxide scale (oxide layer). Furthermore, excessively high annealing temperatures can also lead to coarsening of the grains inside the material, resulting in a decrease in the overall yield strength and tensile strength of the material.
[0035] At relatively low and appropriate annealing temperatures (such as stress-relief annealing or low-temperature full annealing), the oxidation reaction is suppressed, the oxidation reaction on the titanium surface is mild, and the resulting oxide film is extremely thin. Because no thick oxide scale forms on the surface, the original dense surface of titanium metal is preserved, maintaining its metallic color and reflecting light well, thus exhibiting a high gloss on a macroscopic scale.
[0036] It should also be noted that, under appropriate annealing temperatures, the higher the annealing temperature, the better the gloss of the shell, which can better reduce residual stress, improve toughness, and facilitate molding; under appropriate annealing temperatures, the lower the annealing temperature, the worse the gloss of the shell, the greater the residual stress, and the lower the toughness.
[0037] Therefore, gloss is not only a direct reflection of surface morphology, but also a macroscopic mapping of the internal microstructure. This means that by monitoring changes in gloss A, we can inversely deduce the thermal effects experienced by the material.
[0038] This application further adjusts the range of A×X×H, thereby improving the shell's ductility while taking into account its strength and forming stability, ensuring that the shell still has sufficient structural stiffness and resistance to deformation under high ductility.
[0039] Specifically, when the values of A×X×H exceed the upper limit, the proportion of glossiness A, the proportion of phase transformation conversion rate X, or the proportion of sidewall height H in the shell becomes too high. An excessively high proportion of glossiness A intensifies the phase transformation of titanium, making it prone to α-phase to β-phase transformation, leading to a decrease in shell strength. An excessively high proportion of phase transformation conversion rate X results in excessive coarsening of β-phase grains, further reducing shell strength. Furthermore, an excessively high proportion of stretching height leads to increased deformation of the end walls and / or sidewalls, also affecting the structural strength of the shell and increasing the risk of shell breakage during battery vibration. Conversely, when A×X×H is below the lower limit, the proportion of glossiness A, the proportion of phase transformation conversion rate X, or the proportion of sidewall height H becomes too low. A low proportion of glossiness A results in insufficient release of residual stress. A low proportion of phase transformation conversion rate X, meaning a high proportion of α-phase, results in a shell with high strength but poor plasticity and insufficient material ductility, increasing the difficulty of shell molding and making cracking between the end walls and sidewalls during stretching, thus affecting molding yield.
[0040] When the gloss level A of the shell is too low, the residual stress is not fully eliminated, the material has insufficient ductility, and the sidewall 2 is prone to cracks or even tears during the stretching process. When the gloss level A of the shell is too high, the phase transformation of titanium is intensified, the β phase grains coarsen, the shell has good toughness and is easy to form, but it will lead to a decrease in shell strength.
[0041] The higher the phase transformation conversion rate X of the shell, the more significant the phase transformation of titanium from α to β phase, the coarser the β phase grains, and the more significant the decrease in shell strength. Conversely, when the phase transformation conversion rate X is too low, the proportion of α phase grains is too high, the material is brittle, and local fractures are prone to occur during stretching.
[0042] It should be noted that the height H of the sidewall 2 needs to match the design height of the battery cell. When the design height of the battery cell increases, H needs to increase synchronously to ensure that the depth of the receiving cavity 3 is adapted. Therefore, H must meet the functional requirements while taking into account the molding stability and structural reliability.
[0043] When the height H of sidewall 2 is too large, the excessive stretching height will lead to greater deformation of endwall 1. As the material flows, endwall 1 becomes thinner, affecting the structural strength of the casing. Conversely, when the height H of sidewall 2 is too small, the volume of the casing is insufficient, making it difficult to meet installation requirements. Furthermore, when the height H of sidewall 2 is too large, with a constant volume of structural adhesive, the overlap height between the structural adhesive and sidewall 2 is constant. The bonding area of the structural adhesive to the casing during battery installation is relatively small, easily resulting in insufficient constraint on the casing. Moreover, the endwall 1 of the casing is prone to deformation due to excessive deformation, causing the pressure relief valve to open at a higher pressure, leading to excessive pressure inside the casing. When the height H of sidewall 2 is too small, the deformation of endwall 1 of the casing is relatively small, resulting in a thicker endwall 1, poor heat dissipation, and heat accumulation on the bottom surface of the battery, which can easily affect the battery's charging and discharging performance.
[0044] It should be noted that the titanium content in the shell is ≥99.0%. When the titanium content is ≥99.0%, the shell material has sufficient ductility to withstand tensile deformation, which alleviates the stress concentration at the connection between the end wall and the side wall, thereby reducing the risk of crack formation and improving the product molding yield. The titanium content can be controlled by the amount of titanium powder added.
[0045] In addition to titanium, the shell also contains carbon, with the carbon content ranging from 0.01% to 0.08% of the total element content in the titanium shell. This is controlled by the amount of carbon powder incorporated. Other elements may also be present, and their content is controlled by the amount of powdered iron, oxygen, nitrogen, carbon, and sulfur incorporated (the powdered content of these other elements ranges from 0.02% to 0.09% of the total element content in the titanium shell). For example, the Fe content may range from [missing information - likely a percentage] of the total element content in the shell. The carbon content in the battery casing ranges from 0.006% to 0.3%; the oxygen content ranges from 0.005% to 0.25%; the nitrogen content ranges from 0.001% to 0.05%; the sulfur content ranges from 0.0002% to 0.01%. The higher the amount of other elements in powder form, the lower the carbon content in the battery casing; conversely, the lower the amount of other elements in powder form, the higher the carbon content in the battery casing. Test method for the mass content ratio of each element: The mass content of each element in the battery casing is tested according to GB / T17359-2023 standard, and the element content ratio is calculated.
[0046] In this application, the content of titanium can be specifically 99.0%, 99.02%, 99.05%, 99.08%, 99.11%, 99.14%, 99.17%, 99.2%, 99.23%, 99.26%, 99.29%, 99.32%, 99.35%, 99.38%, 99.41%, 99.44%, 99.47%, 99.5%, 99.53%, 99.56%, 99.59%, 99.62%, 99.65%, 99.68%, 99.71%, 99.74%, 99.77%, 99.8%, 99.83%, 99.86%, 99.89%, 99.92%, 99.95%, or 99.99%, etc.
[0047] The specific methods for controlling gloss A are as follows: Within an appropriate annealing temperature range (e.g., stress-relief annealing or low-temperature full annealing), the higher the annealing temperature, the more intense the reaction between the titanium surface and oxygen in the air, the more obvious the surface phase transformation, and the greater the gloss; conversely, the lower the annealing temperature, the milder the annealing oxidation reaction, and the lower the gloss. As a specific example, controlling the annealing temperature at around 940℃ yields finer α-lamellae and higher grain boundary density, which is most beneficial for improving material fatigue performance and microstructure uniformity, resulting in a better gloss A. Alternatively, polishing (physical grinding or electrolyte plasma polishing) can be used. For example, under optimized electrolyte plasma polishing processes (e.g., 280V, 90℃, 40mm immersion depth), surface roughness can be significantly reduced, and gloss can be improved to an extremely high level.
[0048] The specific methods for controlling the phase transition conversion rate are as follows: Addition of alloying elements: Introducing specific alloying elements (such as Al, V, Mo, etc.) can change the phase transformation temperature of the material (such as lowering the β transformation temperature), thereby obtaining different phase transformation conversion rates within the same temperature window.
[0049] Micro-doping: Introducing a small amount of exogenous elements or ions into a crystal can induce local lattice distortion, stress field, or charge rearrangement. This microscopic change can reconstruct the free energy distribution of the system, alter the stability of the metastable state and the phase transition path, thereby precisely controlling the critical point of the phase transition, the conversion rate, and the width of the phase coexistence region.
[0050] The specific control window for phase transition conversion rate is as follows: β-stabilizing element ratio window: By adjusting the percentage of β-stabilizing elements (such as vanadium and molybdenum) (e.g., fine-tuning between 4% and 8%), the β-phase transformation temperature of the material can be precisely set. For example, increasing the content of β-stabilizing elements can enable the material to achieve a higher β-phase transformation rate at a lower annealing temperature.
[0051] Doping concentration window: For novel titanium alloys or special materials, the concentration of trace dopants is usually controlled at an extremely low atomic percentage (e.g., 0.1%-2%). Within this threshold range, doping can effectively induce lattice distortion, stabilize specific metastable phases, or change the hysteresis effect of phase transitions, thereby achieving nonlinear or threshold-type control of the phase transition conversion rate.
