A polytetrafluoroethylene composite film for anti-interference shielded cables
By using a composite structure consisting of a modified polytetrafluoroethylene (PTFE) film layer, an interfacial hot melt adhesive layer, and an aluminum foil layer, the problems of poor interfacial adhesion and water vapor penetration of PTFE films are solved, achieving long-term protection and stable shielding effects in harsh environments.
Patent Information
- Application Number
- CN202611374043.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-09-07
AI Technical Summary
Existing polytetrafluoroethylene (PTFE) films have poor interfacial adhesion to metal shielding layers or other polymer sheathing materials, and are prone to delamination and peeling in high temperature and high humidity environments, resulting in a loose shielding structure and moisture penetration of the cable, which cannot meet the long-term protection requirements in harsh environments.
A composite structure consisting of a modified polytetrafluoroethylene vinyl layer, an interfacial hot melt adhesive layer, and an aluminum foil layer is adopted. By adding hydrophobic modified nano-silica to the modified polytetrafluoroethylene vinyl layer, introducing fluorotitanium-silicon copolymer modified resin into the interfacial hot melt adhesive layer, and treating the modified polytetrafluoroethylene vinyl layer with a specific infrared thermal radiation and quenching process, a low crystallinity surface is formed, which enhances the interfacial bonding force and resistance to water vapor penetration.
It improves the interlayer peel strength and interfacial bonding force, ensuring that the shielding layer is not prone to cracking under bending or thermal cycling conditions, maintaining the integrity of the shielding structure and the stability of dielectric properties, and extending the service life of the anti-interference shielded cable.
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials and cable manufacturing technology, specifically to a polytetrafluoroethylene composite film for anti-interference shielded cables. Background Technology
[0002] With the rapid development of modern communications, aerospace, rail transportation, and high-end electronics manufacturing, the electromagnetic environment in which equipment operates is becoming increasingly complex and variable. This places higher demands on the performance of anti-interference shielded cables. These cables are used to transmit high-frequency signals and power, and must simultaneously possess high signal fidelity, strong anti-electromagnetic interference capabilities, and long-term service stability in harsh environments. The cable structure typically includes a wrapping film, which is wrapped around the insulation layer and utilizes its own metal foil layer to form a shield. This film is a key component ensuring the cable's mechanical strength and shielding effectiveness.
[0003] Polytetrafluoroethylene (PTFE) is an ideal substrate for preparing high-end anti-interference shielding cable wrapping films due to its extremely low dielectric constant, excellent high and low temperature resistance, and excellent chemical stability and insulation properties. However, the highly symmetrical molecular structure of pure PTFE results in extremely low surface energy and exhibits typical chemical inertness. When used as a cable film, it is extremely difficult to form good interfacial adhesion with metal shielding layers or other polymer sheathing materials. In addition, under complex working conditions of long-term high temperature and high humidity, the micropores inside the pure PTFE film are prone to moisture penetration, which leads to fluctuations in the dielectric properties of the cable and a decrease in shielding effectiveness.
[0004] To address these issues, existing technologies typically involve laminating an adhesive material onto the substrate surface to create a composite film. However, current lamination methods suffer from significant technical drawbacks in practical processing and application. If the selected adhesive material is processed at excessively high temperatures, it can exacerbate oxidation of the aluminum foil surface and cause thermal degradation of the adhesive layer during the lamination and calendering process. Conversely, while using ordinary adhesive materials with lower processing temperatures avoids high-temperature degradation, their aging resistance is often poor, and their bonding strength with the PTFE vinyl material is weak. When the cable is under long-term service or subjected to external bending forces, delamination and peeling can easily occur within the composite film. This not only ultimately leads to a loosening of the cable's shielding structure but also allows moisture to re-penetrate through the peeling seams, failing to meet the long-term protection requirements under harsh environments. Summary of the Invention
[0005] To address the problems of poor adhesion performance, easy water vapor permeability, and excessive processing temperature of existing composite layers leading to substrate oxidation and thermal degradation of the adhesive layer, insufficient aging resistance, and easy delamination after long-term use, this invention proposes a polytetrafluoroethylene composite film for anti-interference shielded cables.
[0006] This invention provides a polytetrafluoroethylene composite film for anti-interference shielded cables, employing the following technical solution:
[0007] A polytetrafluoroethylene composite film for anti-interference shielded cables comprises a modified polytetrafluoroethylene vinyl material layer, an interface hot melt adhesive layer, and an aluminum foil layer stacked sequentially, wherein the thickness ratio of the modified polytetrafluoroethylene vinyl material layer, the interface hot melt adhesive layer, and the aluminum foil layer is (4~6):(0.5~1.5):1.
[0008] The modified polytetrafluoroethylene vinyl material layer is prepared from the following raw materials in parts by weight: 100 parts of polytetrafluoroethylene dispersion resin, 3-8 parts of surface hydrophobic modified nano silica, and 0.5-1.5 parts of heptadecafluorodecyltrimethoxysilane.
[0009] The interface hot melt adhesive layer is prepared from the following raw materials in parts by weight: 40-60 parts of tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, 30-45 parts of ethylene-vinyl acetate copolymer, 8-20 parts of fluorotitanium-silicon copolymer modified resin, 0.2-0.8 parts of composite antioxidant, and 1-3 parts of interface stabilizer.
[0010] The fluorotitanium-silicon copolymer modified resin is prepared by copolymerizing monomethylacryloyloxy polydimethylsiloxane, perfluorohexyl ethyl acrylate and γ-methacryloyloxypropyltriethoxysilane under the initiation of azobisisobutyronitrile, and further modifying it by co-hydrolysis condensation with isopropyltris(dioctylpyrophosphate)titanate.
[0011] The modified polytetrafluoroethylene vinyl material layer has a low crystallinity surface on the side near the interface hot melt adhesive layer. The crystallinity of this side surface is lower than that of the internal region of the modified polytetrafluoroethylene vinyl material layer that has not been treated with infrared thermal radiation.
[0012] Preferably, the fluorotitanium-silicon copolymer modified resin in the interfacial hot melt adhesive layer is prepared by the following steps:
[0013] S1. Under nitrogen protection, the monomethacryloxy polydimethylsiloxane is dispersed in the first anhydrous ethyl acetate, the system is heated to 60-70℃ and stirred and homogenized for 30-45 min to obtain a siloxane monomer solution.
[0014] S2. Perfluorohexyl ethyl acrylate, γ-methacryloyloxypropyltriethoxysilane and azobisisobutyronitrile are added to the second anhydrous ethyl acetate and stirred for 20-30 min to dissolve, thus obtaining a mixed monomer solution. Under stirring, the mixed monomer solution is added dropwise to the siloxane monomer solution at a uniform rate over 1-2 h. The system is then heated to 70-75 °C and stirred for another 4-6 h. The system temperature is then lowered to 60-70 °C to obtain an active intermediate solution.
[0015] S3. Under stirring, add deionized water and glacial acetic acid to the active intermediate solution to adjust the pH of the system to 4-5, and then add isopropyl tris(dioctyl pyrophosphate) titanate dropwise. After the addition is complete, continue stirring the reaction at 60-70℃ for 1-1.5h to obtain the modified resin reaction solution.
[0016] S4. After the system is cooled to 45-55℃, the modified resin reaction solution is subjected to desolventizing treatment under reduced pressure and then dried under vacuum to obtain the fluorotitanium-silicon copolymer modified resin.
[0017] Preferably, in step S1, the mass ratio of monomethacryloyloxy polydimethylsiloxane to the first anhydrous ethyl acetate is 1:(1.5~3).
[0018] Preferably, the stirring and homogenization rate in step S1 is 70-120 r / min.
[0019] Preferably, in step S2, the mass ratio of perfluorohexyl ethyl acrylate, γ-methacryloyloxypropyltriethoxysilane, azobisisobutyronitrile, and second anhydrous ethyl acetate is (2.5~4):1:(0.06~0.12):(6~10).
[0020] Preferably, the stirring and dissolving rate in step S2 is 40-80 r / min; the stirring reaction rate is 70-130 r / min.
[0021] Preferably, in step S2, the mass ratio of the mixed monomer solution to the siloxane monomer solution is (1~3):1.
[0022] Preferably, the stirring rate in step S3 is 60-80 r / min.
[0023] Preferably, in step S3, the mass ratio of deionized water, isopropyl tris(dioctylpyrophosphoryloxy)titanate, and active intermediate solution is (0.5~1.0):(2.5~4):100.
[0024] Preferably, the parameters for descaling in step S4 are: vacuum degree -0.08MPa to -0.095MPa, time 1-2h.
[0025] Preferably, the parameters for vacuum drying in step S4 are: temperature 40-55℃, time 8-12h.
[0026] Preferably, the composite antioxidant in the interface hot melt adhesive layer is a mixture of antioxidant 1010 and antioxidant 168.
[0027] Preferably, the composite antioxidant is antioxidant 1010 and antioxidant 168 in a mass ratio of 1:(1~2).
[0028] Preferably, the interface stabilizer in the interface hot melt adhesive layer is a mixture of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate and N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine.
[0029] Preferably, the interface stabilizer is 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarbamate and N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine in a mass ratio of (2~3):1.
