A monolithically integrated dual-active-region tunneling tandem AlGaInP red micro-LED chip and its fabrication method

By using a monolithically epitaxially grown dual-active-region tunnel junction series structure, the efficiency roll-off, heat dissipation, and reliability issues of AlGaInP red Micro-LED chips in automotive applications have been solved, achieving a balance of high brightness, low power consumption, and high reliability, making it suitable for automotive displays and AR-HUD scenarios.

CN122825602BActive Publication Date: 2026-11-17WEIJIU (SUZHOU) OPTOELECTRONICS TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611312916.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17
Estimated Expiration
2046-08-27

AI Technical Summary

Technical Problem

Existing AlGaInP red Micro-LED chips suffer from efficiency roll-off issues, difficulties in micro-area heat dissipation, bonding interface reliability risks, and high power consumption heat dissipation bottlenecks in automotive applications, making it impossible to simultaneously meet the requirements of ultra-high brightness, low power consumption, and high reliability.

Method used

A dual-active-region tunnel junction series structure with monolithic epitaxial growth is adopted to realize carrier transport through the tunnel junction. Combined with the all-monolithic integrated structure, the bonding interface is eliminated, and the driving efficiency and thermal management are optimized.

Benefits of technology

It achieves ultra-high brightness output, reduces driving power consumption, improves the long-term reliability and heat distribution uniformity of the device in the automotive environment, and meets the application requirements of high vibration and high power density in automotive applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122825602B_ABST
    Figure CN122825602B_ABST
Patent Text Reader

Abstract

This application discloses a monolithically integrated dual-active-region tunneling tandem AlGaInP red micro-LED chip and its fabrication method. The chip is grown monolithically using MOCVD epitaxial growth, and from bottom to top, it sequentially integrates a first n-type AlGaInP confinement layer, a first quantum well active region, a p-type AlInP electron blocking layer, a tunneling junction composed of p-type and n-type GaAs / GaInP tunneling layers, a second n-type AlGaInP confinement layer, a second quantum well active region, and a p-type GaP ohmic contact layer. This invention achieves monolithic tandem dual-active-region architecture through the tunneling junction, reducing the current density of a single active region by 50% and raising the efficiency roll-off threshold to 120 A / cm². 2 The tunneling junction voltage is reduced to 0.15~0.25V, and the total operating voltage increases by only 14.3%; the monolithic integration eliminates the thermal resistance at the bonding interface, and the heat distribution uniformity reaches more than 95%, meeting the requirements of ultra-high brightness and high reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor optoelectronic device technology, and in particular to a monolithically integrated dual active region tunneling series AlGaInP red light Micro-LED chip, specifically a monolithically integrated dual active region tunneling series AlGaInP red light Micro-LED chip for automotive ultra-high brightness requirements and its fabrication method. Background Technology

[0002] With the rapid development of intelligent driving and automotive display technologies, the application demands of automotive red Micro-LEDs in scenarios such as intelligent vehicle lights and AR-HUDs (augmented reality head-up displays) continue to increase, placing extremely high requirements on the brightness, efficiency, and environmental reliability of the devices. Existing AlGaInP red Micro-LED technology suffers from three insurmountable technical shortcomings when adapting to the ultra-high brightness requirements of automotive applications: First, mainstream single-active-area AlGaInP red Micro-LEDs have extremely high device operating current densities at the micrometer size, which greatly amplifies the efficiency roll-off problem, resulting in an effective brightness limit far below automotive requirements. At the same time, heat dissipation in the micro-area is difficult, and the risk of thermal reliability increases dramatically under high power density, making it impossible to meet the requirements of long life and high stability in automotive applications.

[0003] Second, the multi-active-region scheme using physical bonding stacking is difficult to guarantee in terms of alignment accuracy and interface uniformity at the micron scale of Micro-LED arrays. The introduced stress and defects will seriously reduce device yield and performance. Especially in the vehicle vibration environment, the bonding interface is prone to failure. At the same time, the bonding interface has high thermal resistance, which becomes a heat dissipation bottleneck under micro-scale high power density, further aggravating the thermal reliability problem.

[0004] Third, the conventional PN junction series connection scheme has extremely high process complexity and extremely low yield in achieving high-quality PN junction series connection within the Micro-LED unit; moreover, the chip operating voltage is nearly doubled after series connection, which will bring serious power consumption and heat dissipation burden in the vehicle battery system, exacerbating the risk of hot spots in the micro-area. At the same time, the uniform injection of current in the multi-junction microstructure also presents significant technical challenges.

[0005] In summary, existing technologies cannot simultaneously achieve ultra-high brightness, low power consumption, and high automotive reliability. There is an urgent need for a novel AlGaInP red Micro-LED chip structure and its fabrication method to systematically address the aforementioned technical challenges. Summary of the Invention

[0006] The purpose of this invention is to provide a monolithically integrated dual-active-region tunneling series AlGaInP red micro-LED chip and its fabrication method. By using a monolithically epitaxially grown tunneling junction series dual-active-region structure, it overcomes the high current density efficiency roll-off bottleneck, eliminates bonding interface reliability risks, and controls the voltage increase of the series structure, thereby achieving a balance between ultra-high brightness, high efficiency, and high reliability in automotive applications.

[0007] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: A monolithically integrated dual-active-region tunneling tandem AlGaInP red micro-LED chip includes an epitaxial layer structure formed by monolithic epitaxial growth. The epitaxial layer structure, from bottom to top, comprises a first n-type AlGaInP confinement layer, a first quantum well active region, a first p-type AlGaInP spacer layer, a p-type AlInP electron blocking layer, a p-type tunneling layer, an n-type tunneling layer, a second n-type AlGaInP confinement layer, a second quantum well active region, a second p-type AlGaInP spacer layer, a second p-type AlInP electron blocking layer, and a p-type GaP ohmic contact layer. The p-type tunneling layer and the n-type tunneling layer are stacked to form a tunneling junction. The tunneling junction is connected in series with the first quantum well active region and the second quantum well active region to realize carrier transport through tunneling mechanism. Both the first and second quantum well active regions employ a periodic quantum well structure with alternating stacks of GaInP well layers and (AlGa)InP barrier layers.