[0052] For example, in this embodiment, the value of A×X×H can be 3.5 or 4.7 or 6.2 or 8.1 or 9.9 or 12.3 or 15.6 or 18.9 or 19.6 or 22.4 or 26.1 or 30.5 or 32.8 or 34.8 or 39.2 or 44.7 or 49.9 or 50.3 or 56.8 or 63.5 or 71.2 or 79.9 or 88.6 or 98.3 or 109.1 or 121.7 or 134.4 or 135.4 or 150.2 or 166.8 or 185.3 or 205.9 or 218.4 or 228.6 or 253.4 or 280.2 or 309.1 or 340.7 or 373.4 or 375.3 or 413.2 or 454.8 or 499.6 or 548.3 or 601.2 or 625.0 or 658.7 or 721.4 or 789.9 or 864.6 or 946.3 or 994.5 or 1035.7 or 1133.2 or 1239.8 or 1356.4 or 1483.9 or 1622.7 or 1630.0 or 1659.8 or 1773.5 or 1911, etc., can also be any range formed by any two of the above values.
[0053] As a further preferred option, the range of values for A×X×H satisfies: 30≤A×X×H≤1400.
[0054] When the formula value of A×X×H satisfies the above preferred range of 30≤A×X×H≤1400, the extensibility of the shell can be better improved, making it easier to form. At the same time, it has a certain structural strength during the forming process and is not prone to cracking.
[0055] For example, when the formula value of A×X×H satisfies the above preferred range of 30≤A×X×H≤1400, the value of A×X×H can be 30 or 37 or 44 or 51 or 58 or 65 or 72 or 79 or 86 or 93 or 100 or 108 or 116 or 124 or 132 or 140 or 148 or 156 or 164 or 172 or 180 or 188 or 196 or 204 or 212 or 220 or 228 or 236 or 244 or 252 or 260 or 268 or 276 or 2 84 or 292 or 300 or 309 or 318 or 327 or 336 or 345 or 354 or 363 or 372 or 381 or 390 or 399 or 408 or 417 or 426 or 435 or 444 or 453 or 462 or 471 or 480 or 489 or 498 or 507 or 516 or 525 or 534 or 543 or 552 or 561 or 570 or 579 or 588 or 597 or 606 or 615 or 624 or 633 or 642 or 651 or 660 or 669 or 678 or 687 or 696 or 705 or 714 or 723 or 732 or 741 or 750 or 760 or 770 or 780 or 790 or 800 or 810 or 820 or 830 or 840 or 850 or 860 or 870 or 880 or 890 or 900 or 911 or 922 or 933 or 944 or 955 or 966 or 977 or 988 or 999 or 1010 or 1021 or 1032 or 1043 or 1054 or 1065 or 1076 or 1087 or 1098 or 1109 or 1120 or 1131 or 1142 or 1153 or 1164 or 1175 or 1186 or 1197 or 1208 or 1219 or 1230 or 1241 or 1252 or 1263 or 1274 or 1285 or 1296 or 1307 or 1318 or 1329 or 1340 or 1351 or 1362 or 1373 or 1384 or 1395 or 1400, etc., or any range formed by any two of the above values.
[0056] It should be noted that the specific measurement method for the gloss A of the casing is as follows: A gloss meter, such as the BGD516 model, is used. The instrument is brought into contact with the surface of the end wall 1 and / or side wall 2 of the housing to be tested, and the readings are taken. Multiple measurements are performed, and the arithmetic mean is taken as the final gloss value. During measurement, ensure that the instrument probe is in close contact with the surface being tested to avoid measurement errors caused by external light interference or probe tilt.
[0057] The method for measuring the phase transition conversion rate X of the shell is as follows: I. Sample Preparation Requirements To ensure the accuracy of the test, sample preparation must meet the following specifications: Shape and size: The shell is processed into a circular shape with a diameter of 3-8mm.
[0058] II. Testing and Data Processing Instrumental testing: The prepared sample and blank sample are placed in the DSC instrument and heated or cooled under a set temperature control program and a specific atmosphere. The blank sample is an empty crucible without any sample.
[0059] Curve analysis: The instrument records the relationship between the difference in heat flow rate (heat power difference) between the supplied sample and the blank sample and temperature or time, generating a DSC curve.
[0060] The area of the endothermic or exothermic peak in the DSC curve represents the total energy (ΔH) released or absorbed during the phase transition process. The specific steps for calculating the phase transition conversion rate at a specific temperature using the DSC curve are as follows: Total enthalpy change (total peak area): Baseline correction and integration are performed on the entire phase transition peak on the DSC curve to obtain the total enthalpy change (i.e., the area of the entire peak, denoted as Atotal or ΔHtotal) when the phase transition process is fully completed.
[0061] Partial enthalpy change (partial peak area): Determine the target temperature point for calculating the conversion rate. Starting from the phase transition initiation point, integrate the peak areas of the DSC curve before that temperature point to obtain the enthalpy change of the phase transition that has already occurred at that temperature (i.e., the area of part of the peaks, denoted as AT or ΔHT).
[0062] Calculate conversion rate: The partial peak area divided by the total peak area gives the phase transition rate (X) at that temperature.
[0063] Calculation formula: X = AT / Atotal (or ΔHT / ΔHtotal).
[0064] The method for measuring the height H mm of sidewall 2 is as follows: Using measuring instruments such as micrometers or calipers, select at least three points evenly along the circumference of the shell, measure the vertical distance from the end of sidewall 2 away from endwall 1 to the end of sidewall 2 close to endwall 1, and take the average value as H; when measuring, ensure that the shell is placed on a horizontal reference platform, the contact surface between the measuring instrument and the reference platform is clean and free of foreign objects, and record the reading after it stabilizes.
[0065] The methods for measuring other dimensions, thicknesses, distances, and areas in this application are as follows: Micrometers, calipers, and other measuring tools can be used to measure dimensions, thicknesses, distances, etc., and the area can be calculated from these dimensions.
[0066] The battery manufacturing method in this embodiment is as follows: (1) Preparation of the positive electrode: The prepared positive electrode active material, conductive agent acetylene black, and binder PVDF are mixed, and solvent NMP is added. The mixture is stirred under vacuum until the system is homogeneous to obtain a positive electrode slurry. The positive electrode slurry is uniformly coated on both surfaces of the positive electrode current collector aluminum foil, air-dried at room temperature, and then transferred to an oven for further drying. Finally, it is cold-pressed and slit to obtain the positive electrode sheet. Specifically, the mass ratio of positive electrode active material: conductive agent: binder satisfies (92~98):(4~1):(4~1).
[0067] (2) Preparation of negative electrode: The negative electrode active material, conductive agent acetylene black, thickener CMC, and binder SBR are mixed, and deionized water is added as a solvent. The mixture is stirred under vacuum until the system is homogeneous to obtain a negative electrode slurry. The negative electrode slurry is uniformly coated on both surfaces of the negative electrode current collector copper foil, air-dried at room temperature, and then transferred to an oven for further drying. After cold pressing and slitting, the negative electrode sheet is obtained. The ratio of negative electrode active material: conductive agent: thickener: binder satisfies (90~96): (4~2): (2~1): (4~1).
[0068] (3) Preparation of electrolyte: Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain an organic solvent. Then, fully dried lithium salt LiPF6 was dissolved in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0069] (4) Preparation of the diaphragm: Polyethylene film is selected as the diaphragm.
[0070] (5) Preparation of the shell: Powder metallurgy is used to prepare titanium-containing blanks from titanium powder, carbon powder and other elemental components (such as iron, oxygen, nitrogen, carbon and sulfur), and then hot stamping is used to form the blanks.
[0071] (6) Battery fabrication: The positive electrode, separator, and negative electrode are stacked in sequence and wound to form a bare battery cell. The bare cell is then placed in a cylindrical battery casing. The battery is dried, injected with electrolyte, and then packaged, allowed to stand, formed, and volume-adjusted to obtain a lithium-ion battery.
[0072] The positive electrode active material can be selected from one or more lithium-containing positive electrode active materials, including lithium iron phosphate, ternary materials containing nickel, cobalt, and manganese, and lithium manganese iron phosphate; the negative electrode active material can be selected from one or more negative electrode active main materials, such as artificial graphite, natural graphite, silicon carbide, silicon oxide, and lithium titanate.
[0073] The adhesive includes, but is not limited to, one or more combinations of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorinated acrylate resin, styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, carboxymethyl chitosan, etc.
[0074] The solvent can be deionized water, NMP (N-methylpyrrolidone), alcohol, ether, ketone or other types of pyrrolidone, etc.
[0075] The positive electrode current collector foil can be a metal foil or a composite current collector. For example, as a metal foil, it can be made of stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel, or titanium with a silver-plated surface. The composite current collector may include a polymer material base layer and a metal layer. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).
[0076] The negative electrode current collector foil can be made of stainless steel, copper, aluminum, nickel, carbon electrodes, or titanium, and can be surface-plated with silver. Composite current collectors may include a polymer base layer and a metal layer. Composite current collectors can be formed by forming metal materials (aluminum, aluminum alloys, copper, nickel, nickel alloys, titanium, titanium alloys, silver and silver alloys, etc.) on a polymer base material (such as polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).
