Crack-free equiaxed heat treatment method and components for additive manufacturing of γ′ phase-strengthened high-temperature-resistant alloys
By employing a multi-stage heat treatment method involving ultra-high temperature solution treatment, controlled slow cooling, and high temperature solution treatment, the problems of liquefaction cracking and microstructure anisotropy in the heat treatment process of additively manufactured γ′ phase-strengthened high-temperature-resistant alloys were solved, achieving a crack-free equiaxed crystal structure and comprehensive mechanical properties of high strength and high toughness.
Patent Information
- Application Number
- CN202611561261.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-10
AI Technical Summary
Additive manufacturing of γ′ phase-strengthened high-temperature-resistant alloys presents problems of liquefaction cracking and microstructure anisotropy during heat treatment. Existing technologies cannot simultaneously achieve crack-free equiaxed crystal structure and excellent mechanical properties.
A multi-stage heat treatment method is adopted, which includes ultra-high temperature solution treatment, controlled slow cooling and high temperature solution treatment. The method includes first-stage solution treatment, controlled slow cooling, second-stage solution treatment and aging treatment. The grain boundary liquid film is re-solidified through the slow cooling time window. Combined with the two-stage aging process, the complete recrystallization and homogenization of the grains are ensured.
It effectively avoids liquefaction cracking during heat treatment, significantly reduces anisotropy, obtains a fully equiaxed crystal structure, and the material exhibits comprehensive mechanical properties of high strength and high toughness at both room temperature and high temperature.
Smart Images

Figure CN123060122A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal additive manufacturing and post-processing technology, and relates to a crack-free equiaxed crystal heat treatment method and components for additive manufacturing of γ′ phase-strengthened high-temperature alloys. It is applicable to the post-processing of γ′ phase-strengthened high-temperature alloy samples and components formed by laser powder bed melting or electron beam powder bed melting. Background Technology
[0002] γ′ phase-reinforced high-temperature-resistance alloys possess excellent high-temperature mechanical properties, oxidation resistance, and corrosion resistance, making them key materials for hot-end components in the aerospace field. Metal additive manufacturing technologies, exemplified by Laser Powder Bed Fusion (LPBF), are based on a discrete-stacking forming concept. They utilize high-energy beams to selectively melt metal powder layer by layer, directly manufacturing complex and intricate structures that are difficult or impossible to achieve using traditional processing methods. This provides unprecedented design freedom and forming capabilities for manufacturing complex γ′ phase-reinforced high-temperature-resistance alloy components.
[0003] However, the inherent rapid melting and cyclic heating characteristics of additive manufacturing technology result in coarse columnar crystals and strong texture in the formed γ′-phase-reinforced high-temperature-resistant alloys such as ZGH451, CM247LC, IN738, and IN939, which have high γ′ content. This leads to significant anisotropy in the mechanical properties of the formed materials in both the transverse and longitudinal directions. Therefore, the mechanical properties of γ′-phase-reinforced high-temperature-resistant alloys in the deposited and printed state cannot meet application requirements, and they must be heat-treated before use.
[0004] Compared to high-temperature alloys manufactured using traditional methods, additively manufactured γ′ phase-strengthened high-temperature-resistance alloys have the following characteristics: (1) Insufficient recrystallization driving force: Unlike forged alloys, additive manufacturing parts lack cold deformation energy storage and rely solely on residual stress to drive recrystallization. Therefore, extremely high solid solution temperatures are required, such as when the solid solution temperature exceeds 1200℃ or even higher, to break grain boundary pinning and achieve the transformation from columnar crystals to equiaxed crystals.
[0005] (2) Severe element segregation at grain boundaries: Due to the non-equilibrium solidification unique to additive manufacturing, elements such as B, C, Ta, and Mo are severely segregated at grain boundaries, resulting in a significant reduction in the non-equilibrium solid phase line at the local melting point of the grain boundaries.
[0006] These two characteristics lead to a core contradiction in the subsequent heat treatment of this type of alloy: a conflict between liquefaction cracking and equiaxed microstructure. Specifically, to achieve equiaxed microstructure and eliminate anisotropy, ultra-high temperature solution treatment is required to provide sufficient recrystallization driving force. However, ultra-high temperatures often exceed the critical temperature at which segregation lowers the liquefaction sensitivity of grain boundaries in that region, causing grain boundary liquefaction. During subsequent rapid cooling (quenching), thermal stress will directly act on the already liquefied and fragile grain boundaries, easily triggering intergranular liquefaction cracking and rendering the part unusable. Conversely, if the solution temperature is lowered to avoid cracking, the recrystallization driving force is insufficient, making complete equiaxed microstructure impossible, and the anisotropy problem remains.
[0007] In the prior art, there are various heat treatment methods for additive manufacturing of high-temperature alloys. For example, Chinese patent CN119525521A discloses a method for preparing high-strength and high-ductility additive manufacturing nickel-based high-temperature alloys. This method uses solution treatment at 1160℃~1200℃ combined with a two-stage aging process. It controls the grain structure and strengthening phase of the alloy through solution treatment and two-stage aging treatment, achieving a synergistic improvement in strength and ductility. Another example is Chinese patent CN119530687A, which discloses a method for controlling the strengthening phase of nickel-based high-temperature alloys based on over-solution treatment. This method designs an over-solution treatment scheme by measuring the γ′ phase transformation temperature to control the precipitation behavior of the γ′ phase and release internal stress in the alloy. However, the above-mentioned prior art mainly focuses on strengthening phase control, residual stress release, and strength and ductility improvement. It has not yet proposed specific control methods for the potential problems of localized grain boundary liquefaction and liquefaction cracking that may occur during the high-temperature solution treatment of high-γ′ content additive manufacturing high-temperature alloys. The existing technology still struggles to simultaneously achieve sufficient equiaxed microstructure and suppression of liquefaction cracking.
