A continuous casting process to prevent nozzle clogging in aluminum-containing steel ladles

By employing argon filling in the tundish, micro-calcium treatment, and full-process argon protection during continuous casting, the problem of nozzle nodule formation was solved, ensuring the purity of the cast billet, simplifying the operation process, and reducing production costs.

CN123060064APending Publication Date: 2026-11-10NANJING IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611268846.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the continuous casting process, the current technology causes nozzle formation to affect the quality of the cast billet, reduce production efficiency and increase production costs. Furthermore, the calcium treatment process has a narrow window, high cost and poor adaptability, making it difficult to effectively prevent nozzle formation in aluminum-containing steel ladles.

Method used

The process of argon filling in the tundish during continuous casting, micro-calcium treatment in the impact zone of the tundish during casting, and argon filling throughout the casting process is adopted. Through high-flow-rate argon replacement and continuous low-flow-rate argon protection, the oxidation of molten steel is prevented, high-melting-point Al2O3 is converted into low-melting-point calcium aluminate, and nozzle nodule formation is prevented.

Benefits of technology

It effectively prevents nozzle clogging, ensures the purity of the cast billet, simplifies the operation process, reduces equipment requirements, avoids complex flow control systems, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060064A_ABST
    Figure CN123060064A_ABST
Patent Text Reader

Abstract

This invention discloses a continuous casting process for preventing tundish nozzle formation in aluminum-containing steel, belonging to the field of steelmaking technology. Specifically, it includes: (1) hoisting the ladle to the rotary table above the tundish and starting to inject argon gas into the tundish; (2) before pouring the ladle, adding silicon-calcium wire to the impact zone of the continuous casting tundish using an existing wire feeder for calcium treatment, and treating the flocculent Al2O3 that may be generated by secondary oxidation of the molten steel during the pouring process to prevent tundish nozzle formation during the pouring process; (3) during the pouring process, the tundish is kept argon-filled throughout to ensure a low-oxidizing atmosphere in the tundish area, preventing the molten steel from oxidizing and generating flocculent Al2O3, which would lead to tundish nozzle formation. This process is based on continuous casting tundish argon filling, micro-calcium treatment of the impact zone of the tundish during the pouring process, and protection of the pouring process in continuous casting technology. It improves the tundish nozzle formation during continuous casting production and solves the problem that tundish nozzle formation in aluminum-containing steel affects the purity of the billet during the production process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a continuous casting process, specifically a continuous casting process for preventing nodule formation at the tundish nozzle of aluminum-containing steel, belonging to the field of steelmaking technology. Background Technology

[0002] In the continuous casting process, the formation of sprue nozzles is a key problem that affects the quality of cast billets, reduces production efficiency, and increases production costs. Severe sprue formation can lead to nozzle deviation or even blockage, affecting the smooth operation of the continuous casting process.

[0003] Current research has revealed the following formation of nodules: In the initial stage of continuous casting, a thin Fe3O4 layer first forms on the surface of the aluminum-carbon refractory material at the nozzle. High-melting-point nodules, Al2O3, then precipitate on the surface of the Fe3O4 layer. Finally, composite inclusions such as calcium aluminate and magnesium aluminum spinel in the molten steel continuously deposit and grow on the Al2O3 surface, eventually leading to a reduction in the flow area of ​​the nozzle or even complete blockage. It can be seen that the nodules mainly originate from alumina inclusions in the molten steel.

[0004] To address this issue, existing LF refining processes typically employ calcium treatment to transform solid Al2O3 and high-melting-point calcium aluminate into low-melting-point liquid calcium aluminate, promoting their flotation and removal or preventing their adhesion to the inner wall of the nozzle. This improves the quality of the molten steel to some extent and reduces the formation of nodules, thus providing a solution for preventing nozzle nodules. However, the control window for calcium treatment is narrow: insufficient calcium addition results in incomplete transformation, and residual high-melting-point inclusions can still induce nodules; excessive calcium addition or high sulfur content in the molten steel can easily generate CaS or high-melting-point C3A (3CaO·Al2O3) phases, which can exacerbate nodules and nozzle blockage. Furthermore, calcium treatment has poor adaptability to high-sulfur steel, exacerbates refractory material erosion, and is costly and complex to operate.