[0077] The following, in conjunction with Table 1, describes the testing of the casing end wall deformation and casing forming rate of the battery provided in this application through several embodiments and comparative tests, in order to verify its qualification.
[0078] Among them, performance 1, the deformation of the shell end wall, is tested using the following method: Following the battery fabrication method described above, batteries were prepared for each embodiment and comparative example. The data for each embodiment and comparative example are shown in Table 1 below, with other structures and test conditions remaining consistent. The end wall of the battery was bonded to a worktable. The surface of the worktable was taken as the XY plane, the direction perpendicular to the XY plane was taken as the Z direction, the geometric center of the end face of the end wall facing the cell was taken as the reference point, and the straight line in the Z direction passing through the reference point was taken as the reference line. Before vibration, the maximum distance between the end face of the end wall away from the cell and the reference line in the plane perpendicular to the Z direction was measured and recorded as distance L1mm.
[0079] According to GB / T2423.43, the battery was mounted on a vibration table, and the testing process was carried out as specified. Random and fixed-frequency vibration loads were applied in each direction, and the loading sequence should preferably be: random z-axis, fixed-frequency z-axis, random y-axis, fixed-frequency y-axis, random x-axis, fixed-frequency x-axis (the direction of the line connecting the front and rear of the battery is the x-axis direction, and the other horizontal direction perpendicular to the x-axis direction is the y-axis direction). The vibration frequency, power spectral density (PSD), vibration time, etc., are shown in the table below.
[0080]
[0081] After vibration, measure again the maximum distance between the end face of the battery wall furthest from the cell and the baseline in the plane perpendicular to the Z direction, and record it as distance L2mm. The deformation of the battery end wall is calculated as |L1-L2|. If the deformation of the battery end wall is greater than 0.2mm, the battery is recorded as unqualified; if the deformation is greater than 0.1mm but less than or equal to 0.2mm, the battery is recorded as qualified; if the deformation is less than or equal to 0.1mm, the battery is recorded as good.
[0082] Among them, performance 2, shell molding rate, is tested using the following methods: According to the battery preparation method described above, for each embodiment and comparative example, the corresponding batteries were prepared. The values for each embodiment and comparative example are shown in Table 1 below. Other structures and test conditions remained the same.
[0083] The size of cracks on the sidewall surface and / or the connection between the sidewall and the endwall of the battery is observed and recorded by scanning electron microscopy. If the crack size is greater than 20 micrometers, the battery is unqualified; otherwise, it is qualified. 100 batteries are made for each embodiment. After the casing is formed, the crack size at the connection between the sidewall and the endwall of the battery is measured, and the overall molding rate of the battery is further calculated. A molding rate of ≥95% is considered good, and a molding rate between 90% and 95% is considered qualified; otherwise, it is unqualified.
[0084] Table 1
[0085] Regarding the test results, referring to Table 1 above, the explanation is as follows: As can be seen from Examples 1-18, when the formula value of A×X×H satisfies the range of 3.5≤A×X×H≤1911, the test results of the shell end wall deformation amount test are all good or qualified, and no unqualified results are found; the test results of the shell forming rate test are all good or qualified, and no unqualified results are found; the performance requirements are met.
[0086] In Comparative Example 1, the value of the formula A×X×H is lower than the lower limit. After the shell forming rate test, the test result is unqualified and cannot meet the performance requirements.
[0087] In Comparative Examples 2 and 3, the values of the formula A×X×H exceeded the upper limit, and the test results for the deformation of the shell end wall were unqualified, failing to meet the performance requirements. It should be noted that in Comparative Example 3, the excessive shell height led to a decrease in the molding yield; therefore, the shell molding rate test result was only qualified.
[0088] In addition, Comparative Examples 4 to 9 were for battery casings with a titanium content of less than 99.0%. Due to the low titanium content, the material's ductility was insufficient, which caused the casing to crack easily when stretched. The casing forming rate test results were all unqualified.
[0089] In Examples 3 to 11, the results of the shell end wall deformation test were all good; the results of the shell forming rate test were all good; and the performance requirements were met.
[0090] In Examples 1 and 2, although A×X×H satisfies the range of 3.5≤A×X×H≤1911, the value of A×X×H is close to the lower limit, which causes the battery to only pass the test when the casing molding rate is tested, but still meets the performance requirements.
[0091] In Examples 12, 13, and 14, although A×X×H satisfies the range of 3.5≤A×X×H≤1911, the value of A×X×H is close to the upper limit. As a result, when the battery casing end wall deformation is tested, the deformation of the battery end wall is greater than 0.1mm but less than or equal to 0.2mm. The test result is only qualified, but still meets the performance requirements.
[0092] In Example 16, although A×X×H satisfies the range of 3.5≤A×X×H≤1911, the value of A is relatively small. As a result, when the battery casing end wall deformation is tested, the deformation is greater than 0.1mm but less than or equal to 0.2mm, and the test result is qualified. When the casing forming rate is tested, the forming rate is between 90% and 95%, and the test result is qualified.
[0093] In Example 17, although the value of X is relatively large, A×X×H satisfies the range of 3.5≤A×X×H≤1911 and is not close to the endpoint value. The test results of the shell end wall deformation amount test are all good; the test results of the shell forming rate test are all good; and the performance requirements are met.
[0094] Combination Figure 1 As shown, the housing in this embodiment also includes a cover plate 5, which is disposed opposite to the end wall 1 and sealed to the opening 4. The cover plate 5 is fixed to the edge of the side wall 2 by means of laser welding or the like to form a complete closed cavity.
[0095] In some embodiments, the end wall 1 has at least one first protrusion 12 on the side facing the receiving cavity 3, and the first protrusion 12 has a first groove 11 on the side facing away from the receiving cavity 3.
[0096] Combination Figure 4 As shown, the first protrusion 12 is integrally formed from the end wall 1 body material by a stamping process. The first protrusion 12 protrudes towards the receiving cavity 3, and the first groove 11 is formed on the side of the first protrusion 12 away from the receiving cavity 3.
[0097] The first groove 11 can be formed on the end wall 1 by stamping after the end wall 1 and side wall 2 of the shell are formed, or it can be formed by stamping simultaneously during the stretching and forming process of the end wall 1.
[0098] The first protrusion 12 protrudes towards one side of the receiving cavity 3, which can enhance the local rigidity of the end wall 1 and release the residual stress of the end wall 1, thus preventing the end wall 1 from warping due to thermal expansion and contraction or compression.
[0099] In this embodiment, when the shell is cylindrical, the first groove 11 can be distributed in a ring shape on the end wall 1; when the shell is square, the first groove 11 can be a rectangular groove surrounding the edge of the end wall 1.
[0100] As a variation, the end wall 1 may also form at least one first protrusion 12 on the side away from the receiving cavity 3, and the first protrusion 12 is provided with a first groove 11, which is formed by the inner surface of the end wall 1 recessed in the direction away from the receiving cavity 3.
[0101] In some embodiments, the width of the first groove 11 is E mm in the direction parallel to the plane of the end wall 1 and perpendicular to the length extension direction of the first groove 11, satisfying: 1 mm ≤ E mm ≤ 5 mm.
[0102] Combination Figure 4 As shown, the width E mm of the first groove 11 refers to the maximum width of the recessed area formed by the first groove 11 in a cross section perpendicular to the plane of the end wall 1 and perpendicular to the extension direction of the first groove 11.
[0103] When the width E mm of the first groove 11 satisfies 1 mm ≤ E mm ≤ 5 mm, it can effectively release the residual stress of the end wall 1, prevent the end wall 1 from warping, and ensure the flatness of the end wall 1.
[0104] When the width E mm of the first groove 11 is lower than the lower limit of the above range, the stress relief effect is weak, the residual stress is large, and the end wall 1 is still prone to warping; when the width E mm of the first groove 11 is higher than the upper limit of the above range, it is easy to affect the flatness of the end wall 1, resulting in poor fit between the end wall 1 and adjacent parts in subsequent assembly, affecting the assembly accuracy.
[0105] For example, in this embodiment, the value of E mm can be 1 mm, 1.4 mm, 1.9 mm, 2.3 mm, 2.8 mm, 3.2 mm, 3.7 mm, 4.1 mm, 4.5 mm, 4.9 mm, or 5 mm, or it can be a range formed by any two of the above values.
[0106] In some embodiments, in a direction perpendicular to the plane of the end wall 1, the first protrusion 12 protrudes from the surface of the end wall 1 toward the receiving cavity 3 by a height of F mm, satisfying: 0.3 mm ≤ F mm ≤ 0.5 mm.
