Microporous membranes modified with MS-PC and B-HC and their preparation method, and zinc-bromine flow batteries
By coating the positive electrode side of the microporous membrane of the zinc-bromine flow battery with MS-PC and the negative electrode side with B-HC, the problems of bromine penetration and zinc dendrite growth were solved, thereby improving the electrochemical performance and cycle life of the battery.
Patent Information
- Application Number
- CN202611422417.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-09-14
AI Technical Summary
Zinc-bromine flow batteries suffer from problems such as bromine penetration, slow bromine kinetics, and zinc dendrite growth, resulting in low coulombic efficiency, low energy efficiency, and short cycle life.
MS-PC coating is applied to the positive electrode side of the microporous membrane and B-HC coating is applied to the negative electrode side. MS-PC forms a physical and chemical dual barrier through its hierarchical porous structure and polar functional groups to prevent the diffusion of bromine species, while B-HC regulates zinc deposition behavior and inhibits zinc dendrite growth through an ion buffer layer.
It significantly improves coulombic efficiency to 91.2%~96.9%, voltage efficiency to 83.3%~87.1%, and energy efficiency to 75.97%~84.40%, extending cycle life and reducing the risk of self-discharge and zinc dendrite puncture.
Smart Images

Figure CN122930970B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrochemical energy storage technology, specifically relating to a microporous membrane modified with mustard seed porous carbon (MS-PC) and bamboo-derived hydrochar (B-HC) and its preparation method, as well as a zinc-bromine flow battery. Background Technology
[0002] Zinc-bromine flow batteries are large-scale energy storage batteries that use zinc and bromine as active materials. The same aqueous solution of zinc bromide is used as the electrolyte at both the positive and negative electrodes. During charging, zinc ions are reduced and deposited as metallic zinc at the negative electrode, while bromide ions (Br₂) are deposited at the negative electrode. - The zinc-bromine flow battery oxidizes to elemental bromine (Br2) at the positive electrode, and the process reverses during discharge. It offers advantages such as low cost, high energy density, safety with an aqueous electrolyte, and no cross-contamination, making it suitable for large-scale energy storage applications.
[0003] However, the industrialization process of zinc-bromine flow batteries is currently constrained by the following three major technical bottlenecks: (1) the active bromine species in the positive electrode (such as Br2 / Br3) - (2) Positive electrode bromine / bromine (Br2 / Br - The redox reaction kinetics of Br2 are slow, involving multiple electron transfer processes and requiring high activation energy. To improve the solubility of Br2, complexing agents are often introduced into the positive electrode, but this makes the reaction path of Br2 more complicated, further slowing down the reaction rate. The resulting high polarization voltage significantly reduces voltage efficiency and power density, ultimately leading to low energy efficiency, limited power output, and difficulty in improving coulombic efficiency. (3) The uneven electric field distribution on the surface of the negative electrode makes it easy for zinc dendrites to form during zinc deposition. Zinc dendrites may not only pierce the separator and cause a short circuit in the battery, but also seriously threaten system safety and limit battery cycle life.
[0004] The aforementioned technological bottlenecks collectively constitute the main obstacles to the industrialization of zinc-bromine flow batteries. Regarding membrane materials, traditional membranes have large pore sizes, resulting in insufficient blocking ability for active bromine species and an inability to effectively inhibit the growth of zinc dendrites. While ceramic membranes exhibit strong bromine blocking performance, their high brittleness and low ionic conductivity limit their practical applications. Recent metal-organic framework (MOF)-based bromine blocking materials primarily rely on pore size sieving mechanisms and lack chemisorption capabilities, thus exhibiting limited bromine blocking effects, a narrow range of applications, and weak inhibition of zinc dendrites.
[0005] In summary, existing zinc-bromine flow battery technology still fails to solve key problems such as bromine breakthrough, sluggish bromine reaction kinetics, and zinc dendrite growth. Summary of the Invention
[0006] To overcome the technical problems of bromine penetration, slow bromine kinetics, and zinc dendrite growth in existing zinc-bromine flow batteries, this invention provides a microporous membrane modified with MS-PC and B-HC, a preparation method thereof, and a zinc-bromine flow battery.
[0007] This invention is achieved through the following technical solution: In a first aspect, the present invention provides a method for preparing a microporous membrane based on MS-PC and B-HC modification, comprising: Mustard seed powder was subjected to a hydrothermal reaction to obtain a hydrothermal carbon precursor; the hydrothermal carbon precursor was pyrolyzed to obtain a carbonized product; the carbonized product was chemically activated with an activator to obtain MS-PC. Bamboo powder was subjected to a hydrothermal carbonization reaction to obtain B-HC; MS-PC was coated on the positive electrode side of the microporous membrane to form an MS-PC coating; B-HC was coated on the negative electrode side of the microporous membrane to form a B-HC coating, thus obtaining a microporous membrane modified with MS-PC and B-HC.
[0008] Preferably, the pyrolysis temperature is 700~900℃.
[0009] Preferably, the activator is H3PO4.
[0010] Preferably, the hydrothermal carbonization reaction of the bamboo powder is carried out at a temperature of 170~230℃.
[0011] Preferably, the MS-PC loading on the positive electrode side of the microporous membrane is 0.4~5.3 mg / cm³. 2 The loading of B-HC on the negative electrode side of the microporous membrane is 0.2~1.0 mg / cm³. 2 .
[0012] Preferably, coating MS-PC onto the positive electrode side of the microporous membrane specifically involves: preparing MS-PC dispersion with water; adding the MS-PC dispersion dropwise onto the positive electrode side of the microporous membrane; and allowing it to stand before drying.
