A cascaded formation method for grid-connected energy storage batteries
By controlling the reaction sequence of additives and main solvent through a step-by-step formation method, the problems of uneven interfacial film and gas retention during the formation of thick electrode energy storage batteries are solved, forming a dense and uniform solid electrolyte interfacial film, which improves the cycle life and safety of the battery.
Patent Information
- Application Number
- CN202611443318.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2046-09-17
AI Technical Summary
In the formation process of large-capacity thick-electrode energy storage batteries, existing processes have difficulty controlling the reaction sequence of additives and main solvents, resulting in uneven interfacial film composition, severe gas retention and local lithium plating, which affect the long-term cycle life and safety of the battery.
By employing a tiered formation method, a uniform solid electrolyte interface film is formed by controlling temperature and pre-tightening pressure, applying a constant micro-current and a gradient current, and monitoring and adjusting the charging current in real time, thereby reducing gas retention and local lithium plating.
This technology enables stepwise reactions between additives and the main solvent within thick electrodes, forming a dense and uniform solid electrolyte interface film. This reduces charge transfer resistance, decreases the risk of localized lithium plating, and improves the battery's long-term capacity retention and safety.
Smart Images

Figure CN122950639B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrochemical energy storage battery manufacturing technology, and specifically to a cascaded formation method for grid energy storage batteries. Background Technology
[0002] Lithium iron phosphate secondary batteries are commonly used energy storage devices in electrochemical energy storage. Their cycle life and operational safety directly affect the application value of energy storage power stations. In order to improve the energy density of the cells and reduce manufacturing costs, energy storage cells usually adopt a large-capacity, thick electrode design. In the battery manufacturing process, the formation process is to cause the electrolyte to undergo an electrochemical reduction reaction on the surface of the negative electrode under the action of an external electric field and form a solid electrolyte interface film. Whether the interface film is dense and whether the composition is uniform will directly affect the interface charge transfer impedance and the long-term cycle life of the battery.
[0003] Thick electrodes have tortuous internal pores and significant solid-liquid mass transfer resistance. During conventional stepped constant current charging, mass transfer lag and polarization potential differences are likely to occur along the thickness of the electrode. The film-forming additives in the electrolyte have different intrinsic reduction potentials from the main solvent. As charging continues, the local potential of the electrode surface may enter the decomposition range of the main solvent earlier, while the additives in the deep pores are limited by diffusion and have not yet fully reacted. This results in uneven composition of the interface film at different locations. If the rate at which the main solvent decomposes and produces gaseous byproducts exceeds the rate at which gas escapes from the porous electrode, the gas is likely to be trapped between electrode layers and in the pores, forming local gas barrier regions. This, in turn, affects ion transport and induces local lithium plating. To address these issues, existing processes typically improve the situation by reducing the charging rate or extending the resting time. However, fixed parameters cannot reflect the real-time changes in the internal reaction state of the battery and will also significantly extend the manufacturing cycle.
[0004] Therefore, for large-capacity thick-electrode energy storage batteries, the technical problem to be solved by this invention is how to control the reaction sequence of additives and main solvents, and adjust the charging current and relaxation process according to the transient polarization state, so as to reduce gas retention and local lithium plating, while forming a solid electrolyte interface film with relatively uniform composition and low impedance at different depths of the thick electrode. Summary of the Invention
[0005] This invention provides a tiered formation method for grid energy storage batteries to solve the problems of uneven phase interface composition, internal gas phase retention, and local lithium plating caused by uncontrolled reaction timing and polarization accumulation during the formation process of large-capacity thick electrode energy storage batteries.
[0006] This invention proposes a cascaded formation method for grid energy storage batteries, comprising the following steps:
[0007] Step S101: Control the energy storage battery to be formed to be in an environment with a temperature of 40°C to 50°C and a pre-tightening pressure of 0.1MPa to 0.3MPa, and apply a constant micro-current of 0.010C to 0.025C to charge it to the first cutoff potential of 2.00V to 2.20V and then cut off.
[0008] Step S102: Apply gradient current to continue charging, collect the charged capacity and closed-circuit voltage of the battery to be formed online, and calculate the differential capacity. When the differential capacity exceeds the characteristic reduction peak of the additive in the potential range of 2.20V to 2.55V and drops to 60% to 70% of the peak intensity, it enters the open-circuit relaxation state. Relaxation is terminated when the open-circuit voltage recovery rate is lower than or equal to 0.10mV / min and the open-circuit relaxation time reaches 5min to 15min. Record the open-circuit reference voltage at the termination time.
[0009] Step S103: Apply a stepped increasing current to charge within the potential range of 2.55V to 3.10V, and calculate the apparent polarization voltage drop between the current closed-circuit voltage and the open-circuit reference voltage in real time during each step charging process. When the apparent polarization voltage drop exceeds the upper limit threshold of polarization of 40mV to 50mV, reduce the current step current by 15% to 20% until the closed-circuit voltage reaches the second cutoff potential of 3.10V.
[0010] In step S104, a main charging current of 0.150C to 0.200C is applied to charge the battery at a constant current until the upper limit cutoff potential of 3.35V to 3.72V is reached, and then constant voltage charging is switched to continue until the charging current decays to the cutoff current threshold of 0.016C to 0.022C, at which point charging is terminated.
[0011] In step S105, the charged energy storage battery to be formed is left to stand in an open circuit in a constant temperature environment. After the gaseous byproducts are discharged, it is sealed under negative pressure and discharged at a constant current of 0.190C to 0.210C until the lower limit cutoff voltage of 2.25V to 2.51V is reached.
[0012] Preferably, in step S101, before the energy storage battery to be formed is placed in an environment with a temperature of 40°C to 50°C and a pre-tightening pressure of 0.1MPa to 0.3MPa, an electrolyte is injected and the battery is allowed to stand and soak at 40°C to 50°C for 22h to 25h; during the charging process in step S101, the pre-tightening pressure is controlled at 0.12MPa to 0.22MPa, the temperature at 40°C to 50°C, the constant micro-current at 0.018C to 0.025C, the first cutoff potential at 2.05V to 2.20V, and the charging duration at 2.0h to 2.5h.
[0013] Preferably, in step S102, the initial current of the gradient current boost is set to 0.020C to 0.030C, and the current is boosted to 0.050C in a linear rate of 0.002C to 0.005C per minute. Within the potential range of 2.20V to 2.55V, the characteristic electrochemical reduction peak of the film-forming additive is identified by differential capacity. When the charging voltage reaches 2.38V to 2.48V and the differential capacity exceeds the characteristic reduction peak of the additive and decreases to 60% to 70% of the characteristic reduction peak of the additive, the applied charging current is cut off and the system enters an open-circuit relaxation state.
[0014] Preferably, in step S102, the duration of the open-circuit relaxation state is set to 5 min to 15 min; in the open-circuit relaxation state, the open-circuit voltage is collected in real time and its rate of change over time is calculated. When the absolute value of the rate of change decreases to the range of 0.05 mV / min to 0.10 mV / min, the relaxation is terminated, and the open-circuit reference voltage is read and stored at the termination time as the reference potential for calculating the apparent polarization voltage drop in step S103.
[0015] Preferably, in step S103, the potential range of 2.55V to 3.10V is the main solvent decomposition potential range, and the step-increasing current includes a first step current of 0.045C to 0.051C, a second step current of 0.076C to 0.082C, and a third step current of 0.113C to 0.121C applied sequentially; the switching voltage node of each step current is set as follows: when the first step current is charged to the closed-circuit voltage of 2.65V to 2.80V, the second step current is switched; when the second step current is charged to the closed-circuit voltage of 2.88V to 2.96V, the third step current is switched.
[0016] Preferably, in step S103, the apparent polarization voltage drop is the difference between the closed-circuit voltage and the open-circuit reference voltage at the current sampling time; during each step current charging process, when the apparent polarization voltage drop exceeds 45mV, the setting value of the current step current level is reduced by 15% to 20%, and the reduced current is maintained to continue charging to the corresponding switching voltage node or the second cutoff potential of 3.10V.
[0017] Preferably, in step S104, the main charging current is 0.180C. After constant charging with the main charging current to the upper limit cutoff potential of 3.65V, the potential of 3.65V is maintained for constant voltage charging until the charging circuit current decays to the cutoff current threshold of 0.020C and then the charging circuit is cut off, thus completing the lithium-ion intercalation in the main phase transition region of the graphite anode.