[0107] Combination Figure 4 As shown, the first groove 11 is recessed in the direction of the receiving cavity 3, that is, the first groove 11 extends at least partially into the receiving cavity 3 from the end wall 1.
[0108] Specifically, the height F mm of the first groove 11 protruding from the surface of the end wall 1 toward the receiving cavity 3 is the height of the first groove 11 protruding from the inner surface of the end wall 1 toward the receiving cavity 3.
[0109] When the height F mm of the first protrusion 12 protruding from the surface of the end wall 1 toward the receiving cavity 3 satisfies 0.3 mm ≤ F mm ≤ 0.5 mm, it can ensure that the first groove 11 has sufficient depth to effectively release the residual stress generated during the molding process, and can also avoid excessive encroachment on the effective space of the receiving cavity 3 due to excessive protrusion height.
[0110] When F mm is higher than the upper limit of the above range, the first groove 11 occupies too much space in the receiving cavity 3, which can easily interfere with the arrangement of the battery cells and affect the overall energy density of the battery. When F mm is lower than the lower limit of the above range, the stress release effect is insufficient, the rigidity of the end wall 1 is limited, and it is still difficult to effectively suppress deformation.
[0111] For example, in this embodiment, the value of F mm can be 0.3 mm, 0.32 mm, 0.34 mm, 0.36 mm, 0.38 mm, 0.41 mm, 0.43 mm, 0.45 mm, 0.47 mm, 0.49 mm, or 0.5 mm, or it can be any range formed by any two of the above values.
[0112] In some embodiments, the first groove 11 is an annular groove.
[0113] In this embodiment, the first groove 11 is constructed as a continuous annular groove. The cross-section of the annular groove can be U-shaped, V-shaped, or semi-circular, which facilitates processing and can meet the stress release requirements while taking into account the structural strength of the shell.
[0114] As a variation, the first groove 11 can also be constructed as a zigzag groove, which is distributed in a sawtooth or stepped manner along the circumference of the end wall 1 to further disperse local stress.
[0115] In some embodiments, the first groove 11 is an arc groove, which includes a plurality of intermittently arranged arc grooves, and the plurality of arc grooves form a ring.
[0116] In this embodiment, the first groove 11 is a plurality of intermittently arranged arc grooves, which together form a ring layout. For example, the first groove 11 may include three arc grooves, each with an equal central angle, and evenly distributed around the end wall 1. The radii of curvature of each arc groove are consistent, and a gap is reserved between adjacent arc grooves.
[0117] By adopting an intermittent circular arc groove layout, both the stress release requirements can be met and the flatness of the end wall 1 can be guaranteed.
[0118] In some embodiments, in the length extension direction parallel to the plane of the end wall 1 and perpendicular to the first groove 11, the minimum distance between the first groove 11 and the side wall 2 is G mm, satisfying: G mm ≥ 4 mm.
[0119] Combination Figure 4 As shown, the minimum distance between the first groove 11 and the side wall 2 refers to the shortest straight-line distance between the outermost edge of the first groove 11 and the inner wall of the side wall 2 in a plane parallel to the end wall 1.
[0120] Due to stress concentration in the connection area between end wall 1 and side wall 2, by limiting the lower limit of the minimum distance G mm between the first groove 11 and side wall 2, structural weakness caused by the groove being too close to the corner can be effectively avoided, and the overall rigidity of end wall 1 can be weakened by the first groove 11 being too close to the side wall 2, thereby preventing cracking when subjected to external impact or internal expansion force.
[0121] For example, in this embodiment, the value of G mm can be 4 mm or 4.5 mm or 5.2 mm or 6 mm or 6.8 mm or 7.5 mm or 8.3 mm or 9.1 mm or 10 mm or 11.2 mm or 12.5 mm or 14 mm or 15.5 mm, or it can be a range formed by any two of the above values.
[0122] In some embodiments, the sidewall 2 and the endwall 1 are connected by a circular arc transition, and the outer radius of the circular arc is Jmm, satisfying: 0.2mm≤Jmm≤2mm.
[0123] It should be noted that the outer radius (R) of the arc refers to the transition arc at the intersection of the outer surface of sidewall 2 and the outer surface of endwall 1.
[0124] The side wall 2 and end wall 1 are connected by a circular arc transition. When the outer radius Jmm of the arc increases, it can better alleviate stress concentration at the connection. However, an excessively large Jmm will weaken the structural rigidity and increase the volume of the casing. Furthermore, since the battery cell needs to be embedded inside the casing, an excessively large radius will also compress the usable space of the battery cell, reducing the volume utilization rate. When Jmm is higher than the upper limit of the above range, it will not only lead to redundancy in the overall size of the casing, resulting in low space utilization, but may also weaken the structural rigidity due to excessive curvature in the transition area. When Jmm is lower than the lower limit of the above range, the stress concentration effect is obvious, which can easily lead to microcracks at the connection between end wall 1 and side wall 2. Especially under conditions of thermal expansion and contraction or frequent vibration, cracks are more likely to occur, leading to structural failure.
[0125] For example, in this embodiment, the value of Jmm can be 0.2mm or 0.35mm or 0.5mm or 0.7mm or 0.9mm or 1.15mm or 1.4mm or 1.65mm or 1.8mm or 1.95mm or 2mm, or it can be any range formed by any two of the above values.
[0126] In some embodiments, the sidewall 2 has at least one second protrusion 22 on the side facing the receiving cavity 3, and the second protrusion 22 has a second groove 21 on the side facing away from the receiving cavity 3. Specifically, the second groove 21 is formed by recessing the outer surface of the sidewall 2 in the direction facing the receiving cavity 3.
[0127] Combination Figure 5 As shown, the second protrusion 22 protrudes towards the receiving cavity 3, and the side of the second protrusion 22 away from the receiving cavity 3 forms a corresponding second groove 21. The second protrusion 22 provided on the side wall 2 can also play a stress-relieving role, thereby alleviating the deformation of the side wall 2 during charge and discharge cycles and improving the overall structural stability of the shell.
[0128] Optionally, the second groove 21 is a straight groove extending along the height direction of the sidewall 2. A straight groove is one whose axis is parallel to the height direction of the sidewall 2 and extends through the entire height of the sidewall 2 or only to a part of the height. The cross-section of the straight groove can be rectangular or U-shaped. The straight grooves can be continuously distributed and extend through the upper and lower edges of the sidewall 2, or they can be distributed intermittently, with a certain distance reserved between each straight groove.
[0129] As a variation, the second groove 21 can also be an annular groove arranged circumferentially along the sidewall 2, and the cross-section of the annular groove can be circular or U-shaped. The annular groove can be arranged continuously or discontinuously along the sidewall 2. The arrangement of the annular groove is particularly suitable for the housing of cylindrical battery cells.
[0130] As a variation, the sidewall 2 may also form at least one second protrusion 22 on the side away from the receiving cavity 3, and the second protrusion 22 is provided with a second groove 21, which is formed by the inner surface of the sidewall 2 recessed in the direction away from the receiving cavity 3.
[0131] Additionally, there may be multiple second grooves 21, which are spaced apart along the height direction of the sidewall 2.
[0132] In some embodiments, the housing is a cylindrical housing, and the second groove 21 extends circumferentially along the sidewall 2.
[0133] In some embodiments, the housing is a cylindrical housing, and along the normal direction of the side wall 2, the second protrusion 22 protrudes from the surface of the side wall 2 toward the receiving cavity 3 by a height of K mm, satisfying: 0.02 mm ≤ K mm ≤ 0.2 mm; Alternatively, the shell is a square shell, and in the plane direction perpendicular to the side wall 2, the second protrusion 22 protrudes from the surface of the side wall 2 toward the receiving cavity 3 by a height of K mm, satisfying: 0.03 mm ≤ K mm ≤ 0.23 mm.
[0134] It should be noted that when the shell is cylindrical, the normal direction of sidewall 2 refers to the radial direction perpendicular to the tangent plane of the cylindrical sidewall; when the shell is square, the direction perpendicular to the plane of sidewall 2 is the thickness direction of the shell.
[0135] By limiting the upper limit of K mm, the second groove 21 can be prevented from protruding excessively and encroaching on the effective space of the cell, thus avoiding excessively low energy density of the battery, while ensuring stress relief. By limiting the lower limit of K mm, the second groove 21 can be ensured to have sufficient structural depth to play a stress relief role, preventing stress concentration in the casing due to insufficient depth.
[0136] When the shell is cylindrical, the second groove 21 protrudes towards the receiving cavity 3 along the normal direction of the side wall 2; when the shell is square, the second groove 21 protrudes towards the receiving cavity 3 in a plane direction perpendicular to the side wall 2.
[0137] Additionally, the protrusion height K mm of the second groove 21 is less than the protrusion height F mm of the first groove 11.