[0013] Preferably, coating B-HC onto the negative electrode side of the microporous membrane specifically involves: preparing a B-HC dispersion using water; adding the B-HC dispersion dropwise to the negative electrode side of the microporous membrane; and allowing it to stand before drying.
[0014] Preferably, the microporous membrane is a polypropylene (PP) membrane, a polyethylene (PE) membrane, or a polyolefin composite membrane.
[0015] Secondly, the present invention provides a microporous membrane based on MS-PC and B-HC modification obtained by the preparation method described above.
[0016] Thirdly, the present invention provides a zinc-bromine flow battery, comprising a microporous membrane modified with MS-PC and B-HC as described above.
[0017] Compared with the prior art, the present invention has the following beneficial effects: This invention involves coating the positive and negative sides of a microporous membrane with MS-PC and B-HC, respectively. The MS-PC is formed from mustard seeds through hydrothermal reaction, pyrolysis, and chemical activation, possessing a hierarchical porous structure of micropores and mesopores. When applied to zinc-bromine flow batteries, the micropores in the MS-PC allow small-sized ions (Br₂, B₃, and Br₂) to pass through. - and Zn 2+ The active bromine species (Br2 / Br3) generated at the positive electrode are passed through, thus allowing them to pass through. - The bromine species are "locked" inside the channels and cage-like cavities, utilizing the pore size sieving effect to hinder the penetration of large molecular active bromine species. This physical confinement prevents the diffusion of active bromine species to the negative electrode, thereby reducing self-discharge and improving coulombic efficiency. Furthermore, MS-PC contains a large amount of CSC and -SO₄ groups. x The presence of polar functional groups such as -COOH can lead to strong chemisorption of active bromine species, forming a dual "adsorption-confinement" barrier with physical confinement, significantly reducing bromine permeation and improving coulombic efficiency. Simultaneously, during MS-PC preparation, the natural sulfur-containing groups of mustard seeds break down, releasing CSC and C-SO4 groups. x When S replaces some C atoms in an aromatic ring, unlike C atoms, S atoms are larger and have more outer electrons. When S replaces C in the aromatic ring, the electron cloud distribution of the CSC bond differs from that of the CCC bond. Electrons shift towards S or rearrange around it, disrupting the originally uniform electron cloud and creating localized electron-rich and electron-deficient regions. - (Negatively charged) are more easily adsorbed and activated by electron-deficient regions, Br2 / Br3 - It can form weak coordination with electron-rich regions, which is beneficial for desorption and transformation, thereby reducing the bromine / bromine ratio (Br2 / Br). - The activation energy of the reaction accelerates the reaction of bromine / bromine (Br2 / Br) -Redox kinetics were studied to overcome the sluggish bromine kinetics. During the hydrothermal carbonization process, B-HC retained abundant oxygen-containing functional groups derived from bamboo powder cellulose, hemicellulose, and lignin, including hydroxyl (-OH), carboxyl (-COOH), and carbonyl (C=O) groups. The -OH and -COOH functional groups on the B-HC surface can interact with Zn. 2+ Weak coordination occurs, forming an ion buffer layer: the ion buffer layer in Zn 2+ Temporary complexation of Zn at high concentrations 2+ In Zn 2+ Zn is replenished by releasing it at low concentrations. 2+ The ion buffer layer smooths the Zn interface. 2+ Concentration fluctuations lead to a more uniform deposition current density distribution, which indirectly results in a more uniform interfacial electric field distribution. This uniform electric field distribution, along with the ion concentration field, promotes the deposition of Zn. 2+ Simultaneous and equal-probability nucleation occurs at all interfaces, increasing the number and uniform distribution of nucleation sites, fundamentally suppressing the initial nucleation of zinc dendrites caused by localized supersaturation. During the zinc deposition and growth stage, B-HC can guide Zn... 2+ B-HC smooths the deposition and buffers the risk of diaphragm puncture, enabling Zn 2+ The diffusion field around the crystal nucleus is more symmetrical, weakening the tip effect and guiding Zn. 2+ It preferentially fills the recessed areas between crystal nuclei, promoting a smoother zinc deposition layer. Even if a small number of zinc dendrites sprout, B-HC can disperse the mechanical stress at the dendrite tips, delaying their penetration into the microporous membrane. Through full-chain intervention in the nucleation, growth, and penetration stages, the B-HC coating effectively inhibits the growth and damage of zinc dendrites. Reducing zinc dendrites serves several purposes. First, it prevents micro-short circuits between the positive and negative electrodes caused by zinc dendrites piercing the microporous membrane, as well as self-discharge caused by the displacement of active bromine species with zinc. It also reduces "dead zinc" formed due to the fracture of zinc dendrite roots, thereby improving the reversible utilization rate and charge conservation efficiency of active zinc. Second, a smooth zinc deposition layer makes the interfacial current distribution more uniform, reducing local activation polarization and concentration polarization. It also reduces the additional contact resistance introduced by zinc dendrites piercing or approaching the microporous membrane, making ohmic polarization controllable. This reduces the charge-discharge voltage difference, promoting a simultaneous improvement in voltage efficiency and energy efficiency. Zinc dendrite suppression can also effectively delay the risk of microporous membrane puncture and electrolyte micro-leakage, maintain the selectivity of the microporous membrane, and reduce the capacity loss rate during long-term cycling by reducing irreversible zinc accumulation. This allows zinc-bromine flow batteries to maintain a higher capacity retention rate and a more stable efficiency decay curve over hundreds to thousands of cycles, extending the cycle life of zinc-bromine flow batteries.
[0018] Furthermore, the pyrolysis temperature during the MS-PC preparation process of this invention is preferably 700~900℃. Within this temperature range, carbonization can be effectively achieved, and the doping state of sulfur in the carbon framework can be controlled to improve bromine inhibition ability and catalytic performance.
