A method for preparing high-purity zinc oxide and synergistic dechlorination

By employing a method involving acid dissolution and hydrothermal dechlorination, deep dechlorination of cuprous oxide using gradient redox potential, and composite precipitation of ammonium bicarbonate and ammonia, the problem of the inability to simultaneously achieve high zinc recovery rate and chloride ion purity in existing technologies has been solved, thus realizing the preparation of high-purity zinc oxide and the resource recovery of chlorine.

CN122748708BActive Publication Date: 2026-11-10HUNAN RUIXIANG NONFERROUS METAL MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611224611.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-13
Publication Date
2026-11-10
Estimated Expiration
2046-08-13

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively suppress chlorine from entering the solution and achieve deep removal and resource recovery of chlorine while ensuring high zinc recovery rates. Furthermore, traditional methods suffer from zinc loss and the discharge of chlorine-containing slag.

Method used

A method combining acid dissolution and hydrothermal dechlorination, gradient redox potential cuprous deep dechlorination, and ammonium bicarbonate and ammonia water composite precipitation is employed. Through differentiated pH control, side-flow crystallization, and low-temperature calcination, selective dissolution of zinc and graded diversion and resource recovery of chlorine are achieved.

Benefits of technology

This method achieves high zinc recovery and high-purity zinc oxide preparation, reduces the chlorine load in the main liquid, decreases the pressure on subsequent deep dechlorination treatment, and realizes the resource utilization of chlorine, significantly improving product purity and recovery rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122748708B_ABST
    Figure CN122748708B_ABST
Patent Text Reader

Abstract

This invention relates to the field of inorganic zinc compound preparation and secondary resource utilization of chlorinated zinc, specifically to a method for preparing high-purity zinc oxide and synergistic dechlorination. The invention discloses a method for preparing high-purity zinc oxide and synergistic dechlorination, comprising: subjecting chlorinated zinc oxide raw material to a first-stage weakly acidic acid dissolution to inhibit the decomposition of basic zinc chloride, yielding a low-chlorine main solution and a chlorine-rich slag; the chlorine-rich slag undergoes low-temperature hydrothermal dechlorination to recover dilute hydrochloric acid and is returned to the acid dissolution stage; the dechlorinated zinc slag enters a second-stage enhanced acid dissolution stage to extract residual zinc; the high-chlorine zinc-containing solution generated from the second-stage acid dissolution stage is combined with the acidic chlorine-containing hydrothermal liquid generated from the first-stage hydrothermal dechlorination stage to form a high-chlorine byproduct; the high-chlorine byproduct undergoes side-flow freeze-crystallization to precipitate zinc chloride byproduct and block the chlorine cycle; the low-chlorine main solution undergoes cuprous dechlorination and copper removal purification with precisely controlled redox potential, followed by the generation of a basic zinc carbonate precursor using ammonium bicarbonate-ammonia water composite precipitant, and finally low-temperature calcination to obtain electronic-grade high-purity zinc oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of inorganic zinc compound preparation and secondary resource utilization of chlorinated zinc, specifically to a method for preparing high-purity zinc oxide and synergistic dechlorination. Background Technology

[0002] Chlorine-containing zinc oxide mainly originates from lead-zinc smelting fumes, zinc-containing dust and sludge from steelmaking, rotary kiln flue gas ash, and enriched products of zinc-containing solid waste. These materials have a high zinc content but also contain impurities such as chlorine, fluorine, lead, cadmium, iron, and copper. Chlorine in these materials typically exists in the form of soluble zinc chloride, basic zinc chloride, and adsorbed chlorine. Conventional acid leaching can improve the zinc leaching rate, but chlorine will enter the leaching solution along with the zinc, increasing the difficulty of subsequent deep purification. If gentle leaching or pre-washing dechlorination is used to reduce the chlorine content, it easily leads to zinc loss and the discharge of chlorine-containing slag.

[0003] To address the aforementioned problems, existing technologies attempt to solve the dechlorination challenge of high-fluoride-chlorinated zinc oxide using ammonia-ammonium carbonate selective leaching technology. For example, CN105129839A discloses a method for producing micron-sized zinc oxide using high-fluoride-chlorinated zinc oxide as a raw material. This method uses ammonia and ammonium carbonate as leaching agents, controlling the final leaching pH to 4.7, allowing Zn, Cl, F, Cd, and some Fe to enter the leaching solution. The solution is then purified through oxidation, zinc powder replacement, and ammonium sulfide purification to obtain a refined solution. This method can prepare zinc oxide from high-fluoride-chlorinated zinc oxide. However, while this method can prepare zinc oxide from high-fluoride-chlorinated zinc oxide, its basic route involves introducing chlorine along with zinc into the ammonia leaching solution followed by purification, failing to achieve graded diversion and targeted treatment of chloride ions according to their concentration gradient within the system.

[0004] In summary, how to innovate a new method that can inhibit chlorine from entering the solution at the source, achieve deep removal and resource recovery of chlorine, reduce calcination temperature, and improve product purity while ensuring high zinc recovery rate has become an urgent technical problem to be solved in this field. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing high-purity zinc oxide and synergistic dechlorination, so as to solve the technical problems in the prior art, such as the inability to achieve high zinc recovery rate and low chloride ion purity, and the high energy consumption of chlorine-containing waste residue disposal.

[0006] The specific technical solution is as follows:

[0007] This invention provides a method for preparing high-purity zinc oxide and synergistically dechlorinating it, comprising the following steps: S1. First-stage acid dissolution and hydrothermal dechlorination: After slurrying the chlorine-containing zinc oxide raw material with water, dilute sulfuric acid is added for a first-stage selective acid dissolution, so that the zinc oxide dissolves preferentially while the chlorine-containing zinc phase is mainly retained in the solid phase. Solid-liquid separation yields low-chlorine zinc sulfate main liquid and a first-stage chlorine-rich slag. The first-stage chlorine-rich slag is subjected to a closed hydrothermal reaction with water. After cooling, solid-liquid separation is performed to obtain dechlorinated zinc slag and acidic chlorine-containing hydrothermal liquid.

[0008] S2, Two-stage acid dissolution and side-flow crystallization: The dechlorinated zinc slag is subjected to two-stage enhanced acid dissolution, and solid-liquid separation is performed to obtain two-stage zinc-containing liquid and final slag; wherein, the portion of the two-stage zinc-containing liquid with a chloride ion concentration higher than a preset threshold is combined with the acidic chlorinated hydrothermal liquid as a high-chlorine auxiliary liquid and enters the high-chlorine branch, and the portion with a chloride ion concentration not higher than the preset threshold is incorporated into the low-chlorine zinc sulfate main liquid; the high-chlorine auxiliary liquid is divided proportionally, a portion is directly recycled back to the first-stage acid dissolution, and the remaining portion is subjected to vacuum evaporation and concentration, and then cooled and crystallized to precipitate hydrated zinc chloride, and the crystallization mother liquor is returned to the high-chlorine branch for recycling.