[0008] Therefore, there is an urgent need to develop a special heat treatment process for additive manufacturing γ′ phase-reinforced high-temperature-resistant alloys that can effectively suppress or avoid heat treatment grain boundary liquefaction cracking, significantly reduce anisotropy, and obtain excellent mechanical properties. Summary of the Invention
[0009] The purpose of this invention is to overcome the shortcomings of the prior art and provide a crack-free equiaxed crystal heat treatment method and component for additive manufacturing of γ′ phase-strengthened high-temperature-resistant alloys. This method can effectively suppress or completely avoid liquefaction cracking during the heat treatment process; significantly reduce the anisotropy of the additive manufacturing structure and obtain a completely equiaxed crystal structure; and enable the treated sample to have a combination of high strength and high toughness in both room temperature and high temperature environments.
[0010] To achieve the above objectives, the first aspect of the present invention provides a crack-free equiaxed grain heat treatment method for additive manufacturing of γ′ phase-strengthened high-temperature-resistant alloys, the heat treatment method comprising the following steps: S1: The additively manufactured γ′ phase reinforced high heat-resistant alloy sample is heated to the first solid solution temperature and held at the temperature to allow the alloy sample to undergo complete recrystallization, transforming the columnar crystals formed by additive manufacturing into equiaxed crystals, and obtaining the first solid solution sample. S2: The first solid solution sample is slowly cooled from the first solid solution temperature to the second solid solution temperature at a first set cooling rate to obtain a slowly cooled sample. S3: The slowly cooled sample is kept at the second solid solution temperature to obtain the second solid solution sample; S4: Cool the second solid solution sample to room temperature to obtain a solid solution sample; S5: The solid solution sample is subjected to aging treatment to obtain a heat-treated alloy.
[0011] Further, in step S1, the first solution temperature satisfies the following relationship: T1=T EL +ΔT; Where T1 is the first solution temperature, T EL ΔT represents the liquefaction initiation temperature of the low-melting-point region at the grain boundaries of the alloy sample, and ΔT is the incremental temperature, ranging from 10 to 50 °C. The first solution treatment is to provide sufficient thermal driving force to drive the printed columnar crystals to undergo complete recrystallization and transform into equiaxed crystals.
[0012] Furthermore, in step S2, the second solution temperature T2 satisfies: T2 < T EL And T2≥T pre Among them, T EL T represents the liquefaction initiation temperature of the low-melting-point region at the grain boundaries of the alloy sample. pre This is the initial precipitation temperature of the γ′ strengthening phase in the alloy sample. The second solution treatment is to ensure complete solidification of the grain boundaries and to bring the matrix alloying elements into a supersaturated solution state.
[0013] Furthermore, the liquefaction initiation temperature of the low melting point region at the grain boundary is the endothermic peak initiation temperature determined by differential thermal analysis (DTA) or differential scanning calorimetry (DSC), and the precipitation initiation temperature is the critical temperature at which the γ′ strengthening phase begins to precipitate, determined by differential thermal analysis or differential scanning calorimetry.
[0014] Further, in step S2, the first set cooling rate is set to the rate at which the liquid film at the grain boundary can completely solidify during the slow cooling process, and the first set cooling rate is 0.1~5℃ / min. Cooling from the first solution temperature to the second solution temperature by the first set cooling rate is to avoid applying excessive quenching stress in the liquid state at the grain boundary, and to utilize the slow cooling time window to allow the diffusion of segregated elements at the grain boundary, thereby promoting the re-solidification of the liquid film at the grain boundary and restoring the solid strength of the grain boundary.
[0015] Further, in step S5, the solid solution sample is subjected to aging treatment to obtain a heat-treated alloy, including: S51: The solid solution sample is heated to the first aging temperature and held at that temperature to obtain the first aging sample; S52: The first aged sample is continuously cooled to the second aging temperature at a second set cooling rate and held at that temperature to obtain the second aged sample; S53: Cool the second aged sample to room temperature to obtain the heat-treated alloy.
[0016] Furthermore, the first-stage aging temperature is 1050℃~1140℃, the second-stage aging temperature is 800℃~900℃, the second set cooling rate is set according to the precipitation kinetics of the γ′ strengthening phase in the alloy sample, the second set cooling rate is 0.5~5℃ / min, and the cooling to room temperature is achieved by air cooling or water cooling.
[0017] Further, the alloy sample is any one of Ni-based superalloys, Co-based superalloys, or high-entropy alloys, wherein the Ni-based superalloy is ZGH451, M247, IN738, or René (such as René 88, René 104, René N5, René N6) series alloys. For M247 and René series alloys, T... EL and T pre The values vary depending on the specific components, and those skilled in the art can adjust the process parameters accordingly after DSC determination using the method disclosed in this invention.
[0018] Furthermore, the holding time for each step is determined based on the effective cross-sectional thickness D of the alloy sample, and satisfies: t ≥ t base +λ×D; where t base Based on the time constant, t corresponding to different steps base It can be selected as a single value, where λ is the thickness coefficient, and the value range is 0.02~0.2h / mm.
[0019] Preferably: during the first stage of solution treatment, t base The time can be 1 to 5 hours; during the second stage of solution treatment, t base The value can be 0.5 to 2 hours; t is used for the first level of timeliness processing. base The value can be 4 to 16 hours; t is used for the second level of timeliness processing. base The value can be 8 to 20 hours.
[0020] The second aspect of the present invention also provides an additively manufactured γ′ phase reinforced high heat-bearing alloy component, which is obtained by the above-mentioned heat treatment method. Its microstructure is a crack-free, fully equiaxed crystal structure, with a room temperature tensile strength ≥1100MPa, an elongation ≥15%, and a difference rate of transverse and longitudinal tensile strength <5% and an elongation difference rate <10% at room temperature and 1000℃.