[0019] Furthermore, the hydrothermal carbonization reaction temperature of the bamboo powder of the present invention is 170~230℃. Within this temperature range, the bamboo powder can be fully carbonized, and at the same time, the polar functional groups such as hydroxyl (-OH) and carboxyl (-COOH) on its surface are largely retained, ensuring the hydrophilicity of B-HC and its coordination ability with zinc ions.
[0020] Furthermore, to balance the functionality and ionic conductivity of the MS-PC coating and the B-HC coating, the MS-PC loading on the positive electrode side of the microporous membrane is 0.408~5.306 mg / cm³. 2 The loading of B-HC on the negative electrode side of the microporous membrane is 0.204~1.020 mg / cm³. 2 Within the aforementioned load range, the MS-PC coating and B-HC coating can fully exert their physicochemical effects without significantly increasing the ohmic impedance due to excessive thickness or blockage of the microporous membrane channels.
[0021] The zinc-bromine flow battery of the present invention uses the microporous membrane based on MS-PC and B-HC modification as the membrane material, which can overcome the problems of bromine permeation, slow bromine kinetic reaction and zinc dendrite growth, and exhibits excellent electrochemical performance with a coulombic efficiency of 91.2%~96.9%, a voltage efficiency of 83.3%~87.1% and an energy efficiency of 75.97%~84.40%. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 The infrared spectra of MS-PC and B-HC prepared in Example 1 are shown.
[0024] Figure 2 The image shows a scanning electron microscope image of the MS-PC prepared in Example 1.
[0025] Figure 3 This is a scanning electron microscope image of B-HC prepared in Example 1. Detailed Implementation
[0026] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0027] It should be noted that the process equipment or apparatus not specifically mentioned in the following embodiments are all conventional equipment or apparatus in the art.
[0028] It should be noted that the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products, or apparatuses. Furthermore, unless otherwise stated, the numbering of each method step is merely a convenient tool for identifying each method step, and not intended to limit the order of the method steps or define the scope of the invention. Changes or adjustments to their relative relationships, without substantially altering the technical content, should also be considered within the scope of the invention.
[0029] Existing membrane materials for zinc-bromine flow batteries have long faced core challenges, including self-discharge caused by bromine penetration on the positive electrode side and short circuits caused by zinc dendrite growth on the negative electrode side. Traditional membranes, due to their uneven pore size distribution, cannot effectively block bromine penetration and lack mechanisms to inhibit zinc dendrite growth. While ceramic membranes can physically block bromine penetration, their high brittleness and low ionic conductivity make them unsuitable for practical applications. Some improved solutions use metal-organic framework materials to prepare membranes, but these rely on a single pore size sieving mechanism and do not introduce chemical adsorption or catalytic functions, thus limiting their bromine blocking effect and failing to inhibit zinc dendrite growth.
[0030] To overcome the above problems, this invention coats the positive and negative sides of the microporous membrane with an MS-PC coating and a B-HC coating, respectively. Studies have found that the MS-PC coating, due to the pore size sieving effect generated by its microporous structure, can directly block Br2 and Br3. - The penetration of large molecular active bromine species enhances the bromine barrier capacity of the microporous membrane; the incorporation of S atoms into aromatic rings in the MS-PC coating causes local charge redistribution, forming electron-deficient and electron-rich regions, thus enabling Br... - More easily adsorbed and activated by electron-deficient regions, Br2 / Br3 - By forming weak coordination with electron-rich regions, the activation energy of the reaction is lowered, the bromine oxidation-reduction kinetics are accelerated, and the catalytic activity is enhanced. The B-HC coating can homogenize the electric field distribution, regulate zinc deposition behavior, and inhibit the growth and damage of zinc dendrites.
[0031] Specifically, the method for preparing a microporous membrane based on MS-PC and B-HC modification provided by this invention includes: Mustard seed powder was subjected to a hydrothermal reaction to obtain a hydrothermal carbon precursor; the hydrothermal carbon precursor was pyrolyzed to obtain a carbonized product; the carbonized product was chemically activated with an activator to obtain MS-PC. Bamboo powder was subjected to a hydrothermal carbonization reaction to obtain B-HC; MS-PC was coated on the positive electrode side of the microporous membrane to form an MS-PC coating; B-HC was coated on the negative electrode side of the microporous membrane to form a B-HC coating, thus obtaining a microporous membrane modified with MS-PC and B-HC.
[0032] The preparation method of MS-PC includes three core steps: hydrothermal reaction, pyrolysis carbonization, and chemical activation pore formation. First, mustard seeds are subjected to a hydrothermal reaction to obtain a hydrothermal carbon precursor; the hydrothermal carbon precursor is pyrolyzed to decompose organic matter and initially form a carbon skeleton; the carbonized product after pyrolysis is activated with an activator, during which the activator etches the carbon skeleton to produce a hierarchical porous structure containing abundant micropores and mesopores.