[0009] S3. Gradient Redox Potential Cuprous Deep Dechlorination: Add copper sulfate to the low-chlorine main solution to achieve a copper ion to chloride ion molar ratio of 1.05:1; activate online redox potential monitoring, add zinc powder suspension dropwise under an inert atmosphere, and adjust the dropping rate according to the online redox potential feedback to reduce copper ions to form cuprous ions, which then react with chloride ions to form cuprous chloride precipitate. After the reaction is complete, filter to remove the cuprous chloride precipitate; then add ammonium sulfide solution to the filtrate to form copper sulfide precipitate from the residual copper ions, and filter to obtain a refined zinc sulfate solution.

[0010] S4. Precipitation and low-temperature calcination: The refined zinc sulfate solution is mixed with ammonium carbonate solution and ammonia water to carry out a precipitation reaction to generate a basic zinc carbonate precursor. The basic zinc carbonate precursor is filtered, washed and calcined to obtain a high-purity zinc oxide product.

[0011] Furthermore, the ammonium carbonate salt is an ammonium bicarbonate solution or an ammonium carbonate solution.

[0012] Further, in S1, the slurrying process takes 20-40 minutes; the selective acid dissolution is performed under the following conditions: reaction temperature 35-45℃, stirring speed 100-200 rpm, final pH controlled at 3.8-4.2, and reaction time 40-80 minutes; the closed hydrothermal reaction is performed under the following conditions: temperature raised to 170-190℃, system pressure raised to 0.7-0.9 MPa, and heat preservation reaction for 1-3 hours; and the cooling process takes place at a temperature of 50-70℃.

[0013] Further, the two-stage enhanced acid dissolution described in S2 is characterized by a reaction temperature of 60-70℃, a stirring speed of 150-250 rpm, a final pH of 2.5-3, and a reaction time of 60-120 minutes; the reduced-pressure evaporation and concentration is characterized by a first-effect temperature of 80-90℃ and a vacuum degree of -0.085 to -0.06 MPa, a second-effect temperature of 60-70℃ and a vacuum degree of -0.095 to -0.07 MPa, and evaporation and concentration until the ZnCl2 concentration reaches 60-65 wt%; the cooling crystallization requires controlling the crystallization temperature at 10-20℃ and maintaining the temperature with stirring for 1-3 hours.

[0014] Further, in step S3, the online ORP monitoring is initiated under the following conditions: initial ORP of +240 to +280 mV, initial dropping rate of 3 to 8 mL / min, maintaining a reaction temperature of 55 to 65 °C, and stirring speed of 100 to 140 rpm. The dropping rate is adjusted based on online redox potential feedback as follows: when the system ORP drops to +90 to +110 mV, the dropping rate is reduced to 1 to 3 mL / min; when the system redox potential drops to +80 to +100 mV, the dropping is stopped. The reaction is completed in a total reaction time of 30 to 50 minutes.

[0015] Further, in S4, the ammonium carbonate solution and ammonia water are mixed, with n(NH4HCO3):n(NH3·H2O) = (5~7):1; the precipitation reaction is carried out at a temperature of 40~50℃, a stirring speed of 80~120rpm, a final pH of 7.5~8.5, and a reaction time of 45~90 minutes; the calcination is carried out by heating to 380~420℃ at a heating rate of 3~8℃ / min and holding for calcination for 1~2 hours.

[0016] Compared with the prior art, the present invention has the following beneficial effects: (1) Reduce the chlorine load of the main liquid: The present invention uses two-stage differential pH acid dissolution. In the first stage, zinc oxide is selectively dissolved and basic zinc chloride is inhibited under weak acid conditions, so that the chloride ion content of the main liquid is significantly reduced compared with the traditional strong acid full dissolution process, which reduces the treatment pressure of subsequent deep dechlorination.

[0017] (2) Achieving chlorine balance and resource utilization: This invention precipitates zinc chloride by-product by side-flow depressurization evaporation-freeze crystallization of the two-stage high-chlorine by-product, effectively blocking the cyclic enrichment of chlorine; at the same time, the chlorine-rich slag is dechlorinated by low-temperature hydrothermal recovery and dilute hydrochloric acid is recycled for acid dissolution process, realizing the resource utilization of chlorine element.

[0018] (3) Obtaining a crystalline precursor: The present invention uses ammonium bicarbonate and ammonia water as a composite precipitant to generate a crystalline basic zinc carbonate precursor, which avoids the problems of difficult filtration and strong adsorption of traditional zinc hydroxide colloids, and the precursor can be completely decomposed at a lower temperature.

[0019] (4) Ensuring high purity and high yield of the product: Through the synergistic combination of two-stage acid dissolution, step-by-step chlorine balance, cuprous / sulfide dechlorination, sodium-free precipitation and low-temperature calcination, the present invention obtains electronic-grade high-purity zinc oxide products while ensuring high zinc recovery rate, and the slag phase is recycled and utilized, with only a small amount of final slag open circuit. Attached Figure Description

[0020] Figure 1 This is a flowchart of a method for preparing high-purity zinc oxide and synergistically dechlorinating according to the present invention.

[0021] Figure 2 The XRD patterns of the raw materials, basic zinc carbonate precursor, and high-purity zinc oxide product in Example 1 of this invention are shown.

[0022] Figure 3 This is a bar chart comparing the Cl / Zn mass ratio of materials in each process stage of Embodiment 1 of the present invention.

[0023] Figure 4 This is the chlorine distribution balance curve for 168 hours of continuous operation of the process in Example 1 of the present invention. Detailed Implementation

[0024] This invention proposes a method for preparing high-purity zinc oxide and synergistically dechlorinating it, such as... Figure 1 The diagram shown is a flowchart of a method for preparing high-purity zinc oxide and synergistically dechlorinating according to the present invention. The detailed preparation steps are as follows: 1. Acid dissolution and hydrothermal dechlorination in one stage Zinc oxide reacts rapidly with sulfuric acid in the pH range of 3.8–4.2 to form soluble zinc sulfate. The layered structure of basic zinc chloride (Zn5(OH)8Cl2·H2O) is highly stable within this pH range, and the protonation rate of its hydroxyl-bridged bonds is much lower than the dissolution rate of zinc oxide. Therefore, most of the chlorine remains in the slag in solid form. After solid-liquid separation, the low-chlorine main liquid directly enters the subsequent purification chain, while the chlorine-rich slag is directly sent to a hydrothermal reactor for treatment at 170–190℃ and 0.7–0.9 MPa. Subcritical water has a lower dielectric constant and a higher ionization constant, exhibiting strong nucleophilic reactivity. This causes the layered structure of basic zinc chloride to collapse, decomposing it according to the reaction Zn5(OH)8Cl2·H2O → 5ZnO + 2HCl + 5H2O. The resulting acidic chlorine-containing hydrothermal liquid is sent to a high-chlorine auxiliary liquid system; the solid product, dechlorinated zinc slag, is transferred to a two-stage acid dissolution extraction system to remove residual zinc.