[0021] Compared with the prior art, the present invention has the following advantages and positive effects: (1) Effectively avoids or suppresses heat treatment liquefaction cracking. This invention adopts a solution treatment scheme of "ultra-high temperature solution treatment, controlled slow cooling, and high temperature solution treatment". By introducing a controlled slow cooling step, the liquid film at the grain boundaries is allowed to re-solidify through solute diffusion during the slow cooling process, fundamentally avoiding intergranular cracking caused by quenching stress. Experiments show that the comparative sample treated with traditional single ultra-high temperature solution treatment (1250℃) followed by direct air cooling produced a large number of intergranular cracks, while the sample treated by the method of this invention was completely crack-free.
[0022] (2) Significantly reduced anisotropy. The first-stage ultra-high temperature solid solution provides a strong driving force for recrystallization, which, combined with the second-stage high-temperature solid solution treatment, promotes complete recrystallization and the full growth and homogenization of equiaxed grains, thereby significantly weakening the anisotropy of the material. Experiments show that after treatment by the method of this invention, the grain morphology of the sample is completely equiaxed, and the transverse and longitudinal tensile property curves at room temperature and 1000℃ almost coincide, with the difference rate of transverse and longitudinal tensile strength <5% and the difference rate of elongation <10%.
[0023] (3) Significantly improved overall performance. Based on the uniform equiaxed, crack-free microstructure obtained by multi-stage solution treatment, combined with the continuous two-stage aging process, the material exhibits higher and more uniform strength and plasticity at both room temperature and high temperature. After treatment by the method of this invention, the sample has a room temperature tensile strength ≥1100MPa and an elongation ≥15%.
[0024] (4) Highly compatible with existing heat treatment equipment. The method of this invention can be directly implemented in conventional vacuum heat treatment furnaces or atmosphere-protected heat treatment furnaces without the need for additional special equipment. The total heat treatment cycle is only increased by a limited time (2-8 hours) of controllable slow cooling section compared to the traditional single-stage solution treatment and aging process. It has extremely high industrial practical value and promising prospects for promotion and application. Attached Figure Description
[0025] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0026] Figure 1 This is a process flow diagram of the additive manufacturing method for crack-free equiaxed grain heat treatment of γ′ phase-reinforced high-temperature-resistant alloys according to the present invention. Figure 2 Comparison diagrams of the final heat-treated metallographic structures of Example 1 and Comparative Examples 1-2. Detailed Implementation
[0027] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments, and those skilled in the art can make several modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.
[0028] In this invention, the term "liquefaction initiation temperature of the low-melting-point region at the grain boundary" refers to the critical temperature at which the low-melting-point region at the grain boundary begins to liquefy during the heating process of an additively manufactured γ′ phase-reinforced high-temperature-resistant alloy. The low-melting-point region at the grain boundary includes elemental segregation regions formed by non-equilibrium solidification during additive manufacturing, low-melting-point second phases, and combinations thereof. Specifically, the elemental segregation regions refer to areas formed by the enrichment of elements such as B, C, Ta, and Mo at the grain boundaries; the low-melting-point second phase includes, but is not limited to, Laves phase, borides, and γ / γ′ eutectic phases. The specific composition of the aforementioned low-melting-point region may vary depending on the alloy grade and additive manufacturing process parameters.
[0029] In the following embodiments, the liquefaction initiation temperature T in the low-melting-point region of the alloy grain boundaries EL and the temperature at which the γ′ strengthening phase begins to precipitate T pre All measurements were performed using differential scanning calorimetry (DSC). The test conditions were: argon protective atmosphere, heating rate 10℃ / min, cooling rate 10℃ / min, sample mass 10–20 mg, Al₂O₃ crucible, and T measured. EL Read the onset temperature of the endothermic peak at time, and measure T. pre The onset temperature of the exothermic peak is read at regular intervals. The process conditions used in the following embodiments are exemplary, and their possible ranges are as shown in the foregoing description of the invention. For process parameters not specifically specified, conventional techniques can be used. The detection methods used in the following embodiments are all conventional detection methods in this industry.
[0030] Before describing the specific embodiments in detail, the process principle of the present invention will be explained first, so as to more clearly understand the design intent and synergistic mechanism of each step.
[0031] I. The contradiction between liquefaction cracking and equiaxed microstructure in the heat treatment of additive manufacturing γ′ phase reinforced high-temperature-resistant alloys Additive manufacturing of γ′ phase-reinforced high-temperature-resistant alloys has two key characteristics: first, a lack of cold deformation energy storage and insufficient recrystallization driving force, requiring ultra-high temperatures (typically exceeding the grain boundary eutectic phase liquefaction temperature T). EL Only by performing the following steps can complete recrystallization be achieved, transforming the printed columnar crystals into equiaxed crystals and thus eliminating anisotropy; secondly, severe segregation of elements such as B, C, Ta, and Mo occurs at the grain boundaries, significantly reducing the local melting point of the grain boundaries. During ultra-high temperature solid solution, the low-melting-point eutectic region at the grain boundaries liquefies, forming a liquid film.
[0032] These two key characteristics determine the core challenge faced by this type of alloy in heat treatment: to achieve complete equiaxation, it is necessary to apply heat exceeding the liquefaction initiation temperature T in the low-melting-point region of the grain boundaries. EL Extremely high temperature (i.e., T1 > T) EL However, extremely high temperatures lead to grain boundary liquefaction and a sharp drop in grain boundary strength. If rapid cooling is applied at this point, thermal stress will cause cracks to initiate and propagate at the grain boundary liquid film, rendering the part unusable. To avoid cracking, the solution temperature is lowered to T... EL Although grain boundary liquefaction can be avoided, the thermal driving force is insufficient to drive complete recrystallization, the columnar crystal texture is partially preserved, and the anisotropy problem still exists.