[0018] Preferably, in step S105, the energy storage battery to be formed after completing the charging in step S104 is transferred to a high-temperature aging chamber at a temperature of 43°C to 47°C and left to stand for 24 to 48 hours with the circuit open; after standing, the air bag is punctured to perform negative pressure evacuation and exhaust, and a second laser sealing is performed; then, under an ambient temperature of 22°C to 27°C, it is discharged at a constant current of 0.19°C to 0.21°C to the lower limit cutoff voltage of 2.42V to 2.51V to complete the electrochemical steady-state shaping.
[0019] Preferably, the energy storage battery to be formed is a lithium iron phosphate battery with a nominal single-cell capacity of not less than 280Ah, the positive electrode sheet has a single-sided active coating with a coating capacity of not less than 3.8mAh / cm², the positive electrode active material layer thickness is 100μm to 140μm, and the electrolyte contains 1.5% to 2.5% by mass of vinylene carbonate and 0.8% to 1.2% by mass of lithium difluorophosphate.
[0020] The beneficial effects of this invention are:
[0021] 1. In the cascade formation of grid-connected energy storage batteries, by controlling the reaction process of film-forming additives in stages, the additives can undergo a more complete reduction reaction before the main solvent decomposes significantly. Open-circuit relaxation can alleviate the concentration difference at different depths of the thick electrode, improving the problem of insufficient additive reaction in deep pores. This allows the additives and the main solvent to react stepwise, reducing the uneven composition of the interfacial film caused by the simultaneous decomposition of both. This is beneficial for forming a denser and more uniform solid electrolyte interfacial film and reducing the charge transfer resistance at the electrode interface.
[0022] 2. During the decomposition of the main solvent and subsequent lithium intercalation, the charging current is dynamically adjusted according to the apparent polarization voltage drop. This can promptly limit the continued accumulation of polarization inside the thick electrode, ensuring a good match between the applied charging intensity and the mass transfer capacity inside the electrode. This helps to reduce local overpotential and uneven potential distribution during high-current charging, and reduces the possibility of excessively low local potential in the negative electrode, thereby reducing the risk of local lithium plating during rapid film formation.
[0023] 3. By coordinating the charging rate and relaxation process at different formation stages, the accumulation of gaseous byproducts generated by the decomposition of the main solvent in a short period of time can be reduced. This allows the generated gas to be discharged more smoothly from the pores of the thick electrode and between the electrode layers, reducing local isolation caused by gas retention and the decrease in effective reaction area. Subsequent static venting and resealing can further remove residual gaseous byproducts inside the battery, ensuring that the electrolyte maintains a good wetting state inside the thick electrode, improving the problem of uneven reaction in different areas of the electrode, and helping to improve the capacity retention capability of the grid energy storage battery during long-term deep charge and discharge processes. Attached Figure Description
[0024] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 This is a flowchart of the stepped formation process of the grid energy storage battery of the present invention;
[0026] Figure 2 This is a diagram showing the flow and interface response interaction during the formation stage of the energy storage battery in this invention. Detailed Implementation
[0027] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0028] A cascaded formation method for grid energy storage batteries includes the following steps:
[0029] Step S101: Control the energy storage battery to be formed to be in an environment with a temperature of 40°C to 50°C and a pre-tightening pressure of 0.1MPa to 0.3MPa, and apply a constant micro-current of 0.010C to 0.025C to charge it to the first cutoff potential of 2.00V to 2.20V and then cut off.
[0030] Step S102: Apply gradient current to continue charging, collect the charged capacity and closed-circuit voltage of the battery to be formed online, and calculate the differential capacity. When the differential capacity exceeds the characteristic reduction peak of the additive in the potential range of 2.20V to 2.55V and drops to 60% to 70% of the peak intensity, it enters the open-circuit relaxation state. Relaxation is terminated when the open-circuit voltage recovery rate is lower than or equal to 0.10mV / min and the open-circuit relaxation time reaches 5min to 15min. Record the open-circuit reference voltage at the termination time.
[0031] Step S103: Apply a stepped increasing current to charge within the potential range of 2.55V to 3.10V, and calculate the apparent polarization voltage drop between the current closed-circuit voltage and the open-circuit reference voltage in real time during each step charging process. When the apparent polarization voltage drop exceeds the upper limit threshold of polarization of 40mV to 50mV, reduce the current step current by 15% to 20% until the closed-circuit voltage reaches the second cutoff potential of 3.10V.
[0032] In step S104, a main charging current of 0.150C to 0.200C is applied to charge the battery at a constant current until the upper limit cutoff potential of 3.35V to 3.72V is reached, and then constant voltage charging is switched to continue until the charging current decays to the cutoff current threshold of 0.016C to 0.022C, at which point charging is terminated.
[0033] In step S105, the charged energy storage battery to be formed is left to stand in an open circuit in a constant temperature environment. After the gaseous byproducts are discharged, it is sealed under negative pressure and discharged at a constant current of 0.190C to 0.210C until the lower limit cutoff voltage of 2.25V to 2.51V is reached.
[0034] Preferably, in step S101, before the energy storage battery to be formed is placed in an environment with a temperature of 40°C to 50°C and a pre-tightening pressure of 0.1MPa to 0.3MPa, an electrolyte is injected and the battery is allowed to stand and soak at 40°C to 50°C for 22h to 25h; during the charging process in step S101, the pre-tightening pressure is controlled at 0.12MPa to 0.22MPa, the temperature at 40°C to 50°C, the constant micro-current at 0.018C to 0.025C, the first cutoff potential at 2.05V to 2.20V, and the charging duration at 2.0h to 2.5h.
[0035] Preferably, in step S102, the initial current of the gradient current boost is set to 0.020C to 0.030C, and the current is boosted to 0.050C in a linear rate of 0.002C to 0.005C per minute. Within the potential range of 2.20V to 2.55V, the characteristic electrochemical reduction peak of the film-forming additive is identified by differential capacity. When the charging voltage reaches 2.38V to 2.48V and the differential capacity exceeds the characteristic reduction peak of the additive and decreases to 60% to 70% of the characteristic reduction peak of the additive, the applied charging current is cut off and the system enters an open-circuit relaxation state.
[0036] Preferably, in step S102, the duration of the open-circuit relaxation state is set to 5 min to 15 min; in the open-circuit relaxation state, the open-circuit voltage is collected in real time and its rate of change over time is calculated. When the absolute value of the rate of change decreases to the range of 0.05 mV / min to 0.10 mV / min, the relaxation is terminated, and the open-circuit reference voltage is read and stored at the termination time as the reference potential for calculating the apparent polarization voltage drop in step S103.
[0037] Preferably, in step S103, the potential range of 2.55V to 3.10V is the main solvent decomposition potential range, and the step-increasing current includes a first step current of 0.045C to 0.051C, a second step current of 0.076C to 0.082C, and a third step current of 0.113C to 0.121C applied sequentially; the switching voltage node of each step current is set as follows: when the first step current is charged to the closed-circuit voltage of 2.65V to 2.80V, the second step current is switched; when the second step current is charged to the closed-circuit voltage of 2.88V to 2.96V, the third step current is switched.
[0038] Preferably, in step S103, the apparent polarization voltage drop is the difference between the closed-circuit voltage and the open-circuit reference voltage at the current sampling time; during each step current charging process, when the apparent polarization voltage drop exceeds 45mV, the setting value of the current step current level is reduced by 15% to 20%, and the reduced current is maintained to continue charging to the corresponding switching voltage node or the second cutoff potential of 3.10V.
[0039] Preferably, in step S104, the main charging current is 0.180C. After constant charging with the main charging current to the upper limit cutoff potential of 3.65V, the potential of 3.65V is maintained for constant voltage charging until the charging circuit current decays to the cutoff current threshold of 0.020C and then the charging circuit is cut off, thus completing the lithium-ion intercalation in the main phase transition region of the graphite anode.
[0040] Preferably, in step S105, the energy storage battery to be formed after completing the charging in step S104 is transferred to a high-temperature aging chamber at a temperature of 43°C to 47°C and left to stand for 24 to 48 hours with the circuit open; after standing, the air bag is punctured to perform negative pressure evacuation and exhaust, and a second laser sealing is performed; then, under an ambient temperature of 22°C to 27°C, it is discharged at a constant current of 0.19°C to 0.21°C to the lower limit cutoff voltage of 2.42V to 2.51V to complete the electrochemical steady-state shaping.