[0033] When applied to zinc-bromine flow batteries, the micropores in MS-PC allow for the production of small-sized ions (Br₂). - and Zn 2+ The active bromine species (Br2 / Br3) generated at the positive electrode are passed through, thus allowing them to pass through. - The bromine species are "locked" inside the channels and cage-like cavities, utilizing the pore size sieving effect to hinder the penetration of large molecular active bromine species. This physical confinement prevents the diffusion of active bromine species to the negative electrode, thereby reducing self-discharge, improving coulombic efficiency, and significantly reducing capacity loss. Furthermore, MS-PC contains a large amount of CSC and -SO₄ compounds. x The presence of polar functional groups such as -COOH can lead to strong chemisorption of active bromine species, forming a dual "adsorption-confinement" barrier with physical confinement, significantly reducing bromine permeation and improving coulombic efficiency. Simultaneously, during MS-PC preparation, the natural sulfur-containing groups of mustard seeds break down, releasing CSC and C-SO4 groups. x When S replaces some C atoms in an aromatic ring, the S atom is larger and has more outer electrons. When S replaces C in the aromatic ring, the electron cloud distribution of the CSC bond differs from that of the CCC bond. Electrons shift towards S or rearrange around it, disrupting the originally uniform electron cloud and creating localized electron-rich and electron-deficient regions. - (Negatively charged) are more easily adsorbed and activated by electron-deficient regions, Br2 / Br3 - It can form weak coordination with electron-rich regions, which is beneficial for desorption and transformation; thereby reducing the bromine / bromine ratio (Br2 / Br). - The activation energy of the reaction accelerates the reaction of bromine / bromine (Br2 / Br) -Redox kinetics. The conductive carbon framework of MS-PC allows electrons to reach the reaction interface in a timely manner, accelerating the reaction of Br. - The charge transfer process of oxidation and Br2 reduction reduces the bromine / bromine ratio (Br2 / Br). - The activation energy of the reaction is reduced, the activation overpotential is decreased, and the problem of slow bromine kinetics is overcome.
[0034] Furthermore, MS-PC possesses both wettability and a hierarchical porous structure, which can accelerate ion transport. Specifically, after coating the positive electrode side of the microporous membrane with MS-PC, the surface polar functional groups (-OH, -COOH, CSC, etc.) can enhance the affinity for electrolytes (containing Br₂)... - Zn 2+ H + The wettability of MS-PC (including H2O) allows the electrolyte to spread and penetrate the porous network of the MS-PC coating, rather than forming gaps at the interface or flowing only along the surface. Furthermore, the hierarchical pores (micropore confinement + mesoporous channels) of MS-PC provide a continuous, short-range diffusion path for ions, reducing concentration polarization. Simultaneously, the MS-PC coating can make close contact with the bipolar plates of the positive electrode, filling some of the voids and making it easier for electrons to cross the interface between the positive electrode and the microporous membrane, thereby reducing the contact resistance at the interface and decreasing overall ohmic polarization. As a carbon-based material, MS-PC possesses similar intrinsic resistance to bromine corrosion, is not easily etched through by Br2, and can maintain the stability of the positive electrode interface during long-term cycling, delaying the performance degradation of the microporous membrane.
[0035] B-HC retains abundant oxygen-containing functional groups derived from bamboo powder cellulose, hemicellulose, and lignin during hydrothermal processing, including hydroxyl (-OH), carboxyl (-COOH), and carbonyl (C=O) groups. The -OH and -COOH functional groups on the B-HC surface can interact with Zn. 2+ Weak coordination occurs, forming an ion buffer layer: the ion buffer layer in Zn 2+ Temporary complexation of Zn at high concentrations 2+ In Zn 2+ Zn is replenished by releasing it at low concentrations. 2+ The ion buffer layer smooths the Zn interface. 2+ Concentration fluctuations lead to a more uniform deposition current density distribution, which indirectly results in a more uniform interfacial electric field distribution. This uniform electric field distribution, along with the ion concentration field, promotes the deposition of Zn. 2+ Simultaneous and equal-probability nucleation occurs at all interfaces, increasing the number and uniform distribution of nucleation sites, fundamentally suppressing the initial nucleation of zinc dendrites caused by local supersaturation. B-HC can guide Zn... 2+ The B-HC coating smooths the deposition and buffers the risk of diaphragm puncture during the zinc deposition growth stage, enabling Zn... 2 + The diffusion field around the crystal nucleus is more symmetrical, weakening the tip effect and guiding Zn.2+ The B-HC coating preferentially fills the recessed areas between crystal nuclei, promoting a smoother zinc deposition layer. Even if a small number of zinc dendrites sprout, B-HC can disperse the mechanical stress at the dendrite tips, delaying their penetration into the microporous membrane. Through full-chain intervention in the nucleation, growth, and penetration stages, the B-HC coating effectively inhibits the growth and damage of zinc dendrites, extending the cycle life of the zinc-bromine flow battery.
[0036] The oxygen-containing functional groups in B-HC are polar functional groups, giving B-HC a strongly hydrophilic surface. When coated on the negative electrode side of a microporous membrane, it significantly reduces the contact angle between the electrolyte and the microporous membrane, allowing the electrolyte to spread evenly on the microporous membrane surface and penetrate into the pores of the B-HC coating. This eliminates interfacial air gaps, reduces interfacial ion transport impedance, and decreases overall ohmic polarization, thereby improving the voltage and energy efficiency of the zinc-bromine flow battery. The excellent hydrophilicity of B-HC enables the electrolyte to form a continuous liquid film on the negative electrode side of the microporous membrane, avoiding poor wettability and localized current density concentration caused by hydrophobic surfaces.
[0037] To obtain an ideal hierarchical porous structure and sulfur doping state to enhance bromine inhibition and catalytic performance, the pyrolysis temperature during the MS-PC preparation process of this invention is preferably 700~900℃, more preferably 700~850℃, for example, 700℃, 750℃, 800℃, 850℃, or 900℃. Within this temperature range, carbonization can be effectively achieved, and the doping form and content of sulfur in the carbon framework can be controlled.
[0038] In the MS-PC preparation process of this invention, the activator used can be H3PO4. H3PO4 can effectively create pores, forming abundant micropores and mesopores.