[0008] In a preferred embodiment, the epitaxial layer structure further includes a GaAs substrate, an n-type GaAs buffer layer, an n-type AlGaInP etch barrier layer, and an n-type GaAs ohmic contact layer disposed below the first n-type AlGaInP confinement layer; the n-type GaAs buffer layer is grown on the surface of the GaAs substrate, and the n-type AlGaInP etch barrier layer is located between the n-type GaAs buffer layer and the n-type GaAs ohmic contact layer; the GaAs substrate has a wafer size of 2 to 12 inches, a thickness of 350 to 650 μm, and a bevel angle of 2 to 15°.

[0009] In a preferred embodiment, the materials of the first n-type AlGaInP confinement layer and the second n-type AlGaInP confinement layer are (Al x1 Ga 1-x1 ) 0.5 In 0.5 P, where x1 ranges from 0.7 to 1, and the doping concentration is 1.0 × 10⁻⁶. 18 ~3.0×10 18 cm -3The thickness of each layer is 150~500nm; both the first and second quantum well active regions contain 1~5 pairs of quantum wells, wherein the GaInP well layer thickness is 1.5~4.5nm, (Al x2 Ga 1-x2 ) 0.5 In 0.5 The thickness of the p-type barrier layer is 4~10 nm, and x2 is 0.7~0.9 nm; the materials of the first p-type AlGaInP spacer layer and the second p-type AlGaInP spacer layer are (Al x3 Ga 1-x3 ) 0.5 In 0.5 P, x3 ranges from 0.8 to 0.9, and the doping concentration is 1.0 × 10⁻⁶. 18 ~2.0×10 18 cm -3 The thickness of each is 30~100nm.

[0010] In a preferred embodiment, the materials of the p-type tunneling layer and the n-type tunneling layer are GaAs or GaInP, and the doping concentration of both is 5.0 × 10⁻⁶. 18 ~1.0×10 19 cm -3 The thickness of each layer is 10~20nm; the operating voltage drop of the tunnel junction is 0.15~0.25V; the materials of the p-type AlInP electron blocking layer and the second p-type AlInP electron blocking layer are Al x4 In 1-x4 P, x4 is 0.5, and the doping concentration is 1.0 × 10⁴. 18 ~3.0×10 18 cm -3 The thickness of each layer is 200~900 nm; the doping concentration of the p-type GaP ohmic contact layer is 3.0 × 10⁻⁶. 18 ~5.0×10 18 cm -3 The thickness is 50~300nm.

[0011] This invention also provides a method for fabricating a monolithically integrated dual-active-region tunneling tandem AlGaInP red micro-LED chip, including an epitaxial growth process and a chip fabrication process; The epitaxial growth process employs MOCVD technology, using hydrogen as the carrier gas, to sequentially grow the following layers monolithically on a GaAs substrate: an n-type GaAs buffer layer, an n-type AlGaInP etch barrier layer, an n-type GaAs ohmic contact layer, a first n-type AlGaInP confinement layer, a first quantum well active region, a first p-type AlGaInP spacer layer, a p-type AlInP electron blocking layer, a p-type tunneling layer, an n-type tunneling layer, a second n-type AlGaInP confinement layer, a second quantum well active region, a second p-type AlGaInP spacer layer, a second p-type AlInP electron blocking layer, and a p-type GaP ohmic contact layer, thus obtaining an epitaxial wafer. The chip fabrication process includes, in sequence: S1, a p-type ITO transparent conductive layer is deposited by electron beam evaporation and then rapidly thermally annealed; S2, deposit a bonding metal layer on the p-type ITO transparent conductive layer, perform metal-to-metal bonding between the epitaxial wafer and the Si-based CMOS driving circuit, and then remove the GaAs substrate by wet etching. S3, spin-coating photoresist and then exposing and developing it under ultraviolet light to form a patterned mask, followed by ICP etching to form a Micro-LED mesa structure; S4 uses PECVD to deposit a SiO2 sidewall passivation layer and ion beam etching to achieve device isolation; S5. A SiO2 mask layer is deposited and patterned to expose the n-type ohmic contact layer. An n-type ITO transparent conductive layer is deposited to achieve n-type interconnection. Finally, an n-type electrode is deposited by electron beam evaporation and patterned by a lift-off process.

[0012] In a preferred embodiment, during the epitaxial growth process: The n-type GaAs buffer layer uses silane as the dopant source and trimethylgallium and arsenide as the growth sources. The growth temperature is 620–700 °C, the growth rate is 0.2–0.7 nm / s, and the doping concentration is 1.0 × 10⁻⁶. 18 ~3.0×10 18 cm -3 The thickness is 100~300nm; The n-type AlGaInP etch barrier layer uses silane as the dopant source and trimethylaluminum, trimethylgallium, trimethylindium, and phosphine as the growth sources. The growth temperature is 700–780 °C, the growth rate is 0.2–0.7 nm / s, and the doping concentration is 1.0 × 10⁻⁶. 18 ~3.0×10 18 cm -3 The thickness is 100~300nm; The n-type GaAs ohmic contact layer uses silane as the dopant source and trimethylgallium and arsine as the growth sources. The growth temperature is 620–700 °C, the growth rate is 0.1–0.3 nm / s, and the doping concentration is 3.0 × 10⁻⁶. 18 ~5.0×10 18 cm -3 The thickness is 10~50nm; Both the first n-type AlGaInP confinement layer and the second n-type AlGaInP confinement layer use silane as the dopant source and trimethylaluminum, trimethylgallium, trimethylindium and phosphine as the growth source, with a growth temperature of 700~780℃ and a growth rate of 0.2~0.5nm / s; Both the first and second quantum well active regions use trimethylaluminum, trimethylgallium, trimethylindium, and phosphine as growth sources, with a growth temperature of 700~780℃ and a growth rate of 0.1~0.2nm / s; both the first and second p-type AlGaInP spacer layers use magnesia-dicenocene as a doping source and trimethylaluminum, trimethylgallium, trimethylindium, and phosphine as growth sources, with a growth temperature of 700~780℃ and a growth rate of 0.2~0.5nm / s. Both the p-type AlInP electron blocking layer and the second p-type AlInP electron blocking layer use magnesia as the dopant source and trimethylaluminum, trimethylindium and phosphine as the growth source, with a growth temperature of 700~780℃ and a growth rate of 0.2~0.5nm / s. The p-type GaP ohmic contact layer uses magnesium pyrocene and carbon tetrabromide as doping sources and trimethylgallium and phosphine as growth sources. The growth temperature is 700~780℃ and the growth rate is 0.2~0.5nm / s.