[0041] Preferably, the energy storage battery to be formed is a lithium iron phosphate battery with a nominal single-cell capacity of not less than 280Ah, the positive electrode sheet has a single-sided active coating with a coating capacity of not less than 3.8mAh / cm², the positive electrode active material layer thickness is 100μm to 140μm, and the electrolyte contains 1.5% to 2.5% by mass of vinylene carbonate and 0.8% to 1.2% by mass of lithium difluorophosphate.
[0042] Example 1: In this example, a positive electrode sheet with a single-sided active coating capacity of 4.2 mAh / cm², a positive active material layer thickness of 125 μm, and a compaction density of 2.45 g / cm³ is assembled with a negative electrode sheet with a coating capacity of 4.6 mAh / cm² and a compaction density of 1.55 g / cm³ to form a lithium iron phosphate grid storage battery with a nominal capacity of 314 Ah. An electrolyte consisting of ethylene carbonate and methyl ethyl carbonate in a volume ratio of 3:7, containing 2% by mass of vinylene carbonate and 1% by mass of lithium difluorophosphate is injected. The battery, after high-temperature static impregnation, is placed in a temperature-controlled fixture set at 45°C. A pre-tightening pressure of 0.2 MPa is applied by an electrode forming machine, and a constant micro-current is applied by a charge / discharge circuit. The corresponding absolute current value is 4.71A, and the constant current charging is carried out for 2.42 hours until the first cutoff potential. After the circuit is cut off, the electrolyte is allowed to penetrate deep into the pores of the thick electrode and establish an initial double-layer electrostatic field at the solid-liquid interface of the negative electrode. In the description of this invention, the charge / discharge rate C is defined as the rate of the battery's nominal capacity, and 1C represents the current value required to fully charge or discharge the battery's nominal capacity within 1 hour.
[0043] A gradient current ramp-up was applied with an initial current of 0.025C, or 7.85A. Subsequent charging was initiated, with the current gradually increased to 0.05C (15.7A) in a linear stepwise manner at a rate of 0.003C (0.942A / min). During this process, sampling was performed at 2-second intervals. Real-time acquisition of battery closed-circuit voltage With the amount of electricity charged Calculate the differential capacity: ,in, and These represent the cumulative charge received at the current sampling time and the previous sampling time, respectively. and These are the closed-circuit voltages at the corresponding sampling times. Using the time sampling interval, when the charging voltage is between 2.20V and 2.55V and reaches 2.38V, the peak value of additive characteristic reduction is detected to be 412Ah / V. Charging continues until the voltage reaches 2.48V, at which point the differential capacity decreases to 265Ah / V, corresponding to a decrease to 64.3% of the peak value of additive characteristic reduction. The control system then cuts off the applied charging current and enters an open-circuit relaxation state. During the open-circuit relaxation state, the rate of change of the open-circuit voltage over time is monitored. When relaxation continues for 8.5 minutes, the open-circuit voltage recovery rate satisfies the following: At this point, the recovery rate was measured to be 0.06 mV / min. The charge and discharge control system then issued a command to the circuit switch relay to maintain the cut-off state and triggered the voltage data latch. At the physical port at the moment of open-circuit relaxation termination, 10 sets of voltage signals were continuously sampled at a resolution of 0.01 mV through a high-precision analog-to-digital conversion channel and the arithmetic average was taken. The stabilized static potential value was written into the controller's non-volatile storage register as the open-circuit reference voltage. This stored value served as the initial static substrate physical quantity for the rebalancing of the additive concentration gradient inside the electrode through free diffusion. It provided the initial bias parameters for the next process step, allowing the additive molecules consumed in the pores deep inside the electrode to be replenished in situ through concentration difference diffusion at the thermodynamic equilibrium potential. Before the main solvent decomposed, a primary passivation layer rich in inorganic components of lithium fluoride and lithium carbonate was constructed.
[0044] Within the main solvent decomposition potential range of 2.55V to 3.10V, charging is performed using a stepped increasing current combined with a dynamic overpotential constraint mode. The stepped current levels are sequentially set to the first stepped current. The first step current ranges from 0.045C to 0.051C, with an absolute value of 15.7A. The second step current... The second-step current ranges from 0.076C to 0.082C, with an absolute value of 25.12A, and the third-step current... The corresponding third-step current ranges from 0.113C to 0.121C, with an absolute value of 37.68A; during each charging step, the current is adjusted online based on the current closed-circuit voltage. With open-circuit reference voltage Calculate the apparent polarization voltage drop: ,in, The charging closed-circuit voltage at the current sampling time. The open-circuit reference voltage at the moment of termination of open-circuit relaxation. For the apparent polarization voltage drop, during the main solvent decomposition and initial lithium intercalation stage (2.55V to 3.10V), the lithium iron phosphate and graphite electrodes have not yet entered the main flat phase transition reaction platform. The solid-phase bulk thermodynamic equilibrium potential rises very gently in this low-charge-state range. The total terminal voltage change inside the thick electrode is mainly dominated by the concentration polarization caused by limited liquid-phase mass transfer and the kinetic overpotential formed by interfacial charge transfer impedance. During this stage, the open-circuit reference voltage obtained at the termination of open-circuit relaxation is used as a unified calculation benchmark. The direct difference between the current closed-circuit voltage and the open-circuit reference voltage during subsequent charging is used as the apparent polarization voltage drop to monitor the polarization changes during the main solvent decomposition and microbubble initiation stages, using the first step current. When the closed-circuit voltage reaches 2.75V, the apparent polarization voltage drop is calculated according to the direct difference relationship mentioned above and compared with the upper limit threshold of 45mV for polarization. If the calculated result is lower than this threshold, the second-step current is switched on. Continue charging; in the engineering analysis of stepped increasing current charging, in order to analyze the evolution mechanism of interface polarization in the deep micro-regions of the electrode, the thermodynamic equilibrium open-circuit voltage measured under the current state of charge is used. As the intrinsic potential base, and through the open-circuit reference voltage Normalization calibration, closing the voltage Response decoupling is ohmic internal resistance voltage drop Pure dynamic polarization overpotential caused by liquid phase mass transfer / interfacial charge transfer Its analytic relation satisfies: Among them, the ohmic internal resistance The real part of the high-frequency AC impedance is calibrated as ; Charge to the first stage At the node, the thermodynamic equilibrium base potential corresponding to the charged state for Subtracting Ohmic polarization voltage drop Then, the pure dynamic polarization overpotential was extracted. for (The project is rounded down as follows) ); Charge to the second stage At the node, the thermodynamic equilibrium basement potential for Subtracting Ohmic polarization voltage drop Then, the pure dynamic polarization overpotential was extracted. for (The project is rounded down as follows) This local dynamic analysis is used to qualitatively analyze the overpotential distribution within the micropores of thick electrode sheets. However, in actual industrial closed-loop control, the online current regulation determination of the apparent polarization voltage drop is still uniformly based on the current closed-loop voltage. With open-circuit reference voltage direct algebraic difference Execute quickly with the second-step current. When the closed-circuit voltage reaches 2.95V, and the calculated apparent polarization voltage drop is still below the upper polarization threshold of 45mV, the third-step current is switched on. Charging; During the third-step current charging process, when the closed-circuit voltage reaches 3.04V, the apparent polarization voltage drop calculated based on the direct difference rises to 48mV and exceeds the upper limit threshold of 45mV for polarization. The control system automatically reduces the current step current level by 20% to 0.096C, i.e., 30.14A, and maintains the reduced current to continue charging until the second cutoff potential. This mechanism balances the generation flux of alkanes and carbon oxides produced by the reduction and decomposition of the main solvent with the resistance to gas-phase seepage from the thick electrode pores, eliminating the isolation cavities caused by gas stagnation. Simultaneously, it maintains the local potential at the negative electrode interface above the lithium metal deposition potential. The mechanism lies in the high tortuosity of the micropores within the 125 μm thick porous electrode with a compaction density of 2.45 g / cm³. This allows alkanes and carbon oxides produced by the electrochemical reduction and decomposition of the main solvent to aggregate and nucleate within the electrode micropores, forming microbubbles. When the macroscopic charging current changes from 0.1... When the current density is reduced by 20% to 0.096C, the electrochemical Faraday reaction rate decreases by 20% instantaneously and proportionally. The molar flux of gas phase generation at the electrode micro-region interface per unit time drops sharply to below the flux discharged by capillary resistance in the micropores. At the same time, the reduction in current density allows the concentration gradient of liquid lithium ions deep in the pores to be rapidly smoothed out by natural diffusion. The electrolyte refills the voids left by the gas phase escape by relying on capillary wetting pressure, eliminating the local insulating gas film formed by the retention of microbubbles in the dead zone of the pores and blocking the lithium plating channel caused by the sharp increase in local current density in the micro-region.