[0030] Preferably, the polytetrafluoroethylene composite film for the anti-interference shielded cable is prepared by a method comprising the following steps:
[0031] Step 1: Weigh out polytetrafluoroethylene dispersion resin, surface hydrophobic modified nano silica, and heptadecafluorodecyltrimethoxysilane by weight. Mix the raw materials at 50-55℃ for 10-15 minutes, then cool to room temperature. Add an extrusion aid at 18-20% of the weight of the polytetrafluoroethylene dispersion resin, mix evenly, and age in a sealed container to obtain the modified polytetrafluoroethylene vinyl layer feedstock. Weigh out tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, ethylene-vinyl acetate copolymer, fluorotitanium-silicon copolymer modified resin, composite antioxidant, and interface stabilizer by weight. Mix the raw materials and homogenize for 15-25 minutes, then melt-blend and granulate using a twin-screw extruder to obtain the hot melt adhesive layer feedstock.
[0032] Step 2: The modified polytetrafluoroethylene vinyl material layer is fed through paste extrusion, calendering, heating to remove extrusion aid, and then sintering and cooling to room temperature to obtain a sintered film; one side of the sintered film is subjected to infrared thermal radiation treatment and then subjected to rapid quenching to obtain a modified polytetrafluoroethylene vinyl material layer with a lower crystallinity on the treated surface than on the interior.
[0033] Step 3: The hot melt adhesive layer is fed through a single screw extruder and a T-die to melt and extrude, and then uniformly cast and coated on the modified polytetrafluoroethylene vinyl material layer. Subsequently, an aluminum foil layer is laminated on top of it to obtain a three-layer composite preform.
[0034] Step 4: The three-layer composite prefabricated film is continuously fed into a hot rolling mill for hot pressing and bonding. After cooling, shaping, trimming and winding, a polytetrafluoroethylene composite film for anti-interference shielded cables is obtained.
[0035] Preferably, the stirring and mixing rate in step 1 is 300-600 r / min; the stirring and homogenization rate is 50-80 r / min.
[0036] Preferably, the extrusion aid is selected from aviation kerosene, dearomatized solvent oil, or isoparaffin.
[0037] Preferably, the sealed aging time in step 1 is 12-24 hours.
[0038] Preferably, in step 1, the length-to-diameter ratio (L / D) of the twin-screw extruder is 36-40:1, the screw speed is 150-250 r / min, and the temperatures of each zone are set as follows: zone 1 140-160℃, zone 2 170-190℃, zone 3 190-210℃, zone 4 210-230℃, zone 5 210-230℃, zone 6 200-220℃, and the die temperature is 190-210℃.
[0039] Preferably, in step 2, the pressing temperature is 35-55℃; the rolling temperature is 45-65℃; and the heating removal temperature is 180-220℃ for 5-15 minutes.
[0040] Preferably, the sintering temperature in step 2 is 370-390℃ and the time is 5-15min.
[0041] Preferably, the infrared thermal radiation treatment in step 2 refers to using an infrared radiation heating device to perform thermal radiation on one side of the film, controlling the thermal radiation time to be 0.4-0.6s, and controlling the heated temperature of that side surface to be 370-390℃.
[0042] Preferably, the specific operation of the rapid quenching in step 2 is as follows: the film is attached to a cold roller with cooling water at 8-10℃ at a speed of 8-12m / min.
[0043] Preferably, in step 3, the length-to-diameter ratio (L / D) of the single-screw extruder is (25~33):1, the screw speed is 20-40 r / min, and the temperatures of each zone are set as follows: feeding section 140-160℃, melting section 170-190℃, metering section 190-210℃, and T-die temperature 200-220℃.
[0044] Preferably, in step 3, the thickness of the modified polytetrafluoroethylene vinyl material layer is 32-72 μm, the thickness of the hot melt adhesive layer is 8-12 μm, and the thickness of the aluminum foil layer is 8-12 μm; and the actual values of the above three should satisfy a thickness ratio of (4~6):(0.5~1.5):1.
[0045] Preferably, the linear speed of the three-layer composite prefabricated membrane conveyed in step 4 is 15-25 m / min.
[0046] Preferably, in step 4, the temperature of the hot rolling mill is 130-150℃ and the linear pressure is 50-70 N / mm.
[0047] Preferably, in step 4, cooling and shaping refers to using a cooling roller to cool the surface of the cooling roller to a temperature of 20-30°C.
[0048] In summary, the present invention has the following beneficial effects:
[0049] 1. This invention integrates modified polytetrafluoroethylene vinyl material, hot melt adhesive layer, and aluminum foil into a single unit. The hydrophobic modified nano-silica added to the substrate fills the internal micropores, reducing water vapor permeability and ensuring stable dielectric properties. Simultaneously, by using a specific ratio of ethylene-vinyl acetate copolymer and tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer in the hot melt adhesive layer, the hot pressing temperature is reduced to a safe range, avoiding metal oxidation on the aluminum foil surface and thermal degradation of the hot melt adhesive layer caused by high temperatures. This also improves the interlayer peel strength, ensuring that the shielding layer remains continuously wrapped after cabling.
[0050] 2. This invention introduces a fluorotitanium-silicon copolymer modified resin into the hot melt adhesive. The covalent bonds formed by the co-hydrolysis condensation reaction firmly graft titanium elements onto the resin skeleton. The fluorine-containing segments in the resin molecules achieve physical wetting with the polytetrafluoroethylene vinyl material, the silicon-containing segments provide flexible buffering, and the titanium-containing segments form chemical bonds with the surface of the aluminum foil layer. This improves the interfacial bonding force from both physical and chemical dimensions, making the adhesive layer less prone to cracking under bending or thermal cycling conditions, maintaining the integrity of the shielding structure, and ensuring stable output of anti-interference performance.
[0051] 3. This invention uses an interface stabilizer composed of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate and N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine. 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate can absorb and neutralize acidic substances produced by the degradation of polymer materials, while N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine can capture free radicals and block the metal-catalyzed oxidation reaction initiated at the aluminum foil layer interface. The two work synergistically to inhibit the aging and embrittlement of the adhesive layer, enabling the composite film to maintain high interlayer adhesion and dielectric properties even after long-term service, thus extending the service life of the anti-interference shielded cable.
[0052] 4. This invention employs a specific infrared thermal radiation and rapid quenching process to treat modified polytetrafluoroethylene (PTFE) materials, resulting in a gradient distribution with low surface crystallinity and high central crystallinity. In this distribution, the central region maintains high crystallinity, thus preserving the original dense barrier properties and good dielectric properties of PTFE. The reduced surface crystallinity increases the proportion of amorphous regions, effectively improving the physical inertness of the pure PTFE surface. This provides ample space for the penetration and entanglement of polymer chains in the hot melt adhesive, significantly enhancing interlayer bonding. Detailed Implementation
[0053] The present invention will be further described in detail below with reference to the embodiments.
[0054] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0055] The key raw materials used in this invention are sourced from the following sources:
[0056] Polytetrafluoroethylene dispersion resin: model F-104, average particle size 500μm, brand Daikin Japan, purchased from Ningbo Rongsu New Materials Co., Ltd.
[0057] Surface-hydrophobically modified nano-silica: specific surface area of 130 m² 2 / g, brand name AEROSIL®R972, brand name Evonik Germany, purchased from Guangzhou Libby New Materials Technology Co., Ltd.;
[0058] Heptadecyltrimethoxysilane: CAS No. 83048-65-1, purchased from Hangzhou Jessica Chemical Co., Ltd.;
[0059] Tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer: Model THV 221, brand 3M (USA), melt index of 20g / 10min and melting point of 120℃ at 265℃ and 5.0 kg, purchased from Shenzhen Zhengfangyuan Plastics Import & Export Co., Ltd.
[0060] Ethylene-vinyl acetate copolymer: grade EA28025, brand LG Chem (Korea), melt index of 25 g / 10 min at 190℃ and 2.16 kg, vinyl acetate (VA) mass fraction of 28%, purchased from Suzhou Lutuo Materials Co., Ltd.
[0061] Monomethacryloyloxy polydimethylsiloxane: CAS No. 58130-03-3, average molecular weight 1500 g / mol, purchased from Hengyu Wuxi Technology Co., Ltd.
[0062] Perfluorohexyl ethyl acrylate: CAS No. 17527-29-6, purchased from Hubei Xingyan New Material Technology Co., Ltd.;
[0063] γ-Methacryloxypropyltriethoxysilane: CAS No. 21142-29-0, purchased from Hubei Xingyan New Material Technology Co., Ltd.;
[0064] Azobisisobutyronitrile: CAS No. 78-67-1, purchased from Shandong Feihong New Materials Co., Ltd.;
[0065] Isopropyl tris(dioctylpyrophosphoryloxy)titanate: CAS No. 67691-13-8, purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.;
[0066] Antioxidant 1010: CAS No. 6683-19-8, purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd.;
[0067] Antioxidant 168: CAS No. 31570-04-4, purchased from Nanjing Milan New Materials Co., Ltd.;
[0068] 3,4-Epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate: CAS No. 2386-87-0, purchased from Hubei Yongkuo Technology Co., Ltd.;
[0069] N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine: CAS No. 32687-78-8, purchased from Hubei Weistin Technology Co., Ltd.;
[0070] Aluminum foil: Commercially available soft aluminum foil, alloy grade 1235-O, purchased from Henan Mingtai Aluminum Co., Ltd.
[0071] Neoalkoxytris(dioctylpyrophosphoryloxy)zirconia ester: CAS No. 103455-10-3, purchased from Wuhan Lingfan Technology Co., Ltd.
[0072] Preparation Examples 1-3 and Comparative Preparation Examples 1-2 provide a method for preparing a fluorotitanium-silicon copolymer modified resin.