[0013] In a preferred embodiment, during the epitaxial growth process, the p-type tunneling layer uses magnesia-3-carbide and carbon tetrabromide as doping sources; when the material is GaAs, it uses trimethylgallium and arsenide as growth sources; and when the material is GaInP, it uses trimethylgallium, trimethylindium, and phosphine as growth sources. The n-type tunneling layer uses disilane as the doping source, and the growth source corresponds to that of the p-type tunneling layer. The growth temperature of both the p-type and n-type tunneling layers is 700~780℃, the growth rate is 0.2~0.5nm / s, and the doping concentration is 5.0×10⁻⁶. 18 ~1.0×10 19 cm -3 The thickness of each is 10~20nm.

[0014] In a preferred embodiment, in step S1, the thickness of the p-type ITO transparent conductive layer is 150 nm, the indium-tin molar ratio of the ITO target is 9:1, the deposition rate is 1 nm / s, and the rapid thermal annealing treatment temperature is 400 °C and the treatment time is 180 s. In step S2, the bonding metal layer is a Cr / Pt / Au stacked structure, with each layer having a thickness of 300nm / 300nm / 200nm, and a deposition rate of 0.1~5nm / s. The temperature for the metal interfusion bonding is 400~700℃, the pressure is 3000~9000kg, and the bonding time is 10~60 minutes. The etching solution for removing the GaAs substrate by wet etching is a mixture of 10% ammonia and 10% hydrogen peroxide at a volume ratio of 4:1, and the etching time is 40 minutes.

[0015] In a preferred embodiment, in step S3, the photoresist is 5214 positive photoresist with a thickness of 500~3000nm, the developer is tetramethylammonium hydroxide aqueous solution, and the development time is 120s; the mask is a periodically arranged square or circular through-hole, corresponding to a Micro-LED mesa with a diameter of 1~50μm and a pixel pitch of 2~75μm; the etching gas for ICP etching is a mixture of Cl2 and BCl3, etching to the surface of the bonding metal layer; In step S4, the thickness of the SiO2 sidewall passivation layer is 10~100nm, the reaction gases for PECVD deposition are N2O and SiH4, the N2O flow rate is 1200sccm, the SiH4 flow rate is 300sccm, the plasma source power is 100W, the deposition temperature is 250℃, and the deposition rate is 1nm / s; the ion beam etching has an etching power of 300W, an etching rate of 2nm / s, and an etching time of 600s, etching through the ITO layer and the bonding metal layer to achieve electrical isolation of the device.

[0016] In a preferred embodiment, in step S5, the SiO2 mask layer has a thickness of 300 nm and is deposited using PECVD. The reactant gases are N2O and SiH4, with an N2O flow rate of 1200 sccm and a SiH4 flow rate of 300 sccm. The plasma source power is 100 W, the deposition temperature is 250 °C, and the deposition rate is 1 nm / s. The SiO2 mask layer in the patterned area is removed by ICP etching to expose the n-type GaAs ohmic contact layer. The etching gases are CF4 and Ar, with a CF4 flow rate of 25 sccm and an etching time of 400 s. The etching rate of SiO2 is 1.2 nm / s. The n-type electrode is a Cr / Pt / Au stacked structure with layer thicknesses of 300 nm / 300 nm / 200 nm, deposited by electron beam evaporation at a deposition rate of 0.1~5 nm / s. The stripping process is achieved by immersion in acetone or isopropanol organic solvent.

[0017] Due to the application of the above technical solution, the beneficial effects of this application compared with the prior art are as follows: 1. Break through the efficiency roll-off bottleneck to achieve ultra-high brightness output.

[0018] This invention adopts a dual active region series structure. Under the same total operating current, the operating current density of a single active region is reduced by 50%, which significantly delays the efficiency roll-off effect and pushes the efficiency roll-off threshold current density to over 120A / cm². The optical output power is doubled, which fully meets the application requirements of ultra-high brightness in automotive applications.

[0019] 2. Extremely low tunneling pressure drop, optimizing drive efficiency.

[0020] This invention employs an ultra-thin tunnel junction with ultra-high doping to achieve efficient carrier transport dominated by quantum tunneling. The operating voltage of a single tunnel junction is reduced to 0.15~0.25V, making the total operating voltage of the chip only 14.3% higher than that of a single junction device. This is far lower than the 100% voltage increase of the traditional PN junction series structure, significantly reducing driving power consumption and heat dissipation pressure, and adapting to the operating characteristics of automotive power systems.

[0021] 3. Monolithic integration enhances thermal management and improves automotive-grade reliability.