[0045] After the battery closed-circuit voltage reaches 3.1V, the process transitions to the main phase transition region of the graphite anode, and the main charging current is applied. That is, constant current charging at 56.52A until the upper limit cutoff potential is reached. Maintain a constant voltage of 3.65V for charging until the charging circuit current decays to the cutoff current threshold. That is, the charging circuit is cut off at 6.28A; the charged battery is transferred to an aging chamber at 45℃ and left to stand open for 36 hours. After the reaction products inside the electrode and the pores are fully balanced, the gas bag is punctured to release the gas phase by-products, and negative pressure sealing and secondary laser sealing are performed; then, under an ambient temperature of 25℃, it is discharged at a constant current of 0.2C, i.e., 62.8A, to the lower limit cutoff voltage of 2.5V to complete the electrochemical steady-state stabilization.
[0046] After the aforementioned step-by-step formation and finalization, the electrochemical performance indicators of the 314Ah grid energy storage battery were measured. The initial coulombic efficiency of the battery reached 94.62%, and the interfacial charge transfer impedance at 50% charge was [not specified]. The resistance is 0.412 mΩ. After continuous constant current charge-discharge cycle testing at 0.5C rate with 100% discharge depth at an ambient temperature of 25℃, the capacity retention rate after 1000 cycles is 96.85%, and the DC internal resistance growth rate is 11.24%. This indicates that a homogeneous low-resistance solid electrolyte interface phase is constructed in the entire depth direction of the thick electrode, which suppresses local lithium plating caused by mass transfer hysteresis and gas phase retention, and improves the service stability of the grid energy storage battery throughout its entire life cycle.
[0047] Example 2: This example verifies the electrochemical response and interface state of the step-formation method under different working boundaries, missing key processes, and parameter deviations. A 314Ah lithium iron phosphate energy storage battery was selected, with a positive electrode single-sided active coating capacity of 4.2 mAh / cm², a positive active material layer thickness of 125 μm, and a compaction density of 2.45 g / cm³, and a negative electrode coating capacity of 4.6 mAh / cm² and a compaction density of 1.55 g / cm³. Ethylene carbonate and ethyl methyl carbonate were injected as solvents in a volume ratio of 3:7. The electrolyte contained 2% vinylene carbonate and 1% lithium difluorophosphate by mass. The battery was then loaded into a device equipped with a force measuring and... A multi-channel charge-discharge test platform for displacement sensors features a voltage measurement resolution of 0.01mV and a measurement accuracy of ±0.1mV, a current output control accuracy of ±0.05%, a temperature control accuracy of ±0.5℃ for the temperature chamber, and a pneumatic clamp pressure control accuracy of ±0.005MPa. A high-frequency random fluctuation signal with a signal-to-noise ratio of 35dB is superimposed in the signal acquisition loop to simulate industrial field interference. A sliding window filtering algorithm with five sampling cycles is used to process the closed-circuit voltage and charged capacity data to reduce the impact of random fluctuations on differential capacity calculation and open-circuit voltage recovery rate determination. Specifically, a first-in-first-out queue is used to maintain the original sampling data for five consecutive sampling cycles in real time. The voltage and charged capacity in the queue are smoothed using a Gaussian centrally symmetric weighted average algorithm, with the weighting coefficient vector set as follows: The filtered output value is expressed as: ;in, For the first The closed-circuit voltage or charged amount after smoothing and filtering in each sampling period For the first The original sampling data for each sampling period, These are weighting coefficients. The offset is relative to the current sampling period. Before performing differential quotient calculation, a voltage micro-step protection threshold is set. When the absolute value of the difference between adjacent filter voltages is less than 0.05mV, the system locks the lower limit of the denominator to 0.05mV or uses the effective smooth slope output of the previous period to suppress the sudden jump of the differential value and the divergence of high-frequency noise when the denominator is close to zero, so that the differential capacity curve can continuously track its extreme value changes.
[0048] Ten independent test groups were set up, with the same physical specifications of the battery cells and electrolyte composition in each group. Test group 1 adopted standard parameter conditions, with the fixture temperature set at 45℃, the preload pressure at 0.2MPa, and a constant microcurrent applied. Charge to the first cutoff potential of 2.15V; then increase the current in steps from 0.025C to 0.05C at a rate of 0.003C per minute. Calculate the differential capacity online. Enter open-circuit relaxation mode when the characteristic reduction peak of the additive is surpassed and the current drops to 64.3% of the peak intensity. Relaxation is terminated when the open-circuit voltage recovery rate reaches 0.06mV / min and the relaxation time reaches 8.5min. Record the open-circuit reference voltage. Within the main solvent decomposition potential range of 2.55V to 3.10V, a first-step current is sequentially applied. Second step current and the third-step current When the apparent polarization voltage drop exceeds 45mV, the current step current is reduced by 20% to 0.096C and charged to the second cutoff potential of 3.10V; then the main charging current is applied. Constant current charging is performed until 3.65V is reached, then constant voltage charging is switched until the cutoff current threshold is reached. After being left to stand at 45℃ for 36 hours with the circuit open and then sealed with exhaust gas, it was discharged at a constant current of 0.2C to 2.50V.
[0049] Experimental group 2 adopted process range boundary condition A, which is biased towards fast-paced production boundary: the fixture temperature was set to the lower limit of 40℃, the preload pressure was set to the lower limit of 0.1MPa, and the constant micro-current was used. The lower limit is set to 0.01C, the first cutoff potential is set to 2.00V, the gradient current ramp rate is set to 0.002C per minute, and the differential capacity decay ratio criterion is set to 60% of the lower limit of the interval. The open-circuit voltage recovery rate termination threshold is set to the upper limit of the numerical interval, 0.10mV / min, which corresponds to the relaxed rate boundary that allows for relatively fast termination of relaxation. The measured relaxation time is 11.2min. The polarization upper limit threshold is set to the lower limit of 40mV, the over-limit reduction is set to 15% of the lower limit, the main charging current is set to the lower limit of 0.15C, and the high-temperature resting time is set to 48h.
[0050] Test group 3 adopted process range boundary condition B, which is biased towards a strict and fully relaxed boundary: the fixture temperature was set to the upper limit of 50℃, the preload pressure was set to the upper limit of 0.3MPa, and the constant microcurrent was used. The upper limit is set to 0.025C, the first cutoff potential is set to the upper limit of 2.20V, the gradient current ramp rate is set to the upper limit of 0.005C per minute, the differential capacity decay ratio criterion is set to the upper limit of 70% of the range, the open circuit voltage recovery rate termination threshold is set to the lower limit of the numerical range of 0.05mV / min, corresponding to the stringent rate boundary of the required high potential smoothness, the measured relaxation time is 6.8min, the polarization upper limit threshold is set to the upper limit of 50mV, the over-limit reduction is set to the upper limit of 20%, the main charging current is set to the upper limit of 0.2C, and the high temperature resting time is set to 24h.
[0051] Control group 1 used conventional fixed-step formation, charging to 2.50V at 0.02C under 45℃ and 0.2MPa conditions, without differential capacity tracking or open-circuit relaxation, then charging to 3.10V with a fixed current of 0.08C, without dynamic current adjustment based on apparent polarization voltage drop, then charging to 3.65V with 0.2C and switching to constant voltage charging until the current drops to 0.02C and is then cut off. After the same static venting process, it was discharged for finalization. Control group 2 canceled differential capacity tracking and open-circuit relaxation, and charging directly across the corresponding potential range. Other parameters were the same as test group 1. Control group 3 canceled dynamic current adjustment based on apparent polarization voltage drop, maintained fixed-step current charging, and did not reduce the current when polarization exceeded the limit. Other parameters were the same as test group 1. Control group 4 used operating conditions below the lower limit of the parameter range, with a preload pressure of 0.05MPa and a constant micro-current. The control group 5 uses a working condition higher than the upper limit of the parameter range, with the upper limit of polarization threshold set to 65mV and the main charging current set to 0.25C. The other parameters are the same as those in the test group 1. The control group 6 changes the additive reaction endpoint criterion, cutting off the current and switching to open-circuit relaxation state when the differential capacity drops to 85% of the characteristic reduction peak intensity of the additive. The other parameters are the same as those in the test group 1. The control group 7 cancels the constant microcurrent and pre-tightening pressure pre-activation stage, and directly applies a 0.05C current for charging after the liquid is injected and allowed to stand. The other parameters are the same as those in the test group 1.