[0073] Preparation Example 1
[0074] The fluorotitanium-silicon copolymer modified resin is prepared by the following steps:
[0075] S1. Under nitrogen protection, the monomethacryloxy polydimethylsiloxane was dispersed in 1.5 times its own mass of anhydrous ethyl acetate, the system was heated to 60°C, and stirred and homogenized at a rate of 70 r / min for 45 min to obtain a siloxane monomer solution.
[0076] S2. The mass ratio of perfluorohexyl ethyl acrylate, γ-methacryloxypropyltriethoxysilane, azobisisobutyronitrile, and second anhydrous ethyl acetate was controlled at 2.5:1:0.06:6. Perfluorohexyl ethyl acrylate, γ-methacryloxypropyltriethoxysilane, and azobisisobutyronitrile were added to the second anhydrous ethyl acetate and stirred at 40 r / min for 30 min to dissolve, obtaining a mixed monomer solution. The mass ratio of the mixed monomer solution to the siloxane monomer solution was controlled at 1:1. The mixed monomer solution was added dropwise to the siloxane monomer solution at a stirring rate of 70 r / min over 2 h. The system was then heated to 70 °C and stirred for another 6 h. The system temperature was then lowered to 60 °C to obtain an active intermediate solution.
[0077] S3. Control the mass ratio of deionized water, isopropyl tris(dioctyl pyrophosphoryloxy) titanate to active intermediate solution to 0.5:2.5:100. Under a stirring rate of 60 r / min, add deionized water and glacial acetic acid to active intermediate solution to adjust the pH of the system to 4. Then add isopropyl tris(dioctyl pyrophosphoryloxy) titanate dropwise. After the dropwise addition is complete, continue stirring the reaction at 60℃ for 1.5 h to obtain modified resin reaction solution.
[0078] S4. After the system cools to 45°C, the modified resin reaction solution is subjected to reduced pressure solvent removal treatment at -0.08MPa for 2 hours, and then baked in a vacuum drying oven at 40°C for 12 hours to obtain fluorotitanium silicon copolymer modified resin.
[0079] Preparation Example 2
[0080] The fluorotitanium-silicon copolymer modified resin is prepared by the following steps:
[0081] S1. Under nitrogen protection, the monomethacryloxy polydimethylsiloxane was dispersed in 2.2 times its own mass of anhydrous ethyl acetate, the system was heated to 65°C, and stirred at 90 r / min for 38 min to obtain a siloxane monomer solution.
[0082] S2. The mass ratio of perfluorohexyl ethyl acrylate, γ-methacryloxypropyltriethoxysilane, azobisisobutyronitrile, and second anhydrous ethyl acetate was controlled at 3.2:1:0.09:8. Perfluorohexyl ethyl acrylate, γ-methacryloxypropyltriethoxysilane, and azobisisobutyronitrile were added to the second anhydrous ethyl acetate and stirred at 60 r / min for 25 min to dissolve, obtaining a mixed monomer solution. The mass ratio of the mixed monomer solution to the siloxane monomer solution was controlled at 2:1. The mixed monomer solution was added dropwise to the siloxane monomer solution at a stirring rate of 93 r / min over 1.5 h. The system was then heated to 72 °C and stirred for another 5 h. The system temperature was then lowered to 65 °C to obtain the active intermediate solution.
[0083] S3. Controlling the mass ratio of deionized water, isopropyl tris(dioctyl pyrophosphoryl oxy) titanate to active intermediate solution to 0.8:3.2:100, deionized water and glacial acetic acid were added to the active intermediate solution at a stirring rate of 70 r / min to adjust the pH of the system to 4.5. Then, isopropyl tris(dioctyl pyrophosphoryl oxy) titanate was added dropwise. After the addition was completed, the reaction was continued to be stirred at 65℃ for 1.2 h to obtain modified resin reaction solution.
[0084] S4. After the system cools to 50°C, the modified resin reaction solution is subjected to reduced pressure solvent removal treatment at -0.088MPa for 1.5 hours, and then baked in a vacuum drying oven at 47°C for 10 hours to obtain fluorotitanium-silicon copolymer modified resin.
[0085] Preparation Example 3
[0086] The fluorotitanium-silicon copolymer modified resin is prepared by the following steps:
[0087] S1. Under nitrogen protection, the monomethacryloxy polydimethylsiloxane was dispersed in three times its own weight of anhydrous ethyl acetate, the system was heated to 70°C, and stirred and homogenized at a rate of 120 r / min for 30 min to obtain a siloxane monomer solution.
[0088] S2. The mass ratio of perfluorohexyl ethyl acrylate, γ-methacryloxypropyltriethoxysilane, azobisisobutyronitrile, and second anhydrous ethyl acetate was controlled at 4:1:0.12:10. Perfluorohexyl ethyl acrylate, γ-methacryloxypropyltriethoxysilane, and azobisisobutyronitrile were added to the second anhydrous ethyl acetate and stirred at 80 r / min for 20 min to dissolve, obtaining a mixed monomer solution. The mass ratio of the mixed monomer solution to the siloxane monomer solution was controlled at 3:1. The mixed monomer solution was uniformly added dropwise to the siloxane monomer solution over 1 h at a stirring rate of 130 r / min. The system was then heated to 75 °C and stirred for 4 h. The system temperature was then lowered to 70 °C to obtain an active intermediate solution.
[0089] S3. Control the mass ratio of deionized water, isopropyl tris(dioctyl pyrophosphoryloxy) titanate to active intermediate solution to 1.0:4:100. Under a stirring rate of 80 r / min, add deionized water and glacial acetic acid to active intermediate solution to adjust the pH of the system to 5. Then add isopropyl tris(dioctyl pyrophosphoryloxy) titanate dropwise. After the dropwise addition is complete, continue stirring the reaction at 70℃ for 1 h to obtain modified resin reaction solution.
[0090] S4. After the system cools to 55°C, the modified resin reaction solution is subjected to reduced pressure solvent removal treatment at -0.095MPa for 1 hour, and then baked in a vacuum drying oven at 55°C for 8 hours to obtain fluorotitanium-silicon copolymer modified resin.
[0091] Comparative Preparation Example 1
[0092] The fluorine-free titanium-silicon copolymer modified resin is prepared by the following steps:
[0093] S1. Under nitrogen protection, the monomethacryloxy polydimethylsiloxane was dispersed in 1.5 times its own mass of anhydrous ethyl acetate, the system was heated to 60°C, and stirred and homogenized at a rate of 70 r / min for 45 min to obtain a siloxane monomer solution.
[0094] S2. The mass ratio of γ-methacryloxypropyltriethoxysilane, azobisisobutyronitrile, and second anhydrous ethyl acetate was controlled at 1:0.06:6. γ-methacryloxypropyltriethoxysilane and azobisisobutyronitrile were added to the second anhydrous ethyl acetate and stirred at 40 r / min for 30 min to dissolve, obtaining a mixed monomer solution. The mass ratio of the mixed monomer solution to the siloxane monomer solution was controlled at 1:1. The mixed monomer solution was uniformly added dropwise to the siloxane monomer solution over 2 h at a stirring rate of 70 r / min. The system was then heated to 70 °C and stirred for another 6 h. The system temperature was then lowered to 60 °C to obtain the active intermediate solution.
[0095] S3. Control the mass ratio of deionized water, isopropyl tris(dioctyl pyrophosphoryloxy) titanate to active intermediate solution to 0.5:2.5:100. Under a stirring rate of 60 r / min, add deionized water and glacial acetic acid to active intermediate solution to adjust the pH of the system to 4. Then add isopropyl tris(dioctyl pyrophosphoryloxy) titanate dropwise. After the dropwise addition is complete, continue stirring the reaction at 60℃ for 1.5 h to obtain modified resin reaction solution.
[0096] S4. After the system cools to 45°C, the modified resin reaction solution is subjected to reduced pressure solvent removal treatment at -0.08MPa for 2 hours, and then baked in a vacuum drying oven at 40°C for 12 hours to obtain fluorine-free chain titanium-silicon copolymer modified resin.
[0097] Comparative Preparation Example 2
[0098] The non-flexible chain fluorotitanium-silicon copolymer modified resin is prepared by the following steps:
[0099] S1. Under nitrogen protection, methyl methacrylate was dispersed in 1.5 times its own weight of anhydrous ethyl acetate, the system was heated to 60°C, and stirred and homogenized at a rate of 70 r / min for 45 min to obtain the basic monomer solution.
[0100] S2. The mass ratio of perfluorohexyl ethyl acrylate, γ-methacryloxypropyltriethoxysilane, azobisisobutyronitrile, and second anhydrous ethyl acetate was controlled at 2.5:1:0.06:6. Perfluorohexyl ethyl acrylate, γ-methacryloxypropyltriethoxysilane, and azobisisobutyronitrile were added to the second anhydrous ethyl acetate and stirred at 40 r / min for 30 min to dissolve, obtaining a mixed monomer solution. The mass ratio of the mixed monomer solution to the basic monomer solution was controlled at 1:1. The mixed monomer solution was uniformly added dropwise to the basic monomer solution over 2 h at a stirring rate of 70 r / min. The system was then heated to 70 °C and stirred for another 6 h. The system temperature was then lowered to 60 °C to obtain the active intermediate solution.
[0101] S3. Control the mass ratio of deionized water, isopropyl tris(dioctyl pyrophosphoryloxy) titanate to active intermediate solution to 0.5:2.5:100. Under a stirring rate of 60 r / min, add deionized water and glacial acetic acid to active intermediate solution to adjust the pH of the system to 4. Then add isopropyl tris(dioctyl pyrophosphoryloxy) titanate dropwise. After the dropwise addition is complete, continue stirring the reaction at 60℃ for 1.5 h to obtain modified resin reaction solution.