[0025] 2. Two-stage acid dissolution and lateral crystallization The zinc slag after hydrothermal dechlorination was subjected to a two-stage acid dissolution under strongly acidic conditions of pH 2.5-3.0 and temperature 60-70℃ to ensure complete dissolution of residual zinc components. The zinc-containing solution from the second stage was tested; if Cl... -If the concentration is ≤0.5g / L, it should be added to the low-chlorine main solution for zinc recovery; if Cl - If the concentration is >0.5 g / L, it is combined with the acidic chlorine-containing hydrothermal liquid produced by the first-stage hydrothermal dechlorination to form a high-chlorine byproduct. The high-chlorine byproduct is split in a 7:3 ratio, with 70% directly recycled back to the first-stage acid dissolution as an acid and zinc source, and the remaining 30% concentrated by vacuum evaporation and then crystallized at low temperature. The crystallization temperature is controlled to allow zinc chloride to precipitate in the form of hydrated zinc chloride crystals. By controlling the side flow rate, the system achieves a net reduction of approximately 30%~40% of chloride ions per batch, avoiding the unlimited enrichment of chlorine in the circulating system, while simultaneously recovering marketable zinc chloride byproducts.

[0026] 3. Gradient ORP cuprous chloride removal Add n(Cu) to the low-chlorine zinc sulfate main solution 2+ ):n(Cl - Add copper sulfate solution at a ratio of 1.05:1 to introduce Cu into the system. 2+ As a dechlorination medium, the dropping rate of zinc powder is controlled in real time using an online ORP monitor to stabilize the system potential within a window of +80 to +100 mV (vs SCE). At this potential, the zinc powder will partially remove Cu. 2+ Reduced to Cu + Meanwhile, another part of Cu 2+ It is reduced to active metallic copper. (Cu) + With Cl in the solution - The copper powder combines to form CuCl precipitate, while the surface of the active copper powder and residual Cu... 2+ Cl - A disproportionation reaction occurs (Cu) 2+ +Cu+2Cl - →2CuCl↓), the two work together to reduce Cl - The concentration of copper ions decreased from 150-300 ppm to 15-25 ppm. The CuCl precipitate generated during the reaction was removed by filtration to obtain a dechlorinated solution. Ammonium sulfide was added to the dechlorinated solution, and the extremely low solubility product of CuS precipitated the residual copper ions to below 1 ppm without introducing sodium ions.

[0027] 4. Precipitation and low-temperature calcination The refined zinc sulfate solution undergoes a precipitation reaction using a composite precipitant of ammonium bicarbonate and ammonia to generate a crystalline basic zinc carbonate precursor. This precursor avoids the problems of difficult filtration and strong adsorption associated with traditional zinc hydroxide colloids. After low-temperature calcination at 380–420°C, electronic-grade high-purity zinc oxide is obtained. The NH3 and CO2 released during the reaction are recovered as (NH4)2SO4 or NH4HCO3 via a dilute sulfuric acid absorption tower, achieving ammonia resource recycling.

[0028] The technical solution designed by this invention to solve the existing problems includes the following key points: 1. Differential pH acid solubility and open-circuit lateral crystallization Traditional acid leaching processes for zinc oxide containing chloride typically control the pH at a strongly acidic level of 1.5–2.5. While this achieves efficient zinc leaching, basic zinc chloride decomposes significantly within this pH range, leading to a large influx of chloride ions into the liquid phase and increasing the subsequent dechlorination load. This invention employs a two-stage differentiated pH acid leaching architecture. The first stage involves selective acid leaching under weakly acidic conditions at pH 3.8–4.2 and temperatures of 35–45°C. This pH range falls within the critical region for complete ZnO dissolution; ZnO can still react with H+ at pH > 3.5. + The reaction produces Zn 2+ The layered structure of basic zinc chloride (Zn5(OH)8Cl2·H2O) exhibits high stability in weakly acidic environments. The protonation rate of its hydroxyl-bridged bonds is significantly lower than the dissolution rate of ZnO. Therefore, ZnO preferentially reacts with sulfuric acid: ZnO + H2SO4 → ZnSO4 + H2O. The acidolysis of basic zinc chloride is inhibited, resulting in a low-chloride zinc sulfate main solution. - The first stage yields only 150-300 ppm of zinc ions. The second stage employs enhanced acid dissolution conditions at pH 2.5-3.0 and a temperature of 60-70℃ to deeply acid dissolve the zinc slag after hydrothermal dechlorination, ensuring the complete dissolution of residual zinc components in the first stage's chlorine-rich slag, achieving a total zinc recovery rate of over 96%. For the high-chlorine byproduct generated during the second-stage acid dissolution, this invention employs a chlorine balance control strategy combining partial circulation and open-circuit side-flow crystallization. 30% of the high-chlorine byproduct volume is used as an open-circuit side-flow, fed into a vacuum evaporation-freeze crystallization unit, with the crystallization temperature controlled at -5-15℃, causing ZnCl2 to precipitate as hydrated zinc chloride crystals, which are then sold as a byproduct. The remaining 70% of the high-chlorine byproduct is returned to the first-stage acid dissolution process as a partial acid and zinc source for reuse. This open-circuit side-flow reduces chloride ions in the system by approximately 30%-40% per batch, although the mother liquor still contains a relatively high concentration of Cl... - However, after returning to a section of acid dissolution, due to the large total volume of the acid dissolution system, the Cl in the mother liquor... - It is diluted to a level that does not affect the chlorine content of the first-stage filtrate. By adjusting the side flow rate, it can be adapted to raw materials with different chlorine contents, achieving long-term stable operation of the system.

[0029] 2. Two-way cascade dechlorination of sludge and liquid Traditional methods for treating chlorine-containing slag mainly involve high-temperature roasting to volatilize chlorides, which suffers from high energy consumption, HCl flue gas corrosion of equipment, and waste of chlorine resources. Liquid-phase dechlorination relies on barium salt precipitation, which is costly and produces difficult-to-treat barium slag. This invention constructs a two-way synergistic dechlorination system between slag and liquid phases. In the slag phase, the chlorine-rich slag produced by acid dissolution is placed in a hydrothermal reactor and treated for 2 hours at 170–190°C and 0.7–0.9 MPa. Under these conditions, water molecules are in a subcritical state, with a decreased dielectric constant and an increased ionization constant, allowing them to dissolve some non-polar substances while maintaining a high H₂ content.+ and OH - The concentration of basic zinc chloride increases, thus exhibiting strong nucleophilic reactivity. In this environment, the interlayer Cl-... - by OH - Through gradual displacement, the layered structure collapses and completely decomposes, proceeding according to the reaction Zn5(OH)8Cl2·H2O → 5ZnO + 2HCl + 5H2O. The HCl produced during decomposition is absorbed by water to obtain 8%–10% dilute hydrochloric acid, which is returned to the acid dissolution process for reuse. The remaining solid product is dechlorinated zinc slag, which is transferred to the second-stage acid dissolution process to extract residual zinc. Acidic chlorinated hydrothermal fluid reacts with Cl... - The two zinc-containing solutions with a concentration higher than 0.5 g / L are combined into a high-chlorine byproduct. 30% of the side stream is taken for vacuum evaporation-freeze crystallization to precipitate hydrated zinc chloride byproduct, thereby realizing the resource recovery of chlorine and the control of system chlorine balance.