[0052] After each group completed the formation and stabilization, the coulombic efficiency of the first charge and discharge was measured at an ambient temperature of 25°C. The battery was then adjusted to 50% state of charge, and AC impedance spectroscopy was performed in the frequency band from 100kHz to 10mHz to extract the charge transfer impedance. The thickness expansion rate of the shaped electrode plate was measured using a laser displacement thickness gauge, and a 1000-cycle charge-discharge test with 100% depth of discharge was conducted at 25℃ and 0.5C. The capacity retention rate and DC internal resistance growth rate were recorded after 1000 cycles. After the test, the electrode roll was disassembled and the lithium deposition state of the micro-area on the negative electrode surface was observed by scanning electron microscopy.
[0053] Under the same test conditions, the initial coulombic efficiency of test group 1 was 94.62%, and the charge transfer impedance was... The resistance was 0.412 mΩ, the thickness expansion rate after shaping was 1.85%, the capacity retention rate after 1000 cycles was 96.85%, the DC internal resistance growth rate after 1000 cycles was 11.24%, no lithium plating was observed on the negative electrode surface, and the interface was uniform and dense. The initial coulombic efficiency of test group 2 was 94.38%, and the charge transfer impedance was... The resistance was 0.435 mΩ, the thickness expansion rate after shaping was 1.96%, the capacity retention rate after 1000 cycles was 96.31%, the DC internal resistance growth rate after 1000 cycles was 12.08%, no lithium plating was observed on the negative electrode surface, the interface was intact, the initial coulombic efficiency of test group 3 was 94.81%, and the charge transfer impedance was... The resistance was 0.398 mΩ, the thickness expansion rate after shaping was 1.78%, the capacity retention rate after 1000 cycles was 97.12%, the DC internal resistance growth rate after 1000 cycles was 10.65%, no lithium plating was observed on the negative electrode surface, and inorganic phase enrichment was observed.
[0054] The results of experimental group 1 were compared with those of experimental groups 2 and 3. Experimental group 1 used the optimized parameter conditions (the measured recovery rate at the open-circuit relaxation termination was 0.06 mV / min). Experimental groups 2 and 3 respectively verified the process adaptability of the open-circuit voltage recovery rate termination threshold at the relaxed rate boundary point (0.10 mV / min) and the strict rate boundary point (0.05 mV / min). The initial coulombic efficiency of all three groups after finalization remained above 94.3%, and the capacity retention rate after 1000 cycles was above 96.3%. No lithium plating was observed on the negative electrode surface. This fully verified that within the open-circuit voltage recovery rate threshold range of 0.05 mV / min to 0.10 mV / min, the additives inside the thick electrode can be effectively ensured to complete in-situ rebalancing through concentration difference diffusion, providing sufficient process window support for the construction of a dense low-resistance passivation layer on the electrode surface.
[0055] After fixed-step formation, control group 1 achieved an initial coulombic efficiency of 92.15% and a charge transfer impedance of [missing information]. The resistance was 0.548 mΩ, the thickness expansion rate after shaping was 4.62%, the capacity retention rate after 1000 cycles was 91.4%, the DC internal resistance growth rate after 1000 cycles was 22.8%, and there were sheet-like dead lithium and vapor phase spots on the negative electrode surface. After canceling differential capacity tracking and open-circuit relaxation in control group 2, the initial coulombic efficiency was 93.04%, and the charge transfer impedance was... The resistance is 0.495 mΩ, the thickness expansion rate after shaping is 3.25%, the capacity retention rate after 1000 cycles is 93.52%, the DC internal resistance growth rate after 1000 cycles is 17.65%, trace lithium plating exists at the edges of local micropores, and after the apparent polarization voltage drop dynamic current adjustment is cancelled in control group 3, the initial coulombic efficiency is 93.28%, and the charge transfer impedance is... The resistance is 0.481 mΩ, the thickness expansion rate after shaping is 3.84%, the capacity retention rate after 1000 cycles is 92.86%, the DC internal resistance growth rate after 1000 cycles is 19.12%, and there are star-shaped lithium deposits in the electrode bending area.
[0056] Under parameter deviation conditions, control group 4, after reducing the preload pressure and constant microcurrent below the parameter range, achieved an initial coulombic efficiency of 92.85% and a charge transfer impedance of [missing information]. The resistance was 0.516 mΩ, the thickness expansion rate after shaping was 3.12%, the capacity retention rate after 1000 cycles was 93.1%, the DC internal resistance growth rate after 1000 cycles was 18.42%, and poor deep wetting and local pitting corrosion of the electrode were observed. In control group 5, after increasing the upper limit of polarization threshold and the main charging current, the initial coulombic efficiency was 93.12%, and the charge transfer impedance was... The resistance was 0.489 mΩ, the thickness expansion rate after shaping was 4.38%, the capacity retention rate after 1000 cycles was 92.15%, the DC internal resistance growth rate after 1000 cycles was 21.05%, dendritic patches appeared in the in-plane high polarization region, and after adjusting the additive reaction endpoint criterion to 85% of the characteristic reduction peak intensity of the additive, the initial coulombic efficiency in control group 6 was 93.41%, and the charge transfer impedance was... The resistance was 0.472 mΩ, the thickness expansion rate after shaping was 2.86%, the capacity retention rate after 1000 cycles was 94.18%, the DC internal resistance growth rate after 1000 cycles was 16.34%, and there was an accumulation of organic solvent decomposition products at the interface. After the constant microcurrent and pre-tightening pressure pre-activation stage was removed in control group 7, the initial coulombic efficiency was 92.46%, and the charge transfer impedance was... The resistance is 0.532 mΩ, the thickness expansion rate after shaping is 4.15%, the capacity retention rate after 1000 cycles is 91.88%, the DC internal resistance growth rate after 1000 cycles is 21.9%, and there is local current density overload accompanied by speckled lithium deposition.
[0057] Comparing the results of experimental group 1 with those of control groups 2 and 3, after canceling differential capacity tracking and open-circuit relaxation, the charge transfer impedance increased and the long-term cycling capacity retention decreased. Under this condition, open-circuit relaxation did not occur at the end of the additive electrochemical reaction window, and the film-forming additive consumed in the deep layer of the electrode pores could not be replenished in time through concentration gradient diffusion, causing the surface potential to enter the main solvent decomposition zone in advance and form a loose and porous organic passivation layer. After canceling the dynamic current adjustment of apparent polarization voltage drop, the thickness expansion rate after shaping and the growth rate of long-term cycling DC internal resistance both increased. After disassembly, speckled lithium plating was observed in the high tortuosity micro-region at the corner of the electrode. Under the action of continuous step current, the gas phase precipitation rate generated by the decomposition of the main solvent exceeded the gas phase permeation escape flux of the porous electrode structure. After the microbubbles were retained, the local lithium ion transport path was blocked, causing transient current overload. The above two types of control results correspond to the additive film formation stage and the step charging stage, respectively, indicating that the additive preferential film formation and multi-stage polarization closed-loop constraint work together to affect the electrode interface state.
[0058] In control group 4, the pre-tightening pressure and constant microcurrent were below the lower limit of the parameter range, which affected the wetting of micropores inside the thick electrode in the low potential range and the orientation of the double layer, resulting in a decrease in the initial coulombic efficiency and an increase in charge transfer impedance. In control group 5, the upper limit of polarization and the main charging current exceeded the upper limit of the parameter range. Under the action of large current, the polarization of the liquid phase concentration in the deep part of the electrode increased, the local transient potential of the negative electrode decreased and side reactions occurred, resulting in an increase in the growth rate of DC internal resistance in long-term cycling. In control group 6, the current was cut off when the differential capacity dropped to only 85% of the peak value. The additive reduction reaction did not proceed fully in the active sites at the full depth of the electrode. The residual additive molecules then competed for reaction in the decomposition stage of the main solvent, resulting in an increase in the interfacial charge transfer impedance. In control group 7, the pre-activation stage was canceled and the electrode was charged directly at 0.05C. Under the action of the initial large current, the electrode surface layer underwent side reactions, resulting in an increase in the thickness expansion rate after shaping and a decrease in the long-term cycling capacity retention rate.
