A method for optimizing the mix design of high-performance concrete
By optimizing the dosage of composite water-reducing agent through nonlinear curve fitting and the median cost principle, the problem of quantitative determination of dosage in the mix design of high-performance concrete is solved, and the synergistic optimization of workability and cost and the improvement of compressive strength are achieved.
Patent Information
- Application Number
- CN202611424783.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-09-15
AI Technical Summary
In the design of high-performance concrete mix proportions, it is difficult to quantitatively determine the dosage of functional components of composite water-reducing agents, which makes it difficult to optimize the workability retention of concrete and production costs in a coordinated manner. Furthermore, the water-cement ratio design does not take into account the impact of composite water-reducing agents on the compressive strength of concrete, resulting in insufficient design accuracy.
By establishing a nonlinear curve fitting between the initial concrete slump expansion and the slump expansion after 2 hours, and combining the pump flow requirements of the project, the initial dosage control range of the functional components of the composite water-reducing agent was determined. The synergistic dosage point K was determined by adopting the cost median value principle. The water-cement ratio calculation formula was modified to quantify the contribution of the composite water-reducing agent to compressive strength and optimize the amount of cementitious materials.
This approach achieves a two-way optimization of the workability retention capacity of concrete after 2 hours and production cost, thereby improving the 28-day compressive strength and slump expansion of concrete, reducing production costs, and enhancing the accuracy and effectiveness of mix design.
Smart Images

Figure CN122930333B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of concrete mix design technology, and specifically relates to a method for optimizing the mix design of high-performance concrete. Background Technology
[0002] High-performance concrete, with its outstanding mechanical, workability, and durability properties, is widely used in various engineering projects. Currently, high-performance concrete is mainly formulated using a cement-mineral powder-fly ash multi-component composite cementitious system. The increased complexity of the cementitious material system makes the interaction mechanism between admixtures and cementitious materials more complex, placing higher demands on the design and dosage of admixtures, and further increasing the difficulty of high-quality concrete mix design. However, existing technologies have significant shortcomings in determining the dosage of functional components in composite water-reducing agents: on the one hand, the influence of functional component dosage on the initial slump spread and 2-hour slump spread of concrete exhibits a non-linear relationship. Traditional empirical methods are insufficient to quantitatively determine the reasonable dosage range of functional components that meet the pump flowability requirements of engineering projects, resulting in a lack of systematic methods for synergistic optimization between workability retention and production costs; on the other hand, existing concrete water-cement ratio design methods do not consider the influence of functional components in composite water-reducing agents on the 28-day compressive strength of concrete, leading to insufficient accuracy in water-cement ratio design and making it difficult to achieve comprehensive optimization of the mix design.
[0003] Therefore, how to provide a method for optimizing the mix design of high-performance concrete is a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0004] The purpose of this invention is to provide a high-performance concrete mix design optimization method to solve the technical problems in the prior art, such as the difficulty in quantitatively determining the dosage of functional components of composite water-reducing agents, the difficulty in synergistically optimizing the workability retention capacity and production cost of concrete, and the insufficient accuracy of mix design due to the failure of existing water-cement ratio design methods to consider the influence of functional components of composite water-reducing agents on the compressive strength of concrete.
[0005] To solve the above technical problems, the present invention includes the following technical solutions:
[0006] A method for optimizing the mix design of high-performance concrete, the method comprising:
[0007] Step S1: Determine the mix design strength of the high-performance concrete. Select the mix design of high-performance concrete prepared with natural aggregates, a composite cementitious material containing both mineral powder and fly ash, and a polycarboxylate superplasticizer as the benchmark mix design. The benchmark mix design is the basis for all subsequent calculations and comparisons, and its mix design strength is determined by the engineering design requirements.
[0008] Step S2: Determine the initial dosage control range U for the functional components. Specifically, based on slump test data, a quantitative relationship between the 2-hour slump expansion of high-performance concrete and the initial slump expansion of concrete under different water content benchmark mix proportions is established through nonlinear curve fitting. The acceptable 2-hour slump expansion control range (A, B) is determined according to the pump flowability requirements of the project, and the initial slump expansion control range (a, b) is obtained by inverse mapping using the aforementioned nonlinear fitting curve. Under the selected benchmark mix proportions, the mass ratio of the functional components in the composite water-reducing agent is gradually changed by a preset adjustment unit, and experiments on the initial slump expansion of concrete under different functional component dosages are conducted to obtain the relationship between the initial slump expansion of concrete and the functional component dosage, and nonlinear curve fitting is performed. Based on the aforementioned nonlinear fitting curve and the initial slump expansion control range (a, b), the initial dosage control range U (e, f) of the functional components in the composite water-reducing agent is obtained. This step, through the dual control constraints of initial slump expansion and 2-hour slump expansion, quantitatively transforms the pump flowability requirements of the project into the functional component dosage constraint range, overcoming the shortcomings of traditional empirical methods that cannot be quantitatively determined.