[0033] like Figure 1 As shown, this embodiment of the invention provides a crack-free equiaxed heat treatment method for additive manufacturing of γ′ phase-strengthened high-temperature-resistant alloys, the method comprising the following steps: S1 (First-stage solution treatment): The additively manufactured γ′ phase-reinforced high-temperature-resistant alloy sample is heated to the first solution temperature and held at that temperature to allow the alloy sample to undergo complete recrystallization, transforming the columnar crystals formed by additive manufacturing into equiaxed crystals, thus obtaining the first solution-state sample.
[0034] In this step, the first solution temperature T1 satisfies T1=T EL +ΔT, where T EL ΔT represents the liquefaction initiation temperature in the low-melting-point region of the alloy grain boundaries, and ΔT is the incremental temperature, ranging from 10 to 50°C. This step provides sufficient recrystallization driving force through ultra-high temperature solid solution, causing the printed columnar crystals to undergo complete recrystallization and transform into equiaxed crystals, thus eliminating anisotropy at its source.
[0035] S2 (Controllable Slow Cooling): The first solid solution sample is slowly cooled from the first solid solution temperature to the second solid solution temperature at a first set cooling rate to obtain a slowly cooled sample.
[0036] This step differs from the conventional multi-stage heat treatment with its rapid temperature rise or stepped heating; it is a controlled, continuous cooling process from the first solution temperature T1 to the second solution temperature T2. During this process, the sample does not undergo rapid quenching, avoiding the application of sudden thermal stress to the grain boundary liquid film. Simultaneously, the time window provided by slow cooling allows grain boundary segregating elements (such as B, C, Ta, Mo, etc.) to diffuse sufficiently. The liquid film at the grain boundaries undergoes solute redistribution and epitaxial resolidification during cooling, thereby eliminating the liquid film and restoring the solid-state strength of the grain boundaries. The first set cooling rate is determined based on the time required for complete solidification of the grain boundary liquid film in the alloy sample, and is typically set to 0.1~5℃ / min.
[0037] S3 (Second-stage solution treatment): The slowly cooled sample is kept at the second solution temperature to obtain the second solution sample.
[0038] In this step, the second solution temperature T2 satisfies T2 < T EL And T2≥T pre T pre This is the initial precipitation temperature of the γ′ strengthening phase. This step ensures complete solidification of the grain boundaries and places the matrix alloying elements in a supersaturated solid solution state, further optimizing the grain morphology.
[0039] S4 (rapid cooling): Cool the second solid solution sample to room temperature to obtain a solid solution sample; S5 (Aging Treatment): The solid solution sample is subjected to aging treatment to obtain the heat-treated alloy.
[0040] In this step, the aging treatment includes: heating the solid solution sample to the first-stage aging temperature T3 (1050℃~1140℃) and holding it at that temperature to obtain the first-aged sample; continuously cooling it to the second-stage aging temperature T4 (800℃~900℃) at a second set cooling rate (0.5~5℃ / min, set according to the precipitation kinetics of the γ′ strengthening phase) and holding it at that temperature to obtain the second-aged sample; and finally cooling it to room temperature. This process enables the γ′ strengthening phase to form an optimized bimodal distribution, while simultaneously precipitating grain boundary carbides, thus comprehensively improving the mechanical properties.
[0041] In the above heat treatment method, the holding time t in each step is determined based on the effective cross-sectional thickness D of the sample, satisfying t ≥ t base +λ×D, where λ is the thickness coefficient, ranging from 0.02 to 0.2 h / mm. t for each step... base The values can be taken independently. For example, the heat preservation time for the solution treatment in step S1 can be 1 to 5 hours, the heat preservation time for the solution treatment in step S3 can be 0.5 to 2 hours, and the heat preservation time for the two-stage aging treatment in step S5 can be 4 to 16 hours and 8 to 20 hours, respectively.
[0042] The present invention further illustrates the above-mentioned crack-free equiaxed crystal heat treatment method through the following specific embodiments.
[0043] Example 1: This embodiment uses ZGH451 high-temperature alloy, a typical representative grade of γ′ phase-strengthened high-temperature-resistant alloys, to provide a crack-free equiaxed grain heat treatment method for laser powder bed melting forming of γ′ phase-strengthened high-temperature-resistant alloys. The specific steps are as follows: Step 1: First-stage solution treatment: The ZGH451 high-temperature alloy sample formed by laser powder bed melting (LPBF) technology is placed in a heat treatment furnace and heated to 1250°C, and held at this temperature for 4 hours to allow the alloying elements to diffuse and homogenize fully and to complete recrystallization, transforming the printed columnar crystals into equiaxed crystals. In this embodiment, the liquefaction initiation temperature T in the low-melting-point region of the grain boundaries of the ZGH451 alloy is... EL The temperature was approximately 1210℃ according to DSC measurement. ΔT was taken as 40℃, and T1 = T. EL +40℃ = 1250℃.
[0044] Step 2: Controlled slow cooling: After completing the first stage of solution treatment, without opening the furnace door, control the furnace cooling rate to 3.5℃ / min, and slowly and uniformly cool the sample to 1180℃ to obtain a slow-cooled sample.
[0045] Step 3: Second-stage solution treatment: Once the furnace temperature reaches 1180℃, immediately hold at this temperature for 1 hour to perform the second-stage solution treatment. In this embodiment, the precipitation temperature T of the γ′ strengthening phase in the ZGH451 alloy is... pre The temperature was approximately 1145℃ according to DSC, and T2 = 1180℃, satisfying T2 ≥ T. pre conditions.