[0138] For example, in this embodiment, when the shell is a cylindrical shell, the value of K mm can be 0.02 mm, 0.035 mm, 0.05 mm, 0.07 mm, 0.09 mm, 0.11 mm, 0.13 mm, 0.15 mm, 0.17 mm, 0.185 mm, or 0.2 mm, or it can be any range formed by any two of the above values.
[0139] For example, in this embodiment, when the shell is a square shell, the value of K mm can be 0.03 mm, 0.05 mm, 0.075 mm, 0.1 mm, 0.12 mm, 0.145 mm, 0.17 mm, 0.19 mm, 0.21 mm, or 0.23 mm, or it can be any range formed by any two of the above values.
[0140] In some embodiments, the height H mm of the sidewall 2 satisfies: 60 mm ≤ H mm ≤ 200 mm.
[0141] When the height H of sidewall 2 is too large, the excessive stretching height will lead to greater deformation of endwall 1. As the material flows, endwall 1 becomes thinner, affecting the structural strength of the casing. Conversely, when the height H of sidewall 2 is too small, the volume of the casing is insufficient, making it difficult to meet installation requirements. Furthermore, when the height H of sidewall 2 is too large, with a constant volume of structural adhesive, the overlap height between the structural adhesive and sidewall 2 is constant. The bonding area of the structural adhesive to the casing during battery installation is relatively small, easily resulting in insufficient constraint on the casing. Moreover, the endwall 1 of the casing is prone to deformation due to excessive deformation, causing the pressure relief valve to open at a higher pressure, leading to excessive pressure inside the casing. When the height H of sidewall 2 is too small, the deformation of endwall 1 of the casing is relatively small, resulting in a thicker endwall 1, poor heat dissipation, and heat accumulation on the bottom surface of the battery, which can easily affect the battery's charging and discharging performance.
[0142] For example, in this embodiment, the value of H mm can be 60 mm, 75 mm, 92 mm, 110 mm, 128 mm, 145 mm, 163 mm, 180 mm, 192 mm, or 200 mm, or it can be any range formed by any two of the above values.
[0143] As a further preferred option, the height H mm of the sidewall 2 satisfies: 80 mm ≤ H mm ≤ 185 mm.
[0144] When the height H mm of the sidewall 2 meets the above preferred range of 80 mm ≤ H mm ≤ 185 mm, it can not only meet the energy requirements of the battery, but also avoid the shell being stretched to an excessive height, thus better preventing cracks or breakage of the shell sidewall.
[0145] For example, when the height H mm of the sidewall 2 satisfies the above-mentioned preferred range of 80 mm ≤ H mm ≤ 185 mm, the value of H mm can be 80 mm or 83 mm or 86 mm or 89 mm or 92 mm or 95 mm or 98 mm or 101 mm or 104 mm or 107 mm or 110 mm or 113 mm or 116 mm or 119 mm or 122 mm or 125 mm or 128 mm or 131 mm or 134 mm or 137 mm or 140 mm or 143 mm or 146 mm or 149 mm or 152 mm or 155 mm or 158 mm or 161 mm or 164 mm or 167 mm or 170 mm or 173 mm or 176 mm or 179 mm or 182 mm or 185 mm, etc., or it can be any range formed by any two of the above values.
[0146] In some embodiments, the thicknesses of end wall 1 and side wall 2 are T1 mm and T2 mm, respectively, satisfying: 1 < T1 / T2 ≤ 2.4.
[0147] Combination Figure 4 As shown, the thickness of end wall 1 refers to the thickness of the solid portion of end wall 1, not the maximum distance between the bottom and top surfaces of end wall 1 in a direction perpendicular to the plane of end wall 1. Similarly, the thickness of side wall 2 refers to the thickness of the solid portion of side wall 2, not the maximum distance between the outer and inner surfaces of side wall 2 in a direction perpendicular to its axis.
[0148] When the ratio of T1 / T2 is higher than the upper limit of the above range, the end wall 1 is too thick and the side wall 2 is too thin, which can easily lead to a low molding yield and a decrease in the heat dissipation efficiency of the end wall 1, causing heat to accumulate at the bottom. When the ratio of T1 / T2 is lower than the lower limit of the above range, the end wall 1 is too thin and the side wall 2 is too thick. In order to ensure molding feasibility and structural strength, the outer R-angle radius needs to be enlarged, which leads to an increase in the overall volume of the shell and a decrease in space utilization.
[0149] For example, in this embodiment, the value of T1 / T2 can be 1.05 or 1.15 or 1.25 or 1.32 or 1.4 or 1.48 or 1.55 or 1.62 or 1.68 or 1.75 or 1.82 or 1.88 or 1.95 or 2.02 or 2.08 or 2.15 or 2.22 or 2.28 or 2.35 or 2.4, etc., or it can be any range formed by any two of the above values.
[0150] In some embodiments, the thickness of end wall 1 is T1mm, satisfying: 0.21mm≤T1mm≤1.44mm; And / or, the thickness of sidewall 2 is T2mm, satisfying: 0.2 mm ≤ T2mm ≤ 0.6 mm.
[0151] This embodiment ensures that the end wall 1 has sufficient structural rigidity to resist internal pressure by limiting the range of its thickness T1mm, while also preventing excessive thickness from hindering heat conduction to the outside. Specifically, by limiting the upper limit of the end wall 1 thickness T1mm, the thermal resistance is prevented from increasing due to excessive thickness, which would affect the battery's heat dissipation efficiency. By limiting the lower limit of the end wall 1 thickness T1mm, sufficient mechanical strength is ensured to withstand internal pressure impacts, ensuring that the end wall 1 does not undergo plastic deformation or breakage when subjected to internal air pressure or external impacts, thus improving safety.
[0152] When T2 is below the lower limit of the above range, the sidewall 2 deforms too much during the molding process, which can easily cause cracks or breakage, reduce the molding yield, and the sidewall 2 has insufficient structural rigidity, affecting the overall pressure resistance of the shell. When T2 is above the upper limit of the above range, the overall weight of the shell increases and the heat dissipation path becomes longer, which leads to increased heat accumulation at the bottom of the battery.
[0153] For example, in this embodiment, the value of T1mm can be 0.21mm or 0.25mm or 0.29mm or 0.33mm or 0.37mm or 0.41mm or 0.45mm or 0.49mm or 0.53mm or 0.57mm or 0.61mm or 0.65mm or 0.69mm or 0.73mm or 0.77mm or 0.81mm or 0.85mm or 0.89mm or 0.93mm or 0.97mm or 1.01mm or 1.06mm or 1.11mm or 1.16mm or 1.21mm or 1.26mm or 1.31mm or 1.35mm or 1.39mm or 1.44mm, or it can be any range formed by any two of the above values.
[0154] For example, in this embodiment, the value of T2mm can be 0.2mm or 0.24mm or 0.29mm or 0.33mm or 0.37mm or 0.42mm or 0.46mm or 0.5mm or 0.54mm or 0.58mm or 0.6mm, or it can be any range formed by any two of the above values.
[0155] In some embodiments, the phase change conversion rate X of the shell satisfies: 0.005 AHX ≤ X AHX ≤ 0.05 AHX.
[0156] The higher the phase transformation conversion rate X of the shell, the more significant the phase transformation of titanium from α to β phase. However, when the phase transformation conversion rate X is higher than the upper limit of the above range, the β phase grains become coarser, and the shell strength decreases significantly. Conversely, when the phase transformation conversion rate X is lower than the lower limit of the above range, the annealing temperature is too low, the residual stress is large, and the proportion of α phase grains is too high, resulting in greater material brittleness and a tendency for localized fracture during stretching.
[0157] In this embodiment, the value of X can be 0.005 AHX, 0.008 AHX, 0.012 AHX, 0.016 AHX, 0.021 AHX, 0.027 AHX, 0.033 AHX, 0.039 AHX, 0.044 AHX, or 0.05 AHX, or it can be any range formed by any two of the above values.
[0158] As a further preferred option, the phase transformation conversion rate X of the shell satisfies: 0.015 AHX≤X AHX≤0.04 AHX.
[0159] When the phase transformation conversion rate X of the shell meets the above preferred range of 0.015 AHX≤X AHX≤0.04 AHX, the phase transformation conversion rate X of the shell is controlled within a certain range, preventing the shell from undergoing a significant phase transformation and better reducing the occurrence of shell strength reduction.
[0160] For example, when the phase change conversion rate X of the shell satisfies the above-mentioned preferred range of 0.015 AHX ≤ X AHX ≤ 0.04 AHX, the value of X can be 0.015 AHX or 0.0165 AHX or 0.018 AHX or 0.019 AHX or 0.02 AHX or 0.021 AHX or 0.0225 AHX or 0.0235 AHX or 0.0245 AHX or 0.0255 AHX or 0.0265 AHX or 0.0275 AHX or 0.0285 AHX or 0.0295 AHX or 0.0305 AHX or 0.0315 AHX or 0.0325 AHX or 0.034 AHX or 0.036 AHX or 0.04 AHX, etc., or it can be any range formed by any two of the above values.