[0030] In the liquid phase, the low-chlorine zinc sulfate main solution first enters the cuprous dechlorination unit with precise redox potential (ORP) control. Under a potential window where the ORP is controlled at +80~+100mV (vs SCE), the zinc powder removes some of the Cu. 2+ Reduced to Cu + Meanwhile, another part of Cu 2+ It is reduced to reactive metallic copper. The newly formed Cu + With Cl in solution - The copper powder combines to form CuCl precipitate, while the surface of the active copper powder reacts with residual Cu in the solution. 2+ Cl - Disproportionation reaction occurs: Cu 2+ +Cu+2Cl - →2CuCl↓. This potential window is set based on the following equilibrium: when the potential is above +150mV, Cu... + It is easily oxidized to Cu 2+ Dechlorination fails; Cu at potential below +50mV + Excessive reduction to Cu prevents the formation of CuCl. The two work synergistically to reduce Cl... - The concentration was reduced to 15-25 ppm. Then (NH₄)₂S was added, and the residual Cu in the solution... + or Cu 2+ With S 2- The reaction produces CuS precipitate, further reducing the Cu concentration to below 1 ppm. This stepwise dechlorination system achieves deep removal of chlorine and copper without introducing sodium ions.

[0031] 3. Preparation of high-purity basic zinc carbonate precursor by sodium-free ammonia-carbon composite precipitation Traditional methods for preparing high-purity zinc oxide often use NaOH as a precipitant to convert zinc sulfate into Zn(OH)₂ before calcination. Zn(OH)₂ is a colloidal precipitate, resulting in slow filtration. Furthermore, its surface is rich in hydroxyl groups, giving it a strong anion adsorption capacity, readily adsorbing Cl₂. - and Na + Washing is difficult. Although single ammonia precipitation avoids the introduction of sodium, Zn(OH)2 will redissolve as [Zn(NH3)4] in excess ammonia. 2+ This results in incomplete precipitation, and the product remains colloidal zinc hydroxide. This invention uses a composite precipitant of ammonium bicarbonate and ammonia, wherein the molar ratio of NH4HCO3 to NH3·H2O is 6:1. Under this ratio, the CO2-NH3-H2O equilibrium system in the solution mainly exists in the form of HCO3-. - and OH - CO3 2- The concentration is moderate. Zinc ions react with bicarbonate and hydroxide ions to form basic zinc carbonate precipitates, typically including Zn4CO3(OH)6·H2O or Zn5(CO3)2(OH)6, belonging to the orthorhombic crystal system. 2- It is embedded between Zn-O layers in a planar triangular coordination manner, forming a regular three-dimensional network structure. Unlike the layered or amorphous structure of Zn(OH)2, basic zinc carbonate is crystalline, with particle sizes typically ranging from 5 to 20 μm, much larger than Zn(OH)2 colloidal particles. Therefore, it has a fast filtration speed, and due to its small specific surface area and low surface hydroxyl density, it is effective against Cl... - and Na + The adsorption capacity is significantly weakened.

[0032] After the reaction, the mixture was aged for another 30 minutes to ensure complete crystal growth and a more uniform particle size distribution. The aged slurry was filtered using a vacuum filter. The mother liquor was collected and sent to a mother liquor treatment system, where it was concentrated by vacuum evaporation to recover the (NH4)2SO4 crystal byproduct. The crystallization mother liquor (containing unreacted NH4HCO3 and NH3) was returned to the precipitation process for recycling. The filter cake was washed three times with deionized water at a liquid-to-solid ratio of 3:1. After each wash, the washing endpoint was measured (to detect Cl in the washing solution). - <5ppm is acceptable), the washed filter cake is the wet-based basic zinc carbonate precursor, with a moisture content of approximately 42%, Cl - <5ppm, Na + Not detected. The NH3 and CO2 released during the reaction enter the dilute sulfuric acid absorption tower through the tail gas pipeline, and are recycled to generate (NH4)2SO4 or NH4HCO3, thus realizing the recycling of ammonia resources.

[0033] Example 1 Table 1 Raw Material Information Table

[0034] A method for preparing high-purity zinc oxide and synergistically dechlorinating it, using raw materials as shown in Table 1, includes the following steps: S1: Take 100 parts of chlorinated zinc oxide flue dust raw material and place it in a reaction vessel. Add deionized water at a liquid-to-solid ratio of 5:1 and slurry for 30 minutes. Then pump in 8% dilute sulfuric acid, control the reaction temperature at 40℃, and stir at 150 rpm for a selective acid dissolution. Control the final pH at 4 and the reaction time at 60 minutes. After the reaction, separate the solid and liquid using a plate and frame filter press to obtain low-chlorinated zinc sulfate main liquid and chlorine-rich slag. Load the chlorine-rich slag into a hydrothermal reaction vessel, add 80 parts of deionized water, seal and heat to 180℃, raise the system pressure to 0.85 MPa, and keep the reaction at this temperature for 2 hours. Then cool to 60℃ and depressurize. Separate the solid and liquid using a centrifuge to obtain dechlorinated zinc slag and acidic chlorine-containing hydrothermal liquid. The acidic chlorine-containing hydrothermal liquid contains hydrogen chloride and a small amount of zinc chloride, and enters the high-chlorine branch for later use.

[0035] S2: The dechlorinated zinc slag is transferred to a two-stage acid dissolution vessel, and 12% (w / w) dilute sulfuric acid is added. The temperature is raised to 65°C, and the stirring speed is 200 rpm for two-stage enhanced acid dissolution. The final pH is controlled at 2.8, and the reaction time is 90 minutes to ensure that the residual zinc components are fully dissolved. After the reaction, the solid and liquid components are separated by a plate and frame filter press to obtain the two-stage zinc-containing solution and the final slag. The Cl content in the two-stage zinc-containing solution is detected. - Concentration, Cl - The portion with a concentration below 0.5 g / L is added to the low-chlorine zinc sulfate main solution to recover the zinc leached in the second stage; the acidic chlorine-containing hydrothermal solution is then reacted with Cl... - The two zinc-containing solutions with a concentration higher than 0.5 g / L were combined into a high-chlorine byproduct. 30% of the high-chlorine byproduct volume was taken as an open-circuit side stream and fed into a double-effect vacuum evaporator. The temperature of the first effect was controlled at 85℃ and the vacuum degree at -0.075 MPa, and the temperature of the second effect was controlled at 65℃ and the vacuum degree at -0.085 MPa. The evaporation and concentration were carried out until the ZnCl2 concentration reached 62 wt%. The concentrate was then transferred to a crystallization kettle, and the crystallization temperature was controlled at 15℃. The mixture was kept at this temperature and stirred for 2 hours to precipitate hydrated zinc chloride crystals. The crystallization slurry was separated by a centrifuge to obtain zinc chloride salt byproducts and crystallization mother liquor. The mother liquor was returned to the high-chlorine branch for circulation via a corrosion-resistant pump.