[0046] Step 4: Rapid Cooling and Continuous Aging Treatment: After completing the second-stage solution treatment, the sample is quickly removed from the heat treatment furnace and cooled to room temperature in still air to obtain a solution-treated sample. The solution-treated sample is then placed back into the heat treatment furnace and heated to 1120℃, held for 4 hours (first-stage aging) to obtain a first-aged sample. Subsequently, without removing the sample, it is directly cooled to 850℃ in the furnace at a controlled rate of 3℃ / min and held at this temperature for 15 hours (second-stage aging) to obtain a second-aged sample. Finally, the sample is removed and cooled to room temperature in still air to obtain the final heat-treated ZGH451 high-temperature alloy sample.
[0047] Comparative Example 1: This comparative example employs a single ultra-high temperature solution treatment process to further investigate the effect of solution temperature on multi-stage treatment. The specific steps are as follows: (1) Solution treatment: The same batch and specification of LPBF-formed ZGH451 high-temperature alloy sample as in Example 1 was used for solution treatment at 1250℃ and held for 4 hours.
[0048] (2) Rapid cooling: After the solution treatment is completed, the sample is directly removed from the furnace and cooled to room temperature in still air to obtain a solution-treated sample. The controlled slow cooling and second-stage solution treatment steps in Example 1 are omitted.
[0049] (3) Continuous aging treatment: The above-mentioned solid solution sample was placed back into the heat treatment furnace and heated to 1120°C with the furnace and held for 4 hours; then cooled to 850°C with the furnace at a controlled rate of 3°C / min and held for 15 hours; finally, it was taken out and air-cooled to room temperature.
[0050] Comparative Example 2: This comparative example employs a single high-temperature solution treatment process to further investigate the effect of solution temperature on multi-stage treatment. The specific steps are as follows: (1) Solution treatment: The same batch and specification of LPBF-formed ZGH451 high-temperature alloy sample as in Example 1 was used for solution treatment at 1180℃ and held for 4 hours.
[0051] (2) Rapid cooling: After the solution treatment is completed, the sample is directly taken out of the furnace and cooled to room temperature in still air to obtain a solution-treated sample. The ultra-high temperature solution treatment and controlled slow cooling steps in Example 1 are omitted.
[0052] (3) Continuous aging treatment: Same as comparative example 1.
[0053] To verify the effect of the above heat treatment method on the microstructure and macroscopic properties of the materials, metallographic observation and mechanical property testing were performed on the samples prepared in Example 1 and Comparative Examples 1-2. The specific test methods and results are as follows.
[0054] I. Testing Method: Room temperature tensile properties: In accordance with GB / T 228.1-2021 "Metallic materials - Tensile testing - Part 1: Test at room temperature", the transverse and longitudinal properties of the samples at room temperature were tested using a universal tensile testing machine.
[0055] High-temperature tensile properties: In accordance with GB / T 228.2-2015 "Metallic materials - Tensile testing - Part 2: High-temperature test method", the transverse and longitudinal properties of the samples at 1000℃ were tested using a universal tensile testing machine equipped with a high-temperature chamber.
[0056] Metallographic analysis: The metallographic structure of the samples in the final heat-treated state was observed and analyzed using a Zeiss Axio Imager metallographic microscope.
[0057] II. Test Results: (a) Anisotropy Contrast The anisotropy of tensile properties of ZGH451 alloy at room temperature and 1000℃ in different states in Example 1 is shown in Table 1 below: Table 1: Comparison of anisotropy of tensile properties of ZGH451 alloy at room temperature and 1000℃ in different states
[0058] As shown in Table 1 above, the LPBF-printed samples exhibited significant differences in transverse and longitudinal tensile properties at room temperature and 1000℃. After treatment using the method described in Example 1 of this invention, the difference in tensile strength between the transverse and longitudinal directions of the ZGH451 alloy at room temperature decreased from 86 MPa to 31 MPa, with the difference rate decreasing from 7.90% to 2.59%. In particular, at 1000℃, the difference in tensile strength between the transverse and longitudinal directions decreased from 182 MPa to 18 MPa, with the difference rate decreasing from 51.12% to 4.39%. Simultaneously, the difference rate of elongation at room temperature decreased from 20.67% to 6.51%, and at 1000℃, the difference rate of elongation decreased from 98.31% to 9.17%, indicating that the anisotropy of the alloy's tensile properties was significantly weakened after heat treatment.
[0059] (II) Microscopic tissue comparison Figure 2 The following are comparison diagrams of the final heat-treated metallographic structures of Example 1 and Comparative Examples 1-2. In the diagram, (1) and (2) are the longitudinal and transverse structures of Example 1; (3) and (4) are the longitudinal and transverse structures of Comparative Example 1; and (5) and (6) are the longitudinal and transverse structures of Comparative Example 2.
[0060] Comparing Example 1 and Comparative Example 1: Both used ultra-high temperature solution treatment at 1250℃, and both underwent sufficient recrystallization. However, Comparative Example 1 produced a large number of heat treatment cracks (including intragranular, transgranular, and grain boundary cracks), while the microstructure of Example 1 was completely crack-free. This demonstrates that "controlled slow cooling + secondary solution treatment" is crucial for suppressing heat treatment liquefaction cracking at ultra-high solution temperatures.
[0061] Comparing Example 1 and Comparative Example 2: neither showed heat treatment cracks. However, the grains in Comparative Example 2 (solution at 1180℃) did not undergo sufficient recrystallization and still retained some oriented columnar crystal structure; while the grains in Example 1 were uniform equiaxed crystals. This proves that the first-stage ultra-high temperature solution (1250℃) is essential for driving complete recrystallization and completely eliminating the original texture.