[0161] In some embodiments, the gloss level A of the housing satisfies: 10 GU ≤ A GU ≤ 200 GU.
[0162] When the gloss A of the shell is lower than the lower limit of the above range, that is, the annealing temperature is too low, the residual stress is not sufficiently eliminated, the material has insufficient ductility, and the sidewall 2 is prone to cracks or even tearing during the stretching process; while when the gloss A of the shell is higher than the upper limit of the above range, that is, the annealing temperature is too high, the phase transformation of titanium element is intensified, the β phase grains are coarsened, the shell has good toughness and is easy to form, but it will lead to a decrease in shell strength.
[0163] For example, in this embodiment, the value of A can be 10 GU or 23 GU or 41 GU or 67 GU or 92 GU or 118 GU or 145 GU or 171 GU or 189 GU or 200 GU, or it can be a range formed by any two of the above values.
[0164] As a further preferred option, the gloss level A of the shell satisfies: 25 GU ≤ A GU ≤ 180 GU.
[0165] When the gloss A of the shell meets the above-mentioned preferred range of 25 GU≤A GU≤180 GU, the residual stress of the shell can be better eliminated, and the shell does not undergo a transitional phase transformation, thus better ensuring the strength of the shell.
[0166] For example, when the gloss level A of the housing meets the preferred range of 25 GU ≤ A GU ≤ 180 GU, the value of A can be 25 GU, 27 GU, 29 GU, 31 GU, 33 GU, 35 GU, 37 GU, 39 GU, 41 GU, 43 GU, 45 GU, 47 GU, 49 GU, 51 GU, 53 GU, 55 GU, 57 GU, 59 GU, 61 GU, 63 GU, 65 GU, 67 GU, 69 GU, 71 GU, 73 GU, 75 GU, 77 GU, 79 GU, 81 GU, 83 GU, 85 GU, 87 GU, 89 GU, 91 GU, 93 GU, 95 GU, 97 GU, 99 GU, 101 GU, 103 GU, 105 GU, or 107 GU. GU or 109 GU or 111 GU or 113 GU or 115 GU or 117 GU or 119 GU or 121 GU or 123 GU or 125 GU or 127 GU or 129 GU or 131 GU or 133 GU or 135 GU or 137 GU or 139 GU or 141 GU or 143 GU or 145 GU or 147 GU or 149 GU or 151 GU or 153 GU or 155 GU or 157 GU or 159 GU or 161 GU or 163 GU or 165 GU or 167 GU or 169 GU or 171 GU or 173 GU or 175 GU or 177 GU or 179 GU or 180 GU, etc., or any range formed by any two of the above values.
[0167] In some embodiments, the gloss of end wall 1 is A1 GU, satisfying: 20 GU≤A1 GU≤200 GU.
[0168] When the gloss A1 of end wall 1 is lower than the lower limit of the above range, i.e., the annealing temperature is too low, the residual stress of end wall 1 is not sufficiently eliminated, which makes end wall 1 prone to microcracks during subsequent assembly or use, affecting the overall reliability of the shell. When the gloss A1 of end wall 1 is higher than the upper limit of the above range, i.e., the annealing temperature is too high, the phase transformation of titanium is intensified, the β phase grains coarsen, the shell has better toughness and is easier to form, but it will lead to a decrease in the strength of end wall 1, thus affecting its impact resistance.
[0169] For example, in this embodiment, the value of A1 GU can be 20 GU or 35 GU or 52 GU or 71 GU or 93 GU or 116 GU or 139 GU or 162 GU or 184 GU or 200 GU, or it can be a range formed by any two of the above values.
[0170] The method for measuring the gloss A1 of end wall 1 is the same as the method for measuring the gloss A of shell.
[0171] In some embodiments, the gloss of the sidewall 2 is A2, satisfying: 10 GU≤A2 GU≤185 GU.
[0172] When the gloss A2 of sidewall 2 is lower than the lower limit of the above range, i.e., the annealing temperature is too low, the residual stress of sidewall 2 is not sufficiently eliminated, which makes sidewall 2 prone to microcracks during subsequent assembly or use, affecting the overall reliability of the shell. When the gloss A2 of sidewall 2 is higher than the upper limit of the above range, i.e., the annealing temperature is too high, the phase transformation of titanium is intensified, the β phase grains coarsen, the shell has better toughness and is easier to form, but it will lead to a decrease in the strength of sidewall 2, thus affecting its impact resistance.
[0173] The method for measuring the gloss A2 of the sidewall 2 is the same as the method for measuring the gloss A of the shell.
[0174] For example, in this embodiment, the value of A2 can be 10 GU or 22 GU or 37 GU or 53 GU or 71 GU or 94 GU or 116 GU or 139 GU or 162 GU or 178 GU or 185 GU, or it can be any range formed by any two of the above values.
[0175] According to embodiments of this application, in conjunction with Figure 1 As shown, on the other hand, a single-cell battery is also provided, comprising: Battery cell; As described above, the battery cell is housed within the housing cavity 3 of the housing.
[0176] The single cell also includes a cover plate 5, which is sealed to the casing by laser welding to form an airtight cavity.
[0177] A single cell is the basic unit that makes up a battery. It stores chemical energy and converts it into electrical energy in a controllable manner. In a recyclable single cell, the active materials can be reactivated by charging after discharge, allowing it to continue to be used. Single cells can be further combined into battery packs. A battery pack contains multiple single cells, and the specific number can be adjusted according to the actual application scenario and capacity requirements.
[0178] A single battery cell includes a casing, a cell, and a cover plate 5. The casing is used to house the cell, and the cover plate 5 has at least one positive electrode post and at least one negative electrode post. The cell includes one or more electrode assemblies, which are formed by stacking or winding positive electrode sheets, negative electrode sheets, and separators.
[0179] The cover plate 5 is a component that seals the opening of the casing to isolate the internal environment of the individual battery cell from the external environment. The cover plate 5 is also made of titanium alloy.
[0180] Terminals are used to electrically connect electrode assemblies located inside the casing to external devices (adjacent batteries or other electrical equipment) located outside the casing. A single battery cell can discharge to external devices through its cell output terminal (tab) and the external device output terminal (terminal assembly). An external power source can charge the battery through the terminals and tabs. Terminals can be directly electrically connected to the cell tabs or connected to the tabs via metal adapters. Terminals are made of metals including, but not limited to, copper, aluminum, aluminum alloys, and copper-aluminum alloys.
[0181] A battery cell is the component in a battery where electrochemical reactions occur; it is the smallest unit in a battery capable of performing electrochemical reactions such as charging and discharging. A battery cell typically consists of a positive electrode, a negative electrode, and a separator. Lithium-ion battery cells primarily function by the movement of lithium ions between the positive and negative electrodes. In cylindrical cells, a three-layer thin-film structure is wound into a cylindrical electrode assembly, while in cuboid cells, the thin-film structure is wound or stacked into an electrode assembly with a roughly cuboid shape.
[0182] A separator is disposed between the positive and negative electrode plates to separate them and prevent short circuits caused by contact. The separator can be at least one of glass fiber, non-woven fabric, polyethylene (PE), polypropylene (PP), and polyvinylidene fluoride. A coating can also be applied to the surface of the separator. The coating can be an inorganic coating and / or an organic coating. The inorganic coating material includes at least one of alumina, silicon oxide, titanium oxide, magnesium oxide, zirconium oxide, and boehmite; the organic coating includes at least one of aramid coating and polyvinylidene fluoride (PVDF) coating.
[0183] The tab is located on one side of the positive / negative current collector and is separately or integrally formed with the current collector. It is electrically connected to the current collector to conduct the current on the corresponding current collector. The tab is made of a metal material with good conductivity (such as copper, aluminum, or nickel).
[0184] The positive electrode is one of the core components in a battery that carries the positive electrode active material. During charging, metal ions (e.g., lithium ions) are released from the positive electrode active material (oxidation reaction), migrate through the electrolyte, and intercalate into the negative electrode. During discharging, metal ions (e.g., lithium ions in a lithium battery) are released from the negative electrode and intercalated into the positive electrode active material (reduction reaction), thus realizing the storage and release of lithium ions.
[0185] A positive electrode generally includes a positive current collector and a positive active material layer. The positive active material layer is coated on at least one surface of the positive current collector and includes: a positive active material, a conductive agent, and a binder. The positive active material includes, but is not limited to, at least one of the following: lithium phosphates, lithium transition metal oxides and their respective modified compounds, or other conventional materials that can be used as positive active materials for batteries. These positive active materials can be used alone or in combination. The lithium phosphates include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also abbreviated as LFP)), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium iron manganese phosphate, and lithium iron manganese phosphate and carbon composites. Lithium transition metal oxides include, but are not limited to, at least one of lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, lithium nickel cobalt manganese oxides, lithium nickel cobalt aluminum oxides, and their modified compounds. Conductive agents include, but are not limited to, one or more combinations of graphite, superconducting carbon, carbon black (such as acetylene black, Ketjen black, Super P, etc.), carbon nanotubes, graphene, and carbon nanofibers. Binders include, but are not limited to, one or more combinations of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorinated acrylate resins, styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, and carboxymethyl chitosan.