[0039] Exemplary preparation method of MS-PC of the present invention includes: washing mustard seeds to remove impurities, drying and mechanically pulverizing them into uniform powder; mixing the powder with water and carrying out hydrothermal reaction at 170~230℃ for 8~12h, naturally cooling and washing until neutral, drying to obtain hydrothermal carbon precursor; placing the hydrothermal carbon precursor in a tube furnace and heating under an inert atmosphere (N2 or Ar) to 700~900℃ at a heating rate of 2~5℃ / min, and holding for pyrolysis for 1~3h; grinding and mixing the obtained carbonized product with activator H3PO4 at a mass ratio of 1:(3~5), placing the resulting mixed powder again under an inert atmosphere and heating to 700~900℃ for 1~2h, rinsing repeatedly with deionized water until the pH of the filtrate is ≈7, and finally vacuum drying at 70~90℃ for 8~10h to obtain MS-PC powder.
[0040] To achieve a suitable degree of carbonization and retain sufficient surface functional groups, the bamboo powder is subjected to a hydrothermal carbonization reaction as described in this invention. The hydrothermal carbonization reaction temperature is 170~230℃, more preferably 170~210℃, for example, 170℃, 190℃, 210℃, or 230℃. Within this temperature range, the bamboo powder can be fully carbonized, while a large number of polar functional groups such as hydroxyl (-OH) and carboxyl (-COOH) groups on its surface are retained, ensuring the hydrophilicity of B-HC and its coordination ability with zinc ions.
[0041] Exemplary preparation method of B-HC of the present invention includes: selecting dried bamboo, removing surface mud and impurities, repeatedly washing with deionized water, drying in an oven at 60~80℃ until constant weight, pulverizing the dried bamboo with a pulverizer, and passing it through a 40~100 mesh sieve to obtain uniform bamboo powder for later use; adding bamboo powder to potassium hydroxide solution according to a set solid-liquid ratio of bamboo powder:potassium hydroxide solution (mass fraction of 3.0%) = 1:(5~10) (w / w), and magnetically stirring for 30~60 minutes to fully mix the bamboo powder and potassium hydroxide solution to form a uniform suspension, avoiding significant sedimentation or agglomeration; transferring the suspension to a reaction vessel, first introducing a small amount of inert gas N2 to remove air from the reaction vessel, and then sealing the reaction vessel. To ensure good airtightness, the reactor was heated to 170-230℃ and kept at this temperature for 10-12 hours. During this time, bamboo powder underwent hydrolysis, dehydration, decarboxylation, and condensation reactions in a hydrothermal environment, gradually forming amorphous carbon. After the reaction, the mixture was allowed to cool naturally to room temperature. The reactor was then opened, and the black suspension was removed and centrifuged at 4000-8000 rpm for solid-liquid separation. The resulting solid was repeatedly washed with deionized water until the filtrate pH was approximately 7 and no obvious soluble organic matter remained. The wet product obtained after washing was dried in a vacuum or forced-air drying oven at 70-90℃ for 8-10 hours, then ground and passed through a 100-200 mesh sieve to obtain uniform and fine B-HC powder. Potassium hydroxide in the potassium hydroxide solution was used as an activator.
[0042] To balance the functionality and ionic conductivity of the MS-PC coating and the B-HC coating, the MS-PC loading on the positive electrode side of the microporous membrane is 0.4~5.3 mg / cm³. 2 More preferably 0.4~4.0 mg / cm³ 2 The loading of B-HC on the negative electrode side of the microporous membrane is 0.2~1.0 mg / cm³. 2 More preferably, it is 0.2~0.8 mg / cm³. 2 Within the aforementioned load range, the MS-PC coating and B-HC coating can fully exert their physicochemical effects without significantly increasing the ohmic impedance due to excessive thickness or blockage of the microporous membrane channels.
[0043] To form a uniform and stable coating, MS-PC is coated onto the positive electrode side of a microporous membrane using a vacuum adsorption method. Specifically, this involves: preparing an MS-PC dispersion using water; adding the MS-PC dispersion dropwise to the positive electrode side of the microporous membrane; allowing it to stand; and then drying. For example, the microporous membrane is laid flat on a vacuum adsorption stage with an adsorption pressure of -0.10 MPa. The MS-PC dispersion is then slowly added dropwise to the positive electrode side of the microporous membrane using a pipette. After standing for 30 minutes, the membrane is placed in a vacuum drying oven at 50–60°C and dried for 12–24 hours to form the MS-PC coating.
[0044] Similarly, B-HC is coated onto the negative electrode side of a microporous membrane using a vacuum adsorption method. Specifically, B-HC is prepared into a B-HC dispersion using water; the B-HC dispersion is then added dropwise to the negative electrode side of the microporous membrane, allowed to stand, and then dried. For example, the microporous membrane is laid flat on a vacuum adsorption stage with an adsorption pressure of -0.10 MPa. The B-HC dispersion is drawn up using a pipette and slowly added dropwise to the negative electrode side of the microporous membrane. After standing for 30 minutes, it is placed in a vacuum drying oven at 50-60°C and dried for 12-24 hours to form a B-HC coating.
[0045] The microporous membrane used in this invention is a commercially available microporous membrane, such as a PP membrane, a PE membrane, or a polyolefin composite membrane. These microporous membranes are low in cost and have good mechanical properties, making them ideal matrix materials. Specifically, the microporous membrane used in the embodiments of this invention is a PP membrane with a size of 3.5cm × 3.5cm, a thickness of 0.6mm, a thickness uniformity of <3%, and an average pore size of <20nm.
[0046] Preferably, before coating MS-PC and B-HC, the microporous membrane is pretreated by ultrasonically cleaning it with ethanol or deionized water for 10-15 minutes to remove impurities and contaminants from the surface, and then drying it in a vacuum drying oven at 60-65°C for 10-12 hours.