[0062] III. Results Analysis and Principle Verification of the Invention The results of Comparative Examples 1 and 2 above profoundly verify the mutually exclusive contradiction between "liquefaction cracking" and "equiaxed microstructure" faced by additively manufactured γ′ phase-strengthened high-temperature-resistant alloys during post-processing: Paradox 1 (as shown in Comparative Example 1): A sufficiently high solution temperature (1250℃) is required to drive complete recrystallization to eliminate anisotropy, but severe stress release and grain boundary liquefaction caused by elemental segregation will result in severe heat treatment cracking.
[0063] Contradiction 2 (as shown in Comparative Example 2): Although lowering the solution temperature (1180℃) can effectively prevent cracking, the thermal driving force is insufficient, the degree of recrystallization is low, and the original columnar crystal structure and anisotropy cannot be eliminated.
[0064] The results of Comparative Examples 1 and 2 above verify the correctness of the aforementioned process principle. This invention successfully reconciles the contradiction between 'liquefaction cracking' and 'equiaxed microstructure' through the synergistic effect of steps S1 to S5. As shown in Table 1, the experimental results fully verify the effectiveness of this invention: while completely suppressing heat treatment cracks (superior to Comparative Example 1), it achieves sufficient recrystallization and microstructure homogenization (superior to Comparative Example 2), ultimately obtaining crack-free, isotropic, high-performance parts.
[0065] Example 2 (different alloy grades IN738): This embodiment verifies the applicability of the method of the present invention to different γ′ phase-strengthened high-temperature-resistant alloys. The IN738 high-temperature alloy sample was formed using LPBF, and the specific steps are as follows: S1: Heat the furnace to 1230℃ and hold for 3 hours. T for IN738 alloy. EL The temperature was measured to be 1195℃ by DSC, and ΔT was taken as 35℃.
[0066] S2: Cool to 1150℃ at 2℃ / min.
[0067] S3: Hold at 1150℃ for 1.5 hours. IN738 alloy T pre The temperature was measured to be 1120℃ by DSC, and T2 = 1150℃, which meets the requirements.
[0068] S4: Air cool to room temperature.
[0069] S5: Heat to 1100℃ in the furnace and hold for 6 hours (first stage aging); cool to 850℃ at 2.5℃ / min and hold for 16 hours (second stage aging); air cool to room temperature.
[0070] Testing revealed that the treated samples formed a fully recrystallized near-equiaxed crystal structure, and no obvious heat treatment cracks were observed. At room temperature, the transverse and longitudinal tensile strengths were approximately 1290 MPa and 1320 MPa, respectively, with a difference of 30 MPa and a difference rate of 2.30%; the transverse and longitudinal elongation were approximately 15.5% and 16.5%, respectively, with a difference of 1.0% and a difference rate of 6.25%. At 1000 °C, the transverse and longitudinal tensile strengths were approximately 365 MPa and 378 MPa, respectively, with a difference of 13 MPa and a difference rate of 3.50%; the transverse and longitudinal elongation were approximately 5.8% and 6.4%, respectively, with a difference of 0.6% and a difference rate of 9.84%. These results demonstrate that the method of this invention significantly weakens anisotropy while achieving a crack-free equiaxed crystal structure, without compromising the material's plasticity.
[0071] Example 3 (Samples with different effective cross-sectional thicknesses): This embodiment verifies the applicability of the method of the present invention to samples of different thicknesses. ZGH451 high-temperature alloy samples formed using LPBF had effective cross-sectional thicknesses D of 10 mm, 30 mm, and 60 mm, respectively. The holding times for each step were set according to t ≥ t. base The calculation is performed using +λ×D, where λ is taken as 0.15 hours / mm, and t is used for each step. base The following values are used: S1 is 2 hours, S3 is 0.5 hours, S5 first-stage aging is 4 hours, and S5 second-stage aging is 8 hours. The process parameters for the remaining steps are the same as in Example 1.
[0072] For samples with a diameter (D) of 10 mm: S1 was maintained at temperature for 4 hours, S3 for 2 hours, S5 was used for the first stage of aging for 6 hours, and S5 was used for the second stage of aging for 10 hours. Testing showed that the microstructure of the treated samples was completely equiaxed and crack-free. At room temperature, the transverse and longitudinal tensile strengths were 1205 MPa and 1172 MPa, respectively, with a difference of 33 MPa and a difference rate of 2.78%. The transverse and longitudinal elongation were 21.0% and 22.5%, respectively, with a difference of 1.5% and a difference rate of 6.90%.
[0073] For samples with a diameter (D) of 30 mm: S1 was maintained for 7 hours, S3 for 5 hours, S5 was used for the first stage of aging for 9 hours, and S5 was used for the second stage of aging for 13 hours. Testing showed that the microstructure of the treated samples was completely equiaxed and crack-free. At room temperature, the transverse and longitudinal tensile strengths were 1188 MPa and 1158 MPa, respectively, with a difference of 30 MPa and a difference rate of 2.55%. The transverse and longitudinal elongations were 20.5% and 22.0%, respectively, with a difference of 1.5% and a difference rate of 7.06%.
[0074] For samples with a diameter (D) of 60 mm: S1 was maintained for 11 hours, S3 for 10 hours, S5 was the first-stage aging for 13 hours, and S5 was the second-stage aging for 17 hours. Testing showed that the microstructure of the treated samples was completely equiaxed and crack-free. At room temperature, the transverse and longitudinal tensile strengths were 1165 MPa and 1138 MPa, respectively, with a difference of 27 MPa and a difference rate of 2.34%. The transverse and longitudinal elongations were 20.0% and 21.3%, respectively, with a difference of 1.3% and a difference rate of 6.30%.