[0022] This invention adopts a fully monolithic epitaxial integrated structure, completely eliminating heterogeneous bonding interfaces and reducing the thermal resistance of the bonding interface by more than 12K / W, thus avoiding the risk of bonding failure at the source. At the same time, the tunneling junction layer also has the function of built-in heat sink, which significantly improves the uniformity of heat distribution inside the chip, increasing the heat distribution uniformity to more than 95%, effectively ensuring the long-term reliability of the device in the harsh environment of high vibration and high power density in automotive applications. Attached Figure Description

[0023] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0024] Figure 1 This is a schematic diagram of the epitaxial structure of the monolithically integrated dual active region tunneling series AlGaInP red micro-LED chip described in this invention. Figure 2 This is a schematic diagram of the complete chip structure after bonding of the Micro-LED chip described in this invention; Figure 3 This is a schematic flowchart of the fabrication method of the monolithically integrated dual active region tunneling series AlGaInP red light Micro-LED chip described in this invention. The components are as follows: 1. GaAs substrate; 2. n-type GaAs buffer layer; 3. n-type AlGaInP etch barrier layer; 4. n-type GaAs ohmic contact layer; 5. First n-type AlGaInP confinement layer; 6. First quantum well active region; 7. First p-type AlGaInP spacer layer; 8. p-type AlInP electron blocking layer; 9. p-type tunneling layer; 10. n-type tunneling layer; 11. Second n-type AlGaInP confinement layer; 12. Second quantum well active region; 13. Second p-type AlGaInP spacer layer; 14. Second p-type AlInP electron blocking layer; 15. p-type GaP ohmic contact layer; 16. Epitaxial wafer; 17. p-type ITO transparent conductive layer; 18. Bonding metal layer; 19. Si-based CMOS driving circuit; 20. SiO2 sidewall passivation layer; 21. n-type ITO transparent conductive layer; 22. n-type electrode. Detailed Implementation

[0025] To enable those skilled in the art to better understand the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present application, and not all embodiments. Based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without creative effort should fall within the scope of protection of the present application.

[0026] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate for the embodiments of this application described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0027] In this application, the terms "upper," "lower," "left," "right," "front," "rear," "top," "bottom," "inner," "outer," "middle," "vertical," "horizontal," "lateral," and "longitudinal" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. These terms are primarily for the purpose of better describing the invention and its embodiments, and are not intended to limit the indicated device, element, or component to having a specific orientation, or to be constructed and operated in a specific orientation.

[0028] Furthermore, in addition to indicating direction or positional relationship, some of the aforementioned terms may also have other meanings. For example, the term "above" may also be used in certain situations to indicate a dependency or connection. Those skilled in the art can understand the specific meaning of these terms in this invention based on the specific circumstances.

[0029] Furthermore, the terms "installation," "setup," "equipped with," "connection," "linking," and "socketing" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral structure; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium, or an internal connection between two devices, components, or parts. Those skilled in the art can understand the specific meaning of these terms in this invention based on the specific circumstances.

[0030] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. This application will now be described in detail with reference to the accompanying drawings and embodiments.

[0031] All epitaxial growth in all embodiments was performed using a commercial MOCVD system, chip fabrication was carried out using standard semiconductor process line equipment, and performance testing was performed using a probe station, integrating sphere, spectrometer, thermal resistance tester, and high and low temperature test chamber.

[0032] Example 1 As attached Figure 1 , Figure 2 As shown, this embodiment provides a monolithically integrated dual-active-region tunneling tandem AlGaInP red Micro-LED chip, specifically a GaAs tunneling junction scheme. This embodiment is a core structure example of the product, and the epitaxial layer structure from bottom to top is as follows: Substrate and underlying transition structure: It uses an n-type GaAs single crystal substrate, with a wafer size of 4 inches, a thickness of 450 μm, and a substrate bevel angle of 10°; Growth occurs sequentially above the substrate: n-type GaAs buffer layer: The n-type doping source is silane, with a doping concentration of 2.0 × 10⁻⁶. 18 cm -3 Thickness 200nm; n-type AlGaInP etch barrier layer: composed of (Al 0.2 Ga 0.8 ) 0.5 In 0.5 P, n-type doping concentration 2.0 × 10⁻⁶ 18 cm -3 Thickness 200nm; n-type GaAs ohmic contact layer: n-type doping concentration 4.0 × 10⁻⁶18 cm -3 Thickness 30nm.

[0033] First light-emitting unit structure: First type n AlGaInP confinement layer: material is (Al0) 0.8 Ga 0.2 ) 0.5 In 0.5 P, n-type doping concentration 2.0 × 10⁻⁶ 18 cm -3 Thickness 300nm; The first quantum well active region consists of three pairs of periodic GaInP well layers / (AlGa)InP barrier layers; the well layers are Ga... 0.5 In 0.5 P, thickness 3nm; barrier layer is (Al0) 0.8 Ga 0.2 ) 0.5 In 0.5 P, thickness 6nm; First p-type AlGaInP spacer layer: material is (Al 0.85 Ga 0.15 ) 0.5 In 0.5 P, p-type doping concentration 1.5 × 10⁻⁶ 18 cm -3 Thickness 60nm; p-type AlInP electron blocking layer: the material is Al 0.5 In 0.5 P, p-type doping concentration 2.0 × 10⁻⁶ 18 cm -3 Thickness 500nm.

[0034] Tunneling junction series structure: p-type tunneling layer: The material is GaAs, and the p-type doping source is co-doped with magnesia-magnesium diazotriene and carbon tetrabromide, with a doping concentration of 8.0 × 10⁻⁶. 18 cm -3 Thickness 15nm; n-type tunneling layer: The material is GaAs, the n-type dopant source is silane, and the doping concentration is 8.0 × 10⁻⁶. 18 cm -3 Thickness 15nm; The p-type tunneling layer and the n-type tunneling layer are stacked to form a tunneling junction, which is connected in series with the first and second quantum well active regions to realize carrier transport through quantum tunneling mechanism. The operating voltage drop of the tunneling junction is about 0.2V.