[0005] Therefore, developing a continuous casting process that can overcome the above defects and prevent nozzle formation in aluminum-containing steel ladles has become a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention

[0006] The technical problem to be solved by this invention is to address the shortcomings of the existing technology by proposing a continuous casting process to prevent tundish nozzle formation in aluminum-containing steel. Based on continuous casting argon filling in the tundish during the initial casting process, micro-calcium treatment of the impact zone in the tundish during the initial casting process, and protective casting process technology, this invention improves the tundish immersion nozzle formation during continuous casting production and solves the problem of tundish immersion nozzle formation affecting the purity of the cast billet in aluminum-containing steel production.

[0007] The technical solution of this invention to solve the above technical problems is: A continuous casting process for preventing nodule formation at the tundish nozzle in aluminum-containing steel, aimed at ensuring the purity of the aluminum-containing steel billet and solving the problem of nodule formation at the tundish submersible nozzle during continuous casting, specifically includes the following steps: (1) The ladle is hoisted to the turntable above the tundish and argon gas is injected into the tundish to ensure a low oxidizing atmosphere inside the tundish; (2) Before the steel ladle is started to pour, calcium treatment is carried out by adding silicon-calcium wire to the impact zone of the continuous casting tundish through the existing wire feeder. The calcium treatment is carried out on the flocculent Al2O3 that may be generated by secondary oxidation of the molten steel during the start of the pouring process to prevent the immersion nozzle from forming nodules during the start of the pouring process. (3) During the steel ladle casting process, the tundish is kept filled with argon throughout to ensure a low oxidizing atmosphere in the tundish area and prevent the molten steel from oxidizing and producing flocculent Al2O3, which would lead to nodule formation at the submerged nozzle.

[0008] The technical solution further defined in this invention is: Furthermore, in the aforementioned continuous casting process for preventing sprue nodules in aluminum-containing steel, during step (1), the argon flow rate is controlled to be greater than 550 L / min and the argon pouring time is greater than 5 min to ensure a low-oxidizing atmosphere in the ladle during the casting process.

[0009] Furthermore, in the aforementioned continuous casting process for preventing nodule formation at the tundish nozzle of aluminum-containing steel, 5-10m of silicon-calcium wire is added during calcium treatment in step (2), which is equivalent to 3-5kg of silicon-calcium wire.

[0010] Furthermore, in the aforementioned continuous casting process for preventing lumps from forming at the tundish nozzle of aluminum-containing steel, the argon flow rate is controlled to be 80-140 L / min during the argon pouring process in step (3).

[0011] The technical effect is that, throughout the entire process from the start of pouring in the ladle to the completion of pouring the molten steel in this furnace, argon gas is continuously injected into the space above the molten steel surface in the tundish without interruption, maintaining a stable replenishment flow rate required for argon gas protection. The continuously injected argon gas creates a slight positive pressure (slightly higher than atmospheric pressure) in the tundish, preventing external air from being sucked in from loose parts such as ladle cover gaps and nozzle connections. The flow rate is controlled at 80-140 liters / minute. Too low a flow rate will not provide an effective seal, while too high a flow rate (such as 550 L / min before pouring) will cause violent churning of the molten steel surface, slag entrapment, and accelerated temperature drop.