[0059] Based on the above-mentioned different parameter conditions, the main charging current is set to 0.15C to 0.2C. When the main charging current is higher than 0.2C, the diffusion flux of solid-phase lithium intercalation inside the thick electrode is limited, the local overpotential at the negative electrode solid-liquid interface drops below 0V, and the risk of local lithium plating increases. When it is lower than 0.15C, the graphite phase transition plateau reaction time is prolonged and no additional interface benefits are obtained. The constant voltage cutoff current threshold is set to 0.016C to 0.022C. When the cutoff current is higher than 0.022C, the lithium intercalation phase transition of the high-order graphite interlayer compound is not fully completed, and the initial coulombic efficiency decreases, falling below 0.016C. Maintaining a high potential constant voltage for a long time will increase the oxidation side reaction of the main solvent in the electrolyte. The lower limit cutoff voltage is set to 2.25V to 2.51V. When it is below 2.25V, the deep part of the electrode is in an excessive delithiation state, which can easily cause trace amounts of transition metals to dissolve from the positive electrode active phase. When it is above 2.51V, the residual active lithium is not fully released and affects the capacity calibration. The current adjustment range of the step current is set to 15% to 20%. When the adjustment range is less than 15%, the continuously accumulated concentration polarization cannot be effectively suppressed. When the adjustment range exceeds 20%, the reaction rate at the electrode interface decreases and the production time is significantly prolonged.
[0060] Example 3: In this example, a positive electrode sheet with a single-sided active coating capacity of 4.2 mAh / cm², a positive active material layer thickness of 125 μm, and a compaction density of 2.45 g / cm³ was selected, along with a negative electrode sheet with a coating capacity of 4.6 mAh / cm² and a compaction density of 1.55 g / cm³. These were assembled into a lithium iron phosphate energy storage battery with a nominal capacity of 314 Ah. An electrolyte solution containing ethylene carbonate and ethyl methyl carbonate (volume ratio 3:7) as a mixed solvent, and containing 2% vinylene carbonate and 1% lithium difluorophosphate by mass, was injected. The battery was placed in a temperature-controlled fixture, and the environment... The temperature was set to 45℃. To determine the initial physical constraint boundary, preload pressures of 0.05MPa, 0.2MPa, and 0.4MPa were used for calibration. The electrolyte retention in the electrode pores and the initial double-layer capacitance were measured. Under a preload pressure of 0.05MPa, a small air gap existed between the electrode layers, and the double-layer formation was delayed. Under a preload pressure of 0.4MPa, the electrode pores were compressed, and deep electrolyte seepage occurred. Under a preload pressure of 0.2MPa, the electrolyte retention and capacitance value in the electrode micropores reached a stable equilibrium. Therefore, a preload pressure of 0.2MPa and an ambient temperature of 45℃ were selected, and a constant microcurrent was applied. That is, constant current charging at 4.71A for 2.42 hours until the first cutoff potential. Afterwards, the deep wetting of the electrode pores and the construction of the electrostatic double layer at the solid-liquid interface were completed.
[0061] A gradient current ramp-up method is adopted, with an initial current of 0.025C and a current ramp-up rate of 0.003C per minute. The current is stepped up to 0.05C; sampling is performed at 2-second intervals. Online acquisition of closed-circuit voltage and charging power The differential capacity was calculated, and the characteristic reduction peak of the additive was identified when the closed-circuit voltage reached 2.38V. To determine the control point of the film-forming reaction, the current was cut off and the system entered an open-circuit relaxation state when the differential capacity decayed from the characteristic reduction peak of the additive to 85%, 65%, and 45% of the peak intensity, respectively. The charge transfer impedance after the stepwise formation and shaping was then measured. Volume of gaseous byproducts; when the current is cut off at 85%, the additive reduction reaction is incomplete, charge transfer impedance. The impedance reached 0.472 mΩ; at 45% current cutoff, the main solvent underwent partial co-decomposition, with a gaseous byproduct volume of 15 mL; at 65% current cutoff, the gaseous byproduct volume was 2 mL, and the charge transfer impedance... The resistance was reduced to 0.412 mΩ, and based on this, 60% to 70% of the peak intensity was taken as the trigger range for transitioning to the open-circuit relaxation state.
[0062] During the determination of gas generation, the outlet pipe of the temporary gas bag at the top of the battery was connected to a constant-temperature liquid displacement drainage meter. The net gas generation in the sealed gas bag was obtained by measuring the volume of the discharged liquid. Based on the porous electrode structure parameters, when the thickness of the positive electrode active material layer is 125 μm and the compaction density is 2.45 g / cm³, the porosity of the positive electrode and the graphite negative electrode is in the range of 28% to 32%. According to the capillary permeation relationship of two-phase flow pores, the maximum allowable generation rate threshold of gas phase capillary escape inside the electrode is 0.12 mL per minute per 100 cm² electrode area. When the differential capacity decays to the characteristic reduction of the additive... The current was cut off when the peak intensity reached 65%. The measured gas production rate was 0.03 mL per minute per 100 cm² electrode area, which is lower than the maximum allowable generation rate threshold. The generated alkane and carbon oxide gaseous byproducts could escape to the external gas bag through the electrode micropores. In this embodiment, when the differential capacity decreased to 64.3% of the characteristic reduction peak intensity of the additive, the applied charging current was cut off and the system entered an open-circuit relaxation state. The open-circuit voltage recovery rate was monitored. When the recovery rate decreased to 0.06 mV / min and the relaxation time reached 8.5 min, the open-circuit relaxation was terminated, and the open-circuit reference voltage at the current moment was recorded and locked. .
[0063] Within the main solvent decomposition potential range where the closed-circuit voltage is between 2.55V and 3.10V, the first step current is applied sequentially. Second step current and the third-step current Perform stepped incremental charging, and adjust the charging based on the current closed-circuit voltage. With open-circuit reference voltage The difference was used to obtain the apparent polarization voltage drop in real time. To determine the polarization tolerance boundary during the stepped charging process, comparative tests were conducted with the upper limit of polarization threshold set at 30mV, 45mV, and 65mV respectively. After disassembling the cell, the surface morphology of the negative electrode was observed using a scanning electron microscope, and the total formation time was recorded. At the 65mV threshold, lithium metal deposition patches appeared in the high tortuosity micro-region at the edge of the negative electrode sheet. At the 30mV threshold, no lithium deposition was observed on the negative electrode surface, but the total formation time was extended by 4.5h due to the increase in the number of current drops. At the 45mV threshold, no lithium metal deposition was observed on the negative electrode surface, and the formation time matched the production cycle. Therefore, 45mV was adopted as the upper limit of polarization threshold.
[0064] When the closed-circuit voltage reaches 3.04V, it will be based on the current closed-circuit voltage. With open-circuit reference voltage The difference calculation showed that the apparent polarization voltage dropped to 48mV, exceeding the upper limit threshold of 45mV. The control system then reduced the current step current by 20% to 0.096C and maintained the reduced current to continue charging until the second cutoff potential. Then apply the main charging current. Constant current charging to the upper limit cutoff potential Maintain a constant voltage of 3.65V for charging until the current decays to the cutoff current threshold. After charging is terminated, the battery is transferred to an open-circuit aging chamber at 45°C and left to stand for 36 hours to remove gaseous byproducts and perform a second negative pressure laser sealing. Then, it is discharged at a constant current of 0.2C at 25°C to the lower limit cutoff voltage of 2.50V to complete the step-by-step formation and shaping.
[0065] Example 4: This example combines Figures 1 to 2 This paper describes a cascaded formation method for grid-connected energy storage batteries, such as... Figure 1 As shown, in step S101, the energy storage battery to be formed is controlled in an environment with a temperature of 40°C to 50°C and a pre-tightening pressure of 0.1MPa to 0.3MPa. A constant micro-current of 0.010C to 0.025C is applied to charge it to the first cutoff potential of 2.00V to 2.20V, and then the charging is stopped. In step S102, a gradient current is applied to continue charging. The charged capacity and closed-circuit voltage of the energy storage battery to be formed are collected online, and the differential capacity is calculated. When the differential capacity exceeds the characteristic reduction peak of the additive in the potential range of 2.20V to 2.55V and drops to 60% to 70% of the peak intensity, it enters the open-circuit relaxation state. Relaxation is terminated when the open-circuit voltage recovery rate is lower than or equal to 0.10mV / min and the open-circuit relaxation time reaches 5min to 15min. The open-circuit reference voltage at the termination time is recorded. In step S103, in the potential range of 2.55V to 3. A stepped increasing current is applied within 10V for charging, and the apparent polarization voltage drop between the current closed-circuit voltage and the open-circuit reference voltage is calculated in real time during each step of charging. When the apparent polarization voltage drop exceeds the upper limit threshold of polarization by 40mV to 50mV, the current step current is reduced by 15% to 20% until the closed-circuit voltage reaches the second cutoff potential of 3.10V. In step S104, a main charging current of 0.150C to 0.200C is applied for constant current charging to the upper limit cutoff potential of 3.35V to 3.72V, and then constant voltage charging is switched until the charging current decays to the cutoff current threshold of 0.016C to 0.022C and then charging is terminated. In step S105, the charged energy storage battery to be formed is left to stand in an open circuit in a constant temperature environment. After the gaseous by-products are discharged, it is sealed under negative pressure and discharged with a discharge current of 0.190C to 0.210C to the lower limit cutoff voltage of 2.25V to 2.51V.