[0186] During battery charging, active ions (such as Li) from the positive electrode are embedded in the negative electrode, while electrons from the positive electrode are transferred to the negative electrode through an external circuit to maintain charge balance. During discharge, active ions (such as lithium ions) previously embedded in the negative electrode can be released, while electrons from the negative electrode are transferred to the negative electrode through an external circuit to maintain charge balance, thus achieving energy storage and release.
[0187] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. The negative electrode current collector is a conductive metal foil, which can be made of stainless steel, copper, aluminum, nickel, carbon electrodes, or titanium with a silver-plated surface. The composite current collector may include a polymer base material and a metal layer. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, copper, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base film layer (such as a base film layer of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.). The negative electrode active material layer includes the negative electrode active material, a conductive agent, and a binder. The negative electrode active material can be carbon-based film material such as graphite, porous carbon, hard carbon, soft carbon, mesophase carbon microspheres, or silicon-based film material such as elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, etc. The conductive agent can be conductive carbon black, carbon nanotubes, etc., and the binder can be styrene-butadiene rubber, polyacrylic acid, etc.
[0188] In some embodiments, the end wall 1 of the housing includes a top wall located at the upper part of the individual battery cell along the height direction.
[0189] In this embodiment, since the side wall 2 extends from one end of the end wall 1 along a direction perpendicular to the plane where the end wall 1 is located; when the end wall 1 serves as the top wall located at the upper part of the single cell along the height direction, the side wall 2 extends downward from the edge of the top wall, together with the bottom wall to form a closed cavity for accommodating the cell assembly, that is, the casing is installed in an inverted form. At this time, the end wall 1 does not need to bear the weight of the cell, and is less likely to be subjected to external impact forces, mainly bearing tensile stress rather than direct impact, which can avoid the risk of increased casing deformation, reduce the risk of casing breakage, and help improve the stability of the casing.
[0190] In some embodiments, the end wall 1 of the housing includes a bottom wall located at the opposite bottom of the single cell along the height direction; the cell is disposed above the bottom wall, and the phase change conversion rate X AHX of the housing satisfies: 0.01AHX≤X AHX≤0.05AHX.
[0191] In this embodiment, when end wall 1 serves as the bottom wall located at the bottom of the individual battery cell along the height direction, the bottom wall directly bears the weight of the cell assembly and potential bottom impact loads. Therefore, the bottom wall typically needs to possess higher structural strength and resistance to deformation. In this case, the upper limit of the phase transformation conversion rate X AHX of the casing needs to be appropriately reduced to minimize the α-phase to β-phase phase transformation of titanium, thereby reducing the proportion of β-phase grains and preventing a decrease in casing strength.
[0192] In this embodiment, the value of X AHX can be 0.01AHX, 0.0115AHX, 0.013AHX, 0.0145AHX, 0.016AHX, 0.017AHX, 0.0175AHX, 0.0185AHX, 0.0195AHX, 0.0205AHX, 0.0215AHX, 0.0225AHX, 0.0235AHX, 0.024AHX, 0.025AHX, or 0. 026AHX or 0.027AHX or 0.028AHX or 0.029AHX or 0.03AHX or 0.031AHX or 0.032AHX or 0.033AHX or 0.034AHX or 0.0355AHX or 0.037AHX or 0.0385AHX or 0.04AHX or 0.043AHX or 0.05AHX, etc., or any range formed by any two of the above values.
[0193] In some embodiments, the single cell includes a cylindrical cell; the end wall 1 of the casing is circular, and the diameter D1 of the end wall 1 satisfies: 18mm≤D1mm≤80mm.
[0194] A cylindrical battery is a single cell with a cylindrical shape, and the end wall 1 of the casing is a circular structure adapted to the shape of the cylindrical battery. By controlling the diameter D1 of the end wall 1 within the aforementioned range, sufficient structural strength can be maintained to withstand internal pressure, while preventing the end wall 1 from easily deforming due to an excessively large diameter. When the diameter D1 of the end wall 1 is lower than the lower limit, the end wall 1 is prone to stress concentration, increasing the risk of cracking, and the internal space is limited, making it difficult to accommodate sufficient active material, resulting in a lower battery energy density. When the diameter D1 is higher than the upper limit, the end wall is more prone to buckling deformation under internal air pressure or external extrusion, thereby weakening the overall structural strength of the casing. In addition, when the diameter D1 is too large, the heat generated inside the battery is greater, increasing the risk of thermal runaway.
[0195] For example, in this embodiment, the value of D1mm can be 18mm or 21mm or 24mm or 27mm or 30mm or 33mm or 36mm or 39mm or 42mm or 45mm or 48mm or 51mm or 54mm or 57mm or 60mm or 63mm or 65mm or 67mm or 69mm or 71mm or 73mm or 75mm or 76.5mm or 77.5mm or 78.5mm or 79mm or 79.3mm or 79.6mm or 79.8mm or 80mm, or it can be any range formed by any two of the above values.
[0196] In some embodiments, the battery cell includes a battery cell body and a tab extending from at least one end of the battery cell body. The tab is electrically connected to the end wall 1. In this case, the height H mm of the side wall 2 satisfies: 60 mm ≤ H mm ≤ 185 mm.
[0197] A tab is a conductive component extending from the battery cell body. The tab is used to conduct the current generated by the battery cell body to the terminal, thereby achieving electrical connection between the battery cell and an external circuit. Specifically, the tab is located on one side of the positive / negative current collector and is separately / integrated with the current collector, electrically connected to it to conduct the current on the corresponding current collector. The tab is made of a highly conductive metal material (such as copper, aluminum, or nickel).
[0198] Since the tabs are electrically connected to the end wall 1, the heat generated by the shell increases after the electrical connection, and the shell is at greater risk of deformation. By reducing the upper limit of the height H mm of the side wall 2, the overall height of the shell can be reduced, the degree of material thinning during the stretching process can be reduced, thereby ensuring the structural strength of the shell. For example, in this embodiment, the value of H mm can be 60 mm, 64 mm, 68 mm, 72 mm, 75 mm, 79 mm, 83 mm, 87 mm, 91 mm, 95 mm, 99 mm, 103 mm, 107 mm, 111 mm, 115 mm, 119 mm, 123 mm, 127 mm, 131 mm, 135 mm, 139 mm, 143 mm, 147 mm, 151 mm, 155 mm, 159 mm, 163 mm, 167 mm, 171 mm, 174 mm, 176 mm, 178 mm, 180 mm, 181 mm, 182 mm, 183 mm, 183.5 mm, 184 mm, 184.5 mm, or 185 mm, etc., or it can be any range formed by any two of the above values.
[0199] According to an embodiment of this application, in another aspect, a battery pack 810 is provided, see [link to embodiment]. Figure 8 , Figure 8 An exploded view of the battery pack in some embodiments of this application is shown; the battery pack 810 includes: The housing 811; and a plurality of individual cells as described above, housed within the housing 811.
[0200] The battery pack 810 also includes a cover 812, which is positioned over the opening of the housing 811 and is sealed to the housing 811 to form a closed chamber for accommodating individual batteries. A sealing element is provided between the cover 812 and the housing 811, extending along the edge of the opening of the housing 811 to fill the gap between the cover 812 and the housing 811. This prevents external moisture, dust, and other impurities from entering the closed chamber, thereby ensuring that the individual batteries operate in a relatively clean and stable environment, and thus improving the overall safety and service life of the battery pack 810.
[0201] The battery pack 810 is configured on an electrical device, such as inside an electric vehicle, and can be installed at the bottom, front, or rear of the vehicle. The battery pack 810 provides electrical support to the electric vehicle, for example, acting as its operating power source. The electric vehicle may also be equipped with a controller and a motor; the controller is used to manage the supply of electrical energy from the battery pack to the motor to meet the power needs of the electric vehicle during starting, navigation, and driving.
[0202] The battery pack 810, as a rechargeable battery, is the power source for new energy vehicles. The battery pack includes a housing 811 and multiple individual battery cells housed within the housing 811. The housing 811 provides space for the individual battery cells and other components, while also providing dustproof, waterproof, and protective functions for the internal components. This reduces the adverse effects of external liquids or foreign objects on the effectiveness and performance of the individual battery cells and other components, effectively extending the battery pack's lifespan. The shape of the housing 811 is not limited; for example, it can be a cuboid, cylinder, etc.