[0047] The microporous membrane based on MS-PC and B-HC modification prepared by the method described above in this invention includes a microporous membrane, wherein the positive electrode side and the negative electrode side of the microporous membrane are coated with MS-PC coating and B-HC coating, respectively.
[0048] The present invention also provides a zinc-bromine flow battery, using the aforementioned microporous membrane based on MS-PC and B-HC modification as the membrane material.
[0049] The zinc-bromine flow battery has a coulombic efficiency of 91.2% to 96.9%, a voltage efficiency of 83.3% to 87.1%, and an energy efficiency of 75.97% to 84.40%.
[0050] Example 1 Step 1: Pretreatment of the microporous membrane: The microporous membrane is ultrasonically cleaned with ethanol for 10 minutes to remove surface impurities and contaminants, and then dried in a vacuum drying oven at 60℃ for 12 hours for later use. The microporous membrane is a PP membrane with dimensions of 3.5cm × 3.5cm, a thickness of 0.6mm, a thickness uniformity of <3%, and an average pore size of <20nm.
[0051] Step 2: Wash 50g of mustard seeds with deionized water to remove impurities, dry at 60℃ for 24h, then mechanically pulverize into a uniform powder and pass through an 80-mesh sieve. Weigh 20g of the sieved powder and add it to a stainless steel reactor with a polytetrafluoroethylene liner at a mass ratio of 1:7. Perform a hydrothermal reaction at 210℃ for 8h. After natural cooling, wash with deionized water until neutral and dry to obtain the hydrothermal carbon precursor. Place the hydrothermal carbon precursor in a tube furnace and heat under a N2 atmosphere at a heating rate of 3℃ / min to the pyrolysis temperature of 700℃, holding for 2h. The obtained carbonized product was ground and mixed with activator H3PO4 at a mass ratio of 1:3. The resulting mixed powder was placed under N2 atmosphere and heated to 800℃ for 1h for activation. After activation, it was repeatedly washed with deionized water until the pH of the filtrate was ≈7. Finally, it was vacuum dried at 70℃ for 10h to obtain MS-PC powder, and a 1.0mg / mL MS-PC dispersion was prepared with deionized water.
[0052] Step 3: Spread the pretreated microporous membrane flat on a vacuum adsorption stage with an adsorption pressure of -0.10 MPa. Use a pipette to take 5 mL of 1.0 mg / mL MS-PC dispersion and slowly add it dropwise to the positive electrode side of the microporous membrane. Let it stand for 30 min and then place it in a vacuum drying oven at 60 °C for 12 h to form an MS-PC coating on the positive electrode side of the microporous membrane, thus obtaining an MS-PC modified microporous membrane.
[0053] Step 4: Select 200g of dried bamboo, wash with deionized water, and dry in an 80℃ oven until constant weight. Crush the dried bamboo using a pulverizer and pass through an 80-mesh sieve to obtain uniform bamboo powder for later use. Weigh 15g of bamboo powder and add it to the potassium hydroxide solution at a solid-liquid ratio of 1:7 (w / w) using a 3.0% potassium hydroxide solution. Stir magnetically for 60 minutes. Transfer the resulting suspension to a stainless steel reactor with a polytetrafluoroethylene liner. First, purge the reactor with inert gas (N2) to remove air, then seal the reactor. Place the reactor in a forced-air drying oven and set the hydrothermal carbonization reaction temperature to 170℃. Maintain the reaction at 170℃ for 12 hours. After the reaction, allow it to cool naturally to room temperature. Remove the resulting black suspension and centrifuge at 6000 rpm for solid-liquid separation. Wash the obtained solid repeatedly with deionized water until the filtrate pH ≈ 7. The washed solid product was placed in a vacuum drying oven and dried at 80°C for 10 hours. Then it was ground with an agate mortar and pestle, passed through a 160-mesh sieve, and prepared into a 0.5 mg / mL B-HC dispersion with deionized water.
[0054] Step 5: The MS-PC modified microporous membrane is laid flat on a vacuum adsorption stage with an adsorption pressure of -0.10 MPa. 5 mL of 0.5 mg / mL B-HC dispersion is slowly added dropwise to the negative electrode side of the MS-PC modified microporous membrane using a pipette. After standing for 30 min, it is placed in a vacuum drying oven at 60 °C for 12 h to form a B-HC coating on the negative electrode side of the microporous membrane, thus obtaining a microporous membrane based on MS-PC and B-HC modification.
[0055] Example 2 It is basically the same as Example 1, except that the concentration of the MS-PC dispersion prepared in step 2 is 4.0 mg / mL.
[0056] Example 3 It is basically the same as Example 1, except that the concentration of the MS-PC dispersion prepared in step 2 is 7.0 mg / mL.
[0057] Example 4 It is basically the same as Example 1, except that the concentration of the MS-PC dispersion prepared in step 2 is 10.0 mg / mL.
[0058] Example 5 It is basically the same as Example 1, except that the concentration of the MS-PC dispersion prepared in step 2 is 13.0 mg / mL.
[0059] Example 6 It is basically the same as Example 1, except that the pyrolysis temperature in step 2 is 750°C and the concentration of MS-PC dispersion is 10.0 mg / mL.
[0060] Example 7 It is basically the same as Example 1, except that the pyrolysis temperature in step 2 is 800°C and the concentration of MS-PC dispersion is 10.0 mg / mL.
[0061] Example 8 It is basically the same as Example 1, except that the pyrolysis temperature in step 2 is 850°C and the concentration of MS-PC dispersion is 10.0 mg / mL.
[0062] Example 9 It is basically the same as Example 1, except that the pyrolysis temperature in step 2 is 900°C and the concentration of MS-PC dispersion is 10.0 mg / mL.