[0066] like Figure 2As shown, in the tiered formation process of the grid energy storage battery, the initial double-layer electrostatic field is first established and the process transitions to a constant micro-current charging stage. From this stage, the process moves to a gradient current ramp-up charging stage. During the gradient current ramp-up charging process, after detecting and reaching the peak state of additive characteristic reduction, the process transitions to a stepped increasing current charging stage. In this stage, dynamic current regulation is implemented to achieve closed-loop control of the formation process. Subsequently, the process transitions to a main charging current constant current and constant voltage charging stage, accompanied by the completion of the graphite anode main phase transition. Then, the process enters an open-circuit resting and constant current discharge stage to complete electrochemical steady-state formation. The grid energy storage battery completed in the open-circuit resting and constant current discharge stages is cyclically connected to the constant micro-current charging process flow loop. Simultaneously, the grid energy storage battery, as the core component of the formation process, corresponds to each of the following process stages: constant micro-current charging, gradient current ramp-up charging, stepped increasing current charging, main charging current constant current and constant voltage charging, and open-circuit resting and constant current discharge.
[0067] Example 5: In this example, a lithium iron phosphate energy storage battery with a nominal capacity of 314Ah was subjected to multi-channel batch formation. To reduce the influence of fixture temperature gradient and electrode wetting differences on the determination of the additive reaction window, the battery was placed in a temperature-controlled pressurization system with a temperature set at 45°C and a pre-tightening pressure set at 0.2MPa, using a constant micro-current with an absolute value of 4.71A. Charge for 2.42 hours to reach the first cutoff potential. The circuit is then disconnected; subsequently, a gradient current ramp-up is applied with an initial current of 0.025C and a ramp-up rate of 0.003C per minute. The current is stepped up to 0.05C, and samples are taken at 2-second intervals. The closed-circuit voltage and charged capacity are collected online, and the differential capacity is calculated. When the closed-circuit voltage reaches 2.38V and the differential capacity drops to 64.3% of the characteristic reduction peak intensity of the additive, the external charging current is cut off and the system enters the open-circuit relaxation state.
[0068] During the open-circuit relaxation process, the rate of change of the open-circuit voltage over time is continuously calculated with a period of 10 seconds, and the termination criterion for the open-circuit voltage recovery rate is calibrated on-site. When the rate of change of the open-circuit voltage is within the range of 0.05mV / min to 0.10mV / min for three consecutive sampling periods, and the open-circuit voltage recovery rate is measured to be 0.06mV / min when the relaxation continues until the 8.5th minute, the open-circuit relaxation is terminated, and the open-circuit reference voltage at the current moment is read. As a benchmark for subsequent calculation of apparent polarization voltage drop, the additive molecules consumed in the deep pores of the thick electrode are replenished through diffusion during open-circuit relaxation and form an inorganic passivation inner layer.
[0069] During on-site calibration, the control system synchronizes the temperature sensor and voltage acquisition channel within the fixture, introducing a temperature drift compensation correction factor of 0.015mV / ℃. This correction factor is obtained by conducting a step-up thermoelectric potential calibration test on the no-current unloaded formation test fixture within the range of 40℃ to 50℃. In each calculation cycle, the thermoelectric potential drift component is subtracted based on the ambient temperature fluctuation. The temperature is maintained within the range of 45℃±0.5℃, and three effective slope values are continuously acquired. When the open-circuit voltage change rate after temperature drift compensation is stable in the range of 0.05mV / min to 0.10mV / min, the open-circuit relaxation termination signal is triggered.
[0070] Within the main solvent decomposition potential range where the closed-circuit voltage is between 2.55V and 3.10V, the first-step current is applied sequentially. Charge to 2.75V, second-stage current. Charge to 2.95V and use the third-step current. Continue step-by-step charging; during each step-by-step charging process, based on the closed-circuit voltage at the current sampling time... With open-circuit reference voltage The difference is calculated in real time to determine the apparent polarization voltage drop when the third-step current is used. When the closed-circuit voltage reaches 3.04V, the apparent polarization voltage drops to 48mV, exceeding the upper limit threshold of 45mV. The control system responds within 100ms, reducing the current step current by 20% to 0.096C and maintaining the reduced current to continue charging until the second cutoff potential. .
[0071] During dynamic current adjustment, after the control system completes a 20% current reduction, it locks the current level in one direction. Even if subsequent sampling detects that the apparent polarization voltage drop has fallen below 45mV, the current level is maintained and not adjusted upwards to avoid interface polarization fluctuations caused by repeated current switching. If, after a current reduction, the apparent polarization voltage drop still exceeds the 45mV polarization upper limit threshold within 5 consecutive sampling cycles, the secondary current reduction protection is triggered, and the current is reduced by another 10% until the apparent polarization voltage drop falls below the threshold or the closed-circuit voltage reaches the second cutoff potential of 3.10V, before proceeding to the next stage of charging.
[0072] Apply main charging current Constant current charging to the upper limit cutoff potential It then switches to 3.65V constant voltage charging until the circuit current decays to the cutoff current threshold. Then, the charging was terminated; the battery was transferred to an aging chamber at 45°C and left to stand open for 36 hours to remove gaseous byproducts and perform a second negative pressure laser sealing. Then, it was discharged at a constant current of 0.2C at 25°C to the lower limit cutoff voltage of 2.50V to complete the step-by-step formation and shaping.
[0073] Example 6: In this example, a 314Ah lithium iron phosphate grid storage battery was selected, with a positive electrode single-sided active coating capacity of 4.2 mAh / cm², a positive active material layer thickness of 125 μm and a compaction density of 2.45 g / cm³, and a negative electrode single-sided coating capacity of 4.6 mAh / cm² and a compaction density of 1.55 g / cm³. An electrolyte containing a 3:7 volume ratio of ethylene carbonate and methyl ethyl carbonate, and 2% by mass of vinylene carbonate and 1% lithium difluorophosphate was injected. The battery was placed in a fixture with the temperature controlled at 45°C, and a pre-tightening pressure of 0.2 MPa was applied mechanically. A constant micro-current was applied using a charge / discharge circuit. That is, constant current charging at 4.71A to the first cutoff potential. The circuit is then disconnected; subsequently, a gradient current of 7.85A (0.025C) is applied. The current is stepped up to 0.05C (15.7A) at a rate of 0.003C per minute, with sampling intervals of 2 seconds during this period. Online acquisition of closed-circuit voltage With the amount of electricity charged Calculate the differential capacity: ,in, and These represent the charge input at the current time and the previous sampling time, respectively. and These are the closed-circuit voltages at the corresponding sampling times. The time sampling interval is denoted as .
[0074] During online calculations at industrial charging and discharging sites, the control system employs first-order differential sign inversion and continuous multi-point confirmation logic to track the peak value of additive feature reduction in real time. It continuously calculates the first-order slope of the differential capacity with a fixed sampling period of 2 seconds. When the slope changes from positive to negative, and the subsequent three consecutive sampling points maintain a negative slope, it is determined that the local maximum peak has been exceeded, and the differential capacity at the inflection point is locked and stored as the peak intensity of additive feature reduction. Subsequently, it continuously calculates the ratio of the differential capacity at the current sampling point to this peak intensity. When this ratio monotonically decreases from a high point to a preset ratio range of 60% to 70%, the control system responds within 100ms and issues a current cut-off command to determine the endpoint of the film-forming additive reduction reaction online under strong background electrical noise interference.