[0009] Step S3: Within the control interval U(e, f), calculate the unit production cost of concrete under the corresponding functional component dosage. Take the mass ratio of the functional component corresponding to the median cost as the synergistic dosage point K. The median cost principle ensures that the determined K value not only meets the engineering requirements for maintaining workability but also achieves a reasonable balance in production cost, realizing two-way constraint optimization of workability and cost.
[0010] Step S4: Design the water-cement ratio of concrete based on the strength variation coefficient V. High-performance concrete is prepared using a composite water-reducing agent with a functional component mass ratio of K, and its 28-day compressive strength is measured and denoted as... Concrete was prepared using the reference mix proportion, and its 28-day compressive strength was measured and denoted as . The intensity variation coefficient V is calculated using the following formula:
[0011] ,
[0012] Substitute the strength variation coefficient V into the following formula to calculate the water-cement ratio of high-performance concrete:
[0013] ,
[0014] The strength variation coefficient V quantifies the actual contribution of the functional components in the composite water-reducing agent to the 28-day compressive strength of concrete. By introducing V into the Balromy water-cement ratio calculation formula, the shortcomings of the existing method in not considering the influence of the strength of functional components are corrected, making the water-cement ratio design more accurate.
[0015] Step S5: Based on the water-cement ratio obtained above, calculate the total amount of cementitious materials, and then calculate the amount of the three cementitious materials according to the ratio of cement, mineral powder and fly ash, and calculate the amount of sand and gravel aggregate to complete the mix design optimization of high-performance concrete.
[0016] Furthermore, when determining the initial dosage control range U of the functional components, the preset adjustment unit is 0.1 of the total mass of the composite water-reducing agent. This step size takes into account both experimental efficiency and range accuracy. When determining the synergistic dosage point K, the adjustment unit is 0.02 of the total mass of the composite water-reducing agent. The smaller step size ensures the accuracy of K value determination.
[0017] Furthermore, the reference mix proportion adopts a ternary composite cementitious material system composed of silicate cement, slag powder and fly ash. The synergistic effect of the three can improve the workability, mechanical properties and durability of concrete.
[0018] Furthermore, all parameters in the water-cement ratio calculation formula, except for the strength variation coefficient V, are selected in accordance with the provisions of the industry standard "Specification for Mix Proportion Design of Ordinary Concrete" (JGJ55-2011), and the amount of sand and gravel aggregate is also calculated and determined in accordance with the provisions of this specification, thereby ensuring the effective connection between the method of the present invention and the current industry standards.
[0019] Specifically, this invention also provides a composite water-reducing agent for high-performance concrete, which is composed of polycarboxylate superplasticizer mother liquor and functional components. The mass proportion of the functional components is K, which is given by the synergistic dosage point K determined in the above-mentioned high-performance concrete mix proportion optimization design method. The mass proportion of the functional components in this composite water-reducing agent is systematically optimized through workability dual control and cost median principle, which can achieve reasonable control of production costs while meeting the pump flowability requirements of engineering projects.
[0020] Furthermore, the functional component in the composite water-reducing agent is lignocal water-reducing agent or CSH gel.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0022] (1) The high-performance concrete mix design method provided by the present invention combines the dual control constraint of initial concrete slump expansion and slump expansion over 2 hours with nonlinear curve fitting, and quantitatively maps the pump flowability requirement of the project into the functional component dosage constraint interval U(e,f). This overcomes the shortcomings of traditional empirical methods in making it difficult to quantitatively determine the dosage of functional components, and transforms the determination of the dosage of functional components from qualitative empirical judgment to quantitative system design.
[0023] (2) The high-performance concrete mix design method provided by the present invention determines the synergistic admixture point K by adopting the cost median value principle within the control range U, thereby achieving two-way constraint optimization of the concrete’s workability retention capacity after 2 hours and unit production cost, avoiding the one-sided design problem of only pursuing workability retention while ignoring cost, or only pursuing low cost while sacrificing workability.
[0024] (3) The high-performance concrete mix design method provided by the present invention modifies the Balromy water-cement ratio calculation formula by introducing the strength variation coefficient V, quantifies the actual contribution of the functional components of the composite water-reducing agent to the 28-day compressive strength of concrete, makes up for the defect of the existing water-cement ratio design method that does not consider the influence of the strength of the functional components, and significantly improves the accuracy of mix design.