[0035] Second light-emitting unit structure: The second n-type AlGaInP confinement layer is completely identical to the first n-type AlGaInP confinement layer in terms of material, doping, and thickness. The second quantum well active region has the same structure and parameters as the first quantum well active region, and adopts a periodic quantum well structure with alternating stacks of GaInP well layers and (AlGa)InP barrier layers. The second p-type AlGaInP spacer layer has parameters that are completely identical to those of the first p-type AlGaInP spacer layer. The second p-type AlInP electron blocking layer has the same parameters as the lower p-type AlInP electron blocking layer.

[0036] Top contact layer: p-type GaP ohmic contact layer: The p-type doping source is co-doped with magnesia-magnesium diacene and carbon tetrabromide, with a doping concentration of 4.0 × 10⁻⁶. 18 cm -3 Thickness 200nm.

[0037] Example 2 This embodiment provides a monolithically integrated dual-active-region tunneling tandem AlGaInP red Micro-LED chip, specifically a GaInP tunneling junction scheme. This embodiment is a product extension structure embodiment, and the overall stack-up order is the same as that in Embodiment 1. The core difference is: Tunneling junction: Both the p-type and n-type tunneling layers are made of Ga. 0.5 In 0.5 P, with a doping concentration of 6.0 × 10⁻⁶. 18 cm -3 The thickness of each is 12nm, and the working voltage drop of the tunnel junction is approximately 0.22V; Active region: Both the first and second quantum well active regions employ a 5-pair quantum well structure, with a GaInP well layer thickness of 4 nm. 0.75 Ga 0.25 ) 0.5 In 0.5 The P-barrier layer thickness is 8nm; The materials, components, doping concentrations, and thicknesses of the remaining layers are consistent with those in Example 1.

[0038] Example 3 As attached Figure 3 As shown, this embodiment provides a method for fabricating a monolithically integrated dual-active-region tunneling tandem AlGaInP red Micro-LED chip. This embodiment is based on the chip structure of Embodiment 1 and fully executes the entire process of epitaxial growth and chip fabrication.

[0039] I. Epitaxial growth process (MOCVD process, hydrogen as carrier gas): Substrate pretreatment: A 4-inch n-type GaAs substrate is placed into the reaction chamber, the chamber pressure is evacuated to below 100 Pa, high-purity hydrogen is introduced, and the temperature is raised to 650℃ and kept at a constant temperature for 10 min to remove the surface oxide layer and organic contaminants.

[0040] n-type GaAs buffer layer growth: reaction chamber temperature 650℃, chamber pressure 100mbar, trimethylgallium, arsenide and disilane introduced, growth rate 0.5nm / s, growth thickness 200nm, doping concentration controlled at 2.0×10⁻⁶. 18 cm -3 .

[0041] n-type AlGaInP etch barrier layer growth: Temperature is increased to 750℃, and trimethylaluminum, trimethylgallium, trimethylindium, phosphine, and silane are introduced to regulate the composition (Al). 0.2 Ga 0.8 ) 0.5 In 0.5 P, growth rate 0.4 nm / s, growth thickness 200 nm, doping concentration 2.0 × 10⁻⁶ 18 cm -3 .

[0042] n-type GaAs ohmic contact layer growth: Cooling to 650℃, introducing trimethylgallium, arsenide, and disilane, growth rate 0.2 nm / s, growth thickness 30 nm, doping concentration 4.0 × 10⁻⁶ 18 cm -3 .

[0043] First type n AlGaInP confinement layer growth: Temperature increased to 750℃, trimethylaluminum, trimethylgallium, trimethylindium, phosphine, and silane were introduced. The composition (Al...) 0.8 Ga 0.2 ) 0.5 In 0.5 P, growth rate 0.3 nm / s, growth thickness 300 nm, doping concentration 2.0 × 10⁻⁶ 18 cm -3 .

[0044] Growth of the first quantum well active region: Maintaining 750℃, alternately introducing growth sources for the well layer and barrier layer, for a total of 3 cycles; Ga well layer 0.5 In 0.5 P growth rate 0.15 nm / s, thickness 3 nm; barrier layer (Al) 0.8 Ga 0.2 ) 0.5 In 0.5 P growth rate: 0.15 nm / s, thickness: 6 nm.

[0045] First p-type AlGaInP spacer layer growth: Maintain 750℃, introduce trimethylaluminum, trimethylgallium, trimethylindium, phosphine and magnesium pyrocene, composition (Al 0.85 Ga 0.15 ) 0.5 In 0.5P, growth rate 0.3 nm / s, growth thickness 60 nm, doping concentration 1.5 × 10⁻⁶ 18 cm -3 .

[0046] p-type AlInP electron blocking layer growth: Maintain 750℃, turn off the trimethylgallium source, and introduce trimethylaluminum, trimethylindium, phosphine, and magnesium pyrocene. Al composition... 0.5 In 0.5 P, growth rate 0.3 nm / s, growth thickness 500 nm, doping concentration 2.0 × 10⁻⁶ 18 cm -3 .

[0047] Tunnel junction growth: Maintaining a temperature of 750℃, a p-type GaAs tunnel layer was first grown by introducing trimethylgallium, arsenide, magnesia-diocene, and carbon tetrabromide. The growth rate was 0.3 nm / s, the thickness was 15 nm, and the doping concentration was 8.0 × 10⁻⁶. 18 cm -3 A new n-type GaAs tunneling layer was grown by introducing trimethylgallium, arsenide, and disilane at a growth rate of 0.3 nm / s, a thickness of 15 nm, and a doping concentration of 8.0 × 10⁻⁶. 18 cm -3 .