[0075] The above results show that the room temperature tensile strength of the three thickness samples is ≥1100MPa, the elongation is ≥20%, the difference rate of transverse and longitudinal tensile strength is <3%, and the difference rate of transverse and longitudinal elongation is <8%, indicating that the method of the present invention has good adaptability to samples with different cross-sectional thicknesses and the anisotropy is significantly weakened.
[0076] Example 4 (Different Cooling Methods): This embodiment verifies the applicability of different cooling methods in the method of the present invention. In steps S4 and S53, cooling to room temperature can be achieved using air cooling and water cooling, or any other feasible cooling method can be selected; the present invention does not limit this method. The remaining process parameters are the same as in Example 1. Testing showed that the final heat-treated samples obtained by air cooling and water cooling showed no heat-treatment cracks, indicating that rapid cooling after the grain boundaries have fully healed is safe and reliable.
[0077] Example 5 (Boundary verification of aging temperature range): This embodiment verifies the effectiveness of the aging temperature range boundary in the method of the present invention. ZGH451 high-temperature alloy samples formed using LPBF were subjected to the same solution treatment parameters as in Example 1, and the aging treatment was performed under the following three sets of conditions: (1) T3=1050℃ / T4=800℃ (lower limit combination): First stage aging at 1050℃ for 4 hours, cooling to 800℃ at 3℃ / min and holding for 15 hours, followed by air cooling. The microstructure of the treated sample was found to be completely equiaxed and without cracks. The transverse and longitudinal tensile strengths at room temperature were 1185 MPa and 1155 MPa, respectively, with a difference of 30 MPa and a difference rate of 2.56%; the transverse and longitudinal elongation were 21.6% and 23.0%, respectively, with a difference of 1.4 percentage points and a difference rate of 6.28%; the transverse and longitudinal tensile strengths at 1000℃ were 406 MPa and 391 MPa, respectively, with a difference of 15 MPa and a difference rate of 3.76%; the transverse and longitudinal elongation were 5.4% and 4.9%, respectively, with a difference of 0.5 percentage points and a difference rate of 9.71%.
[0078] (2) T3=1140℃ / T4=900℃ (upper limit combination): First stage aging at 1140℃ for 4 hours, cooling to 900℃ at 3℃ / min and holding for 15 hours, followed by air cooling. The microstructure of the treated sample was found to be completely equiaxed and without cracks. The transverse and longitudinal tensile strengths at room temperature were 1178 MPa and 1148 MPa, respectively, with a difference of 30 MPa and a difference rate of 2.58%; the transverse and longitudinal elongation were 22.1% and 23.5%, respectively, with a difference of 1.4 percentage points and a difference rate of 6.14%; the transverse and longitudinal tensile strengths at 1000℃ were 404 MPa and 389 MPa, respectively, with a difference of 15 MPa and a difference rate of 3.78%; the transverse and longitudinal elongation were 5.8% and 5.3%, respectively, with a difference of 0.5 percentage points and a difference rate of 9.01%.
[0079] (3) T3=1080℃ / T4=820℃ (intermediate combination): First-stage aging at 1080℃ for 4 hours, followed by cooling to 820℃ at 3℃ / min and holding for 15 hours, then air cooling. The microstructure of the treated sample was found to be completely equiaxed and without cracks. The transverse and longitudinal tensile strengths at room temperature were 1198 MPa and 1168 MPa, respectively, with a difference of 30 MPa and a difference rate of 2.54%; the transverse and longitudinal elongation were 21.2% and 22.6%, respectively, with a difference of 1.4 percentage points and a difference rate of 6.39%; the transverse and longitudinal tensile strengths at 1000℃ were 414 MPa and 398 MPa, respectively, with a difference of 16 MPa and a difference rate of 3.94%; the transverse and longitudinal elongation were 5.6% and 5.1%, respectively, with a difference of 0.5 percentage points and a difference rate of 9.35%.
[0080] The above results show that all three groups of samples meet the performance indicators of tensile strength ≥1100MPa and elongation ≥15% at room temperature. Meanwhile, the differences in transverse and longitudinal tensile strength at room temperature were 2.56%, 2.58%, and 2.54%, respectively, all less than 5%, and the differences in transverse and longitudinal elongation were 6.28%, 6.14%, and 6.39%, respectively, all less than 10%. At 1000℃, the differences in transverse and longitudinal tensile strength were 3.76%, 3.78%, and 3.94%, respectively, all less than 5%, and the differences in transverse and longitudinal elongation were 9.71%, 9.01%, and 9.35%, respectively, all less than 10%. This indicates that the aging temperature ranges T3=1050~1140℃ and T4=800~900℃ defined in this invention have good boundary effectiveness.
[0081] In one embodiment, the present invention also provides a heat treatment control system for additive manufacturing of γ′ phase-strengthened high-temperature-resistant alloys, including a temperature control module and a cooling rate control module. The temperature control module controls the heat treatment furnace to operate according to a preset temperature-time curve; the cooling rate control module controls the cooling rate of the alloy sample during the heat treatment process.
[0082] Specifically, the preset temperature-time curve includes at least the following control segments executed sequentially: In the first solution treatment stage, the alloy sample is heated to the first solution temperature and held at that temperature. The first solution temperature is higher than the liquefaction initiation temperature of the low melting point region of the alloy grain boundary. In the first controllable slow cooling section, the material is cooled to the second solid solution temperature at a first set cooling rate. The second solid solution temperature is lower than the liquefaction initiation temperature of the low melting point region of the alloy grain boundary and higher than the precipitation initiation temperature of the γ′ strengthening phase in the alloy sample. The second solution treatment stage involves holding the sample at the second solution temperature; the rapid cooling stage involves cooling the alloy sample held at the second solution temperature to room temperature to obtain a solution-treated sample. In the first aging treatment stage, the alloy sample is heated to the first-stage aging temperature and held at that temperature. A controllable transition section continuously cools the temperature from the first aging temperature to the second aging temperature at a second set cooling rate. In the second aging treatment stage, the temperature is maintained at the second-stage aging temperature, and then cooled to room temperature.