[0075] When the charging voltage is between 2.20V and 2.55V and reaches 2.38V, the identified additive characteristic reduction peak is 412Ah / V. When charging continues to 2.48V, the differential capacity decreases to 265Ah / V, which is 64.3% of the peak value. The control system cuts off the charging current and enters an open-circuit relaxation state. During this state, the rate of change of the open-circuit voltage over time is monitored. When relaxation continues for 8.5 minutes and the open-circuit voltage recovery rate decreases to 0.06mV / min, the following condition is met: The termination condition is to terminate open-circuit relaxation and read the open-circuit reference voltage at the current moment. During open-circuit relaxation, the film-forming additive molecules consumed in the deep pores of the electrode are replenished in situ through concentration gradient diffusion at the thermodynamic equilibrium potential, and form a dense inorganic passivation layer before the main solvent decomposes.
[0076] Within the main solvent decomposition potential range of 2.55V to 3.10V, the first-step current is applied sequentially. That is, charging from 15.7A to 2.75V, the second step current. That is, charging to 2.95V at 25.12A, using the third-step current. That is, continue step charging at 37.68A; during each step charging process, based on the closed-circuit voltage at the current sampling time... With open-circuit reference voltage Calculate the apparent polarization voltage drop: When using the third-step current When the closed-circuit voltage reaches 3.04V, the calculated apparent polarization voltage drop rises to 48mV and exceeds the upper polarization threshold of 45mV. The control system then reduces the current step current by 20% to 0.096C, or 30.14A, and maintains the reduced current to charge to the second cutoff potential. This balances the gas generation rate with the outflow flux through the electrode pores; subsequently, the main charging current is applied. That is, constant current charging at 56.52A until the upper limit cutoff potential is reached. It then switches to 3.65V constant voltage charging until the circuit current decays to the cutoff current threshold. That is, the charging circuit is cut off at 6.28A; the charged battery is transferred to an open-circuit aging chamber at 45℃ and left to stand for 36 hours to remove gaseous byproducts and perform secondary negative pressure laser sealing; then it is discharged at a constant current of 0.2C (62.8A) at an ambient temperature of 25℃ to the lower limit cutoff voltage of 2.5V to complete the step-by-step formation and shaping.
[0077] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for grading of a battery for grid energy storage, characterized in that, Includes the following steps: Step S101: Control the energy storage battery to be formed to be in an environment with a temperature of 40°C to 50°C and a pre-tightening pressure of 0.1MPa to 0.3MPa, and apply a constant micro-current of 0.010C to 0.025C to charge it to the first cutoff potential of 2.00V to 2.20V and then cut off. Step S102: Apply gradient current to continue charging, collect the charged capacity and closed-circuit voltage of the battery to be formed online, and calculate the differential capacity. When the differential capacity exceeds the characteristic reduction peak of the additive in the potential range of 2.20V to 2.55V and drops to 60% to 70% of the peak intensity, it enters the open-circuit relaxation state. Relaxation is terminated when the open-circuit voltage recovery rate is lower than or equal to 0.10mV / min and the open-circuit relaxation time reaches 5min to 15min. Record the open-circuit reference voltage at the termination time. Step S103: Apply a stepped increasing current to charge within the potential range of 2.55V to 3.10V, and calculate the apparent polarization voltage drop between the current closed-circuit voltage and the open-circuit reference voltage in real time during each step charging process. When the apparent polarization voltage drop exceeds the upper limit threshold of polarization of 40mV to 50mV, reduce the current step current by 15% to 20% until the closed-circuit voltage reaches the second cutoff potential of 3.10V. In step S104, a main charging current of 0.150C to 0.200C is applied to charge the battery at a constant current until the upper limit cutoff potential of 3.35V to 3.72V is reached, and then constant voltage charging is switched to continue until the charging current decays to the cutoff current threshold of 0.016C to 0.022C, at which point charging is terminated. In step S105, the charged energy storage battery to be formed is left to stand in an open circuit in a constant temperature environment. After the gaseous byproducts are discharged, it is sealed under negative pressure and discharged at a constant current of 0.190C to 0.210C until the lower limit cutoff voltage of 2.25V to 2.51V is reached.
2. The cascaded formation method for grid energy storage batteries according to claim 1, characterized in that, In step S101, before the energy storage battery to be formed is placed in an environment with a temperature of 40°C to 50°C and a pre-tightening pressure of 0.1MPa to 0.3MPa, it is first injected with electrolyte and allowed to stand and soak at 40°C to 50°C for 22h to 25h; during the charging process in step S101, the pre-tightening pressure is controlled at 0.12MPa to 0.22MPa, the temperature at 40°C to 50°C, the constant micro-current at 0.018C to 0.025C, the first cutoff potential at 2.05V to 2.20V, and the charging duration at 2.0h to 2.5h.
3. The cascaded formation method for grid energy storage batteries according to claim 1, characterized in that, In step S102, the initial current of the gradient current boost is set to 0.020C to 0.030C, and the current is boosted to 0.050C in a linear rate of 0.002C to 0.005C per minute. Within the potential range of 2.20V to 2.55V, the characteristic electrochemical reduction peak of the film-forming additive is identified by differential capacity. When the charging voltage reaches 2.38V to 2.48V and the differential capacity exceeds the characteristic reduction peak of the additive and decreases to 60% to 70% of the characteristic reduction peak of the additive, the applied charging current is cut off and the system enters an open-circuit relaxation state.
4. The cascaded formation method for grid energy storage batteries according to claim 1, characterized in that, In step S102, the duration of the open-circuit relaxation state is set to 5 min to 15 min. During the open-circuit relaxation state, the open-circuit voltage is collected in real time and its rate of change over time is calculated. When the absolute value of the rate of change decreases to the range of 0.05 mV / min to 0.10 mV / min, the relaxation is terminated. At the termination time, the open-circuit reference voltage is read and stored as the reference potential for calculating the apparent polarization voltage drop in step S103.
5. The cascaded formation method for grid energy storage batteries according to claim 1, characterized in that, In step S103, the potential range of 2.55V to 3.10V is the main solvent decomposition potential range, and the step-increasing current includes a first step current of 0.045C to 0.051C, a second step current of 0.076C to 0.082C, and a third step current of 0.113C to 0.121C applied sequentially. The switching voltage node of each step current is set as follows: when the first step current is charged to the closed-circuit voltage of 2.65V to 2.80V, the second step current is switched; when the second step current is charged to the closed-circuit voltage of 2.88V to 2.96V, the third step current is switched.
6. The cascaded formation method for grid energy storage batteries according to claim 1, characterized in that, In step S103, the apparent polarization voltage drop is the difference between the closed-circuit voltage and the open-circuit reference voltage at the current sampling time. During each step current charging process, when the apparent polarization voltage drop exceeds 45mV, the setting value of the current step current level is reduced by 15% to 20%, and the reduced current is maintained to charge to the corresponding switching voltage node or the second cutoff potential of 3.10V.
7. The cascaded formation method for grid energy storage batteries according to claim 1, characterized in that, In step S104, the main charging current is 0.180C. After constant charging with the main charging current to the upper limit cutoff potential of 3.65V, the potential of 3.65V is maintained for constant voltage charging until the charging circuit current decays to the cutoff current threshold of 0.020C and then the charging circuit is cut off, thus completing the lithium-ion intercalation in the main phase transition region of the graphite anode.
8. The cascaded formation method for grid energy storage batteries according to claim 1, characterized in that, In step S105, the energy storage battery to be formed after completing the charging in step S104 is transferred to a high-temperature aging chamber at a temperature of 43°C to 47°C and left to stand for 24 to 48 hours with the circuit open. After standing, the air bag is punctured to perform negative pressure evacuation and exhaust, and a second laser sealing is performed. Then, under an ambient temperature of 22°C to 27°C, it is discharged at a constant current of 0.19°C to 0.21°C to the lower limit cutoff voltage of 2.42V to 2.51V to complete the electrochemical steady-state shaping.
9. A cascaded formation method for grid energy storage batteries according to claim 1, characterized in that, The energy storage battery to be formed is a lithium iron phosphate battery with a nominal single-cell capacity of not less than 280Ah. Its positive electrode sheet has a single-sided active coating with a coating capacity of not less than 3.8mAh / cm², a positive electrode active material layer thickness of 100μm to 140μm, and an electrolyte containing 1.5% to 2.5% by mass of vinylene carbonate and 0.8% to 1.2% by mass of lithium difluorophosphate.
Citation Information
Patent Citations
Formation method for improving cycling stability of silicon-containing soft package lithium ion battery
CN120376798A
Dynamic depolarization balancing process
CN122716464A