[0025] (4) The high-performance concrete mix design method provided by the present invention, as verified by examples, shows that compared with the standard mix design of ordinary high-performance concrete, the C50 high-performance concrete designed by the method of the present invention has a 28-day compressive strength increased by 5.7 MPa, an initial slump flow increased by 100 mm, a 2-hour slump flow increased by 110 mm, a 28-day shrinkage strain decreased by 35 με, and a unit production cost decreased by 23 yuan / m³. 3 This achieves synergistic optimization of overall performance and production costs. Attached Figure Description
[0026] Figure 1 This is a schematic diagram of the relationship between the time-dependent concrete slump expansion and the initial concrete slump expansion according to an embodiment of the present invention.
[0027] Figure 2 This is a schematic diagram of the relationship between the initial concrete slump expansion and the dosage of functional components according to an embodiment of the present invention.
[0028] Figure 3 This is a schematic diagram showing the relationship between the unit cost and the amount of functional component in an embodiment of the present invention. Detailed Implementation
[0029] The following detailed description, in conjunction with the accompanying drawings and specific embodiments, provides a method for optimizing the mix design of high-performance concrete according to the present invention. The advantages and features of the present invention will become clearer from the following description.
[0030] The following is combined Figures 1 to 3 This invention provides a detailed description of the high-performance concrete mix design optimization method.
[0031] In the following examples, the P.O42.5 silicate cement, S95 grade slag powder, Class II C fly ash, natural sand, gravel, polycarboxylate superplasticizer mother liquor, and lignosulfonate superplasticizer used were all commercially available products. The initial slump flow and 2-hour slump flow of the concrete were determined according to GB / T 50080; the 28-day compressive strength was determined according to GB / T 50081; the 28-day shrinkage strain was determined according to GB / T 50082; and the unit production cost was calculated based on the actual amount of raw materials used and the market unit price. Functional components refer to organic or inorganic retarding and thickening components that can improve the workability retention of concrete over time, including but not limited to lignosulfonate superplasticizer and CSH gel. The synergistic dosage point K refers to the optimal mass ratio of the functional component determined based on the cost median principle within the initial dosage control range U of the functional component.
[0032] Example 1
[0033] Please refer to Figures 1 to 3 This embodiment uses C50 high-performance concrete as the object and employs the method of this invention for mix proportion optimization design, with lignocal water-reducing agent selected as the functional component. Of course, the functional component can also be CSH gel or other organic or inorganic retarding and thickening components that can improve the workability retention of concrete over time. When CSH gel is used as the functional component, the same method and steps as in Example 1 can be followed. Figures 1 to 3 The illustration shown is one of the preferred embodiments of this invention and is not the only limitation on the technical solution of this invention.
[0034] First, the baseline mix proportion and strength were determined. The high-performance concrete mix proportion prepared using a composite cementitious material with natural aggregates, mineral powder and fly ash, and polycarboxylate superplasticizer was selected as the baseline mix proportion. The specific dosages are shown in Table 1.
[0035] Table 1. Mix proportions of ordinary high-performance concrete (kg / m³) 3 )
[0036] P.O42.5 cement water S95 grade slag powder Class II, Category C fly ash natural sand pebbles Polycarboxylate superplasticizer Water-to-glue ratio 270 208 110 105 780 980 3.6 0.43
[0037] Concrete prepared according to the above-mentioned standard mix proportions was found to have a 28-day compressive strength of 50.4 MPa, an initial slump flow of 580 mm, a 2-hour slump flow of 510 mm, a 28-day shrinkage strain of 546 με, and a unit production cost of 385 yuan / m³. 3 .
[0038] Secondly, the initial dosage control range U of the functional components was determined. The initial slump flow of the concrete was controlled by varying the water content. Based on slump test data, the relationship between the 2-hour slump flow of high-performance concrete and the initial slump flow was obtained under different water content benchmark mix proportions. Nonlinear curve fitting was then performed, and the results are as follows: Figure 1As shown.
[0039] Based on the pump flowability requirements of the project, the acceptable slump spread control range (A, B) of concrete after 2 hours is determined, where A = 593 mm and B = 644 mm. Figure 1 The nonlinear fitting curve shown is used to obtain the initial concrete slump expansion control range (a, b) by inverse mapping, where a = 671 mm and b = 700 mm.