[0036] S3: Take the low-chlorine zinc sulfate main solution according to n(Cu) 2+ ):n(Cl -Add 0.5 mol / L copper sulfate solution at a ratio of 1.05:1, transfer the solution to a reactor equipped with an online ORP electrode, purge the air with high-purity nitrogen to maintain a slight positive pressure of 0.02 MPa inside the reactor, control the reaction temperature at 60℃, and the stirring speed at 120 rpm. Using a saturated calomel electrode as a reference electrode, the initial ORP was measured to be +265 mV. Start the precision metering pump and continuously add zinc powder suspension at a flow rate of 5 mL / min, while maintaining the reaction temperature at 60℃ and the stirring speed at 120 rpm. When the system ORP decreases... When the ORP reached +100mV, the precision metering pump was reduced to 2mL / min and the addition continued. When the ORP dropped to +85mV, the addition was stopped, with a total reaction time of 38 minutes. After the reaction, the slurry was filtered through a 0.22μm PTFE precision membrane filter to obtain a dechlorinated solution and a CuCl filter cake. A 5wt% ammonium sulfide solution was added to the dechlorinated solution, the amount being 1.10 times the theoretical precipitate of residual copper. The pH was controlled at 4.2 and the temperature at 45℃, and the reaction was allowed to proceed for 30 minutes to allow residual copper ions to precipitate as copper sulfide. After filtration, a refined zinc sulfate solution was obtained. The refined zinc sulfate solution contained Cl... - The content decreased to about 20 mg / L, and the Cu content was less than 1 mg / L.

[0037] S4: Pump the refined zinc sulfate solution into the precipitation vessel, control the reaction temperature at 45℃, and the stirring speed at 100 rpm. Simultaneously add 1.5 mol / L ammonium bicarbonate solution and 8 mol / L ammonia water at a ratio of n(NH4HCO3):n(NH3·H2O) = 6:1. Control the pH at the reaction endpoint at 8, and the reaction time at 60 minutes. After the reaction, continue aging for 30 minutes, then filter using a vacuum filter. Wash the filter cake three times with deionized water at a liquid-to-solid ratio of 3:1 to detect the Cl content in the washing solution. - <5ppm is considered acceptable, yielding a wet-based basic zinc carbonate precursor. The wet-based basic zinc carbonate precursor is placed in an electrically heated box furnace and heated to 400℃ at a heating rate of 5℃ / min, then held at that temperature for 1.5 hours. The basic zinc carbonate decomposes at low temperature, and after cooling, an electronic-grade high-purity zinc oxide product is obtained.

[0038] XRD was used to analyze the raw materials, basic zinc carbonate precursor, and final high-purity zinc oxide product to determine the phase composition and crystal structure of the samples. The test results are shown in [Figure number missing]. Figure 2 The diffraction patterns of the raw materials simultaneously show standard characteristic peaks for both ZnO and Zn5(OH)8Cl2·H2O, proving that the chlorine in the raw materials is mainly combined into basic zinc chloride. The diffraction peaks of the basic zinc carbonate precursor correspond to the Zn5(CO3)2(OH)6 standard card, indicating that the product has a single phase and good crystallinity. The high-purity zinc oxide product only shows the characteristic peak of hexagonal wurtzite ZnO, with no obvious impurity peaks, indicating that the precursor is completely decomposed under low-temperature calcination conditions, resulting in a high-purity zinc oxide product without impurity phases.

[0039] As shown by the XRD characterization above, chlorine in the raw material is stably hosted in the sparingly soluble basic zinc chloride solid phase. This invention achieves selective separation of chlorine and zinc through a step-by-step acid dissolution-hydrothermal decomposition process. To quantitatively evaluate the dechlorination separation capacity of each process step, the Cl / Zn mass ratio of the materials in the key stages of the entire process was measured. The results are shown in […]. Figure 3 The raw material has a Cl / Zn ratio of 0.186; after the first stage of acid dissolution, the low-chlorine main liquid has a ratio of only 0.0221, while chlorine is enriched in the chlorine-rich slag (1.0463); the chlorine-rich slag is hydrothermally decomposed to separate an ultra-high-chlorine hydrothermal liquid with a Cl / Zn ratio as high as 3.5; the combined materials are then acid-dissolved in the second stage to obtain a high-chlorine byproduct liquid (1.0333), which can be crystallized to produce zinc chloride; after purification, the Cl / Zn ratio of the zinc sulfate solution is reduced to 0.0013, and the final high-purity zinc oxide has a Cl / Zn ratio of <0.0003, which meets the requirements for low-chlorine in electronic-grade applications.

[0040] The static tests described above verified the efficient dechlorination and separation effect of a single batch of materials. To further verify the stability of the process during continuous industrial operation, a 168-hour long-term continuous pilot-scale test was conducted to track the changes in the chlorine element distribution ratio within the system. The results are shown in […]. Figure 4 During the operating cycle, approximately 83% of the raw material chlorine enters the high-chlorine recovery branch, of which 74% is converted into zinc chloride byproduct, and about 8.5% of the chlorine is recycled with the mother liquor; less than 8.5% of the chlorine remains in the product system. The proportions of each component fluctuate very little throughout the process, the process has good stability during continuous operation, and simultaneously achieves deep dechlorination of the product and resource recovery of chlorine.

[0041] Example 2 The preparation method is the same as in Example 1, except that: S1: Slurry for 20 minutes; control the reaction temperature at 35℃ and the stirring speed at 100 rpm; control the final pH at 3.8 and the reaction time at 40 minutes; raise the temperature to 170℃, raise the system pressure to 0.7MPa, and keep the reaction at this temperature for 1 hour; release the pressure after cooling to 50℃. S2: Heat to 60℃, stir at 150 rpm; control the final pH at 2.5, and the reaction time at 60 minutes; control the first effect temperature at 80℃ and the vacuum degree at -0.085 MPa, the second effect temperature at 60℃ and the vacuum degree at -0.095 MPa, and evaporate and concentrate until the ZnCl2 concentration reaches 60 wt%; control the crystallization temperature at 10℃ and keep it at this temperature while stirring for 1 hour. S3: Initial ORP is +240mV; zinc powder suspension is continuously added dropwise at a flow rate of 3mL / min; maintain reaction temperature at 55℃ and stirring speed at 100rpm; when the system ORP drops to +90mV, the precision metering pump is reduced to 1mL / min and the addition continues; when the system ORP drops to +80mV, the addition is stopped, and the total reaction time is 30 minutes. S4: Control the reaction temperature at 40℃ and the stirring speed at 80 rpm; n(NH4HCO3):n(NH3·H2O)=5:1; control the pH at the reaction endpoint at 7.5 and the reaction time at 45 minutes; raise the temperature to 380℃ at a rate of 3℃ / min and keep it at that temperature for 1 hour. All other steps are the same.

[0042] Example 3 The preparation method is the same as in Example 1, except that: S1: Slurry for 40 minutes; control reaction temperature at 45℃ and stirring speed at 200 rpm; control final pH at 4.2 and reaction time at 80 minutes; raise temperature to 190℃, increase system pressure to 0.9 MPa, and maintain temperature for 3 hours; release pressure after cooling to 70℃. S2: Heat to 70℃, stir at 250 rpm; control the final pH at 3, and the reaction time at 120 minutes; control the first effect temperature at 90℃ and the vacuum degree at -0.06 MPa, the second effect temperature at 70℃ and the vacuum degree at -0.07 MPa, and evaporate and concentrate until the ZnCl2 concentration reaches 65 wt%; control the crystallization temperature at 20℃ and keep it warm and stir for 3 hours. S3: Initial ORP is +280mV; zinc powder suspension is continuously added dropwise at a flow rate of 8mL / min; maintain reaction temperature at 65℃ and stirring speed at 140rpm; when the system ORP drops to +110mV, the precision metering pump is reduced to 3mL / min and the addition continues; when the system ORP drops to +100mV, the addition is stopped, and the total reaction time is 50 minutes. S4: Control the reaction temperature at 50℃ and the stirring speed at 120 rpm; n(NH4HCO3):n(NH3·H2O)=7:1; control the pH at the reaction endpoint at 8.5 and the reaction time at 90 minutes; raise the temperature to 420℃ at a rate of 8℃ / min and keep it at that temperature for 2 hours. All other steps are the same.