[0012] The beneficial effects of this invention are: Compared with the existing technology that commonly uses calcium wire fed in with the flow throughout the process, the present invention adopts centralized treatment before casting. 5-10m of silicon-calcium wire is added to the impact zone at one time before casting. The operation is simpler and the equipment requirements are lower. There is no need for a complex flow matching control system. In addition, even with the protection of step (1), the impact of the steel flow at the moment of casting may still entrain a very small amount of air, or there may be a small amount of oxidation products in the ladle itself. These newly generated Al2O3 are solid, high melting point and very easy to adhere. Calcium treatment can transform these solid Al2O3 into liquid calcium aluminate (such as 12CaO·7Al2O3) that is not easy to adhere to, and cannot be deposited on the inner wall of the nozzle.

[0013] This invention employs a pre-filling + continuous protection argon gas introduction method, involving high-flow-rate replacement (argon flow rate greater than 550 L / min) before casting and a two-stage argon gas protection maintained throughout the casting process. Under safe conditions, this effectively ensures a low-oxidizing atmosphere within the ladle, preventing the formation of flocculent Al2O3 due to steel oxidation, which could lead to nodule formation at the submerged entry nozzle. Specifically: If the tundish is filled with air, when the high-temperature molten steel is poured from the ladle, the Al in the molten steel will react with the oxygen in the air, instantly generating a large number of flocculent Al2O3 (alumina) inclusions. These high-melting-point inclusions are the culprits that cause nozzle nodules. Creating a low-oxygen protective atmosphere in the tundish before pouring can prevent the high-temperature molten steel from coming into contact with air and undergoing secondary oxidation, thus generating Al2O3 inclusions that cause nozzle nodules. This is the first line of defense against nozzle nodules. The argon gas used for continuous protection in the later stage maintains a long-term oxidizing atmosphere inside the ladle, preventing the molten steel from being continuously oxidized throughout the entire casting cycle. At this time, a relatively small and stable flow rate of argon gas is sufficient, as long as it can maintain positive pressure and prevent air backflow. Excessive flow rate will cause the molten steel surface to churn violently, which may instead cause slag entrainment.

[0014] This invention addresses the problem of tundish nozzle formation in the continuous casting process of aluminum-containing steel. By employing argon injection into the tundish during the initial casting stage, micro-calcium treatment of the impact zone in the tundish during the initial casting stage, and argon injection throughout the casting process, this invention prevents tundish nozzle formation in aluminum-containing steel and ensures the purity of the cast billet. Attached Figure Description

[0015] Figure 1 This is a schematic diagram of the opening stopper rod curve in Embodiment 1 of the present invention; Figure 2 This is a schematic diagram of the comparative opening and closing curve of the stopper rod of the present invention. Detailed Implementation

[0016] To make the objectives, technical solutions, and advantages of this application clearer, the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments. The described embodiments should not be considered as limitations on this application. All other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of this application. Unless otherwise defined, all technical and scientific terms used in the embodiments of this application have the same meaning as commonly understood by those skilled in the art. The terminology used in the embodiments of this application is for the purpose of describing the embodiments of this application only and is not intended to limit this application. Example 1

[0017] To ensure the purity of aluminum-containing steel billets and solve the problem of tumbler formation on the tumbler nozzle during continuous casting, this embodiment provides a continuous casting process to prevent tumbler formation on aluminum-containing steel billets, specifically including the following steps: (1) Continuous casting process: A 250*300mm cross-section 4-strand casting machine is adopted; an integral submerged entry nozzle (inner diameter of nozzle: φ45mm) is used. (2) The ladle is hoisted to the turntable above the tundish and argon gas is injected into the tundish. The argon gas injection rate is 575 L / min and the injection time is 6 min to ensure a low oxidizing atmosphere in the ladle during the pouring process. (3) Before the steel ladle is started to pour, 5m of silicon-calcium wire is added to the impact zone of the continuous casting ladle through the existing wire feeder for calcium treatment. This calcium treatment is used to treat the flocculent Al2O3 that may be generated by secondary oxidation of the molten steel during the start of the ladle, and to prevent the immersion nozzle from forming nodules during the start of the pouring process. (4) During the steel ladle casting process, the tundish is kept filled with argon throughout the process, with an argon seal of 100L / min, to ensure a low oxidizing atmosphere in the tundish area and prevent the molten steel from oxidizing and producing flocculent Al2O3, which would lead to nodule formation at the submerged nozzle. (5) During the casting process, the liquid level in the ladle is controlled at 43 tons. After the ladle, the liquid is transported by the submerged nozzle and enters the crystallizer and the second cooling zone to become a billet. The billet is pulled out at a constant speed of 0.85m / min.