[0063] Example 10 It is basically the same as Example 8, except that the concentration of B-HC dispersion in step 4 is 1.0 mg / mL.
[0064] Example 11 It is basically the same as Example 8, except that the concentration of B-HC dispersion in step 4 is 1.5 mg / mL.
[0065] Example 12 It is basically the same as Example 8, except that the concentration of B-HC dispersion in step 4 is 2.0 mg / mL.
[0066] Example 13 It is basically the same as Example 8, except that the concentration of B-HC dispersion in step 4 is 2.5 mg / mL.
[0067] Example 14 It is basically the same as Example 8, except that the hydrothermal carbonization reaction temperature in step 4 is 190°C and the concentration of B-HC dispersion is 2.0 mg / mL.
[0068] Example 15 It is basically the same as Example 8, except that the hydrothermal carbonization reaction temperature in step 4 is 210°C and the concentration of B-HC dispersion is 2.0 mg / mL.
[0069] Example 16 It is basically the same as Example 8, except that the hydrothermal carbonization reaction temperature in step 4 is 230°C and the concentration of B-HC dispersion is 2.0 mg / mL.
[0070] Comparative Example 1 Comparative Example 1 only performed step 1 of Example 1, thus obtaining a microporous membrane without MS-PC and B-HC modification.
[0071] Figure 1 The infrared spectra of MS-PC and B-HC prepared in Example 1 are shown. Figure 1 It can be seen that for MS-PC, 700~710cm -1 The characteristic peak at 1120–1200 cm⁻¹ belongs to the CSC of thiophene. -1 The characteristic peak at that location is attributed to the sulfonyl group (-SO). x ), 1210~1320cm -1 The characteristic peak at 3200–3600 cm⁻¹ is attributed to CO in the carboxyl group; for β-HC, the peak is 3200–3600 cm⁻¹. -1 The characteristic peak at 1650~1700 cm⁻¹ is attributed to the hydroxyl group (-OH). -1 The characteristic peak at 1210~1320 cm⁻¹ is attributed to the C=O group in the ester group. -1 The characteristic peak at that location is attributed to CO in the carboxyl group.
[0072] Figure 2 The image shows a scanning electron microscope image of the MS-PC prepared in Example 1. As can be seen from the image, the surface morphology of the MS-PC material is irregular, with a large number of pores of different sizes distributed on it. The overall structure is composed of pores of various sizes.
[0073] Figure 3 The image shows a scanning electron microscope image of B-HC prepared in Example 1. As can be seen from the image, the overall morphology of the B-HC material is relatively smooth, with a certain regular shape, as well as certain pores and textures.
[0074] To test the performance of the microporous membranes in Examples 1-16 and Comparative Example 1, zinc-bromine flow batteries were assembled using conventional electrode materials and electrolyte systems found in zinc-bromine flow batteries. The electrodes were commercially available carbon-plastic bipolar plates with an electrode area of 9 cm². 2 The electrolyte was a 2.0 mol / L zinc bromide aqueous solution, containing 2 mol / L potassium chloride and 0.2 mol / L 1-methyl-1-ethylpyrrolidine ammonium bromide. Charge-discharge tests were performed on a battery testing system with a charge-discharge rate of 20 mA / cm². 2 The charging time was 2 hours and the test temperature was 25°C. The synthesis conditions of the microporous membranes obtained in different embodiments are shown in Table 1. The electrochemical performance test results of the zinc-bromine flow batteries corresponding to the microporous membranes obtained in different embodiments are shown in Table 2.
[0075] Table 1 Synthesis conditions of microporous membranes in different embodiments
[0076] Table 2 Electrochemical performance of zinc-bromine flow batteries corresponding to microporous membranes obtained in different embodiments
[0077] As can be seen from Table 2, Examples 1-16 all exhibited better electrochemical performance than Comparative Example 1. That is, the microporous membranes modified with MS-PC and B-HC showed better electrochemical performance as zinc-bromine flow battery membranes than the unmodified microporous membranes. This indicates that MS-PC and B-HC help improve the voltage efficiency, coulombic efficiency, and energy efficiency of zinc-bromine flow batteries. Furthermore, it shows that the microporous membranes modified with MS-PC and B-HC have a significant impact on improving bromine inhibition, accelerating the bromine kinetic reaction rate, and inhibiting zinc dendrite formation.
[0078] Comparing Examples 1-5, it can be seen that, under the same conditions, within a certain concentration range, the electrochemical performance of the zinc-bromine flow battery gradually improves with increasing MS-PC dispersion concentration. This indicates that the introduction of MS-PC has a significant impact on improving bromine inhibition capacity, accelerating bromine kinetics, and reducing ohmic internal resistance. However, when the MS-PC dispersion concentration exceeds 10.0 mg / mL, the electrochemical performance of the zinc-bromine flow battery decreases. This may be because the MS-PC coating is too thick and carbon particles penetrate into the micropores of the microporous membrane surface, partially blocking the intrinsic ion channels of the microporous membrane. + Zn 2+ ,Br - Increased migration resistance exacerbates concentration polarization.
[0079] Comparing Examples 4 and 6-9, it can be seen that the zinc-bromine flow battery corresponding to Example 8 exhibits the best energy efficiency, voltage efficiency, and coulombic efficiency, demonstrating better electrochemical performance. In other words, as the pyrolysis temperature during MS-PC preparation increases, the electrochemical performance (including energy efficiency, voltage efficiency, and coulombic efficiency) of the corresponding zinc-bromine flow battery first increases and then decreases. This indicates that increasing the pyrolysis temperature during MS-PC preparation has a significant impact on improving bromine inhibition capability, accelerating the bromine kinetic reaction rate, and reducing ohmic internal resistance. However, when the pyrolysis temperature during MS-PC preparation exceeds 850℃, it may cause carbon wall sintering, micropores merging into macropores or closed pores, effectively sieving Br2 / Br3. - The pore size distribution is disrupted, the physical barrier to bromine decreases, and the retention rate of sulfur at 900℃ also decreases, which affects the extent to which the bromine kinetic reaction rate increases.