[0043] Example 4 The preparation method is the same as in Example 1, except that: S4: Replace the ammonium bicarbonate solution with an ammonium carbonate solution, both of which are ammonium carbonate salts; All other steps are the same.

[0044] Comparative Example 1 High-purity zinc oxide was prepared using a traditional acid-dissolution-alkali precipitation process for zinc oxide containing chlorine. The preparation method is as follows: 100 parts of zinc oxide containing chlorine were slurried with deionized water at a liquid-to-solid ratio of 5:1. 15% (w / w) dilute sulfuric acid was pumped in, and the reaction temperature was controlled at 75℃. The final pH was 1.5. The reaction was carried out for 120 minutes with strong acid dissolution to fully dissolve the zinc oxide and basic zinc chloride. The solution was filtered to obtain zinc sulfate, and the filter residue was stored. At 65℃, 2.5 times the theoretical amount of zinc powder was added to displace and remove heavy metals. After filtration, a purified zinc sulfate solution was obtained. At 50℃, 20% NaOH solution was added to adjust the final pH to 8.5, precipitating Zn(OH)₂. The solution was filtered, and the filter cake was washed three times with deionized water at a liquid-to-solid ratio of 3:1. The solution was calcined at 600℃ for 2 hours to obtain the zinc oxide product.

[0045] Comparative Example 2 The preparation method is the same as in Example 1, except that: S1, S2: The two-stage differential pH acid dissolution step is omitted. 100 parts of chlorine-containing zinc oxide dust are subjected to only one-stage acid dissolution, with the pH controlled at 1.8 and the temperature at 70℃. After the reaction, solid and liquid are separated to obtain zinc sulfate main solution and chlorine-rich slag. The chlorine-rich slag is not subjected to hydrothermal dechlorination treatment, but is directly washed with water and then stored. Since the two-stage acid dissolution step is not performed, no two-stage zinc-containing solution or high-chlorine byproduct is generated. All other steps are the same.

[0046] Comparative Example 3 The preparation method is the same as in Example 1, except that: S2: Omit the side-flow crystallization open-circuit step, and mix the high-chlorine byproduct from step S2, i.e., the acidic chlorine-containing hydrothermal liquid, with Cl... - The combined solution of the two zinc-containing solutions with a concentration of >0.5 g / L was directly recycled back to the S1 first-stage acid dissolution process without vacuum evaporation and crystallization separation. The acid consumption was replenished with an equal amount of fresh sulfuric acid to maintain the acidity conditions of the acid dissolution system. This process was repeated for 5 batches. All other steps are the same.

[0047] Comparative Example 4 The preparation method is the same as in Example 1, except that: S3: Omit the gradient ORP control step and replace it with a fixed ratio, based on the Cl content in the solution. - Add zinc powder in 1.5 times the molar amount at once, react for 30 minutes, and then filter directly. All other steps are the same.

[0048] Comparative Example 5 The preparation method is the same as in Example 1, except that: S4: Replace the precipitant prepared in a ratio of n(NH4HCO3):n(NH3·H2O)=6:1 with ammonia water at a concentration of 8 mol / L, without adding ammonium bicarbonate, and control the pH at the reaction endpoint at 8.0; All other steps are the same.

[0049] Experimental Example 1 The high-purity zinc oxide products prepared in Examples 1-4 and Comparative Examples 1-5 were tested: (1) ZnO main content (purity): Referring to GB / T 4372.1-2014 "Direct Method for Chemical Analysis of Zinc Oxide - Part 1: Determination of Zinc Oxide Content by Na2EDTA Titration", accurately weigh 0.25g of zinc oxide sample dried to constant weight at 105℃, place it in a 250mL beaker, add 15mL of hydrochloric acid and heat at low temperature to dissolve, cool and transfer to a 250mL volumetric flask, dilute with water to the mark, mix well, and filter dry. Transfer 50mL of filtrate to a 250mL conical flask, add 20mL of water, 10mL of potassium fluoride solution, 5mL of triethanolamine and 2 drops of xylenol orange indicator, adjust the solution with ammonia water to a stable rose red, then adjust with hydrochloric acid to yellow, add 1 drop of hydrochloric acid, add 10mL of hexamethylenetetramine buffer solution, and titrate with 0.02mol / L Na2EDTA standard titration solution until the solution changes from purple-red to bright yellow as the endpoint. The main content of zinc oxide is expressed as mass fraction. Each group should have no fewer than 5 valid samples, and the final result should be the average.

[0050] (2) Cl - Content: Referring to GB / T 3051-2025 "General Methods for Determination of Chloride Content in Inorganic Chemical Products—Mercurometric Method and Ion Chromatography", accurately weigh 0.2~1.0g of zinc oxide sample, place it in a 100mL beaker, add an appropriate amount of water to moisten, slowly add nitric acid solution until the sample is completely dissolved, heat to boiling to remove CO2, cool, transfer to a 100mL volumetric flask, dilute with water to the mark, and mix well. Transfer an appropriate amount of the test solution through a 0.22μm filter membrane and inject it into an ion chromatograph. Use a sodium carbonate-sodium bicarbonate mixed solution as the eluent, detect with a conductivity detector, and quantify using the external standard method. The chloride ion content is expressed as a mass fraction. At least 5 parallel samples should be tested in each group, and the average value should be taken.

[0051] (3) Total zinc recovery rate: Refer to YS / T 1171.1-2017 "Chemical Analysis Methods for Recycled Zinc Raw Materials—Part 1: Determination of Zinc Content by Na2EDTA Titration" to determine the mass fraction of zinc in the raw material. Accurately weigh 0.30 g of the raw material sample that has been dried to constant weight at 105℃, place it in a 250 mL beaker, moisten it with a small amount of water, add 2 mL of ammonium fluoride solution and 10 mL of hydrochloric acid, and heat at low temperature to decompose it; add 5 mL of nitric acid and 5 mL of sulfuric acid, continue heating until white fumes of sulfuric acid are emitted, remove and cool, dilute with water to about 50 mL, heat to a gentle boil, cool and let stand for 2 h, filter with slow-speed filter paper, and wash with sulfuric acid. Adjust the filtrate with ammonia water until precipitation is complete and add 10 mL in excess, heat to a gentle boil for 1~2 min, filter while hot, and wash with hot ammonium chloride washing solution. The filtrate was concentrated to approximately 100 mL, cooled, and then 0.1 g ascorbic acid, 25 mL acetate-sodium acetate buffer solution, 5 mL potassium fluoride solution, 10 mL sodium thiosulfate solution, and 2 drops xylenol orange indicator were added. Titration was performed with 0.02 mol / L Na₂EDTA standard titration solution until the solution changed from purple-red to bright yellow. The mass fraction of zinc was calculated based on the volume of Na₂EDTA consumed. The total zinc recovery rate was calculated using the following formula: Total zinc recovery rate (%) = (Final zinc oxide product mass × Mass fraction of zinc in the final product) / (Raw material mass × Mass fraction of zinc in the raw material) × 100%; whereby the mass fraction of zinc in the final product was determined according to the method described in GB / T 4372.1-2014 "Direct Method for Chemical Analysis of Zinc Oxide—Part 1: Determination of Zinc Oxide Content by Na₂EDTA Titration". At least 5 parallel samples were tested in each group, and the average value was taken.