[0018] (6) After the initial pouring, the stopper rod curve is stable as shown. Figure 1 As shown, the stopper rod opening degree did not increase. Specific parameters of the adsorbate inside the four runners after production stopped for seven heats are as follows: Figure 1 As shown, its average thickness is 0.58 mm.

[0019] Table 1. Thickness of adsorbate inside the four water outlets in Example 1

[0020] Comparative Example 1 (1) Continuous casting process: A 250*300mm cross-section 4-strand casting machine is adopted; an integral submerged entry nozzle (inner diameter of nozzle: φ45mm) is used. (2) The ladle is hoisted to the turntable above the tundish and argon gas is injected into the tundish at a rate of 575 L / min for 6 min. (3) No silicon-calcium wire is added to the impact zone of the tundish in the initial continuous casting process; (4) During the steel ladle casting process, the tundish is kept filled with argon throughout the process, with an argon sealing rate of 100L / min; (5) During the casting process, the liquid level in the ladle is controlled at 43 tons. After the ladle, the liquid is transported by the submerged nozzle and enters the crystallizer and the second cooling zone to become a billet. The billet is pulled out at a constant speed of 0.85m / min.

[0021] (6) The stopper curve after pouring is as follows Figure 2 As shown, the stopper rod rose abnormally and the opening degree of the stopper rod increased. The adsorbent inside the four runners after the 7th furnace was stopped is shown in Table 2, with an average thickness of 4.8 mm.

[0022] Table 2. Thickness of adsorbate inside the four water outlets in the comparative example.

[0023] As can be seen from Table 1-2, the thickness of the adsorbent inside the final runner of the comparative scheme is much greater than that of the runner after the process of the present invention. The present invention prevents the problem of nodule formation in the immersion runner of aluminum steel and ensures the purity of the aluminum steel billet.

[0024] Based on the existing processes of the steel plant, combined with the argon gas sealing of the ladle to prevent secondary oxidation of molten steel, and the operation of constant ladle liquid level and constant casting speed to ensure the relative stability of molten steel in the continuous casting ladle, the problem of immersion-type nodule formation in the ladle for aluminum-containing steel grades can be basically solved.

[0025] In addition to the embodiments described above, the present invention may have other implementations. All technical solutions formed by equivalent substitution or equivalent transformation fall within the protection scope claimed by the present invention.

Claims

1. A continuous casting process for preventing nodule formation at the tundish nozzle of aluminum-containing steel, characterized in that, Specifically, the following steps are included: (1) The ladle is hoisted to the turntable above the tundish, and argon gas is injected into the tundish to ensure a low oxidizing atmosphere inside the tundish; (2) Before the steel ladle is started to pour, a silicon-calcium wire is added to the impact zone of the continuous casting ladle for calcium treatment; (3) During the ladle casting process, the tundish is kept filled with argon throughout to ensure a low oxidizing atmosphere in the tundish area.

2. The continuous casting process for preventing nodule formation in the tundish nozzle of aluminum-containing steel according to claim 1, characterized in that: In step (1), the argon flow rate is controlled to be greater than 550 L / min and the argon filling time is greater than 5 min.

3. The continuous casting process for preventing nodule formation in the tundish nozzle of aluminum-containing steel according to claim 1, characterized in that: In step (2), 5-10m of silicon-calcium wire is added during calcium treatment.

4. The continuous casting process for preventing nodule formation in the tundish nozzle of aluminum-containing steel according to claim 1, characterized in that: During the pouring process in step (3), the argon flow rate is controlled to be 80-140 L / min.