[0102] S4. After the system cools to 45°C, the modified resin reaction solution is subjected to reduced pressure solvent removal treatment at -0.08MPa for 2 hours, and then placed in a vacuum drying oven at 40°C for 12 hours to obtain a non-flexible chain fluorotitanium silicon copolymer modified resin.
[0103] Comparative preparation example 3
[0104] The zirconium-substituted fluorosilicone copolymer modified resin is prepared by the following steps:
[0105] S1. Under nitrogen protection, the monomethacryloxy polydimethylsiloxane was dispersed in 1.5 times its own mass of anhydrous ethyl acetate, the system was heated to 60°C, and stirred and homogenized at a rate of 70 r / min for 45 min to obtain a siloxane monomer solution.
[0106] S2. The mass ratio of perfluorohexyl ethyl acrylate, γ-methacryloxypropyltriethoxysilane, azobisisobutyronitrile, and second anhydrous ethyl acetate was controlled at 2.5:1:0.06:6. Perfluorohexyl ethyl acrylate, γ-methacryloxypropyltriethoxysilane, and azobisisobutyronitrile were added to the second anhydrous ethyl acetate and stirred at 40 r / min for 30 min to dissolve, obtaining a mixed monomer solution. The mass ratio of the mixed monomer solution to the siloxane monomer solution was controlled at 1:1. The mixed monomer solution was added dropwise to the siloxane monomer solution at a stirring rate of 70 r / min over 2 h. The system was then heated to 70 °C and stirred for another 6 h. The system temperature was then lowered to 60 °C to obtain an active intermediate solution.
[0107] S3. Control the mass ratio of deionized water, neoalkoxytris(dioctylpyrophosphoryloxy)zirconia ester, and active intermediate solution to 0.5:2.5:100. Under a stirring rate of 60 r / min, add deionized water and glacial acetic acid to the active intermediate solution to adjust the pH of the system to 4. Then add neoalkoxytris(dioctylpyrophosphoryloxy)zirconia ester dropwise. After the addition is complete, continue stirring the reaction at 60℃ for 1.5 h to obtain the modified resin reaction solution.
[0108] S4. After the system cools to 45°C, the modified resin reaction solution is subjected to reduced pressure solvent removal treatment at -0.08MPa for 2 hours, and then baked in a vacuum drying oven at 40°C for 12 hours to obtain zirconium-substituted fluorosilicone copolymer modified resin.
[0109] Example 1
[0110] A polytetrafluoroethylene composite film for anti-interference shielded cables comprises a modified polytetrafluoroethylene vinyl material layer, an interface hot melt adhesive layer, and an aluminum foil layer stacked sequentially. The formulations and preparation methods of each layer are as follows:
[0111] Step 1: Preparation of modified polytetrafluoroethylene vinyl layer feedstock: Weigh 100 parts of polytetrafluoroethylene dispersion resin, 3 parts of surface hydrophobic modified nano silica, and 0.5 parts of heptadecafluorodecyltrimethoxysilane. Mix the raw materials at 50°C and 300 r / min for 15 min. After cooling to room temperature, add No. 3 aviation kerosene, which is 18% of the weight of polytetrafluoroethylene dispersion resin. Mix evenly and age in a sealed container for 12 h to obtain the modified polytetrafluoroethylene vinyl layer feedstock.
[0112] Preparation of interfacial hot melt adhesive layer feed: Weigh 40 parts of tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, 30 parts of ethylene-vinyl acetate copolymer, 8 parts of the fluorotitanium-silicon copolymer modified resin obtained in Preparation Example 1, 0.2 parts of composite antioxidant (including antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1), and 1 part of interfacial stabilizer (including 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate and N,N'-bis[3-(3,5- [di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine] The raw materials were stirred and homogenized at a rate of 50 r / min for 25 min, and then added to a twin-screw extruder (length to diameter ratio L / D of 36:1). The screw speed was 150 r / min, and the temperatures of each zone were set as follows: zone 1 140℃, zone 2 170℃, zone 3 190℃, zone 4 210℃, zone 5 210℃, zone 6 200℃, and the die temperature was 190℃. After melt blending and granulation in the twin-screw extruder, the hot melt adhesive layer feed was obtained.
[0113] Step 2: The modified polytetrafluoroethylene vinyl material layer is fed into the feed at 35°C and pressed with paste. Then it is calendered at a roller temperature of 45°C, heated at 180°C for 15 minutes to remove aviation kerosene, and then sintered at 370°C for 15 minutes. After cooling to room temperature, a sintered film is obtained. An infrared radiation heating device is used to subject one side of the sintered film to instantaneous heat radiation for 0.4 seconds, so that the surface temperature of that side reaches 370°C. Then it is attached to a cold roller with cooling water at 8 m / min for rapid quenching, resulting in a modified polytetrafluoroethylene vinyl material layer with a lower crystallinity on the treated surface than the interior.
[0114] Step 3: Feed the hot melt adhesive layer into a single screw extruder (L / D ratio of 25:1), with a screw speed of 20 r / min. The temperature of each zone is set as follows: feeding section 140℃, melting section 170℃, metering section 190℃, and T-die temperature 200℃. The material is melt-extruded through the T-die and uniformly cast onto a 32μm thick modified polytetrafluoroethylene vinyl material layer. The coating thickness is controlled to be 12μm. Then, an 8μm thick aluminum foil layer is laminated on top to obtain a three-layer composite preform.
[0115] Step 4: The three-layer composite preform is continuously fed to a hot rolling mill at 130°C and 50 N / mm at a linear speed of 15 m / min for hot pressing and bonding. Then it is cooled and shaped by a cooling roller at 20°C, trimmed, and wound up to obtain a polytetrafluoroethylene composite film for anti-interference shielding cables.
[0116] Example 2
[0117] A polytetrafluoroethylene composite film for anti-interference shielded cables comprises a modified polytetrafluoroethylene vinyl material layer, an interface hot melt adhesive layer, and an aluminum foil layer stacked sequentially. The formulations and preparation methods of each layer are as follows:
[0118] Step 1: Preparation of modified polytetrafluoroethylene vinyl layer feedstock: Weigh 100 parts of polytetrafluoroethylene dispersion resin, 6 parts of surface hydrophobic modified nano silica, and 1 part of heptadecafluorodecyltrimethoxysilane. Mix the raw materials at 53°C and 450 r / min for 12 min, then cool to room temperature. Add No. 3 aviation kerosene, which is 19% of the weight of polytetrafluoroethylene dispersion resin. Mix evenly and age in a sealed container for 18 h to obtain the modified polytetrafluoroethylene vinyl layer feedstock.
[0119] Preparation of the interfacial hot melt adhesive layer: Weigh 50 parts of tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, 38 parts of ethylene-vinyl acetate copolymer, 14 parts of the fluorotitanium-silicon copolymer modified resin obtained in Preparation Example 2, 0.6 parts of composite antioxidant (including antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.5), and 2 parts of interfacial stabilizer (including 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate and N,N'-bis[3-(3, [5-Di-tert-butyl-4-hydroxyphenyl)propionylhydrazine] The raw materials were stirred and homogenized at a rate of 68 r / min for 20 min, and then added to a twin-screw extruder (L / D ratio of 38:1). The screw speed was 200 r / min, and the temperatures of each zone were set as follows: Zone 1 150℃, Zone 2 180℃, Zone 3 200℃, Zone 4 220℃, Zone 5 220℃, Zone 6 210℃, and the die temperature was 200℃. The mixture was melt-blended and granulated in the twin-screw extruder to obtain the hot melt adhesive layer feed.
[0120] Step 2: The modified polytetrafluoroethylene vinyl material layer is fed into the feed at 35°C and pressed with paste. Then it is calendered at a roller temperature of 45°C, heated at 180°C for 15 minutes to remove aviation kerosene, and then sintered at 380°C for 10 minutes. After cooling to room temperature, a sintered film is obtained. An infrared radiation heating device is used to subject one side of the sintered film to instantaneous heat radiation for 0.5 seconds, so that the surface temperature of that side reaches 380°C. Then it is attached to a cold roller with 9°C cooling water at a speed of 10 m / min for rapid quenching, resulting in a modified polytetrafluoroethylene vinyl material layer with a lower crystallinity on the treated surface than the interior.
[0121] Step 3: Feed the hot melt adhesive layer into a single screw extruder (L / D ratio of 28:1), with a screw speed of 30 r / min. The temperature of each zone is set as follows: feeding zone 150℃, melting zone 180℃, metering zone 200℃, and T-die temperature 210℃. The material is melt-extruded through the T-die and uniformly cast onto a 50 μm thick modified polytetrafluoroethylene vinyl material layer. The coating thickness is controlled to be 10 μm. Then, a 10 μm thick aluminum foil layer is laminated on top to obtain a three-layer composite preform.
[0122] Step 4: The three-layer composite preform is continuously fed to a hot rolling mill at 140℃ and 60N / mm at a linear speed of 20m / min for hot pressing and bonding. Then it is cooled and shaped by a cooling roller at 25℃, trimmed and wound up to obtain a polytetrafluoroethylene composite film for anti-interference shielding cables.