[0048] Growth of the second light-emitting unit: Repeat steps 5 to 8 to grow the second n-type AlGaInP confinement layer, the second quantum well active region, the second p-type AlGaInP spacer layer, and the second p-type AlInP electron blocking layer in sequence, with process parameters completely consistent with the corresponding layers of the first light-emitting unit.

[0049] p-type GaP ohmic contact layer growth: Maintain 750℃, turn off the trimethylaluminum and trimethylindium sources, and introduce trimethylgallium, phosphine, magnesia-diocene, and carbon tetrabromide. Growth rate: 0.3 nm / s, growth thickness: 200 nm, doping concentration: 4.0 × 10⁻⁶. 18 cm -3 .

[0050] Cooling annealing: After growth is complete, the reaction source is turned off, and the temperature is gradually reduced to room temperature under a hydrogen atmosphere. After in-situ annealing for 30 minutes, the epitaxial wafer is removed to obtain a complete epitaxial wafer.

[0051] II. Chip fabrication process Preparation and annealing of S1, p-type ITO transparent conductive layer: A 150 nm thick p-type ITO transparent conductive layer was deposited on the surface of the p-type GaP ohmic contact layer using electron beam evaporation. The indium-tin molar ratio of the ITO target was 9:1, and the deposition rate was 1 nm / s. After deposition, a rapid thermal annealing treatment was performed at a temperature of 400 °C for 180 s to form a good ohmic contact.

[0052] S2, Bonding and Substrate Removal: Electron beam evaporation was used to sequentially deposit 300 nm Cr / 300 nm Pt / 200 nm Au on the surface of p-type ITO to form a bonding metal layer at a deposition rate of 1 nm / s. Simultaneously, a bonding metal layer with the same structure was deposited on the front side of the Si-based CMOS driving circuit. The front side of the epitaxial wafer was aligned and bonded to the front side of the driving circuit, and metal hot-pressing fusion bonding was performed using a wafer-level bonding machine at a bonding temperature of 500℃, a bonding pressure of 4500 kg, and a bonding time of 30 min. After bonding, the GaAs substrate was removed by wet etching. The etching solution was a mixture of 10% ammonia and 10% hydrogen peroxide in a volume ratio of 4:1. The etching time was 40 minutes, and the etching stopped when the n-type AlGaInP etching barrier layer was reached. Then the n-type GaAs buffer layer was removed to expose the n-type GaAs ohmic contact layer.

[0053] S3, Micro-LED mesa fabrication: 5214 positive photoresist was spin-coated onto the exposed epitaxial surface with a thickness of 1500 nm. After pre-baking and curing, it was exposed to ultraviolet light and developed with tetramethylammonium hydroxide aqueous solution for 120 s to form a periodically arranged circular mesa mask pattern; the mesa diameter was 10 μm and the pixel pitch was 15 μm. The epitaxial layer of the patterned area is removed by inductively coupled plasma (ICP) etching process. The etching gas is a mixture of Cl2 and BCl3. The etching stops at the surface of the bonding metal layer. After etching, the remaining photoresist is removed by sequential cleaning with acetone and isopropanol to form an independent Micro-LED mesa structure.

[0054] S4, sidewall passivation and device isolation: A 50 nm thick SiO2 sidewall passivation layer was deposited on the overall surface of the sample using PECVD. The reaction gases were N2O and SiH4, with an N2O flow rate of 1200 sccm and a SiH4 flow rate of 300 sccm. The plasma source power was 100 W, the deposition temperature was 250 °C, and the deposition rate was 1 nm / s. Subsequently, an ion beam etching process was used to etch the mesa gap region, penetrating the ITO layer and the bonding metal layer to achieve electrical isolation between adjacent pixels; the etching power was 300W, the etching rate was 2nm / s, and the etching time was 600s.

[0055] S5, n-type interconnect and electrode fabrication: A 300 nm thick SiO2 mask layer was deposited using PECVD, with process parameters identical to those for the passivation layer deposition in step S4. The n-type electrode contact window was then formed via photolithography and ICP etching, exposing the n-type GaAs ohmic contact layer. The etching gases were CF4 and Ar, with a CF4 flow rate of 25 sccm, an etching time of 400 s, and an etching rate of 1.2 nm / s for SiO2. Subsequently, an n-type ITO transparent conductive layer is deposited to achieve current expansion in the n-type region; then, an electron beam evaporation process is used to deposit a 300nm Cr / 300nm Pt / 200nm Au stack, and a patterned n-type electrode is formed by an acetone immersion and stripping process to complete the chip fabrication.

[0056] Example 4 Performance testing and effect verification: Using the 10μm pixel-size Micro-LED chip prepared in Example 1 as the test sample, and a conventional single-active-area AlGaInP red Micro-LED chip of the same size as the comparative example, the results are as follows, compared under the same test conditions: Brightness and efficiency roll-off: 20A / cm 2 At the injected current density, the optical output power of this embodiment is 1.92 times that of the comparative example; the efficiency roll-off threshold current density reaches 128 A / cm². 2 This represents a 113% improvement over the control, effectively suppressing efficiency degradation under high current density.

[0057] Voltage characteristics: The operating voltage of this embodiment is 1.62V, while the operating voltage of the comparative single-junction chip is 1.42V, with a voltage increase of about 14.1%, which is far lower than the 100% increase of the traditional double PN junction series structure; the tunnel junction voltage drop is 0.2V, which meets the design expectations.

[0058] Thermal and Reliability: The thermal resistance at the bonding interface is reduced by 13.2 K / W compared to physical bonding stacking schemes, and the uniformity of internal heat distribution of the chip reaches 96.2%; 85℃ high temperature, 20A / cm 2 In constant current aging tests, the lifespan of the T50 was extended by 71% compared to the control, meeting the high reliability requirements for automotive applications.