[0040] Under the above-mentioned benchmark mix proportions, using 0.1% of the total mass of the composite water-reducing agent as the adjustment unit, the mass proportion of lignosulfonate water-reducing agent in the composite water-reducing agent was gradually changed. Initial slump flow tests were conducted with different functional component dosages to obtain the relationship between the initial slump flow and the functional component dosage, and nonlinear curve fitting was performed. The results are as follows: Figure 2 As shown.
[0041] according to Figure 2 The nonlinear fitting curves and the initial concrete slump expansion control range (a=671mm, b=700mm) shown indicate the initial dosage control range U(e, f) of the calcium lignosulfonate water-reducing agent in the composite water-reducing agent, where e=0.32 and f=0.44.
[0042] Within the control interval U (0.32, 0.44), calculate the unit production cost of concrete under the corresponding functional component dosage, and plot the relationship curve of cost versus functional component dosage, as shown below. Figure 3 As shown. Figure 3 Among them, the highest cost (approximately 380 yuan / m³) is achieved when the functional component dosage is e=0.32. 3 The lowest cost (approximately 344 yuan / m³) is achieved when the functional component dosage is f=0.44. 3 ).
[0043] Take the median cost of 362 yuan / m 3 The corresponding functional component mass percentage is taken as the synergistic doping point K, by Figure 3 K was set at 0.36. This K value achieved a reasonable balance in production cost control while meeting the pump flow requirements of the project.
[0044] Subsequently, the water-cement ratio of the concrete was designed based on the strength variation coefficient V. High-performance concrete was prepared using a composite water-reducing agent with a functional component (calcium lignosulfonate water-reducing agent) having a mass ratio of K=0.36, and its 28-day compressive strength was measured to be 60.5 MPa according to GB / T 50081.
[0045] Substitute the above values into the following formula to calculate the intensity variation coefficient V:
[0046] We find that V is approximately equal to 1.2.
[0047] Substitute the strength variation coefficient V=1.2 into the following formula to calculate the water-cement ratio of high-performance concrete:
[0048] ,
[0049] In the above formula, all parameters except the strength variation coefficient V are selected in accordance with the provisions of the "Specification for Mix Proportion Design of Ordinary Concrete" (JGJ 55-2011), and the water-cement ratio is calculated to be 0.41.
[0050] Finally, based on a water-cement ratio of 0.41, the total amount of cementitious materials was calculated, and then the amount of the three cementitious materials was calculated according to the ratio of cement, slag powder and fly ash. The amount of sand and gravel aggregate was calculated and determined according to the "Specification for Mix Proportion Design of Ordinary Concrete" (JGJ55-2011). The optimized mix proportion of C50 high-performance concrete was obtained, and the specific amounts are shown in Table 2.
[0051] Table 2 Optimized mix proportions of C50 high-performance concrete (kg / m³) 3 )
[0052] P.O42.5 cement water S95 grade slag powder Class II, Category C fly ash natural sand pebbles Composite high-efficiency water-reducing agent (calcium lignosulfonate synergistic ratio 0.36) Water-to-glue ratio 282 208 115 110 780 980 3.6 0.41
[0053] The performance of the optimized mix proportion concrete was tested, and the results are shown in Table 3.
[0054] Table 3. Performance and cost test results of optimized C50 high-performance concrete
[0055] Performance indicators Optimized measurement values Benchmark measurement Change 28-day compressive strength (MPa) 56.1 50.4 +5.7 Initial collapse spread (mm) 680 580 +100 Slump spread over 2 hours (mm) 620 510 +110 28d contraction strain (με) 511 546 -35 <![CDATA[Unit production cost (CNY / m 3 )]]> 362 385 -23
[0056] Comparative Example 1
[0057] This comparative example is ordinary C50 high-performance concrete, prepared using the benchmark mix proportions shown in Table 1. That is, polycarboxylate superplasticizer is used without introducing functional components for synergistic dosage optimization, and the strength variation coefficient V is not used to correct the water-cement ratio, keeping the water-cement ratio at 0.43.
[0058] Concrete was prepared according to the standard mix proportion, and the following performance indicators were measured: 28-day compressive strength 50.4 MPa, initial slump flow 580 mm, 2-hour slump flow 510 mm, 28-day shrinkage strain 546 με, and production cost per cubic meter 385 yuan / m³. 3 .
[0059] A comparison of Example 1 and Comparative Example 1 shows that after optimizing the mix design using the method of the present invention, the 28-day compressive strength of high-performance concrete increased by 5.7 MPa, the initial slump flow increased by 100 mm, the 2-hour slump flow increased by 110 mm, the 28-day shrinkage strain decreased by 35 με, and the unit production cost decreased by 23 yuan / m³. 3This achieves synergistic optimization of overall performance and production costs.