[0123] Example 3
[0124] A polytetrafluoroethylene composite film for anti-interference shielded cables comprises a modified polytetrafluoroethylene vinyl material layer, an interface hot melt adhesive layer, and an aluminum foil layer stacked sequentially. The formulations and preparation methods of each layer are as follows:
[0125] Step 1: Preparation of modified polytetrafluoroethylene vinyl layer feedstock: Weigh 100 parts of polytetrafluoroethylene dispersion resin, 8 parts of surface hydrophobic modified nano silica, and 1.5 parts of heptadecafluorodecyltrimethoxysilane. Mix the raw materials at 55°C and 600 r / min for 10 min, then cool to room temperature. Add No. 3 aviation kerosene, which is 20% of the weight of polytetrafluoroethylene dispersion resin. Mix evenly and age in a sealed container for 24 h to obtain the modified polytetrafluoroethylene vinyl layer feedstock.
[0126] Preparation of interfacial hot melt adhesive layer feed: Weigh 60 parts of tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, 45 parts of ethylene-vinyl acetate copolymer, 20 parts of the fluorotitanium-silicon copolymer modified resin obtained in Preparation Example 3, 0.8 parts of composite antioxidant (including antioxidant 1010 and antioxidant 168 in a mass ratio of 1:2), and 3 parts of interfacial stabilizer (including 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate and N,N'-bis[3-(3,5- (di-tert-butyl-4-hydroxyphenyl)propionylhydrazine) All raw materials were stirred and homogenized at a rate of 80 r / min for 15 min, and then added to a twin-screw extruder (length-to-diameter ratio L / D of 40:1). The screw speed was 250 r / min, and the temperatures of each zone were set as follows: zone 1 160℃, zone 2 190℃, zone 3 210℃, zone 4 230℃, zone 5 230℃, zone 6 220℃, and the die temperature was 210℃. The mixture was melt-blended and granulated in the twin-screw extruder to obtain the hot melt adhesive layer feed.
[0127] Step 2: The modified polytetrafluoroethylene vinyl material layer is fed into the feed at 55°C and pressed with paste. Then it is calendered at a roller temperature of 65°C, heated at 220°C for 5 minutes to remove aviation kerosene, and then sintered at 390°C for 5 minutes. After cooling to room temperature, a sintered film is obtained. An infrared radiation heating device is used to subject one side of the sintered film to instantaneous thermal radiation for 0.6 seconds, and the surface temperature of that side reaches 390°C. Then it is attached to a cold roller with 10°C cooling water at a speed of 12 m / min for rapid quenching, resulting in a modified polytetrafluoroethylene vinyl material layer with a lower crystallinity on the treated surface than the interior.
[0128] Step 3: Feed the hot melt adhesive layer into a single screw extruder (L / D ratio of 33:1), with a screw speed of 40 r / min. The zones are set as follows: feeding section 160°C, melting section 190°C, metering section 210°C, and T-die temperature 220°C. The material is melt-extruded through the T-die and uniformly cast onto a 72 μm thick modified polytetrafluoroethylene vinyl material layer. The coating thickness is controlled to be 9 μm. Then, a 12 μm thick aluminum foil layer is laminated on top to obtain a three-layer composite preform.
[0129] Step 4: The three-layer composite preform is continuously fed to a hot rolling mill at 150°C and 70 N / mm at a linear speed of 25 m / min for hot pressing and bonding. Then, it is cooled and shaped by a cooling roller at 30°C, trimmed, and wound up to obtain a polytetrafluoroethylene composite film for anti-interference shielding cables.
[0130] To verify the comprehensive performance of the polytetrafluoroethylene composite film for anti-interference shielded cables provided by the present invention, comparative examples 1-5 were set up, wherein:
[0131] Comparative Example 1
[0132] Comparative Example 1 is the same as Example 1, except that the fluorotitanium-silicon copolymer modified resin prepared in Preparation Example 1 is replaced with the fluorine-free titanium-silicon copolymer modified resin prepared in Comparative Preparation Example 1. Specifically:
[0133] A polytetrafluoroethylene composite film for anti-interference shielded cables comprises a modified polytetrafluoroethylene vinyl material layer, an interface hot melt adhesive layer, and an aluminum foil layer stacked sequentially. The formulations and preparation methods of each layer are as follows:
[0134] Step 1: Preparation of modified polytetrafluoroethylene vinyl layer feedstock: Weigh 100 parts of polytetrafluoroethylene dispersion resin, 3 parts of surface hydrophobic modified nano silica, and 0.5 parts of heptadecafluorodecyltrimethoxysilane. Mix the raw materials at 50°C and 300 r / min for 15 min. After cooling to room temperature, add No. 3 aviation kerosene, which is 18% of the weight of polytetrafluoroethylene dispersion resin. Mix evenly and age in a sealed container for 12 h to obtain the modified polytetrafluoroethylene vinyl layer feedstock.
[0135] Preparation of interfacial hot melt adhesive layer feed: Weigh 40 parts of tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, 30 parts of ethylene-vinyl acetate copolymer, 8 parts of the fluorine-free chain titanium-silicon copolymer modified resin prepared in Comparative Preparation Example 1, 0.2 parts of composite antioxidant (including antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1), and 1 part of interfacial stabilizer (including 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate and N,N'-bis[3-(3, [5-Di-tert-butyl-4-hydroxyphenyl)propionylhydrazine] The raw materials were stirred and homogenized at a rate of 50 r / min for 25 min, and then added to a twin-screw extruder (L / D ratio of 36:1). The screw speed was 150 r / min, and the temperatures of each zone were set as follows: Zone 1 140℃, Zone 2 170℃, Zone 3 190℃, Zone 4 210℃, Zone 5 210℃, Zone 6 200℃, and the die temperature was 190℃. The mixture was melt-blended and granulated by the twin-screw extruder to obtain the hot melt adhesive layer feed.
[0136] Step 2: The modified polytetrafluoroethylene vinyl material layer is fed into the feed at 35°C and pressed with paste. Then it is calendered at a roller temperature of 45°C, heated at 180°C for 15 minutes to remove aviation kerosene, and then sintered at 370°C for 15 minutes. After cooling to room temperature, a sintered film is obtained. An infrared radiation heating device is used to subject one side of the sintered film to instantaneous heat radiation for 0.4 seconds, so that the surface temperature of that side reaches 370°C. Then it is attached to a cold roller with cooling water at 8 m / min for rapid quenching, resulting in a modified polytetrafluoroethylene vinyl material layer with a lower crystallinity on the treated surface than the interior.
[0137] Step 3: Feed the hot melt adhesive layer into a single screw extruder (L / D ratio of 25:1), with a screw speed of 20 r / min. The temperature of each zone is set as follows: feeding section 140℃, melting section 170℃, metering section 190℃, and T-die temperature 200℃. The material is melt-extruded through the T-die and uniformly cast onto a 32μm thick modified polytetrafluoroethylene vinyl material layer. The coating thickness is controlled to be 12μm. Then, an 8μm thick aluminum foil layer is laminated on top to obtain a three-layer composite preform.
[0138] Step 4: The three-layer composite preform is continuously fed to a hot rolling mill at 130°C and 50 N / mm at a linear speed of 15 m / min for hot pressing and bonding. Then it is cooled and shaped by a cooling roller at 20°C, trimmed, and wound up to obtain a polytetrafluoroethylene composite film for anti-interference shielding cables.
[0139] Comparative Example 2
[0140] Comparative Example 2 is the same as Example 1, except that the fluorotitanium-silicon copolymer modified resin prepared in Preparation Example 1 is replaced with the non-flexible chain fluorotitanium-silicon copolymer modified resin prepared in Comparative Preparation Example 2. Specifically:
[0141] A polytetrafluoroethylene composite film for anti-interference shielded cables comprises a modified polytetrafluoroethylene vinyl material layer, an interface hot melt adhesive layer, and an aluminum foil layer stacked sequentially. The formulations and preparation methods of each layer are as follows:
[0142] Step 1: Preparation of modified polytetrafluoroethylene vinyl layer feedstock: Weigh 100 parts of polytetrafluoroethylene dispersion resin, 3 parts of surface hydrophobic modified nano silica, and 0.5 parts of heptadecafluorodecyltrimethoxysilane. Mix the raw materials at 50°C and 300 r / min for 15 min. After cooling to room temperature, add No. 3 aviation kerosene, which is 18% of the weight of polytetrafluoroethylene dispersion resin. Mix evenly and age in a sealed container for 12 h to obtain the modified polytetrafluoroethylene vinyl layer feedstock.
[0143] Preparation of the interfacial hot melt adhesive layer: Weigh 40 parts of tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, 30 parts of ethylene-vinyl acetate copolymer, 8 parts of the non-flexible chain fluorotitanium-silicon copolymer modified resin obtained in Comparative Preparation Example 2, 0.2 parts of composite antioxidant (including antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1), and 1 part of interfacial stabilizer (including 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate and N,N'-bis[3-(3, [5-Di-tert-butyl-4-hydroxyphenyl)propionylhydrazine] The raw materials were stirred and homogenized at a rate of 50 r / min for 25 min, and then added to a twin-screw extruder (L / D ratio of 36:1). The screw speed was 150 r / min, and the temperatures of each zone were set as follows: Zone 1 140℃, Zone 2 170℃, Zone 3 190℃, Zone 4 210℃, Zone 5 210℃, Zone 6 200℃, and the die temperature was 190℃. The mixture was melt-blended and granulated by the twin-screw extruder to obtain the hot melt adhesive layer feed.
[0144] Step 2: The modified polytetrafluoroethylene vinyl material layer is fed into the feed at 35°C and pressed with paste. Then it is calendered at a roller temperature of 45°C, heated at 180°C for 15 minutes to remove aviation kerosene, and then sintered at 370°C for 15 minutes. After cooling to room temperature, a sintered film is obtained. An infrared radiation heating device is used to subject one side of the sintered film to instantaneous heat radiation for 0.4 seconds, so that the surface temperature of that side reaches 370°C. Then it is attached to a cold roller with cooling water at 8 m / min for rapid quenching, resulting in a modified polytetrafluoroethylene vinyl material layer with a lower crystallinity on the treated surface than the interior.