[0059] Finally, it should be noted that the above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A monolithically integrated dual-active-region tunneling tandem AlGaInP red Micro-LED chip, characterized in that, This includes epitaxial layer structures formed by monolithic epitaxial growth; The epitaxial layer structure, from bottom to top, comprises a first n-type AlGaInP confinement layer, a first quantum well active region, a first p-type AlGaInP spacer layer, a p-type AlInP electron blocking layer, a p-type tunneling layer, an n-type tunneling layer, a second n-type AlGaInP confinement layer, a second quantum well active region, a second p-type AlGaInP spacer layer, a second p-type AlInP electron blocking layer, and a p-type GaP ohmic contact layer. The p-type tunneling layer and the n-type tunneling layer are stacked to form a tunneling junction. The tunneling junction is connected in series with the first quantum well active region and the second quantum well active region to realize carrier transport through tunneling mechanism. Both the first and second quantum well active regions employ a periodic quantum well structure with alternating stacks of GaInP well layers and (AlGa)InP barrier layers.

2. The monolithically integrated dual-active-region tunneling tandem AlGaInP red Micro-LED chip according to claim 1, characterized in that, The epitaxial layer structure further includes a GaAs substrate, an n-type GaAs buffer layer, an n-type AlGaInP etch barrier layer, and an n-type GaAs ohmic contact layer disposed below the first n-type AlGaInP confinement layer; the n-type GaAs buffer layer is grown on the surface of the GaAs substrate, and the n-type AlGaInP etch barrier layer is located between the n-type GaAs buffer layer and the n-type GaAs ohmic contact layer; the wafer size of the GaAs substrate is 2 to 12 inches, the thickness is 350 to 650 μm, and the bevel angle is 2 to 15°.

3. The monolithically integrated dual-active-region tunneling series AlGaInP red Micro-LED chip according to claim 1, characterized in that, The materials of the first n-type AlGaInP confinement layer and the second n-type AlGaInP confinement layer are (Al x1 Ga 1-x1 ) 0.5 In 0.5 P, where x1 ranges from 0.7 to 1, and the doping concentration is 1.0 × 10⁻⁶. 18 ~3.0×10 18 cm -3 The thickness of each layer is 150~500nm; both the first and second quantum well active regions contain 1~5 pairs of quantum wells, wherein the GaInP well layer thickness is 1.5~4.5nm, (Al x2 Ga 1-x2 ) 0.5 In 0.5 The thickness of the p-type barrier layer is 4~10 nm, and x2 is 0.7~0.9 nm; the materials of the first p-type AlGaInP spacer layer and the second p-type AlGaInP spacer layer are (Al x3 Ga 1-x3 ) 0.5 In 0.5 P, x3 ranges from 0.8 to 0.9, and the doping concentration is 1.0 × 10⁻⁶. 18 ~2.0×10 18 cm -3 The thickness of each is 30~100nm.

4. The monolithically integrated dual-active-region tunneling series AlGaInP red Micro-LED chip according to claim 1, characterized in that, The p-type tunneling layer and the n-type tunneling layer are made of GaAs or GaInP, and both have a doping concentration of 5.0 × 10⁻⁶. 18 ~1.0×10 19 cm -3 The thickness of each layer is 10~20nm; the operating voltage drop of the tunnel junction is 0.15~0.25V; the materials of the p-type AlInP electron blocking layer and the second p-type AlInP electron blocking layer are Al x4 In 1-x4 P, x4 is 0.5, and the doping concentration is 1.0 × 10⁴. 18 ~3.0×10 18 cm -3 The thickness of each layer is 200~900 nm; the doping concentration of the p-type GaP ohmic contact layer is 3.0 × 10⁻⁶. 18 ~5.0×10 18 cm -3 The thickness is 50~300nm.

5. A method for fabricating a monolithically integrated dual-active-region tunneling tandem AlGaInP red Micro-LED chip according to any one of claims 1 to 4, characterized in that, This includes epitaxial growth processes and chip fabrication processes; The epitaxial growth process employs MOCVD technology, using hydrogen as the carrier gas, to sequentially grow the following layers monolithically on a GaAs substrate: an n-type GaAs buffer layer, an n-type AlGaInP etch barrier layer, an n-type GaAs ohmic contact layer, a first n-type AlGaInP confinement layer, a first quantum well active region, a first p-type AlGaInP spacer layer, a p-type AlInP electron blocking layer, a p-type tunneling layer, an n-type tunneling layer, a second n-type AlGaInP confinement layer, a second quantum well active region, a second p-type AlGaInP spacer layer, a second p-type AlInP electron blocking layer, and a p-type GaP ohmic contact layer, thus obtaining an epitaxial wafer. The chip fabrication process includes, in sequence: S1, a p-type ITO transparent conductive layer is deposited by electron beam evaporation and then rapidly thermally annealed; S2, deposit a bonding metal layer on the p-type ITO transparent conductive layer, perform metal-to-metal bonding between the epitaxial wafer and the Si-based CMOS driving circuit, and then remove the GaAs substrate by wet etching. S3, spin-coating photoresist and then exposing and developing it under ultraviolet light to form a patterned mask, followed by ICP etching to form a Micro-LED mesa structure; S4 uses PECVD to deposit a SiO2 sidewall passivation layer and ion beam etching to achieve device isolation; S5. A SiO2 mask layer is deposited and patterned to expose the n-type ohmic contact layer. An n-type ITO transparent conductive layer is deposited to achieve n-type interconnection. Finally, an n-type electrode is deposited by electron beam evaporation and patterned by a lift-off process.