[0203] The material of the 811 enclosure can also be flexibly selected, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc.
[0204] In this embodiment, the battery pack 810 includes multiple battery groups 813. Each sub-accommodation space of the housing 811 is provided with a battery group 813. Each battery group 813 includes multiple stacked individual cells. The stacking direction of the individual cells can be a direction parallel to the plane of the bottom plate of the housing 811.
[0205] The battery pack 810 also includes a battery management system (BMS), a thermal management system, an electrical connection system (high-voltage / low-voltage connectors, wiring harnesses, etc.), structural components (casing, brackets, etc.), and protective components. These components are housed within a casing 811 and sealed by a cover 812, forming a complete functional unit capable of directly outputting electrical energy. The battery management system (BMS) is used to detect the operating status of the battery pack and its individual cells, and to manage the battery modules and their individual cells. The battery management system includes a battery management unit (BMU), a cell measurement circuit (CMC), sensors, and some electronic control devices. The battery management system includes at least one processor and a memory. The memory can be built into the battery management system or externally located outside the battery management system. The memory can also be remotely configured and connected to the battery management system via a network.
[0206] According to an embodiment of this application, in another aspect, a battery device is also provided, comprising: One or more battery packs 810 as described above.
[0207] The battery device 800 can serve as an operating power source for electrical devices, or as a driving power source for electrical devices, replacing or partially replacing fuel or natural gas to provide driving power for vehicles.
[0208] Electrical devices include energy storage equipment, electric ships, aircraft, laptops, power tools, electric bicycles, electric motorcycles, electric cars, military equipment, aerospace and many other technological fields.
[0209] The following uses vehicle 900 as a specific example of an electrical device for illustration. See also Figure 7 , Figure 7 The diagram illustrates the structure of a vehicle in some embodiments of this application. The vehicle 900 can be a new energy vehicle, encompassing various types such as pure electric vehicles, hybrid electric vehicles, and range-extended electric vehicles. The battery device 800 can be located at the bottom, front, or rear of the vehicle 900, providing electrical support to the vehicle 900, for example, acting as the vehicle 900's operating power source. Furthermore, the vehicle 900 typically also includes a controller 700, which manages the discharge process of the battery device 800 to cover various power needs during vehicle start-up, navigation, and driving.
[0210] In some embodiments, the battery device 800 comprises one or more battery packs 810, which can be connected in series, parallel, or a hybrid configuration. A hybrid configuration refers to the simultaneous presence of series and parallel connections in the connection of multiple battery packs 810. In other embodiments, the battery device 800 is a cluster-level battery architecture composed of multiple battery packs 810 connected in series, wherein the number of battery packs 810 in each cluster is strictly configured according to voltage and capacity requirements. More specifically, the battery unit of the battery device 800 includes multiple batteries, some of which are connected in series to form a cluster that meets a preset power supply voltage requirement, and at least one spare battery among the multiple batteries is bypassed.
[0211] Obviously, the above embodiments are merely examples for clear illustration and are not intended to limit the implementation. Although embodiments of this application have been described in conjunction with the accompanying drawings, those skilled in the art can make various modifications and variations without departing from the spirit and scope of this application, and all such modifications and variations fall within the scope defined by this application.
Claims
1. A housing, characterized in that, include: The end wall (1) and side wall (2) are integrally formed. The side wall (2) is formed by extending one end of the end wall (1) in a direction perpendicular to the flat end wall surface where the end wall (1) is located. The side wall (2) and the end wall (1) enclose and form a receiving cavity (3). The titanium content in the shell is ≥99.0%; the gloss of the shell is A GU; and the phase transformation conversion rate of the shell is XAHX. Along the direction perpendicular to the plane where the end wall (1) is located, the height of the side wall (2) is H mm; It satisfies: 3.5≤A×X×H≤1911.
2. The housing according to claim 1, characterized in that, The end wall (1) forms at least one first protrusion (12) on the side facing the receiving cavity (3), and the first protrusion (12) is provided with a first groove (11) on the side away from the receiving cavity (3).
3. The housing according to claim 2, characterized in that, In the direction of the first groove (11) extending parallel to the plane of the end wall (1) and perpendicular to the length of the first groove (11), the width of the first groove (11) is E mm, which satisfies: 1 mm ≤ E mm ≤ 5 mm.
4. The housing according to claim 2, characterized in that, In the direction perpendicular to the plane of the end wall (1), the height of the first protrusion (12) protruding from the surface of the end wall (1) toward the receiving cavity (3) is F mm, which satisfies: 0.3 mm ≤ F mm ≤ 0.5 mm.
5. The housing according to claim 2, characterized in that, The first groove (11) is an annular groove.
6. The housing according to claim 2, characterized in that, The first groove (11) is an arc groove, which includes multiple intermittently arranged arc grooves, and the multiple arc grooves form a ring.
7. The housing according to claim 2, characterized in that, In the length extension direction parallel to the plane where the end wall (1) is located and perpendicular to the first groove (11), the minimum distance between the first groove (11) and the side wall (2) is G mm, which satisfies: G mm ≥ 4 mm.
8. The housing according to claim 1, characterized in that, The sidewall (2) and the endwall (1) are connected by a circular arc transition, and the outer radius of the circular arc is Jmm, satisfying: 0.2mm≤Jmm≤2mm.
9. The housing according to claim 1, characterized in that, The sidewall (2) has at least one second protrusion (22) on the side facing the receiving cavity (3), and the second protrusion (22) has a second groove (21) on the side facing away from the receiving cavity (3).
10. The housing according to claim 9, characterized in that, The shell is a cylindrical shell, and the second groove (21) extends circumferentially along the side wall (2).
11. The housing according to claim 9, characterized in that, The shell is a cylindrical shell. Along the normal direction of the side wall (2), the second protrusion (22) protrudes from the surface of the side wall (2) toward the receiving cavity (3) by a height of K mm, satisfying: 0.02 mm ≤ K mm ≤ 0.2 mm; Alternatively, the housing is a square housing, and in the plane direction perpendicular to the side wall (2), the second protrusion (22) protrudes from the surface of the side wall (2) toward the receiving cavity (3) by a height of K mm, satisfying: 0.03 mm ≤ K mm ≤ 0.23 mm.
12. The housing according to any one of claims 1 to 11, characterized in that, The thicknesses of the end wall (1) and the side wall (2) are T1mm and T2mm respectively, satisfying: 1<T1 / T2≤2.
4.
13. The housing according to any one of claims 1 to 11, characterized in that, The thickness of the end wall (1) is T1mm, which satisfies: 0.21mm≤T1mm≤1.44mm; And / or, the thickness of the sidewall (2) is T2mm, satisfying: 0.2 mm≤T2mm≤0.6 mm.
14. The housing according to any one of claims 1 to 11, characterized in that, The phase transition conversion rate X of the shell satisfies: 0.005 AHX ≤ X AHX ≤ 0.05 AHX; And / or, the gloss level A of the housing satisfies: 10 GU ≤ A GU ≤ 200 GU; And / or, the height H mm of the sidewall (2) satisfies: 60 mm ≤ H mm ≤ 200 mm.
15. The housing according to any one of claims 1 to 11, characterized in that, The gloss of the end wall (1) is A1GU, which satisfies: 20 GU≤A1 GU≤200 GU.
16. The housing according to any one of claims 1 to 11, characterized in that, The gloss of the sidewall (2) is A2, which satisfies: 10 GU≤A2 GU≤185 GU.
17. A single-cell battery, characterized in that, include: Battery cell; And a housing as described in any one of claims 1 to 16 above, wherein the battery cell is disposed within the receiving cavity (3) of the housing.
18. The single-cell battery according to claim 17, characterized in that, The end wall (1) of the housing includes a top wall located at the upper part of the individual battery cell along the height direction.
19. The single-cell battery according to claim 17, characterized in that, The end wall (1) of the housing includes a bottom wall located at the opposite bottom of the single cell along the height direction; the cell is disposed above the bottom wall, and the phase change conversion rate X AHX of the housing satisfies: 0.01 AHX≤X AHX≤0.05 AHX.
20. The single-cell battery according to claim 17, characterized in that, The single cell includes a cylindrical cell; the end wall (1) of the casing is circular, and the diameter D1 of the end wall (1) satisfies: 18mm≤D1mm≤80mm.
21. The single-cell battery according to claim 20, characterized in that, The battery cell includes a battery cell body and a tab extending from at least one end of the battery cell body. The tab is electrically connected to the end wall (1). At this time, the height H mm of the side wall (2) satisfies: 60 mm ≤ H mm ≤ 185 mm.
22. A battery pack, characterized in that, include: A housing (811); and a plurality of individual cells as described in any one of claims 17 to 21, disposed within the housing (811).
Citation Information
Patent Citations
Battery and electric device comprising same
CN119542632A
Battery shell and battery