[0145] Step 3: Feed the hot melt adhesive layer into a single screw extruder (L / D ratio of 25:1), with a screw speed of 20 r / min. The temperature of each zone is set as follows: feeding section 140℃, melting section 170℃, metering section 190℃, and T-die temperature 200℃. The material is melt-extruded through the T-die and uniformly cast onto a 32μm thick modified polytetrafluoroethylene vinyl material layer. The coating thickness is controlled to be 12μm. Then, an 8μm thick aluminum foil layer is laminated on top to obtain a three-layer composite preform.
[0146] Step 4: The three-layer composite preform is continuously fed to a hot rolling mill at 130°C and 50 N / mm at a linear speed of 15 m / min for hot pressing and bonding. Then it is cooled and shaped by a cooling roller at 20°C, trimmed, and wound up to obtain a polytetrafluoroethylene composite film for anti-interference shielding cables.
[0147] Comparative Example 3
[0148] Comparative Example 3 is the same as Example 1, except that the fluorotitanium-silicon copolymer modified resin prepared in Preparation Example 1 is replaced with the zirconium-substituted fluorosilicon copolymer modified resin prepared in Comparative Preparation Example 3. Specifically:
[0149] A polytetrafluoroethylene composite film for anti-interference shielded cables comprises a modified polytetrafluoroethylene vinyl material layer, an interface hot melt adhesive layer, and an aluminum foil layer stacked sequentially. The formulations and preparation methods of each layer are as follows:
[0150] Step 1: Preparation of modified polytetrafluoroethylene vinyl layer feedstock: Weigh 100 parts of polytetrafluoroethylene dispersion resin, 3 parts of surface hydrophobic modified nano silica, and 0.5 parts of heptadecafluorodecyltrimethoxysilane. Mix the raw materials at 50°C and 300 r / min for 15 min. After cooling to room temperature, add No. 3 aviation kerosene, which is 18% of the weight of polytetrafluoroethylene dispersion resin. Mix evenly and age in a sealed container for 12 h to obtain the modified polytetrafluoroethylene vinyl layer feedstock.
[0151] Preparation of interfacial hot melt adhesive layer feed: Weigh 40 parts of tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, 30 parts of ethylene-vinyl acetate copolymer, 8 parts of zirconium-fluorinated silicone copolymer modified resin prepared in Comparative Preparation Example 3, 0.2 parts of composite antioxidant (including antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1), and 1 part of interfacial stabilizer (including 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate and N,N'-bis[3-(3,5-)-carboxylate in a mass ratio of 2:1). (-di-tert-butyl-4-hydroxyphenyl)propionylhydrazine) After the raw materials are stirred and homogenized at a rate of 50 r / min for 25 min, they are added to a twin-screw extruder (length-to-diameter ratio L / D is 36:1). The screw speed is 150 r / min, and the temperatures of each zone are set as follows: zone 1 140℃, zone 2 170℃, zone 3 190℃, zone 4 210℃, zone 5 210℃, zone 6 200℃, and the die temperature is 190℃. The hot melt adhesive layer feed is obtained by melt blending and granulation in the twin-screw extruder.
[0152] Step 2: The modified polytetrafluoroethylene vinyl material layer is fed into the feed at 35°C and pressed with paste. Then it is calendered at a roller temperature of 45°C, heated at 180°C for 15 minutes to remove aviation kerosene, and then sintered at 370°C for 15 minutes. After cooling to room temperature, a sintered film is obtained. An infrared radiation heating device is used to subject one side of the sintered film to instantaneous heat radiation for 0.4 seconds, so that the surface temperature of that side reaches 370°C. Then it is attached to a cold roller with cooling water at 8 m / min for rapid quenching, resulting in a modified polytetrafluoroethylene vinyl material layer with a lower crystallinity on the treated surface than the interior.
[0153] Step 3: Feed the hot melt adhesive layer into a single screw extruder (L / D ratio of 25:1), with a screw speed of 20 r / min. The temperature of each zone is set as follows: feeding section 140℃, melting section 170℃, metering section 190℃, and T-die temperature 200℃. The material is melt-extruded through the T-die and uniformly cast onto a 32μm thick modified polytetrafluoroethylene vinyl material layer. The coating thickness is controlled to be 12μm. Then, an 8μm thick aluminum foil layer is laminated on top to obtain a three-layer composite preform.
[0154] Step 4: The three-layer composite preform is continuously fed to a hot rolling mill at 130°C and 50 N / mm at a linear speed of 15 m / min for hot pressing and bonding. Then it is cooled and shaped by a cooling roller at 20°C, trimmed, and wound up to obtain a polytetrafluoroethylene composite film for anti-interference shielding cables.
[0155] Comparative Example 4
[0156] Comparative Example 4 is the same as Example 1, except that the interface stabilizer is only 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate. Details are as follows:
[0157] A polytetrafluoroethylene composite film for anti-interference shielded cables comprises a modified polytetrafluoroethylene vinyl material layer, an interface hot melt adhesive layer, and an aluminum foil layer stacked sequentially. The formulations and preparation methods of each layer are as follows:
[0158] Step 1: Preparation of modified polytetrafluoroethylene vinyl layer feedstock: Weigh 100 parts of polytetrafluoroethylene dispersion resin, 3 parts of surface hydrophobic modified nano silica, and 0.5 parts of heptadecafluorodecyltrimethoxysilane. Mix the raw materials at 50°C and 300 r / min for 15 min. After cooling to room temperature, add No. 3 aviation kerosene, which is 18% of the weight of polytetrafluoroethylene dispersion resin. Mix evenly and age in a sealed container for 12 h to obtain the modified polytetrafluoroethylene vinyl layer feedstock.
[0159] Preparation of interfacial hot melt adhesive layer feed: Weigh 40 parts of tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, 30 parts of ethylene-vinyl acetate copolymer, 8 parts of fluorotitanium-silicon copolymer modified resin prepared in Preparation Example 1, 0.2 parts of composite antioxidant (including antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1), and 1 part of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate. After stirring and homogenizing each raw material at a rate of 50 r / min for 25 min, add it to a twin-screw extruder (length-to-diameter ratio L / D of 36:1). The screw speed is 150 r / min, and the temperatures of each zone are set as follows: Zone 1 140℃, Zone 2 170℃, Zone 3 190℃, Zone 4 210℃, Zone 5 210℃, Zone 6 200℃, and the die temperature is 190℃. After melt blending and granulation in a twin-screw extruder, the hot melt adhesive layer feed is obtained.
[0160] Step 2: The modified polytetrafluoroethylene vinyl material layer is fed into the feed at 35°C and pressed with paste. Then it is calendered at a roller temperature of 45°C, heated at 180°C for 15 minutes to remove aviation kerosene, and then sintered at 370°C for 15 minutes. After cooling to room temperature, a sintered film is obtained. An infrared radiation heating device is used to subject one side of the sintered film to instantaneous heat radiation for 0.4 seconds, so that the surface temperature of that side reaches 370°C. Then it is attached to a cold roller with cooling water at 8 m / min for rapid quenching, resulting in a modified polytetrafluoroethylene vinyl material layer with a lower crystallinity on the treated surface than the interior.
[0161] Step 3: Feed the hot melt adhesive layer into a single screw extruder (L / D ratio of 25:1), with a screw speed of 20 r / min. The temperature of each zone is set as follows: feeding section 140℃, melting section 170℃, metering section 190℃, and T-die temperature 200℃. The material is melt-extruded through the T-die and uniformly cast onto a 32μm thick modified polytetrafluoroethylene vinyl material layer. The coating thickness is controlled to be 12μm. Then, an 8μm thick aluminum foil layer is laminated on top to obtain a three-layer composite preform.
[0162] Step 4: The three-layer composite preform is continuously fed to a hot rolling mill at 130°C and 50 N / mm at a linear speed of 15 m / min for hot pressing and bonding. Then it is cooled and shaped by a cooling roller at 20°C, trimmed, and wound up to obtain a polytetrafluoroethylene composite film for anti-interference shielding cables.
[0163] Comparative Example 5
[0164] Comparative Example 5 is the same as Example 1, except that the interface stabilizer is only N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine. Specifically:
[0165] A polytetrafluoroethylene composite film for anti-interference shielded cables comprises a modified polytetrafluoroethylene vinyl material layer, an interface hot melt adhesive layer, and an aluminum foil layer stacked sequentially. The formulations and preparation methods of each layer are as follows:
[0166] Step 1: Preparation of modified polytetrafluoroethylene vinyl layer feedstock: Weigh 100 parts of polytetrafluoroethylene dispersion resin, 3 parts of surface hydrophobic modified nano silica, and 0.5 parts of heptadecafluorodecyltrimethoxysilane. Mix the raw materials at 50°C and 300 r / min for 15 min. After cooling to room temperature, add No. 3 aviation kerosene, which is 18% of the weight of polytetrafluoroethylene dispersion resin. Mix evenly and age in a sealed container for 12 h to obtain the modified polytetrafluoroethylene vinyl layer feedstock.