[0060] The aforementioned effects are attributed to the synergistic effect of the three core technical features of this invention: by quantitatively determining the initial dosage control range U of the functional components through workability dual control constraints and nonlinear curve fitting, the blindness of traditional empirical methods is avoided; by determining the synergistic dosage point K within the control range U through the cost median principle, the dual constraint optimization of workability maintenance and production cost is achieved; and by introducing the strength variation coefficient V to correct the Balromy water-cement ratio calculation formula, the actual contribution of the composite water-reducing agent functional components to the 28-day compressive strength is quantified, making the water-cement ratio design more accurate.
[0061] In particular, the composite cementitious material system in the benchmark mix proportion is not limited to the ternary system of silicate cement, slag powder and fly ash. All high-performance concretes prepared using natural aggregates and composite cementitious material systems can be optimized for mix proportion design using the method of this invention.
[0062] The above examples are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. The above embodiments only illustrate several implementations of the present invention, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the invention patent. It should be noted that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this patent should be determined by the appended claims.
Claims
1. A method for optimizing the mix design of high-performance concrete, characterized in that, The method includes the following steps: Step S1: Determine the mix design strength of high-performance concrete and select the mix design of high-performance concrete prepared with composite cementitious materials and polycarboxylate superplasticizer as the benchmark mix design. Step S2: Determine the initial dosing control range U for the functional components. The specific steps are as follows: The first step is to obtain the relationship between the slump expansion of high-performance concrete after 2 hours and the initial slump expansion of concrete under different water content benchmark mix proportions based on slump test data, and to perform nonlinear curve fitting. The second step is to determine the control range (A, B) of the concrete slump expansion after 2 hours based on the pump flow requirements of the project; and to obtain the initial concrete slump expansion control interval (a, b) by inverse mapping based on the nonlinear fitting curve obtained in the first step. The third step is to select the benchmark mix proportion, gradually change the mass ratio of functional components in the composite water-reducing agent with preset adjustment units, conduct the initial slump flow test of concrete under different functional component dosages, obtain the relationship between the initial slump flow of concrete and the dosage of functional components, and perform nonlinear curve fitting. The fourth step is to obtain the initial dosage control range U(e,f) of the functional components in the composite water-reducing agent based on the nonlinear fitting curve obtained in the third step and the initial concrete slump expansion control range (a, b) obtained in the second step. Step S3: Determine the synergistic dosing point K of the functional components. The specific steps are as follows: Within the control interval U(e, f), calculate the unit production cost of concrete under the corresponding functional component dosage, and take the mass ratio of the functional component corresponding to the median cost value as the synergistic dosage point K. Step S4: Design the water-cement ratio of concrete based on the strength variation coefficient V. The specific steps are as follows: Step 1: High-performance concrete was prepared using a composite water-reducing agent with a functional component mass ratio of K, and its 28-day compressive strength was measured and recorded as follows. Concrete was prepared using the reference mix proportion determined in step S1, and its 28-day compressive strength was measured and denoted as f. cu,28 ; Step 2: Calculate the intensity variation coefficient V using the following formula: ; Step 3: Substitute the strength variation coefficient V into the following formula to calculate the water-cement ratio of high-performance concrete: ; Step S5: Based on the water-cement ratio obtained in step S4, calculate the total amount of cementitious materials, and then calculate the amount of the three cementitious materials according to the ratio of cement, mineral powder and fly ash, and calculate the amount of sand and gravel aggregate to complete the mix design optimization of high-performance concrete.
2. The method according to claim 1, characterized in that, In step S1, a composite cementitious material made by mixing natural aggregates, mineral powder and fly ash is used.
3. The method according to claim 1, characterized in that, In the third step, the functional component is an organic or inorganic retarding and thickening component that can improve the workability retention of concrete over time.
4. The method according to claim 3, characterized in that, The functional component is a lignocal water-reducing agent.
5. The method according to claim 3, characterized in that, The functional component is CSH gel.
6. The method according to claim 1, characterized in that, In the third step, when determining the synergistic dosage point K, the adjustment unit is 0.02 of the total mass of the composite water-reducing agent.
7. The method according to claim 2, characterized in that, The composite cementitious material system includes a ternary composite cementitious material system composed of silicate cement, slag powder and fly ash.
8. The method according to claim 1, characterized in that, In step S4, the amount of sand and gravel aggregate is calculated and determined in accordance with the provisions of the industry standard "Specification for Mix Proportion Design of Ordinary Concrete".
Citation Information
Patent Citations
Design method for mixing proportion of self-compacting concrete mixture
CN105224727A
Full-hole slag concrete collaborative deformation design method