[0080] Comparing Examples 10-13 with Example 8, it can be seen that, under the same conditions, within a certain concentration range, the electrochemical performance (including energy efficiency, voltage efficiency, and coulombic efficiency) of the zinc-bromine flow battery gradually improves with increasing B-HC dispersion concentration. This indicates that the addition of B-HC has a significant impact on the ability of the microporous membrane to suppress zinc dendrites and reduce ohmic resistance. However, when the B-HC dispersion concentration exceeds 2.0 mg / mL, the electrochemical performance of the zinc-bromine flow battery decreases. This may be because excessive B-HC microspheres penetrate into the micropores on the surface of the microporous membrane, filling the pores and compressing the originally reasonable pore size distribution of the microporous membrane, increasing the tortuosity of ion transport and exacerbating concentration polarization.
[0081] Comparing Examples 12 and 14-16, it can be seen that the zinc-bromine flow battery corresponding to Example 15 has the best electrochemical performance. That is, as the hydrothermal carbonization reaction temperature used in the preparation of B-HC increases, the coulombic efficiency, voltage efficiency, and energy efficiency of the zinc-bromine flow battery corresponding to the modified microporous membrane first increase and then decrease. This indicates that increasing the hydrothermal carbonization reaction temperature during the B-HC preparation process has a significant impact on improving the ability of the microporous membrane to suppress zinc dendrites and reducing ohmic resistance. However, when the hydrothermal carbonization reaction temperature during the B-HC preparation process is too high, -COOH and some -OH are easily decarboxylated / dehydrated, causing a decrease in surface polarity and hydrophilicity, as well as its interaction with Zn. 2+ The weakened coordination ability is not conducive to uniform nucleation and the formation of ion buffer layers; the higher hydrothermal carbonization reaction temperature also intensifies the condensation inside B-HC microspheres, partially closes the pores, and reduces the specific surface area, which has an adverse effect on electrochemical performance.
[0082] In summary, this invention effectively improves bromine permeation and slow bromine kinetics by modifying the positive electrode side of the microporous membrane with MS-PC, accelerating bromine conversion and reducing side reactions. Furthermore, modifying the negative electrode side of the microporous membrane with B-HC further optimizes the electric field distribution and prevents localized deposition, thereby improving zinc dendrite growth. The synergistic effect of MS-PC and B-HC comprehensively enhances the bromine barrier performance, bromine reaction kinetics, and zinc dendrite suppression of the microporous membrane.
[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a microporous membrane based on MS-PC and B-HC modification, characterized in that, include: Mustard seed powder was subjected to a hydrothermal reaction to obtain a hydrothermal carbon precursor; the hydrothermal carbon precursor was then pyrolyzed to obtain carbonized products. The carbonization product was chemically activated using an activating agent to obtain MS-PC; the MS-PC has a hierarchical porous structure of micropores and mesopores. Bamboo powder was subjected to a hydrothermal carbonization reaction to obtain B-HC; MS-PC was coated on the positive electrode side of the microporous membrane, and B-HC was coated on the negative electrode side of the microporous membrane to obtain a microporous membrane modified with MS-PC and B-HC.
2. The method for preparing a microporous membrane based on MS-PC and B-HC modification according to claim 1, characterized in that, The pyrolysis temperature is 700~900℃.
3. The method for preparing a microporous membrane based on MS-PC and B-HC modification according to claim 1, characterized in that, The activator is H3PO4.
4. The method for preparing a microporous membrane based on MS-PC and B-HC modification according to claim 1, characterized in that, The bamboo powder is subjected to a hydrothermal carbonization reaction at a temperature of 170~230℃.
5. The method for preparing a microporous membrane based on MS-PC and B-HC modification according to claim 1, characterized in that, The MS-PC loading on the positive electrode side of the microporous membrane is 0.4~5.3 mg / cm³. 2 The loading of B-HC on the negative electrode side of the microporous membrane is 0.2~1.0 mg / cm³. 2 .
6. The method for preparing a microporous membrane based on MS-PC and B-HC modification according to claim 1, characterized in that, The process of coating MS-PC onto the positive electrode side of the microporous membrane specifically involves: preparing an MS-PC dispersion using water; adding the MS-PC dispersion dropwise onto the positive electrode side of the microporous membrane; and allowing it to stand before drying.
7. The method for preparing a microporous membrane based on MS-PC and B-HC modification according to claim 1, characterized in that, The process of coating B-HC onto the negative electrode side of the microporous membrane specifically involves: preparing a B-HC dispersion using water; adding the B-HC dispersion dropwise onto the negative electrode side of the microporous membrane; and allowing it to stand before drying.
8. The method for preparing a microporous membrane based on MS-PC and B-HC modification according to claim 1, characterized in that, The microporous membrane is a polypropylene membrane, a polyethylene membrane, or a polyolefin composite membrane.
9. A microporous membrane based on MS-PC and B-HC modification obtained by the preparation method according to any one of claims 1 to 8.
10. A zinc-bromine flow battery, characterized in that, Includes the microporous membrane based on MS-PC and B-HC modification as described in claim 9.
Citation Information
Patent Citations
Antibiotic, flame-resistant and environmentally-friendly wood plastic material used for intelligent homed device installation
CN105924816A
Functional composite membrane for zinc-bromine flow battery as well as preparation and application of functional composite membrane
CN116154206A