[0167] Preparation of interfacial hot melt adhesive layer feed: Weigh 40 parts of tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, 30 parts of ethylene-vinyl acetate copolymer, 8 parts of the fluorotitanium-silicon copolymer modified resin prepared in Preparation Example 1, 0.2 parts of composite antioxidant (including antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1), and 1 part of N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine. After the material is stirred and homogenized at a rate of 50 r / min for 25 min, it is added to a twin-screw extruder (length-to-diameter ratio L / D is 36:1). The screw speed is 150 r / min, and the temperature of each zone is set as follows: zone 1 140℃, zone 2 170℃, zone 3 190℃, zone 4 210℃, zone 5 210℃, zone 6 200℃, and the die temperature is 190℃. After being melt-blended and granulated by the twin-screw extruder, the hot melt adhesive layer feed is obtained.
[0168] Step 2: The modified polytetrafluoroethylene vinyl material layer is fed into the feed at 35°C and pressed with paste. Then it is calendered at a roller temperature of 45°C, heated at 180°C for 15 minutes to remove aviation kerosene, and then sintered at 370°C for 15 minutes. After cooling to room temperature, a sintered film is obtained. An infrared radiation heating device is used to subject one side of the sintered film to instantaneous heat radiation for 0.4 seconds, so that the surface temperature of that side reaches 370°C. Then it is attached to a cold roller with cooling water at 8 m / min for rapid quenching, resulting in a modified polytetrafluoroethylene vinyl material layer with a lower crystallinity on the treated surface than the interior.
[0169] Step 3: Feed the hot melt adhesive layer into a single screw extruder (L / D ratio of 25:1), with a screw speed of 20 r / min. The temperature of each zone is set as follows: feeding section 140℃, melting section 170℃, metering section 190℃, and T-die temperature 200℃. The material is melt-extruded through the T-die and uniformly cast onto a 32μm thick modified polytetrafluoroethylene vinyl material layer. The coating thickness is controlled to be 12μm. Then, an 8μm thick aluminum foil layer is laminated on top to obtain a three-layer composite preform.
[0170] Step 4: The three-layer composite preform is continuously fed to a hot rolling mill at 130°C and 50 N / mm at a linear speed of 15 m / min for hot pressing and bonding. Then it is cooled and shaped by a cooling roller at 20°C, trimmed, and wound up to obtain a polytetrafluoroethylene composite film for anti-interference shielding cables.
[0171] The comprehensive performance of the polytetrafluoroethylene composite films for anti-interference shielded cables prepared in Examples 1-3 and Comparative Examples 1-5 of this invention was tested respectively.
[0172] 1. Water vapor transmission rate test
[0173] Referring to GB / T 26253-2010 standard, the composite film prepared by this invention was cut into circular samples with a diameter of 100 mm and clamped between the two chambers of a moisture transilluminator. The wet side was controlled at 38±0.5℃ and relative humidity at 90±2%, while the dry side was maintained under low-humidity carrier gas conditions as specified in the standard. After the permeation data stabilized, the water vapor transmission rate (g / (m³)) was measured. 2 ·24h)).
[0174] 2. Interlayer bonding strength test
[0175] According to GB / T 2791-1995 standard, the film prepared by this invention was cut into strips of 25mm×200mm. The substrate and aluminum foil layer were T-shaped peeled at 250mm / min using a universal testing machine at room temperature of 25℃ to obtain the initial normal peel strength. Then, another set of samples of the same specifications were placed in a high and low temperature alternating test chamber and subjected to 50 cycles of extreme thermal shock between -40℃ and 85℃. Each time, the extreme temperature point was strictly held for 30min. After the alternating cycle was completed and the sample was left to stand at room temperature for 24h, the peel test was performed again to obtain the peel strength after aging (N / 25mm).
[0176] 3. Flexural fatigue test
[0177] Referring to ASTM D2176 standard, the composite film prepared in this invention was cut into strips of 15mm × 150mm in length. The samples were vertically fixed between the upper and lower clamps of the MIT flexural strength tester, and a constant tension load of 4.9N was suspended from the lower clamp. The instrument was then started to continuously flex and break the samples within a range of ±135° at a frequency of 175 times / min. The critical number of bends (times) when the aluminum foil layer first showed visible cracks or when the interface just began to delaminate was closely observed and recorded.
[0178] 4. Dielectric property thermal aging stability test
[0179] The dielectric substrate, which has not yet been coated with aluminum foil in step 3 of this invention, is flattened and cut into square samples with a size of 50mm×50mm. It is placed in a standard room temperature environment of 25°C and 50% relative humidity. The initial relative permittivity is measured and recorded using a broadband dielectric spectrometer at a test frequency of 1MHz, in accordance with the GB / T 1409-2006 standard. The sample is then placed in an electric heating drying oven at 150°C for 168h. After the thermal aging is completed, the sample is taken out and placed in the above standard room temperature environment for 24h to recover. The relative permittivity of the sample after thermal aging is measured using the same instrument at the same frequency.
[0180] 5. Electromagnetic shielding effectiveness test after mechanical stress
[0181] Referring to ASTM D4935-18, the film prepared in this invention was cut into standard circular specimens with an outer diameter of 133 mm. Using a vector network analyzer connected to a flange coaxial test fixture, the initial electromagnetic shielding effectiveness (dB) of the specimen at 1.0 GHz was measured within a wide frequency range of 30 MHz to 1.5 GHz. Subsequently, the specimen was fixed on a dynamic bending fatigue testing machine and subjected to 1000 consecutive bends with a bending radius of 2 mm and a bending angle of 180°. After bending, the specimen was removed and flattened on a flat surface to ensure that there were no severe wrinkles in the test area that would cause leakage of electromagnetic waves from the fixture. Then, using the same testing instrument in the same scanning frequency band, the shielding effectiveness of the specimen at 1.0 GHz was measured again.
[0182] 6. Surface and central crystallinity characterization tests
[0183] The modified polytetrafluoroethylene (PTFE) vinyl material samples prepared in the embodiments and comparative examples of this invention were used to cut out the surface sample after quenching treatment and the internal sample unaffected by thermal radiation using a precision micro-slicing and peeling method. Subsequently, the two sets of samples were placed in a differential scanning calorimeter (DSC) and subjected to initial temperature scanning analysis at a heating rate of 10 °C / min under a nitrogen atmosphere. After the test was completed, the integral area (i.e., enthalpy of fusion) of the first melting endothermic peak of each sample was calculated using the instrument analysis software and compared with the standard enthalpy of 100% crystalline PTFE to obtain the crystallinity percentage of the surface sample and the internal sample.
[0184] The test results are shown in Table 1-2:
[0185] Table 1. Water vapor transmission rate test, interlayer bonding strength test, and flexural fatigue test data for Examples 1-3 and Comparative Examples 1-5.
[0186] Test Project <![CDATA[Water vapor transmission rate (g / (m 2 ·24h))]]> Initial peel strength (N / 25mm) Peel strength after thermal shock (N / 25mm) Fatigue life under bending (cycles) Example 1 0.36 8.9 7.8 345 Example 2 0.32 9.6 8.7 412 Example 3 0.28 10.4 9.5 485 Comparative Example 1 0.44 7.2 5.6 282 Comparative Example 2 0.47 5.3 2.1 256 Comparative Example 3 0.49 4.8 1.9 278 Comparative Example 4 0.41 8.7 4.6 335 Comparative Example 5 0.43 8.8 4.2 340
[0187] Table 2. Data on dielectric properties, thermal aging stability, and electromagnetic shielding effectiveness under mechanical stress in Examples 1-3 and Comparative Examples 1-5.
[0188] Test Project Initial relative permittivity (@1MHz) Relative permittivity after aging (@1MHz) Initial shielding effectiveness (@1GHz, dB) Shielding effectiveness after bending (@1GHz, dB) Surface crystallinity (%) Internal crystallinity (%) Example 1 2.14 2.17 74 70 22.4 46.5 Example 2 2.12 2.14 76 73 18.6 45.8 Example 3 2.11 2.12 78 75 15.2 45.2 Comparative Example 1 2.18 2.33 71 46 22.5 46.4 Comparative Example 2 2.15 2.28 72 38 22.3 46.6 Comparative Example 3 2.21 2.37 70 42 22.1 46.2 Comparative Example 4 2.17 2.36 73 58 22.6 46.3 Comparative Example 5 2.19 2.34 71 55 22.2 46.7
[0189] As shown in Table 1-2, the polytetrafluoroethylene composite film for anti-interference shielded cables prepared in Examples 1-3 of this invention has excellent water vapor barrier properties, extremely high interlayer bonding strength, and excellent mechanical fatigue life. At the same time, after undergoing severe thermal aging and mechanical bending, it can still maintain a highly stable dielectric constant and electromagnetic shielding effectiveness, and has excellent overall environmental tolerance.
[0190] Further analysis of the crystallinity data in Table 2 reveals that this invention successfully constructed a gradient structure with low surface crystallinity and high internal crystallinity in the modified polytetrafluoroethylene (PTFE) material layer through specific infrared thermal radiation and rapid quenching treatment. This special design, on the one hand, utilizes the high crystallinity region in the center to retain the original dense barrier and excellent dielectric properties of PTFE; on the other hand, the reduction in surface crystallinity increases the amorphous regions on the substrate surface, breaking the physical inertia of the highly crystalline and dense surface of pure PTFE. This provides ample free space for the penetration and entanglement of polymer chains in the hot melt adhesive layer, laying the foundation for improving interlayer bonding from the perspective of the physical state of the substrate.