[0052] Table 2 Comparison of experimental results of Examples 1-4 and Comparative Examples 1-5

[0053] The experimental results of Examples 1-4 and Comparative Examples 1-5 are shown in Table 2. The high-purity zinc oxide product obtained in Example 1 of this invention has a ZnO main content of 99.91% and a Cl content of 99.91%. - With a content as low as 15 ppm and a total zinc recovery rate of 96.30%, the technical solution of this invention demonstrates its comprehensive superiority in improving product purity, deep dechlorination, and increasing zinc recovery rate.

[0054] Example 2, using a lower reaction temperature and shorter reaction time, resulted in a decrease in the total zinc recovery rate to 95.78%. This is because the decomposition rate of basic zinc chloride is significantly slowed down under low-temperature conditions, and insufficient second-stage acid dissolution time also prevented the residual zinc in the chlorine-rich slag from fully dissolving, demonstrating that appropriate reaction conditions are crucial to ensuring recovery. Example 3 increased the reaction temperature to 45°C and 70°C, and extended the time to 80 minutes and 120 minutes, allowing the Cl... -The content was further reduced to 12 ppm, and the total zinc recovery rate increased to 96.82%. High-temperature, long-duration conditions not only promoted the complete decomposition of basic zinc chloride but also enhanced the thermodynamic driving force of the cuprous dechlorination reaction. This result indicates that appropriately enhancing reaction conditions based on optimized parameters can further improve the process efficiency, but energy consumption costs must be balanced. Example 4 used ammonium carbonate instead of ammonium bicarbonate as the precipitant; the ZnO content and Cl content... - The content and recovery rate were very close to those of Example 1. Ammonium carbonate hydrolysis in solution can also provide carbonate ions and adjust pH. After the ratio is adjusted, its precipitation effect is basically equivalent to that of ammonium bicarbonate. This proves that the two ammonium salts are versatile in sodium-free ammonia-carbon precipitation systems and can be flexibly selected according to the availability of raw materials.

[0055] Comparative Examples 1-5, lacking key technologies, showed varying degrees of reduced overall performance compared to the examples. Comparative Example 1, employing a traditional strong acid-to-alkali precipitation process, lacked crucial technologies such as two-stage differentiated pH acid dissolution for chlorine control, open-circuit side-flow crystallization to prevent chlorine enrichment, gradient ORP cuprous dechlorination, and sodium-free ammonia-carbon precipitation, resulting in lower product Cl. - The content was as high as 1252 ppm, the main ZnO content was only 99.19%, and the recovery rate was 93.48%, all of which were significantly worse than those of Example 1. Comparative Example 2 omitted the two-stage enhanced acid dissolution step, and the chloride-rich slag was directly stockpiled without secondary zinc extraction, resulting in a large loss of residual zinc in the slag, and the total zinc recovery rate dropped to 91.22%. At the same time, the high concentration of chloride ions introduced by the first-stage acid dissolution was not effectively diluted and diverted, and the product Cl - The content was as high as 848 ppm, with ZnO content as low as 99.34%; Comparative Example 3 omitted the open-circuit crystallization step of the high-chlorine byproduct liquid, and recycled all the high-chlorine byproduct liquid generated in the second stage acid dissolution back to the first stage acid dissolution, resulting in the batch-by-batch enrichment of chloride ions in the system. When running to the 5th batch, the product Cl - The zinc content accumulated to 422 ppm, and the main ZnO content decreased to 99.42%. Although the total zinc recovery rate was only slightly affected, the chlorine content of the product could no longer meet the electronic grade standard, proving that the open-circuit side flow plays an irreplaceable role in maintaining the chlorine balance of the system. Comparative Example 4 omitted gradient ORP control and adopted a fixed feeding method of adding zinc powder all at once, which resulted in the cuprous dechlorination reaction not being able to proceed within the optimal potential window. + Generation rate and Cl - Precipitation efficiency mismatch, product Cl -The content was 86 ppm, the main ZnO content was 99.68%, and the total zinc recovery rate was 94.71%. Although this was better than other comparative examples, it was still significantly worse than Example 1, proving that precise control of gradient ORP is a key technical feature for achieving deep dechlorination. Comparative Example 5 used a single ammonia solution for precipitation without adding ammonium bicarbonate, resulting in a precipitate of colloidal zinc hydroxide rather than crystalline basic zinc carbonate. Colloidal zinc hydroxide has a large specific surface area and abundant surface hydroxyl groups, exhibiting a strong adsorption capacity for chloride ions and impurity metal ions. Although it was washed three times, the product still showed good adsorption of chloride ions and impurity metal ions. - The zinc content remained at 46 ppm, the main ZnO content was only 99.53%, and the total zinc recovery rate was 94.49%. These results indicate that the addition of ammonium bicarbonate is key to forming crystalline basic zinc carbonate precursors and achieving low-chlorine, high-purity products.

[0056] Table 3. Impurity element content of high-purity zinc oxide product in Example 1

[0057] Note: The contents of Pb, Cd, Cu, Fe, Al, Na, K, and As were determined by ICP-MS, the contents of S were determined by infrared carbon-sulfur analyzer, and the contents of F were determined by ion chromatography.

[0058] The high-purity zinc oxide product obtained in Example 1 was tested for impurity element content, and the results are shown in Table 3. Table 3 shows that the contents of heavy metal impurities such as lead, cadmium, copper, iron, and aluminum in the product are all lower than the standard reference values ​​for electronic-grade zinc oxide; the contents of alkali metal impurities such as sodium and potassium are lower than 5 mg / kg; the fluorine content is lower than 0.5 mg / kg; and the arsenic content is lower than 0.5 mg / kg. This indicates that the present invention effectively removes heavy metals, alkali metals, and harmful impurities from the raw materials through multi-stage purification steps including two-stage acid dissolution, zinc powder replacement, cuprous chloride removal, copper removal by sulfidation, and sodium-free ammonia carbon precipitation, achieving product purity that meets electronic-grade requirements.