[0083] The control system can be directly integrated into the control cabinet of an existing vacuum heat treatment furnace or atmosphere-protected heat treatment furnace without requiring structural modifications to the furnace body.
[0084] The present invention provides a crack-free equiaxed grain heat treatment method for additive manufacturing of γ′ phase-strengthened high-temperature-resistant alloys, and components produced by this method. This method can be widely applied to the post-processing of hot-end components in the aerospace field, and is particularly suitable for the heat treatment of complex components such as γ′ phase-strengthened high-temperature alloy turbine blades, combustion chamber liners, and guide vanes formed by laser powder bed melting or electron beam powder bed melting. This method is simple to operate, highly compatible with existing heat treatment equipment, requires no additional special equipment, and can be directly implemented in conventional vacuum heat treatment furnaces or atmosphere-protected heat treatment furnaces, possessing extremely high industrial practical value and promising prospects for widespread application.
[0085] In specific industrial applications, it is necessary to ensure good contact between the thermocouple and the sample surface during furnace loading. Samples of different thicknesses should maintain a uniform spacing (e.g., ≥20mm) within the furnace to ensure atmosphere flow and temperature uniformity. This method is applicable to additive manufacturing alloy components with an effective cross-sectional thickness of 5~100mm. For components exceeding this range, appropriate adjustments can be made by referring to the general formula for calculating the holding time disclosed in this invention. The total heat treatment cycle of this invention (including solution treatment, slow cooling, and aging) is approximately 12~36 hours depending on the cooling rate and temperature range. Compared with the existing single-stage solution treatment + aging process, it only adds a limited time (2~8 hours) to the controllable slow cooling section, but achieves significant gains in crack-free equiaxed grain structure and high comprehensive mechanical properties, demonstrating good economic efficiency.
[0086] Obviously, those skilled in the art should understand that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Various modifications and variations of the embodiments of the present invention are possible for those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A crack-free equiaxed heat treatment method for additive manufacturing of γ′ phase-strengthened high-temperature-resistant alloys, characterized in that, include: The additively formed γ′ phase reinforced high heat-resistant alloy sample is heated to the first solid solution temperature and held at that temperature to allow the alloy sample to undergo complete recrystallization, transforming the columnar crystals formed by additive manufacturing into equiaxed crystals, thus obtaining the first solid solution sample. The first solid solution sample is slowly cooled from the first solid solution temperature to the second solid solution temperature at a first set cooling rate to obtain a slowly cooled sample. The slowly cooled sample is kept at the second solid solution temperature to obtain the second solid solution sample; The second solid solution sample was cooled to room temperature to obtain a solid solution sample; The solid solution sample was subjected to aging treatment to obtain a heat-treated alloy.
2. The heat treatment method according to claim 1, characterized in that, The first solution temperature satisfies the following relationship: T1 = T EL +ΔT; where T1 is the first solution temperature, T EL The liquefaction initiation temperature is the low-melting-point region of the alloy grain boundary in the alloy sample, and ΔT is the incremental temperature, ranging from 10 to 50℃.
3. The heat treatment method according to claim 1, characterized in that, The second solution temperature satisfies: T2 < T EL And T2≥T pre Where T2 is the second solution temperature, T EL T represents the liquefaction initiation temperature of the low-melting-point region at the grain boundaries of the alloy sample. pre The temperature at which the γ′ strengthening phase begins to precipitate in the alloy sample is denoted as γ′.
4. The heat treatment method according to claim 3, characterized in that, The liquefaction initiation temperature of the low melting point region of the alloy grain boundary is the endothermic peak initiation temperature determined by differential thermal analysis or differential scanning calorimetry, and the precipitation initiation temperature is the critical temperature at which the γ′ strengthening phase begins to precipitate, determined by differential thermal analysis or differential scanning calorimetry.
5. The heat treatment method according to claim 1, characterized in that, The first set cooling rate is 0.1~5℃ / min.
6. The heat treatment method according to claim 1, characterized in that, The heat-treated alloy is obtained by aging the solution-treated sample, comprising: The solid solution sample is heated to the first aging temperature and held at that temperature to obtain the first aging sample. The first aged sample is continuously cooled to the second aging temperature at a second set cooling rate and held at that temperature to obtain the second aged sample. The second aged sample was cooled to room temperature to obtain the heat-treated alloy.
7. The heat treatment method according to claim 6, characterized in that, The first stage aging temperature is 1050℃~1140℃, the second stage aging temperature is 800℃~900℃, and the second set cooling rate is 0.5~5℃ / min.
8. The heat treatment method according to claim 1, characterized in that, The holding time t is determined based on the effective cross-sectional thickness D of the alloy sample, and satisfies: t ≥ t base +λ×D; where t base The base time constant is λ, which is the thickness coefficient, ranging from 0.02 to 0.2 h / mm.
9. The heat treatment method according to claim 1, characterized in that, The alloy sample is any one of Ni-based superalloy, Co-based superalloy, or high-entropy alloy, wherein the Ni-based superalloy is ZGH451, M247, IN738, or René series alloy.
10. An additively manufactured γ′ phase reinforced high-temperature-resistant alloy component, characterized in that, The microstructure obtained by the heat treatment method according to any one of claims 1 to 9 is a crack-free, fully equiaxed crystal structure.
Citation Information
Patent Citations
Preparation method of high-strength and high-plasticity additive manufacturing nickel-based superalloy
CN119525521A
Method for regulating and controlling strengthening phase of nickel-based superalloy based on over-solid solution
CN119530687A