[0191] As shown in Example 1 and Comparative Examples 1, 2, and 3: Comparative Example 1 uses a fluorine-free titanium-silicon copolymer modified resin, which lacks fluorine-containing segments in the system. This results in severely insufficient wetting and spreading ability of the adhesive layer on the polytetrafluoroethylene vinyl material, leading to a significant decrease in initial peel strength. Comparative Example 2 uses a non-flexible fluorine-titanium-silicon copolymer modified resin. While maintaining the silane crosslinking network, a rigid monomer replaces the long polysiloxane chain, causing the adhesive layer to lose the flexible buffering effect of the macromolecules and become brittle overall. Under repeated mechanical stress, it is prone to cracking, and its flexural fatigue life is significantly reduced. Comparative Example 3 uses a zirconium-substituted fluorine-silicon copolymer modified resin, demonstrating that even with the substitution of zirconium from the same group, it lacks the specificity of forming a stable chemical bond between the titanium-containing structure and the aluminum foil surface. After undergoing thermal cycling, it is prone to interfacial delamination, leading to a severe loss of electromagnetic shielding effectiveness after bending. Therefore, the synergy of the three functional segments—fluorine, titanium, and silicon—is indispensable; the absence of any single segment will disrupt the mechanical and bonding balance of the composite film.
[0192] As can be seen from Example 1 and Comparative Examples 4 and 5: Comparative Example 4 only uses 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, and the system loses its ability to capture free radicals, resulting in the inability to effectively block the catalytic oxidation reaction at the aluminum interface; Comparative Example 5 only uses N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, which lacks a corresponding acid neutralization mechanism, resulting in the inability to absorb the acidic byproducts generated by the degradation of the adhesive layer at high temperature, which continue to erode the substrate. The two work synergistically to achieve dual protection against oxidation and neutralization of acidic substances, effectively blocking the aging and degradation of the adhesive layer, thereby ensuring the dielectric stability and excellent interlayer peel strength of the composite film under harsh environments.
[0193] It should be noted that the flexural fatigue test (MIT method) in Table 1 was conducted under a constant tension of 4.9N and a destructive folding angle of ±135°. These conditions were extremely demanding, resulting in microcracks or initial delamination in the sample specimens after approximately 300-500 folds. In contrast, the 1000 dynamic bending tests in Table 2 involved no additional tensile stress. Thanks to the strong interfacial chemical bonding and flexible buffering effect provided by the fluorotitanium-silicon copolymer modified resin in the hot melt adhesive layer of this invention, even after fatigue microcracks appeared in the aluminum foil layer after 1000 folds, it remained firmly anchored to the polytetrafluoroethylene material without macroscopic falling off, breaking, or large-area peeling. Because the aluminum foil layer macroscopically maintained a continuous Faraday cage structure and did not form wide gaps larger than the wavelength of high-frequency electromagnetic waves, its electromagnetic shielding effectiveness only experienced a slight decrease due to surface microcracks (e.g., only a decrease from 74dB to 70dB in Example 1), maintaining excellent anti-interference capabilities.
[0194] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they are within the scope of the claims of the present invention.
Claims
1. A polytetrafluoroethylene composite film for anti-interference shielded cables, characterized in that, It comprises a modified polytetrafluoroethylene vinyl material layer, an interface hot melt adhesive layer, and an aluminum foil layer stacked sequentially, wherein the thickness ratio of the modified polytetrafluoroethylene vinyl material layer, the interface hot melt adhesive layer, and the aluminum foil layer is 4-6:0.5-1.5:1; The modified polytetrafluoroethylene vinyl material layer is prepared from the following raw materials in parts by weight: 100 parts of polytetrafluoroethylene dispersion resin, 3-8 parts of surface hydrophobic modified nano silica, and 0.5-1.5 parts of heptadecafluorodecyltrimethoxysilane. The interface hot melt adhesive layer is prepared from the following raw materials in parts by weight: 40-60 parts of tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, 30-45 parts of ethylene-vinyl acetate copolymer, 8-20 parts of fluorotitanium-silicon copolymer modified resin, 0.2-0.8 parts of composite antioxidant, and 1-3 parts of interface stabilizer. The fluorotitanium-silicon copolymer modified resin is prepared by copolymerizing monomethylacryloyloxy polydimethylsiloxane, perfluorohexyl ethyl acrylate and γ-methacryloyloxypropyltriethoxysilane under the initiation of azobisisobutyronitrile, and further modifying it by co-hydrolysis condensation with isopropyltris(dioctylpyrophosphate)titanate. The interface stabilizer in the interface hot melt adhesive layer is a mixture of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate and N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine; The modified polytetrafluoroethylene vinyl material layer has a low crystallinity surface on the side near the interface hot melt adhesive layer. The low crystallinity surface is formed by treating the modified polytetrafluoroethylene vinyl material with infrared thermal radiation and quenching process. The crystallinity of this side surface is lower than that of the internal region of the modified polytetrafluoroethylene vinyl material layer.
2. The polytetrafluoroethylene composite film for anti-interference shielded cables according to claim 1, characterized in that, The fluorotitanium-silicon copolymer modified resin in the interfacial hot melt adhesive layer is prepared by the following steps: S1. Under nitrogen protection, the monomethacryloxy polydimethylsiloxane is dispersed in the first anhydrous ethyl acetate, the system is heated to 60-70℃ and stirred and homogenized for 30-45 min to obtain a siloxane monomer solution. S2. Perfluorohexyl ethyl acrylate, γ-methacryloyloxypropyltriethoxysilane and azobisisobutyronitrile are added to the second anhydrous ethyl acetate and stirred for 20-30 min to dissolve, thus obtaining a mixed monomer solution. Under stirring, the mixed monomer solution is added dropwise to the siloxane monomer solution at a uniform rate over 1-2 h. The system is then heated to 70-75 °C and stirred for another 4-6 h. The system temperature is then lowered to 60-70 °C to obtain an active intermediate solution. S3. Under stirring, add deionized water and glacial acetic acid to the active intermediate solution to adjust the pH of the system to 4-5, and then add isopropyl tris(dioctyl pyrophosphate) titanate dropwise. After the addition is complete, continue stirring the reaction at 60-70℃ for 1-1.5h to obtain the modified resin reaction solution. S4. After the system is cooled to 45-55℃, the modified resin reaction solution is subjected to desolventizing treatment under reduced pressure and then dried under vacuum to obtain the fluorotitanium-silicon copolymer modified resin.
3. The polytetrafluoroethylene composite film for anti-interference shielded cables according to claim 2, characterized in that, In step S2, the mass ratio of perfluorohexyl ethyl acrylate, γ-methacryloyloxypropyltriethoxysilane, azobisisobutyronitrile, and second anhydrous ethyl acetate is 2.5-4:1:0.06-0.12:6-10.
4. The polytetrafluoroethylene composite film for anti-interference shielded cables according to claim 2, characterized in that, In step S2, the mass ratio of the mixed monomer solution to the siloxane monomer solution is 1-3:
1.
5. The polytetrafluoroethylene composite film for anti-interference shielded cables according to claim 2, characterized in that, In step S3, the mass ratio of deionized water, isopropyl tris(dioctylpyrophosphoryloxy)titanate, and active intermediate solution is 0.5-1.0:2.5-4:
100.
6. The polytetrafluoroethylene composite film for anti-interference shielded cables according to claim 2, characterized in that, The parameters for descaling in step S4 are: vacuum degree -0.08MPa to -0.095MPa, time 1-2h.
7. The polytetrafluoroethylene composite film for anti-interference shielded cables according to claim 2, characterized in that, The parameters for vacuum drying are: temperature 40-55℃, time 8-12h.
8. The polytetrafluoroethylene composite film for anti-interference shielded cables according to claim 1, characterized in that, The interface stabilizer is 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarbamate and N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine in a mass ratio of 2-3:
1.
9. A method for preparing a polytetrafluoroethylene composite film for anti-interference shielded cables as described in any one of claims 1-8, characterized in that, Includes the following steps: Step 1: Weigh out polytetrafluoroethylene dispersion resin, surface hydrophobic modified nano silica, and heptadecafluorodecyltrimethoxysilane by weight. Mix the raw materials at 50-55℃ for 10-15 minutes, then cool to room temperature. Add an extrusion aid at 18-20% of the weight of the polytetrafluoroethylene dispersion resin, mix evenly, and age in a sealed container to obtain the modified polytetrafluoroethylene vinyl layer feedstock. Weigh out tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride terpolymer, ethylene-vinyl acetate copolymer, fluorotitanium-silicon copolymer modified resin, composite antioxidant, and interface stabilizer by weight. Mix the raw materials and homogenize for 15-25 minutes, then melt-blend and granulate using a twin-screw extruder to obtain the hot melt adhesive layer feedstock. Step 2: The modified polytetrafluoroethylene vinyl material layer is fed through paste extrusion, calendering, heating to remove extrusion aid, and then sintering and cooling to room temperature to obtain a sintered film; one side of the sintered film is subjected to infrared thermal radiation treatment and then subjected to rapid quenching to obtain a modified polytetrafluoroethylene vinyl material layer with a lower crystallinity on the treated surface than on the interior. Step 3: The hot melt adhesive layer is fed through a single screw extruder and a T-die to melt and extrude, and then uniformly cast and coated on the modified polytetrafluoroethylene vinyl material layer. Subsequently, an aluminum foil layer is laminated on top of it to obtain a three-layer composite preform. Step 4: The three-layer composite prefabricated film is continuously fed into a hot rolling mill for hot pressing and bonding. After cooling, shaping, trimming and winding, a polytetrafluoroethylene composite film for anti-interference shielded cables is obtained.
Citation Information
Patent Citations
Polypropylene film, preparation method thereof and paper-plastic thermal composite base material
CN115284706A
Fluorosilicone modified acrylic resin and preparation method thereof
CN118006064A