[0059] In summary, this invention constructs a complete chlorine balance system through a two-stage differentiated pH acid dissolution gradient chlorine control, high-chlorine byproduct side-flow crystallization open circuit, low-temperature hydrothermal dechlorination and recycling of the slag phase, liquid-phase gradient ORP cuprous / sulfide gradient chlorine removal, and sodium-free ammonia-carbon composite precipitation. This system achieves a total zinc recovery rate ≥96% while ensuring the product Cl... - The content is stably controlled below 40 ppm, and the main ZnO content is increased to over 99.5%, while simultaneously achieving resource recovery of chlorine and recycling of slag. Compared with traditional acid-dissolution-alkali precipitation processes and comparative examples, this invention has significant advantages in dechlorination depth, product purity, zinc recovery rate, and environmental friendliness, providing an economically feasible technical path for the high-value utilization of chlorine-containing zinc oxide dust.

[0060] Those skilled in the art will readily understand that the present invention is perfectly suited to achieving the stated objectives, fulfilling the purposes, and realizing the advantages inherent in the invention as described above. The chemical substances, methods, steps, processes, molecules, and specific compounds mentioned herein are presently representative of preferred embodiments and are exemplary, and should not be construed as limiting the scope of the invention. Various variations and other applications will occur to those skilled in the art, all of which are included within the spirit of the invention and are defined by the scope of the claims.

[0061] It will be apparent to those skilled in the art that various substitutions and modifications can be made to the invention disclosed herein without departing from the scope and spirit of the invention.

Claims

1. A method for preparing high-purity zinc oxide and synergistically dechlorinating it, characterized in that, Includes the following steps: S1. First-stage acid dissolution and hydrothermal dechlorination: After slurrying the chlorine-containing zinc oxide raw material with water, dilute sulfuric acid is added for a first-stage selective acid dissolution, which allows the zinc oxide to dissolve preferentially while the chlorine-containing zinc phase is mainly retained in the solid phase. Solid-liquid separation yields low-chlorine zinc sulfate main liquid and a first-stage chlorine-rich slag. The first-stage chlorine-rich slag is then subjected to a closed hydrothermal reaction with water. After cooling, solid-liquid separation is performed to obtain dechlorinated zinc slag and acidic chlorine-containing hydrothermal liquid. S2, Two-stage acid dissolution and side-flow crystallization: The dechlorinated zinc slag undergoes two-stage enhanced acid dissolution, and solid-liquid separation yields two-stage zinc-containing solutions and final slag; wherein, the portion of the two-stage zinc-containing solutions with a chloride ion concentration higher than a preset threshold, together with the acidic chlorinated hydrothermal fluid, enters the high-chlorine branch as a high-chlorine auxiliary liquid, and the portion with a chloride ion concentration not higher than the preset threshold is incorporated into the low-chlorine zinc sulfate main liquid; the high-chlorine auxiliary liquid is divided proportionally, a portion is directly recycled back to the first-stage acid dissolution, and the remaining portion is subjected to vacuum evaporation and concentration, and then cooled and crystallized to precipitate hydrated zinc chloride, and the crystallization mother liquor is returned to the high-chlorine branch for recycling; S3. Gradient Redox Potential Cuprous Deep Dechlorination: Add copper sulfate to the low-chlorine main solution to achieve a copper ion to chloride ion molar ratio of 1.05:1; activate online redox potential monitoring, add zinc powder suspension dropwise under an inert atmosphere, and adjust the dropping rate according to the online redox potential feedback to reduce copper ions to form cuprous ions, which then react with chloride ions to form cuprous chloride precipitate. After the reaction is complete, filter to remove the cuprous chloride precipitate; then add ammonium sulfide solution to the filtrate to form copper sulfide precipitate from the residual copper ions, and filter to obtain a purified zinc sulfate solution. S4. Precipitation and calcination: The refined zinc sulfate solution is mixed with ammonium carbonate solution and ammonia water to carry out a precipitation reaction to generate a basic zinc carbonate precursor. The basic zinc carbonate precursor is filtered, washed and calcined to obtain a high-purity zinc oxide product.

2. The method for preparing high-purity zinc oxide and synergistically dechlorinating it as described in claim 1, characterized in that, The ammonium carbonate salt is an ammonium bicarbonate solution or an ammonium carbonate solution.

3. The method for preparing high-purity zinc oxide and synergistically dechlorinating it as described in claim 1, characterized in that, The slurrying process described in S1 takes 20-40 minutes; the selective acid dissolution process is characterized by a reaction temperature of 35-45°C, a stirring speed of 100-200 rpm, a final pH of 3.8-4.2, and a reaction time of 40-80 minutes.

4. The method for preparing high-purity zinc oxide and synergistically dechlorinating it as described in claim 1, characterized in that, The closed hydrothermal reaction described in S1 is characterized by the following conditions: heating to 170~190℃, system pressure to 0.7~0.9MPa, and holding the reaction at this temperature for 1~3 hours; the cooling temperature is 50~70℃.

5. The method for preparing high-purity zinc oxide and synergistically dechlorinating it as described in claim 1, characterized in that, The two-stage enhanced acid dissolution described in S2 is set under the following conditions: reaction temperature 60~70℃, stirring speed 150~250rpm, final pH controlled at 2.5~3, and reaction time 60~120 minutes.

6. The method for preparing high-purity zinc oxide and synergistically dechlorinating it as described in claim 1, characterized in that, The reduced pressure evaporation concentration described in S2 is set under the following conditions: first effect temperature 80~90℃, vacuum degree -0.085~-0.06MPa, second effect temperature 60~70℃, vacuum degree -0.095~-0.07MPa, evaporation concentration until the ZnCl2 concentration reaches 60~65wt%; the cooling crystallization requires controlling the crystallization temperature at 10~20℃ and maintaining the temperature with stirring for 1~3 hours.

7. The method for preparing high-purity zinc oxide and synergistically dechlorinating it as described in claim 1, characterized in that, S3 describes the start of online redox potential monitoring, with the following conditions: initial redox potential of +240~+280mV, initial dropping rate of 3~8mL / min, maintaining reaction temperature of 55~65℃, and stirring speed of 100~140rpm.

8. The method for preparing high-purity zinc oxide and synergistically dechlorinating it as described in claim 1, characterized in that, S3 describes adjusting the dropping rate based on online redox potential feedback, specifically as follows: when the system's redox potential drops to +90~+110mV, the dropping rate is reduced to 1~3mL / min; when the system's redox potential drops to +80~+100mV, the dropping is stopped; the reaction is complete, and the total reaction time is 30~50 minutes.

9. The method for preparing high-purity zinc oxide and synergistically dechlorinating it as described in claim 1, characterized in that, The ammonium carbonate solution and ammonia water in S4 are mixed, with n(NH4HCO3):n(NH3·H2O)=(5~7):1; the precipitation reaction is carried out at a temperature of 40~50℃, a stirring speed of 80~120rpm, a final pH of 7.5~8.5, and a reaction time of 45~90 minutes.

10. The method for preparing high-purity zinc oxide and synergistically dechlorinating it as described in claim 1, characterized in that, The calcination described in S4 requires heating to 380-420°C at a rate of 3-8°C / min and holding for 1-2 hours.

Citation Information

Patent Citations

  • Method for producing micron-grade zinc oxide with high fluorine and chlorine crude zinc oxide as raw material

    CN105129839A

  • Synergistic resource utilization method for solid waste and wastewater of iron and steel plant

    CN120515789A

  • Method for preparing nano active zinc oxide from low grade zinc containing material

    CN1418972A