6. The preparation method according to claim 5, characterized in that, In the epitaxial growth process: The n-type GaAs buffer layer uses silane as the dopant source and trimethylgallium and arsenide as the growth sources. The growth temperature is 620–700 °C, the growth rate is 0.2–0.7 nm / s, and the doping concentration is 1.0 × 10⁻⁶. 18 ~3.0×10 18 cm -3 The thickness is 100~300nm; The n-type AlGaInP etch barrier layer uses silane as the dopant source and trimethylaluminum, trimethylgallium, trimethylindium, and phosphine as the growth sources. The growth temperature is 700–780 °C, the growth rate is 0.2–0.7 nm / s, and the doping concentration is 1.0 × 10⁻⁶. 18 ~3.0×10 18 cm -3 The thickness is 100~300nm; The n-type GaAs ohmic contact layer uses silane as the dopant source and trimethylgallium and arsine as the growth sources. The growth temperature is 620–700 °C, the growth rate is 0.1–0.3 nm / s, and the doping concentration is 3.0 × 10⁻⁶. 18 ~5.0×10 18 cm -3 The thickness is 10~50nm; Both the first n-type AlGaInP confinement layer and the second n-type AlGaInP confinement layer use silane as the dopant source and trimethylaluminum, trimethylgallium, trimethylindium and phosphine as the growth source, with a growth temperature of 700~780℃ and a growth rate of 0.2~0.5nm / s; Both the first and second quantum well active regions use trimethylaluminum, trimethylgallium, trimethylindium, and phosphine as growth sources, with a growth temperature of 700~780℃ and a growth rate of 0.1~0.2nm / s; both the first and second p-type AlGaInP spacer layers use magnesia-dicenocene as a doping source and trimethylaluminum, trimethylgallium, trimethylindium, and phosphine as growth sources, with a growth temperature of 700~780℃ and a growth rate of 0.2~0.5nm / s. Both the p-type AlInP electron blocking layer and the second p-type AlInP electron blocking layer use magnesia as the dopant source and trimethylaluminum, trimethylindium and phosphine as the growth source, with a growth temperature of 700~780℃ and a growth rate of 0.2~0.5nm / s. The p-type GaP ohmic contact layer uses magnesium pyrocene and carbon tetrabromide as doping sources and trimethylgallium and phosphine as growth sources. The growth temperature is 700~780℃ and the growth rate is 0.2~0.5nm / s.

7. The preparation method according to claim 5, characterized in that, In the epitaxial growth process, the p-type tunneling layer uses magnesia-3-carbide and carbon tetrabromide as doping sources; when the material is GaAs, it uses trimethylgallium and arsenide as growth sources; and when the material is GaInP, it uses trimethylgallium, trimethylindium, and phosphine as growth sources. The n-type tunneling layer uses disilane as the doping source, and the growth source corresponds to that of the p-type tunneling layer. The growth temperature of both the p-type and n-type tunneling layers is 700~780℃, the growth rate is 0.2~0.5nm / s, and the doping concentration is 5.0×10⁻⁶. 18 ~1.0×10 19 cm -3 The thickness of each is 10~20nm.

8. The preparation method according to claim 5, characterized in that, In step S1, the thickness of the p-type ITO transparent conductive layer is 150 nm, the indium-tin molar ratio of the ITO target is 9:1, the deposition rate is 1 nm / s, the rapid thermal annealing temperature is 400 °C, and the processing time is 180 s. In step S2, the bonding metal layer is a Cr / Pt / Au stacked structure, with each layer having a thickness of 300nm / 300nm / 200nm, and a deposition rate of 0.1~5nm / s. The temperature for the metal interfusion bonding is 400~700℃, the pressure is 3000~9000kg, and the bonding time is 10~60 minutes. The etching solution for removing the GaAs substrate by wet etching is a mixture of 10% ammonia and 10% hydrogen peroxide at a volume ratio of 4:1, and the etching time is 40 minutes.

9. The preparation method according to claim 5, characterized in that, In step S3, the photoresist is 5214 positive photoresist with a thickness of 500~3000nm, the developer is tetramethylammonium hydroxide aqueous solution, and the development time is 120s; the mask is a periodically arranged square or circular through-hole, corresponding to a Micro-LED mesa with a diameter of 1~50μm and a pixel pitch of 2~75μm; the etching gas for ICP etching is a mixture of Cl2 and BCl3, which is used to etch to the surface of the bonding metal layer; In step S4, the thickness of the SiO2 sidewall passivation layer is 10~100nm, the reaction gases for PECVD deposition are N2O and SiH4, the N2O flow rate is 1200sccm, the SiH4 flow rate is 300sccm, the plasma source power is 100W, the deposition temperature is 250℃, and the deposition rate is 1nm / s; the ion beam etching has an etching power of 300W, an etching rate of 2nm / s, and an etching time of 600s, etching through the ITO layer and the bonding metal layer to achieve electrical isolation of the device.

10. The preparation method according to claim 5, characterized in that, In step S5, the SiO2 mask layer has a thickness of 300 nm and is deposited using PECVD. The reaction gases are N2O and SiH4, with an N2O flow rate of 1200 sccm and a SiH4 flow rate of 300 sccm. The plasma source power is 100 W, the deposition temperature is 250 °C, and the deposition rate is 1 nm / s. The SiO2 mask layer in the patterned area is removed by ICP etching to expose the n-type GaAs ohmic contact layer. The etching gases are CF4 and Ar, with a CF4 flow rate of 25 sccm and an etching time of 400 s. The etching rate of SiO2 is 1.2 nm / s. The n-type electrode is a Cr / Pt / Au stacked structure with layer thicknesses of 300 nm / 300 nm / 200 nm, respectively. Electron beam evaporation deposition is used, with a deposition rate of 0.1~5 nm / s. The stripping process is achieved by immersion in acetone or isopropanol organic solvent.

Citation Information

Patent Citations

  • AlGaInP-base light emitting diode epitaxial wafer, AlGaInP-base light emitting diode chip and preparation method thereof

    CN106384771A

  • Tunnel junction for multi-junction LED, multi-junction LED and preparation method thereof

    CN107482091A